Method and system for preparing sulfuric acid and calcium carbonate from gypsum solid waste at low temperature

The method for preparing sulfuric acid and calcium carbonate at low temperatures solves the problems of high energy consumption and low resource utilization in gypsum solid waste treatment, and realizes the high-value conversion and near-zero emission of sulfur and calcium resources, which is suitable for industrial application.

CN123128307APending Publication Date: 2026-11-20JINAN LINYUAN RESOURCE RECYCLING TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611481400.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing gypsum solid waste treatment technologies suffer from high energy consumption, large investment, and stringent requirements for raw material quality. They also make it difficult to achieve the low-temperature conversion of sulfur and calcium resources into high-value-added products. Furthermore, the added value of gypsum solid waste in building materials is low, its disposal capacity is limited, and it poses environmental risks.

Method used

A low-temperature method for preparing sulfuric acid and calcium carbonate involves generating calcium carbonate precipitate and ammonium sulfate solution through a metathesis reaction, followed by two-stage thermal decomposition of ferrous ammonium sulfate to produce ammonia, sulfur dioxide, and ferric sulfate. This method achieves high-value conversion of sulfur and calcium resources and constructs a closed-loop cycle for ammonia and iron components.

Benefits of technology

Significantly reduce energy consumption and equipment investment, realize the conversion of sulfur resources into high-value-added sulfuric acid products, and calcium resources into high-purity calcium carbonate. The products can be directly used as inorganic fillers, achieving near-zero emissions and efficient resource utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128307A_ABST
    Figure CN123128307A_ABST
Patent Text Reader

Abstract

This application provides a method and system for preparing sulfuric acid and calcium carbonate from gypsum solid waste at low temperature. The method uses gypsum solid waste, whose main component is calcium sulfate dihydrate, as raw material. After slurrying with water, it undergoes metathesis with ammonium carbonate at 40-50℃ and normal pressure to generate calcium carbonate and ammonium sulfate solutions. Calcium carbonate is obtained by pressure filtration. Ferrous sulfate is added to the ammonium sulfate filtrate to generate ferrous ammonium sulfate precipitate. This ferrous ammonium sulfate precipitate undergoes two-stage thermal decomposition at 150-200℃ and 450-550℃ to obtain ammonia, sulfur dioxide, and ferric sulfate. Sulfur dioxide is purified, catalytically oxidized, and absorbed to produce sulfuric acid. Ammonia and carbon dioxide are absorbed to regenerate ammonium carbonate, and ferric sulfate is reduced with iron powder to regenerate ferrous sulfate, achieving a closed-loop cycle of ammonia and iron components. Simultaneously, it achieves high-value conversion of both sulfur and calcium resources. The method provided in this application has mild reaction conditions, low energy consumption, and achieves waste-to-waste treatment, high-value conversion of sulfur and calcium resources, and near-zero emissions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of industrial solid waste resource utilization technology, and relates to a method and system for preparing sulfuric acid and calcium carbonate from gypsum solid waste at low temperature. Background Technology

[0002] Gypsum solid waste is a type of industrial solid waste with calcium sulfate dihydrate as its main component. It mainly includes phosphogypsum, a byproduct of wet-process phosphoric acid production; desulfurization gypsum, a byproduct of calcium-based flue gas desulfurization; fluorogypsum, a byproduct of hydrofluoric acid production; titanium gypsum, a byproduct of titanium dioxide production; and salt gypsum, a byproduct of salt chemical industry. my country is a major producer of gypsum solid waste, and a large amount of it is disposed of through stockpiling, occupying land resources and posing environmental risks of dust and leaching pollution. With increasingly stringent environmental protection requirements, the large-scale, high-value disposal of gypsum solid waste has become a prominent issue facing industries such as phosphate chemicals, power generation, and titanium dioxide production.

[0003] Currently, the utilization of gypsum solid waste is mainly concentrated in the building materials sector: after purification, dehydration, and calcination, gypsum solid waste is used to produce gypsum board, gypsum blocks, plaster, and other gypsum building materials; it is also used as a cement retarder in cement production. However, the above utilization methods are basically limited to the low-value transformation of waste into materials, and the sulfur and calcium resources in gypsum solid waste have not been converted into high-value products. Regarding the recovery of sulfur resources from gypsum solid waste, existing technologies mainly employ a high-temperature reduction pyrolysis route, namely the process of producing sulfuric acid from phosphogypsum and co-producing cement. However, while the above-mentioned process achieves the recovery of sulfur resources, it has the following shortcomings: First, the decomposition temperature is as high as 1100℃ or above, resulting in high energy consumption, large equipment investment, and high operating costs; Second, it has strict requirements on the content of impurities such as phosphorus and fluorine in the raw materials. Excessive phosphorus and fluorine content will inhibit the formation of cement clinker minerals and aggravate ring formation and equipment corrosion in rotary kilns, resulting in poor raw material adaptability; Third, the concentration of sulfur dioxide in the furnace gas is low and fluctuates greatly, requiring a large-scale purification and conversion device, and the process flow is long; Fourth, the calcium in the kiln slag exists in the form of cement minerals such as calcium silicate, and the calcium resources are fixed in low-value cement clinker, making it impossible to obtain high-value-added calcium-based fine chemicals, and failing to achieve full resource utilization.

