A method of controlling rolling edge cracking of a dual phase steel and the resulting dual phase steel

By adopting a front-end centralized cooling and stacking cooling treatment method in the production of high-strength duplex steel, the content of alloying elements is controlled to ensure the uniformity of bainite and ferrite structures, thus solving the edge cracking problem in the cold rolling process of high-strength duplex steel and improving production efficiency and yield.

CN123128317APending Publication Date: 2026-11-20HUNAN VALIN LIANYUAN IRON & STEEL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611277758.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively control edge cracking during the cold rolling process of high-strength duplex steel, resulting in low production efficiency and low yield.

Method used

Laminar flow cooling with a front-end centralized cooling mode is adopted to avoid edge obstruction. Combined with ultra-fast cooling and stacking cooling, the chemical composition of the billet is optimized, the content of alloying elements is controlled, the uniformity of bainite and ferrite structure is ensured, and the microstructure difference caused by alloying element segregation is reduced.

Benefits of technology

It significantly reduces edge cracking during cold rolling, improves production efficiency and yield, reduces production costs, and meets the strength and formability requirements of automotive steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128317A_ABST
    Figure CN123128317A_ABST
Patent Text Reader

Abstract

The application provides a method for controlling rolling edge cracks of dual-phase steel and the obtained dual-phase steel, and comprises the following steps: providing a steel billet; heating the steel billet to 1200-1280 DEG C and keeping the temperature, then respectively performing rough rolling and finish rolling to obtain a finish rolling plate strip; cooling the finish rolling plate strip, wherein the cooling comprises ultrafast cooling and laminar cooling, the laminar cooling adopts a front concentrated cooling mode, and no edge shielding is adopted during the laminar cooling, then performing coiling treatment, the coiling temperature is 500-560 DEG C, and a hot-rolled strip steel is obtained; performing stack cooling treatment on the coiled hot-rolled strip steel to room temperature, then performing pickling and cold rolling to obtain a cold-rolled strip steel, and then performing galvanizing to obtain the dual-phase steel. The method is simple and convenient to operate, the production cost is effectively reduced while the product quality is ensured, and the method has a good industrial application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of duplex steel production technology, and in particular to a method for controlling edge cracking during duplex steel rolling and the resulting duplex steel. Background Technology

[0002] High-strength duplex steel is widely used in automobiles, home appliances, machinery, hardware and other fields due to its excellent strength and plasticity. With the transformation and upgrading of related industries and the increasing demand for green manufacturing, the application ratio of high-strength duplex steel continues to increase, and the strength grades are also constantly increasing. However, high-strength duplex steel usually contains high levels of alloying elements (such as Si, Mn, Nb, Ti, Cr, etc.). High alloy content easily leads to element segregation during solidification and hot rolling. During subsequent laminar cooling and phase transformation, the segregated regions are more prone to forming coarse martensitic (M) hard phase structures at the edges of the strip due to alloy enrichment. In traditional processes, laminar flow cooling and edge shielding measures are usually used to prevent the temperature of the strip edge from dropping too quickly. However, this actually leads to higher edge temperatures, exacerbating the difference in cooling rate between the inner and outer rings and the edge after the steel coil is coiled. This causes a large number of coarse martensite phases to be generated at the segregation points. As a result, microcracks are easily generated at the interface between the ferrite (F) and martensite (M) phases during the subsequent cold rolling process of the hot-rolled strip. After the cracks expand, they form macroscopic edge cracks. In severe cases, the length of the edge cracks can reach nearly 100mm, resulting in a large amount of rework and edge trimming losses, which seriously restricts production efficiency and yield.

[0003] In existing technologies, most methods employ edge shielding to control edge temperature drop during strip steel production, but these methods fail to fundamentally solve the problem of edge cracking during cold rolling of high-strength duplex steel. Therefore, this invention provides a method for controlling edge cracking during duplex steel rolling and the resulting duplex steel, thereby addressing the existing problems of uncontrollable edge cracking, low production efficiency, and low yield in the cold rolling of high-strength duplex steel. Summary of the Invention

[0004] The main objective of this invention is to provide a method for controlling edge cracking during the rolling of duplex steel and the resulting duplex steel, aiming to solve the technical problems of difficult edge cracking, low production efficiency, and low yield in the cold rolling of high-strength duplex steel.