[0004] Therefore, existing technologies for the resource utilization of gypsum solid waste share the following common bottlenecks: First, the added value of building material utilization is low, the disposal capacity is limited, and stockpiling and disposal occupy land and pose environmental risks; Second, the high-temperature acid production route has high energy consumption, large investment, and stringent requirements for raw material quality, making it difficult to match with low-quality gypsum solid waste containing impurities; Third, there is a lack of systematic technical solutions that can convert sulfur and calcium resources in gypsum solid waste into sulfuric acid and high-value-added calcium carbonate products at low temperatures, and achieve closed-loop recycling and near-zero emissions of ammonia and iron auxiliary components. Summary of the Invention

[0005] The purpose of this invention is to provide a method and system for preparing sulfuric acid and calcium carbonate from gypsum solid waste at low temperature, so as to solve the problem that existing gypsum solid waste treatment cannot achieve the complete recovery of sulfur and calcium resources.

[0006] To achieve the above objectives, the present invention adopts the following technical solution: In a first aspect, this application provides a method for preparing sulfuric acid and calcium carbonate from gypsum solid waste at low temperature, the method comprising: After impurities are removed, gypsum solid waste is slurried with water to form gypsum slurry. The gypsum slurry undergoes a metathesis reaction with ammonium carbonate to generate calcium carbonate precipitate and ammonium sulfate solution. The ammonium sulfate solution reacts with ferrous sulfate to produce ferrous ammonium sulfate precipitate and filtrate; The ferrous ammonium sulfate precipitate undergoes a two-stage thermal decomposition to yield ammonia, sulfur dioxide, and ferric sulfate. The sulfur dioxide reacts with oxygen to produce sulfur trioxide, which is then absorbed by concentrated sulfuric acid to obtain a sulfuric acid solution. The ammonia and carbon dioxide react with the filtrate, and the resulting ammonium carbonate is reused to react with the gypsum slurry. The ferric sulfate reacts with iron, and the resulting ferrous sulfate is reused to react with the ammonium sulfate solution.

[0007] Secondly, this application provides a system for preparing sulfuric acid and calcium carbonate from gypsum solid waste at low temperature, including a metathesis reaction unit, an ammonium sulfate reaction unit, a thermal decomposition unit, and a regeneration and recycling unit connected in series.

[0008] The present invention has the following beneficial effects: (1) Low energy consumption: This application converts calcium sulfate, which is difficult to decompose thermally, into ferrous ammonium sulfate, which is easily decomposed thermally, through a double decomposition reaction at 40-50℃ and normal pressure. The sulfur element is released through a two-stage thermal decomposition of ferrous ammonium sulfate at 150-200℃ and 450-550℃, which greatly reduces the high-temperature reduction thermal decomposition temperature of traditional gypsum above 1100℃. Compared with the process of producing sulfuric acid and cement from phosphogypsum with a calcination temperature of 1100-1450℃, the maximum operating temperature of this application is reduced by about 600℃, which greatly reduces energy consumption and equipment investment, and avoids the risk of secondary pollution from sulfur dioxide tail gas in the high-temperature process.

[0009] (2) High-value conversion of sulfur and calcium resources: This application converts sulfate in gypsum solid waste into ammonium sulfate through metathesis, and then releases sulfur in the form of sulfur dioxide through two-stage thermal decomposition of ferrous ammonium sulfate, thus realizing the chemical-grade high-value recovery of sulfur resources; at the same time, calcium in gypsum solid waste is directly converted into calcium carbonate products through metathesis, which has a significantly higher added value than the gypsum building material utilization route. The product has high purity and high whiteness and can be directly used as inorganic filler and other applications.

[0010] (3) Using waste to treat waste and turn waste into treasure: This application uses gypsum solid waste, which is difficult to dispose of at high value, as raw material and converts it into sulfuric acid and calcium carbonate, two high value-added products, under mild conditions. This fundamentally solves the problems of gypsum solid waste storage, land occupation, environmental risks and low-value disposal.

[0011] (4) Closed-loop circulation and near-zero discharge of ammonia and iron components: In this application, the ammonia gas released by the decomposition of ferrous ammonium sulfate is absorbed and carbon dioxide is used to regenerate ammonium carbonate and return it to the metathesis process. The generated ferrous sulfate is reduced by iron powder to regenerate ferrous sulfate and return it to the precipitation process, thus constructing a closed-loop circulation of ammonia and iron components. There is no process waste liquid discharged throughout the process, realizing the resource utilization of near-zero discharge.

[0012] (5) Mild conditions, continuous operation, and easy industrialization: All reaction processes in this application are carried out under mild conditions and conventional chemical equipment. The raw materials are fed quantitatively through buffer silos, sieves and belt conveyors, which is suitable for continuous production and easy to scale up and promote industrial application. Attached Figure Description

[0013] Figure 1 This is a schematic diagram of the system for preparing sulfuric acid and calcium carbonate from gypsum solid waste using a low-temperature method, as provided in the embodiments of this application. Symbolic representation: 1-Double decomposition reactor, 2-Calcium carbonate filter press, 3-Ammonium sulfate liquid tank, 4-Ammonium sulfate transfer pump, 5-Ammonium sulfate reactor, 6-Precipitation filter press, 7-Filtrate tank, 8-Filtrate transfer pump, 9-Rotary kiln, 10-Elevator, 11-Ferrous sulfate silo, 12-Ferrous sulfate regeneration reactor, 13-Ammonium carbonate regeneration reactor, 14-Screw feeder. Detailed Implementation

[0014] This application provides a method for preparing sulfuric acid and calcium carbonate from gypsum solid waste at low temperature, the method comprising: S01: The gypsum solid waste after impurity removal is slurried with water to form gypsum slurry. The gypsum slurry undergoes a metathesis reaction with ammonium carbonate to generate calcium carbonate precipitate and ammonium sulfate solution.

[0015] The temporarily stored gypsum solid waste with a calcium sulfate dihydrate content of not less than 50% by mass is added to a sieve with a sieve aperture diameter of 20 mm to remove large impurities. Then, it is fed quantitatively by a belt conveyor to ensure uniform and stable feeding, meeting the needs of continuous production. The impurity-removed gypsum solid waste is added to water to prepare a gypsum slurry with a solid content of 25-35%. In the embodiments of this application, the gypsum solid waste includes one or more of phosphogypsum, desulfurized gypsum, fluorogypsum, and titanium gypsum.

[0016] The prepared gypsum slurry and ammonium carbonate are fed into a double decomposition reactor. Under conditions of 40-50℃, atmospheric pressure, and a stirring speed of 20-40 r / min, the calcium sulfate in the gypsum slurry undergoes a double decomposition reaction with the ammonium carbonate for 0.5-1.5 hours, producing a slurry containing calcium carbonate precipitate and ammonium sulfate solution. The amount of ammonium carbonate added is 105-115% of the stoichiometric ratio of calcium sulfate dihydrate in the gypsum slurry. The core reaction equation for the double decomposition reaction is: CaSO4+(NH4)2CO3→CaCO3↓+(NH4)2SO4.

[0017] The slurry is separated by pressure filtration to obtain calcium carbonate filter cake and ammonium sulfate solution, thus achieving separation between the two. The calcium carbonate filter cake produced by separation is washed and dried multiple times to obtain calcium carbonate product with a purity ≥98% and whiteness ≥92; the ammonium sulfate solution then enters step S02.

[0018] In the embodiments of this application, in the initial stage of the metathesis reaction, the ammonium carbonate used is purchased ammonium carbonate or prepared from ammonia and carbon dioxide; when the reaction proceeds to step S05, the ammonium carbonate used in the metathesis reaction stage is the ammonium carbonate generated in step S05.

[0019] S02: The ammonium sulfate solution reacts with ferrous sulfate to produce ferrous ammonium sulfate precipitate and filtrate.

[0020] Ferrous sulfate and ammonium sulfate solution were added to an ammonium sulfate reaction vessel and reacted at 40-50℃ and pH 1-3 for 0.5-1.5 h. The reaction product was separated by pressure filtration to obtain ferrous ammonium sulfate precipitate and filtrate. The molar ratio of ferrous sulfate to ammonium sulfate in the solution was 1:0.9-1.2. The core reaction equation is as follows: (NH4)2SO4+FeSO4+6H2O→(NH4)2Fe(SO4)2·6H2O↓.

[0021] S03: The ferrous ammonium sulfate precipitate undergoes two-stage thermal decomposition to yield ammonia, sulfur dioxide, and ferric sulfate.

[0022] Ferrous ammonium sulfate precipitate is added to a rotary kiln and heated to 150-200℃. The ferrous ammonium sulfate decomposes to remove its water of crystallization, releasing ammonia gas and generating a basic ferrous sulfate intermediate. Once no more gas is produced, heating continues to 450-550℃. The basic ferrous sulfate intermediate decomposes thermally, releasing sulfur dioxide gas and generating ferric sulfate. Thus, ammonia, sulfur dioxide, and ferric sulfate are obtained through a two-stage thermal decomposition process, heating sequentially to 150-200℃ and then 450-550℃. The core reaction equation is as follows: 2(NH4)2Fe(SO4)2·6H2O→4NH3↑+SO2↑+Fe2(SO4)3+14H2O↑.

[0023] S04: The sulfur dioxide reacts with oxygen to produce sulfur trioxide, which is then absorbed by concentrated sulfuric acid to obtain a sulfuric acid solution.