[0005] To achieve the above objectives, the present invention provides a method for controlling edge cracking during the rolling of duplex steel, comprising the following steps: S1: Provide a steel billet, the chemical composition of which, by mass fraction, comprises: C 0.08~0.13%, Si 0.2~0.8%, Mn 1.8~2.2%, Als 0.025~0.060%, Nb 0.01~0.05%, Ti 0.015~0.04%, Cr 0.1~0.7%, S≤0.010%, P≤0.020%, with the balance being Fe and unavoidable impurities.

[0006] S2: The steel billet is heated to 1200~1280℃ and held at that temperature, and then roughed and finished rolled to obtain a finished strip.

[0007] S3: Cool the finished strip, including ultra-fast cooling and laminar flow cooling. The laminar flow cooling adopts a front-end centralized cooling mode, and no edge shielding is used during the laminar flow cooling process. Then, the strip is coiled at a temperature of 500~560℃ to obtain hot-rolled strip steel.

[0008] S4: The hot-rolled strip steel after coiling is subjected to a stacking cooling treatment to room temperature, followed by pickling and cold rolling to obtain cold-rolled strip steel, which is then galvanized to obtain the duplex steel.

[0009] According to an embodiment of this application, the thickness of the steel billet is 230~240mm.

[0010] The total heating time for the steel billet is 160~320 minutes.

[0011] The heating rate of the steel billet is 4.8~9.8℃ / min.

[0012] The heat preservation time is 30-70 minutes.

[0013] According to an embodiment of this application, the roughing process involves 5 to 7 passes.

[0014] The temperature of the intermediate billet at the exit of the roughing mill is 1070~1120℃.

[0015] According to an embodiment of this application, the inlet temperature of the finishing mill is 1020~1090℃.

[0016] The exit temperature of the finishing mill is 860~890℃.

[0017] According to an embodiment of this application, the microstructure of the edge of the cooled precision-rolled strip includes bainite and ferrite.

[0018] The volume fraction of bainite is 60-80%.

[0019] According to an embodiment of this application, the thickness of the hot-rolled strip is 2.0~6.0 mm.

[0020] The ultra-fast cooling rate is 60~110℃ / s.

[0021] The laminar flow cooling rate is 10~20℃ / s.

[0022] According to an embodiment of this application, the reduction rate of the cold rolling is 45-60%.

[0023] The thickness of the cold-rolled strip is 1.0~2.5mm.

[0024] According to an embodiment of this application, the stacking cooling method includes: naturally stacking the coiled hot-rolled strip steel in a steel coil warehouse and cooling it to room temperature.

[0025] During the stack cooling process, forced air blowing and / or water cooling are prohibited for accelerated cooling.

[0026] This invention provides a dual-phase steel, which is prepared using the above-described method for controlling edge cracking during rolling of dual-phase steel.

[0027] According to the embodiments of this application, the yield strength of the duplex steel is 440~500MPa, the tensile strength is 780~840MPa, and the elongation is 22~30%.