[0024] The sulfur dioxide generated in step S03 is washed with water, dried with 93-98% concentrated sulfuric acid, and filtered through an acid-resistant metal filter. Then, under the action of a vanadium-based catalyst, the sulfur dioxide and oxygen react at 400-500°C to generate sulfur trioxide. This sulfur trioxide is then absorbed by concentrated sulfuric acid to prepare a sulfuric acid solution. In the embodiments of this application, the vanadium-based catalyst includes: vanadium pentoxide catalyst, S101 type low-temperature vanadium catalyst, S107 type low-temperature vanadium catalyst, S108 type low-temperature vanadium catalyst, etc.

[0025] S05: The ammonia and carbon dioxide react with the filtrate, and the resulting ammonium carbonate is reused to react with the gypsum slurry.

[0026] The ammonia and carbon dioxide generated in step S03 are mixed with the filtrate generated in step S02 at a molar ratio of 2:1. The water in the filtrate absorbs the ammonia and carbon dioxide, and the core reaction equation 2NH3+CO2+H2O→(NH4)2CO3 occurs, generating ammonium carbonate. This ammonium carbonate is recycled as a product in step S01.

[0027] S06: The ferric sulfate reacts with iron, and the resulting ferrous sulfate is reused to react with the ammonium sulfate solution.

[0028] The ferrous sulfate produced in step S03, the filtrate from step S02, and iron powder are added to the ferrous sulfate regeneration reactor, where the core reaction equation, Fe2(SO4)3 + Fe → 3FeSO4, occurs, producing ferrous sulfate. The molar ratio of ferrous sulfate to iron powder is 1:1-1.2. This ferrous sulfate is recycled as a product in step S02, and excess ferrous sulfate is sold as a byproduct. When excess ferrous sulfate is sold as a byproduct, the iron and sulfur losses are replenished by purchasing ferrous sulfate or iron powder according to the stoichiometric ratio.

[0029] In addition, this application also provides a system for the low-temperature preparation of sulfuric acid and calcium carbonate from gypsum solid waste using the above method. This system includes interconnected metathesis reaction units, ammonium sulfate reaction units, thermal decomposition units, and regeneration and recycling units, as shown in the attached figure. Figure 1 As shown.

[0030] Specifically, the metathesis reaction unit is used to react the purified and pulped gypsum solid waste with ammonium carbonate in a metathesis reaction. In this embodiment, the metathesis reaction unit includes a metathesis reaction vessel 1, a calcium carbonate filter press 2, an ammonium sulfate tank 3, and an ammonium sulfate transfer pump 4, all connected in sequence. The pulped gypsum solid waste reacts with ammonium carbonate in the metathesis reaction vessel 1, producing calcium carbonate precipitate and ammonium sulfate solution. The resulting product is passed into the calcium carbonate filter press 2 for filtration separation, yielding a calcium carbonate filter cake and an ammonium sulfate solution, thus achieving separation between the two. The ammonium sulfate solution is stored in the ammonium sulfate tank 3 and then pumped by the ammonium sulfate transfer pump 4 to the ammonium sulfate reaction vessel 5 in the ammonium sulfate reaction unit.

[0031] The ammonium sulfate reaction unit is a component that reacts ammonium sulfate produced by the metathesis reaction unit with ferrous sulfate. In this embodiment, the ammonium sulfate reaction unit includes an ammonium sulfate reactor 5, a precipitation filter press 6, a filtrate tank 7, and a filtrate transfer pump 8, all connected in sequence. Ammonium sulfate and ferrous sulfate react in the ammonium sulfate reactor 5 to produce a product consisting of ferrous ammonium sulfate precipitate and filtrate. This product is separated by filtration in the precipitation filter press 6 to obtain ferrous ammonium sulfate precipitate and filtrate. The ferrous ammonium sulfate precipitate is fed into the thermal decomposition unit, and the filtrate, after temporary storage in the filtrate tank 7, is pumped by the filtrate transfer pump 8 to the ammonium carbonate regeneration reactor 13 in the regeneration and circulation unit.

[0032] The thermal decomposition unit is a component that performs a two-stage thermal decomposition of the ferrous ammonium sulfate precipitate produced by the ammonium sulfate reaction unit. In this embodiment, the thermal decomposition unit includes a rotary kiln 9, an elevator 10, and a ferrous sulfate silo 11 connected in sequence. The ferrous ammonium sulfate precipitate is first heated to 150-200°C in the rotary kiln 9, where it loses its water of crystallization and decomposes to release ammonia gas, generating a basic ferrous sulfate intermediate. The generated ammonia gas is discharged into the ammonium carbonate regeneration reactor 13 of the regeneration circulation unit. When no more gas is generated, the rotary kiln 9 continues to heat to 450-550°C, where the basic ferrous sulfate intermediate decomposes, releasing sulfur dioxide gas and generating ferric sulfate. The released sulfur dioxide gas is washed with water, dried with 93-98% concentrated sulfuric acid, and filtered through an acid-resistant metal filter. Under the action of a vanadium-based catalyst, sulfur dioxide and oxygen react at 400-500°C to generate sulfur trioxide. This sulfur trioxide is absorbed by concentrated sulfuric acid to prepare a sulfuric acid solution. Ferric sulfate is lifted by elevator 10 to ferric sulfate silo 11 for temporary storage.

[0033] The regeneration and recycling unit is a component for regenerating and recycling ammonia and ferric sulfate produced by the pyrolysis unit. In the embodiments of this application, the regeneration and recycling unit includes a ferrous sulfate regeneration reactor 12 and an ammonium carbonate regeneration reactor 13. The ferrous sulfate regeneration reactor 12 is connected to the ferric sulfate silo 11, the filtrate transfer pump 8, and the ammonium sulfate reactor 5, respectively. The ammonium carbonate regeneration reactor 13 is connected to the rotary kiln 9, the filtrate transfer pump 8, and the metathesis reactor 1, respectively.

[0034] In this process, ammonia gas generated by the thermal decomposition unit, filtrate generated by the ammonium sulfate reaction unit, and carbon dioxide react in the ammonium carbonate regeneration reactor 13 to produce ammonium carbonate. This ammonium carbonate is then pumped to the metathesis reactor 1 of the metathesis reaction unit to participate in the metathesis reaction of the slurryed gypsum solid waste.

[0035] Ferrous sulfate temporarily stored in ferric sulfate silo 11 is conveyed to ferrous sulfate regeneration reactor 12 via screw feeder 14. There, it reacts with iron powder and the filtrate from step S02 to generate ferrous sulfate. This ferrous sulfate is recycled as a product and used in the ammonium sulfate reactor 5 of the ammonium sulfate reaction unit. Excess ferrous sulfate is sold as a byproduct.

[0036] The technical solution of the present invention will be further explained and described below through specific embodiments.

[0037] Example 1 This application provides a method for preparing sulfuric acid and calcium carbonate from gypsum solid waste at low temperature. The method uses phosphogypsum solid waste, a byproduct of wet-process phosphoric acid production in a phosphate chemical enterprise, as the gypsum solid waste. The phosphogypsum solid waste (dry basis) contains 78% calcium sulfate dihydrate by mass, 22% impurities such as phosphorus, fluorine, and acid-insoluble matter, and has a moisture content of approximately 12%. The method includes: S101: Phosphogypsum solid waste is added to a sieve with a sieve aperture diameter of 20 mm to remove large impurities. Then, it is quantitatively added to water via a belt conveyor to prepare a gypsum slurry with a solid content of 30%. The prepared gypsum slurry and ammonium carbonate are fed into a double decomposition reactor 1. Under conditions of 45℃, atmospheric pressure, and a stirring speed of 30 r / min, the calcium sulfate in the gypsum slurry undergoes a double decomposition reaction with ammonium carbonate for 1 hour, generating a slurry containing calcium carbonate precipitate and ammonium sulfate solution. The amount of ammonium carbonate added is 110% of the stoichiometric ratio of calcium sulfate dihydrate in the gypsum slurry. This slurry is then filtered by a calcium carbonate filter press 2 at a pressure of 0.4 MPa to obtain a calcium carbonate filter cake and an ammonium sulfate solution.

[0038] S102: According to the molar ratio of ferrous sulfate to ammonium sulfate of 1:1.05, ferrous sulfate and ammonium sulfate solutions are added to ammonium sulfate reaction vessel 5 and reacted for 1 hour at a temperature of 45℃ and a pH of 2. The reaction products are separated by filtration using a precipitation filter press 6 to obtain ferrous ammonium sulfate precipitate and filtrate.

[0039] S103: Ferrous ammonium sulfate precipitate is added to rotary kiln 9 and heated to 160°C. Ferrous ammonium sulfate removes water of crystallization and decomposes to release ammonia gas, generating basic ferrous sulfate intermediate. When no gas is generated, the temperature is further increased to 500°C. The basic ferrous sulfate intermediate decomposes under heat, releasing sulfur dioxide gas and generating ferric sulfate.

[0040] S104: After sulfur dioxide gas is washed with water, dried with 93-98% concentrated sulfuric acid, and filtered through an acid-resistant metal filter, sulfur dioxide and oxygen react at 430°C under the action of vanadium pentoxide catalyst to produce sulfur trioxide. The sulfur trioxide is then absorbed by concentrated sulfuric acid to prepare a sulfuric acid solution.

[0041] S105: Ammonia, carbon dioxide and the filtrate produced in step S02 are added to the ammonium carbonate regeneration reactor 13 according to the molar ratio of ammonia to carbon dioxide of 2:1. The water in the filtrate absorbs ammonia and carbon dioxide to generate ammonium carbonate, which is recycled as a product in step S01.

[0042] S106: Ferric sulfate, iron powder, and the filtrate from step S02 are added to the ferrous sulfate regeneration reactor 12 at a molar ratio of ferrous sulfate to iron powder of 1:1.1 to react and generate ferrous sulfate. This ferrous sulfate is recycled as a regenerated product and used in step S02; excess ferrous sulfate is sold as a byproduct.