[0028] Compared with the prior art, the beneficial effects of the present invention are as follows: The aforementioned method for controlling edge cracking during dual-phase steel rolling and the resulting dual-phase steel employ a front-end centralized cooling mode without edge shielding during laminar flow cooling. This allows the finished strip to complete its main temperature drop and rapidly pass through the phase transformation zone before cooling, effectively shortening the difference in residence time between the edge and center of the finished strip in the high-temperature zone. This significantly reduces the microstructure differences between the edge and center caused by alloy element segregation and uneven cooling, thereby refining the grains and improving the ability to generate crack initiation and prevent crack propagation. Simultaneously, the coiling temperature of 500~560℃ allows the edge of the finished strip to generate a fine-grained bainite and ferrite multiphase microstructure at a relatively fast cooling rate. This multiphase microstructure has strong coordinating deformation capabilities, fundamentally improving the microstructure uniformity at the edge. The process effectively suppresses edge cracking during subsequent cold rolling, avoiding the cold rolling edge cracking problems caused by increased martensite ratio and grain coarsening due to higher edge temperatures and faster cooling rates of the inner and outer rings of the coil after coiling, which are common in traditional edge shielding processes. Furthermore, by subjecting the hot-rolled strip to stacking cooling treatment after coiling, the process promotes the full diffusion and escape of hydrogen in the steel and the uniform release of residual stress, further reducing edge crack sensitivity. Simultaneously, by optimizing the chemical composition of the billet, adding Nb and Ti microalloying elements to the C-Si-Mn-Cr system while controlling the content of impurity elements such as S and P, the resulting dual-phase steel possesses excellent comprehensive mechanical properties, combining high strength and good formability, meeting the requirements for a balance between strength and formability in automotive steel and other applications.

[0029] The method of this invention is simple and easy to operate. The edge crack repair rate of cold-rolled high-strength duplex steel can be reduced from 50% to 0%, avoiding the repair process of trimming or cutting off the length of the edge crack. This increases the production efficiency of the cold rolling mill by 20%, saves 50 yuan / ton in repair process costs, and improves the overall yield by 2.5%. The entire process is simple and efficient, requiring no additional edge trimming or complex edge heating devices. It effectively reduces production costs while ensuring product quality and has good prospects for industrial application. Attached Figure Description

[0030] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.

[0031] Figure 1 This is a photograph of the duplex steel obtained in Example 1; Figure 2 This is a photograph of the duplex steel prepared in Comparative Example 1.

[0032] The realization of the objective, functional characteristics and advantages of the present invention will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation

[0033] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0034] Furthermore, the technical solutions of the various embodiments of the present invention can be combined with each other, but only if they are based on the ability of those skilled in the art to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such combination of technical solutions does not exist and is not within the scope of protection claimed by the present invention.

[0035] To achieve the above objectives, the present invention provides a method for controlling edge cracking during the rolling of duplex steel, comprising the following steps: S1: Provide a steel billet, the chemical composition of which, by mass fraction, comprises: C 0.08~0.13%, Si 0.2~0.8%, Mn 1.8~2.2%, Als 0.025~0.060%, Nb 0.01~0.05%, Ti 0.015~0.04%, Cr 0.1~0.7%, S≤0.010%, P≤0.020%, with the balance being Fe and unavoidable impurities.

[0036] In some embodiments, the chemical composition of the steel billet, by mass fraction, includes: C 0.09~0.10%, Si 0.30~0.50%, Mn 1.98~2.10%, Als 0.035~0.040%, Nb 0.015~0.020%, Ti 0.015~0.025%, Cr 0.20~0.50%, S≤0.007%, P 0.011~0.014%, with the balance being Fe and unavoidable impurities.

[0037] S2: The steel billet is heated to 1200~1280℃ and held at that temperature, and then roughed and finished rolled to obtain a finished strip.

[0038] In some embodiments, the steel billet is heated to 1225~1250℃, and the total furnace time is 180~240min, wherein the heat soaking time is 40~60min, and the average heating rate of the heating section is 4.8~9.5℃ / min; then rough rolling and finish rolling are performed sequentially to obtain finish rolled strip.

[0039] S3: Cool the finished strip, including ultra-fast cooling and laminar flow cooling. The laminar flow cooling adopts a front-end centralized cooling mode, and no edge shielding is used during the laminar flow cooling process. Then, the strip is coiled at a temperature of 500~560℃ to obtain hot-rolled strip steel.

[0040] In some embodiments, the winding temperature is 530~550°C.

[0041] S4: The hot-rolled strip steel after coiling is subjected to a stacking cooling treatment to room temperature, followed by pickling and cold rolling to obtain cold-rolled strip steel, which is then galvanized to obtain the duplex steel.