[0043] Example 2 This application provides a method for preparing sulfuric acid and calcium carbonate from gypsum solid waste at low temperature. The method uses desulfurized gypsum, a byproduct of calcium-based desulfurization in a power plant, as the gypsum solid waste. The desulfurized gypsum (dry basis) contains 90% calcium sulfate dihydrate and 10% impurities. The phosphogypsum solid waste has a moisture content of approximately 12%. The method includes: S201: Desulfurized gypsum is added to a sieve with a sieve diameter of 20 mm to remove large impurities. Then, it is quantitatively added to water via a belt conveyor to prepare a gypsum slurry with a solid content of 25%. The prepared gypsum slurry and ammonium carbonate are fed into a double decomposition reactor 1. Under conditions of 48℃, atmospheric pressure, and a stirring speed of 35 r / min, the calcium sulfate in the gypsum slurry undergoes a double decomposition reaction with ammonium carbonate for 1.5 h, generating a slurry containing calcium carbonate precipitate and ammonium sulfate solution. The amount of ammonium carbonate added is 115% of the stoichiometric ratio of calcium sulfate dihydrate in the gypsum slurry. This slurry is then filtered by a calcium carbonate filter press 2 at a pressure of 0.4 MPa to obtain a calcium carbonate filter cake and an ammonium sulfate solution.

[0044] S202: According to the molar ratio of ferrous sulfate to ammonium sulfate of 1:0.9, ferrous sulfate and ammonium sulfate solutions are added to ammonium sulfate reaction vessel 5 and reacted at a temperature of 48℃ and a pH of 1 for 1.5h. The reaction products are separated by filtration using a precipitation filter press 6 to obtain ferrous ammonium sulfate precipitate and filtrate.

[0045] S203: Ferrous ammonium sulfate precipitate is added to rotary kiln 9 and heated to 180°C. Ferrous ammonium sulfate removes water of crystallization and decomposes to release ammonia gas and generate basic ferrous sulfate intermediate. When no gas is generated, the temperature is further increased to 520°C. The basic ferrous sulfate intermediate decomposes under heat, releasing sulfur dioxide gas and generating ferric sulfate.

[0046] S204: After sulfur dioxide gas is washed with water, dried with 93-98% concentrated sulfuric acid, and filtered through an acid-resistant metal filter, sulfur dioxide and oxygen react at 450°C under the action of S101 type low-temperature vanadium catalyst to generate sulfur trioxide. This sulfur trioxide is then absorbed by concentrated sulfuric acid to prepare a sulfuric acid solution.

[0047] S205: Ammonia, carbon dioxide and the filtrate produced in step S02 are added to the ammonium carbonate regeneration reactor 13 according to the molar ratio of ammonia to carbon dioxide of 2:1. The water in the filtrate absorbs ammonia and carbon dioxide to generate ammonium carbonate, which is recycled as a product in step S01.

[0048] S206: Ferric sulfate, iron powder, and the filtrate from step S02 are added to the ferrous sulfate regeneration reactor 12 at a molar ratio of ferrous sulfate to iron powder of 1:1, and react to generate ferrous sulfate. This ferrous sulfate is recycled as a regenerated product and used in step S02; excess ferrous sulfate is sold as a byproduct.

[0049] Example 3 This application provides a method for preparing sulfuric acid and calcium carbonate from gypsum solid waste at low temperature. The method uses titanium gypsum, a byproduct of a titanium dioxide plant, as the gypsum solid waste. The titanium gypsum (dry basis) contains 55% calcium sulfate dihydrate and 45% impurities such as iron, titanium, and acid-insoluble substances. The phosphogypsum solid waste has a moisture content of approximately 10%. The method includes: S301: Titanium gypsum is added to a sieve with a sieve diameter of 20 mm to remove large impurities. Then, it is quantitatively added to water via a belt conveyor to prepare a gypsum slurry with a solid content of 35%. The prepared gypsum slurry and ammonium carbonate are fed into a double decomposition reactor 1. Under conditions of 42℃, atmospheric pressure, and a stirring speed of 25 r / min, the calcium sulfate in the gypsum slurry undergoes a double decomposition reaction with ammonium carbonate for 1.5 h, generating a slurry containing calcium carbonate precipitate and ammonium sulfate solution. The amount of ammonium carbonate added is 105% of the stoichiometric ratio of calcium sulfate dihydrate in the gypsum slurry. This slurry is then filtered by a calcium carbonate filter press 2 at a pressure of 0.4 MPa to obtain a calcium carbonate filter cake and an ammonium sulfate solution.

[0050] S302: According to the molar ratio of ferrous sulfate to ammonium sulfate of 1:1.2, ferrous sulfate and ammonium sulfate solutions are added to ammonium sulfate reaction vessel 5 and reacted at a temperature of 42℃ and a pH of 3 for 0.5h. The reaction products are separated by filtration using a precipitation filter press 6 to obtain ferrous ammonium sulfate precipitate and filtrate.

[0051] S303: Ferrous ammonium sulfate precipitate is added to rotary kiln 9 and heated to 150°C. Ferrous ammonium sulfate removes water of crystallization and decomposes to release ammonia gas, generating basic ferrous sulfate intermediate. When no gas is generated, the temperature is further increased to 450°C. The basic ferrous sulfate intermediate decomposes under heat, releasing sulfur dioxide gas and generating ferric sulfate.

[0052] S304: After sulfur dioxide gas is washed with water, dried with 93-98% concentrated sulfuric acid, and filtered through an acid-resistant metal filter, sulfur dioxide and oxygen react at 400°C under the action of S107 type low-temperature vanadium catalyst to generate sulfur trioxide. The sulfur trioxide is then absorbed by concentrated sulfuric acid to prepare a sulfuric acid solution.

[0053] S305: Ammonia, carbon dioxide and the filtrate produced in step S02 are added to the ammonium carbonate regeneration reactor 13 according to the molar ratio of ammonia to carbon dioxide of 2:1. The water in the filtrate absorbs ammonia and carbon dioxide to generate ammonium carbonate, which is then recycled as a product in step S01.

[0054] S306: Ferric sulfate, iron powder, and the filtrate from step S02 are added to the ferrous sulfate regeneration reactor 12 at a molar ratio of ferrous sulfate to iron powder of 1:1.2, and react to generate ferrous sulfate. This ferrous sulfate is recycled as a regenerated product and used in step S02; excess ferrous sulfate is sold as a byproduct.

[0055] Comparative Example 1 This application provides a comparative example of a method for treating gypsum solid waste, wherein the gypsum solid waste in this method is the same as that in Example 1, and the method includes: Phosphogypsum solid waste is added to a sieve with a 20mm aperture to remove large impurities. Then, it is quantitatively added to water via a belt conveyor to produce a gypsum slurry with a solid content of 30%. The prepared gypsum slurry is dehydrated to a moisture content of ≤12%, and then further dehydrated at 165-175℃ to produce β-hemihydrate gypsum. This β-hemihydrate gypsum is used in the production of cement retarders or gypsum building materials.

[0056] Comparative Example 2 This application provides a comparative example of a method for treating gypsum solid waste, wherein the gypsum solid waste in this method is the same as that in Example 1, and the method includes: Phosphogypsum is mixed with coke, clay, and sand in a specific mass ratio and then calcined in a rotary kiln at 1150-1350℃ to produce sulfur dioxide furnace gas and kiln slag. The sulfur dioxide furnace gas is purified to produce acid, and the kiln slag is cooled and ground to produce cement clinker.

[0057] Based on 1 ton of dry gypsum solid waste, the yield, purity, and other data of sulfuric acid, calcium carbonate, and ferrous sulfate prepared in Examples 1-3 of this application are statistically analyzed and obtained in Table 1.

[0058] Table 1: Data on yield, purity, etc. As shown in Table 1, the method provided in this application can prepare sulfuric acid with a mass fraction ≥98% and a purity ≥98.5%, calcium carbonate with a whiteness ≥92 and a purity ≥98.6%, and ferrous sulfate byproduct. Taking 1 ton of dry-based gypsum solid waste as an example, when the mass fraction of dihydrate calcium sulfate in the gypsum solid waste increases from 55% to 90%, the sulfuric acid yield increases from 0.14t to 0.23t, the calcium carbonate yield increases from 0.30t to 0.50t, and the ferrous sulfate yield increases from 0.44t to 0.73t. That is, the product yield increases synchronously with the increase in the dihydrate calcium sulfate content in the raw materials. The entire process involves no discharge of process waste liquid and achieves high-value conversion of sulfur under low-temperature conditions, while simultaneously realizing the high-value resource utilization of gypsum solid waste.

[0059] In addition, the titanium gypsum used in Example 3 is a gypsum solid waste with high impurity content. However, after being treated by the method provided in this application, its sulfuric acid mass fraction can still reach 98% and its calcium carbonate purity can reach 98.6%. This shows that the method provided in this application has good adaptability to low-grade gypsum solid waste such as titanium gypsum with low calcium sulfate dihydrate content.

[0060] In Comparative Example 1, phosphogypsum's high content of phosphorus, fluorine, and acid-insoluble impurities limits its compatibility in building materials, resulting in low added value as a cement retarder. When used as a gypsum building material, the market's capacity to absorb it is limited, requiring large quantities of phosphogypsum to be stockpiled and disposed of. Furthermore, the sulfur and calcium resources in the gypsum do not undergo high-value chemical conversion, and no sulfuric acid or calcium carbonate products are produced throughout the process. In contrast, the method provided in this application can convert the sulfur and calcium elements in phosphogypsum into sulfuric acid and calcium carbonate, respectively, resulting in significant economic and environmental benefits.