[0042] The aforementioned method for controlling edge cracks in duplex steel rolling employs a front-end centralized cooling mode and eliminates edge shielding during laminar flow cooling. This allows the finished strip to complete its main temperature drop and rapidly pass through the phase transformation zone before cooling, effectively shortening the difference in residence time between the edge and center of the finished strip in the high-temperature zone. This significantly reduces the microstructure differences between the edge and center caused by alloy element segregation and uneven cooling, thereby refining the grain size and improving the ability to generate crack initiation and prevent crack propagation. Simultaneously, the coiling temperature of 500~560℃, combined with a rapid cooling rate, allows the edge of the finished strip to generate a fine-grained bainite and ferrite-based multiphase microstructure. This multiphase microstructure possesses strong coordinating deformation capabilities, fundamentally improving the microstructure uniformity and plasticity of the edge. This effectively suppresses edge cracking during subsequent cold rolling, avoiding the cold rolling edge cracking problems caused by increased martensite ratio and grain coarsening due to higher edge temperatures and faster cooling rates of the inner and outer rings of the coil after coiling, which are common in traditional edge shielding processes. Furthermore, by subjecting the hot-rolled strip to stacking cooling treatment after coiling, the full diffusion and escape of hydrogen in the steel and the uniform release of residual stress are promoted, further reducing edge crack sensitivity. Simultaneously, by optimizing the chemical composition of the billet, adding Nb and Ti microalloying elements to the C-Si-Mn-Cr system while controlling the content of impurity elements such as S and P, the resulting dual-phase steel possesses excellent comprehensive mechanical properties, combining high strength and good formability, meeting the requirements for a balance between strength and formability in automotive steel and other applications.

[0043] In some embodiments, the thickness of the steel billet is 230~240mm.

[0044] The total heating time for the steel billet is 160~320 minutes.

[0045] The heating rate of the steel billet is 4.8~9.8℃ / min.

[0046] The heat preservation time is 30-70 minutes.

[0047] In some embodiments, the total heating time of the billet includes a heating stage and a soaking stage, wherein the holding time is the duration of the soaking stage.

[0048] In some embodiments, the roughing rolling process consists of 5 to 7 passes.

[0049] The temperature of the intermediate billet at the exit of the roughing mill is 1070~1120℃.

[0050] In some embodiments, the temperature of the intermediate billet exiting the roughing mill is 1075~1090°C.

[0051] In some embodiments, the inlet temperature of the finishing mill is 1020~1090℃.

[0052] The exit temperature of the finishing mill is 860~890℃.

[0053] In some embodiments, the inlet temperature of the finishing mill is 1035~1050°C.

[0054] The exit temperature of the finishing mill is 870~890℃.

[0055] In some embodiments, the microstructure of the edge of the cooled finished strip includes bainite and ferrite.

[0056] The volume fraction of bainite is 60-80%.

[0057] In some embodiments, the volume fraction of bainite and the volume fraction of ferrite in the edge of the cooled finished strip are 60-80% and 20-40%, respectively.

[0058] In some embodiments, the volume fraction of bainite in the edge of the cooled finished strip is 70-75%, with the remainder being ferrite.

[0059] In some embodiments, the thickness of the hot-rolled strip is 2.0~6.0 mm.

[0060] The ultra-fast cooling rate is 60~110℃ / s.

[0061] The laminar flow cooling rate is 10~20℃ / s.

[0062] In some embodiments, the thickness of the hot-rolled strip is 2.5~5.0 mm.

[0063] In some embodiments, the thickness of the hot-rolled strip is 2.6 to 4.2 mm.

[0064] In some embodiments, the ultra-fast cooling rate is 70~90℃ / s.

[0065] In some embodiments, the laminar cooling rate is 12~18°C / s.

[0066] In some embodiments, the cold rolling reduction rate is 45-60%.

[0067] The thickness of the cold-rolled strip is 1.0~2.5mm.

[0068] In some embodiments, the cold rolling reduction rate is 50-53.8%.

[0069] In some embodiments, the thickness of the cold-rolled strip is 1.2~2.0 mm.