[0061] The treatment method provided in Comparative Example 2 requires a decomposition temperature of over 1150°C. For treating the same volume and composition of phosphogypsum solid waste, the energy consumption of the method in Comparative Example 2 is more than three times that of the method in Example 1 of this application. Furthermore, the high-temperature decomposition treatment method in Comparative Example 2 is sensitive to the phosphorus and fluorine impurities in the raw materials, has a high risk of ring formation and corrosion in the rotary kiln, and requires significant investment. The calcium in the kiln slag exists in the form of cement minerals such as calcium silicate, making it impossible to directly obtain high-purity calcium carbonate. In contrast, the method provided in Example 1 of this application involves metathesis reactions and other reactions at 40-50°C, with only a portion of the rotary kiln requiring medium-temperature operation at 450-550°C. This significantly reduces energy consumption and investment, and directly co-produces high-purity calcium carbonate.

[0062] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A method for preparing sulfuric acid and calcium carbonate from gypsum solid waste at low temperature, characterized in that, include: After impurities are removed, gypsum solid waste is slurried with water to form gypsum slurry. The gypsum slurry undergoes a metathesis reaction with ammonium carbonate to generate calcium carbonate precipitate and ammonium sulfate solution. The ammonium sulfate solution reacts with ferrous sulfate to produce ferrous ammonium sulfate precipitate and filtrate; The ferrous ammonium sulfate precipitate undergoes a two-stage thermal decomposition to yield ammonia, sulfur dioxide, and ferric sulfate. The sulfur dioxide reacts with oxygen to produce sulfur trioxide, which is then absorbed by concentrated sulfuric acid to obtain a sulfuric acid solution. The ammonia and carbon dioxide react with the filtrate, and the resulting ammonium carbonate is reused to react with the gypsum slurry. The ferric sulfate reacts with iron, and the resulting ferrous sulfate is reused to react with the ammonium sulfate solution.

2. The method for preparing sulfuric acid and calcium carbonate from gypsum solid waste at low temperature according to claim 1, characterized in that, The metathesis reaction is carried out at a temperature of 40-50℃, a pressure of atmospheric pressure, a stirring speed of 20-40 r / min, and a reaction time of 0.5-1.5 h.

3. The method for preparing sulfuric acid and calcium carbonate from gypsum solid waste at low temperature according to claim 1, characterized in that, The reaction temperature of the ammonium sulfate solution with ferrous sulfate is 40-50℃, the pH value is 1-3, and the reaction time is 0.5-1.5h.

4. The method for preparing sulfuric acid and calcium carbonate from gypsum solid waste at low temperature according to claim 1, characterized in that, The temperatures for the two-stage thermal decomposition are 150-200℃ and 450-550℃, respectively.

5. The method for preparing sulfuric acid and calcium carbonate from gypsum solid waste at low temperature according to claim 1, characterized in that, The amount of ammonium carbonate added is 105-115% of the stoichiometric ratio of calcium sulfate dihydrate in the gypsum slurry.

6. The method for preparing sulfuric acid and calcium carbonate from gypsum solid waste at low temperature according to claim 1, characterized in that, The molar ratio of ferrous sulfate to ammonium sulfate in the ammonium sulfate solution is 1:0.9-1.

2.

7. The method for preparing sulfuric acid and calcium carbonate from gypsum solid waste at low temperature according to claim 1, characterized in that, Under the action of a vanadium-based catalyst, sulfur dioxide and oxygen react at 400-500℃ to produce sulfur trioxide.

8. The method for preparing sulfuric acid and calcium carbonate from gypsum solid waste at low temperature according to claim 1, characterized in that, The gypsum solid waste includes one or more of phosphogypsum, desulfurized gypsum, fluorogypsum, and titanium gypsum; the mass fraction of calcium sulfate dihydrate in the gypsum solid waste is not less than 50%.

9. A system for preparing sulfuric acid and calcium carbonate from gypsum solid waste using a low-temperature method according to any one of claims 1-8, characterized in that, It includes interconnected double decomposition reaction units, ammonium sulfate reaction units, thermal decomposition units, and regeneration cycle units.

10. The system for preparing sulfuric acid and calcium carbonate from gypsum solid waste using a low-temperature method according to claim 9, characterized in that, The metathesis reaction unit includes a metathesis reaction vessel (1), a calcium carbonate filter press (2), an ammonium sulfate tank (3), and an ammonium sulfate transfer pump (4) connected in sequence. The ammonium sulfate reaction unit includes an ammonium sulfate reactor (5), a precipitation filter press (6), a filtrate tank (7), and a filtrate transfer pump (8) connected in sequence. The pyrolysis unit includes a rotary kiln (9), an elevator (10), and a ferric sulfate silo (11) connected in sequence. The regeneration cycle unit includes a ferrous sulfate regeneration reactor (12) and an ammonium carbonate regeneration reactor (13). The ferrous sulfate regeneration reactor (12) is connected to the ferrous sulfate silo (11), the filtrate delivery pump (8), and the ammonium sulfate reactor (5), respectively. The ammonium carbonate regeneration reactor (13) is connected to the rotary kiln (9), the filtrate delivery pump (8), and the metathesis reactor (1), respectively.