[0070] In some embodiments, the stacking cooling method includes: naturally stacking the coiled hot-rolled strip steel in a steel coil warehouse and cooling it to room temperature.

[0071] During the stack cooling process, forced air blowing and / or water cooling are prohibited for accelerated cooling.

[0072] The method of this invention is simple and easy to operate. The edge crack repair rate of cold-rolled high-strength duplex steel can be reduced from 50% to 0%, avoiding the repair process of trimming or cutting off the length of the edge crack. This increases the production efficiency of the cold rolling mill by 20%, saves 50 yuan / ton in repair process costs, and improves the overall yield by 2.5%. The entire process is simple and efficient, requiring no additional edge trimming or complex edge heating devices. It effectively reduces production costs while ensuring product quality and has good prospects for industrial application.

[0073] This invention provides a dual-phase steel, which is prepared using the above-described method for controlling edge cracking during rolling of dual-phase steel.

[0074] In some embodiments, the yield strength of the duplex steel is 440-500 MPa, the tensile strength is 780-840 MPa, and the elongation is 22-30%.

[0075] In some embodiments, the duplex steel has a yield strength of 457-475 MPa, a tensile strength of 785-798 MPa, and an elongation of 24.5-26%.

[0076] To further illustrate the present invention, the following examples are provided: Example 1 A method for controlling edge cracking during rolling of 2.6mm thick duplex steel, comprising the following steps: S1: Provides a steel billet with the following chemical composition by mass fraction: C 0.1%, Si 0.3%, Mn 1.98%, Als 0.035%, Nb 0.015%, Ti 0.025%, Cr 0.2%, S 0.0012%, P 0.014%, with the balance being Fe and unavoidable impurities; the billet thickness is 230 mm.

[0077] S2: The steel billet is heated to 1225℃ and held for 40 minutes, with a total heating time of 180 minutes. It should be noted that the heating process for the same steel billet is controlled by zones, with each zone having a heating rate of 6.0~9.5℃ / min. After exiting the furnace, the steel billets undergo roughing and finishing rolling. Roughing is performed in 5 passes to obtain an intermediate billet. The intermediate billet exiting the roughing mill has a temperature of 1080℃. The intermediate billet is then subjected to 7-stand finishing rolling, with an entry temperature of 1040℃ and an exit temperature of 890℃ to obtain finished strip.

[0078] S3: The finished strip is subjected to ultra-fast cooling and laminar flow cooling. The ultra-fast cooling rate is 80℃ / s, and the laminar flow cooling rate is 15℃ / s. The laminar flow cooling adopts a front-end centralized cooling mode, and no edge shielding is used during the laminar flow cooling process. Then, it is coiled at a temperature of 550℃ to obtain hot-rolled strip steel. The microstructure of the edge of the cooled finished strip steel is 70% bainite and 30% ferrite by volume, and the thickness of the hot-rolled strip steel is 2.6mm.

[0079] S4: After being uncoiled from the coiler, the hot-rolled strip steel coils are rapidly transported to the coil warehouse via a coil conveyor chain. They are then naturally stacked and cooled to room temperature. During the stacking cooling process, forced air blowing and / or water cooling are prohibited for accelerated cooling, resulting in hot-rolled strip. The hot-rolled strip undergoes pickling and cold rolling with a reduction rate of 53.8%, yielding a 1.2mm thick cold-rolled strip. This strip is then galvanized to obtain duplex steel. Furthermore, no edge cracks are generated during the cold rolling process, resulting in a high-strength duplex steel product that meets quality standards.

[0080] Tests showed that the yield strength of the duplex steel prepared in Example 1 was 457 MPa, the tensile strength was 785 MPa, and the elongation was 24.5%.

[0081] Example 2 A method for controlling edge cracking during rolling of 3.6mm thick duplex steel, comprising the following steps: S1: Provides a steel billet with the following chemical composition by mass fraction: C 0.1%, Si 0.4%, Mn 2.05%, Als 0.038%, Nb 0.020%, Ti 0.015%, Cr 0.3%, S 0.0010%, P 0.012%, with the balance being Fe and unavoidable impurities; the billet thickness is 230 mm.

[0082] S2: The steel billet is heated to 1240℃ and held for 50 minutes, with a total heating time of 210 minutes. The heating process for the same billet is controlled by zones, with each zone having a heating rate of 5.0~8.0℃ / min. After exiting the furnace, the billets undergo roughing and finishing rolling. Roughing is performed in 5 passes to obtain intermediate billets. The intermediate billet exiting the roughing mill has a temperature of 1090℃. The intermediate billets are then finished using a 7-stand finishing mill, with an entry temperature of 1050℃ and an exit temperature of 870℃, yielding finished strip.

[0083] S3: The finished strip undergoes ultra-rapid cooling and laminar flow cooling. The ultra-rapid cooling rate is 70℃ / s, and the laminar flow cooling rate is 12℃ / s. The laminar flow cooling adopts a front-end centralized cooling mode, and no edge shielding is used during the laminar flow cooling process. The strip is then coiled at a temperature of 530℃ to obtain hot-rolled strip steel. The microstructure of the edge of the cooled finished strip steel consists of 75% bainite and 25% ferrite by volume. The thickness of the hot-rolled strip steel is 3.6mm.

[0084] S4: After being uncoiled from the coiler, the hot-rolled strip steel coils are rapidly transported to the coil warehouse via a coil conveyor chain. They are then naturally stacked and cooled to room temperature. During the stacking cooling process, forced air blowing and / or water cooling are prohibited for accelerated cooling, resulting in hot-rolled strip. The hot-rolled strip undergoes pickling and cold rolling with a 50% reduction rate to obtain a 1.8mm thick cold-rolled strip, which is then galvanized to obtain duplex steel. No edge cracks are generated during the cold rolling process, resulting in a high-strength duplex steel product that meets quality standards.

[0085] Tests showed that the yield strength of the duplex steel prepared in Example 2 was 475 MPa, the tensile strength was 798 MPa, and the elongation was 25.5%.

[0086] Example 3 A method for controlling edge cracking during rolling of 4.2mm thick duplex steel, comprising the following steps: S1: Provides a steel billet with the following chemical composition by mass fraction: C 0.09%, Si 0.5%, Mn 2.1%, Als 0.040%, Nb 0.018%, Ti 0.025%, Cr 0.5%, S 0.007%, P 0.011%, with the balance being Fe and unavoidable impurities; the billet thickness is 230 mm.

[0087] S2: The steel billet is heated to 1250℃ and held for 60 minutes, with a total heating time of 240 minutes. The heating process for the same billet is controlled by zones, with each zone having a heating rate of 4.8~7.0℃ / min. After exiting the furnace, the billets undergo roughing and finishing rolling. Roughing is performed in 7 passes to obtain an intermediate billet. The intermediate billet exits the roughing mill at 1075℃. The intermediate billet then undergoes 7-stand finishing rolling, with the entry temperature at 1035℃ and the exit temperature at 870℃, yielding a finished strip.

[0088] S3: The finished strip undergoes ultra-rapid cooling and laminar flow cooling. The ultra-rapid cooling rate is 90℃ / s, and the laminar flow cooling rate is 18℃ / s. The laminar flow cooling adopts a front-end centralized cooling mode, and no edge shielding is used during the laminar flow cooling process. The strip is then coiled at a temperature of 530℃ to obtain hot-rolled strip steel. The microstructure of the edge of the cooled finished strip steel consists of 70% bainite and 30% ferrite by volume. The thickness of the hot-rolled strip steel is 4.2mm.

[0089] S4: After being uncoiled from the coiler, the hot-rolled strip steel coils are rapidly transported to the coil warehouse via a coil conveyor chain. They are then naturally stacked and cooled to room temperature. During the stacking cooling process, forced air blowing and / or water cooling are prohibited for accelerated cooling, resulting in hot-rolled strip. The hot-rolled strip undergoes pickling and cold rolling with a reduction rate of 52.4%, yielding a 2.0mm thick cold-rolled strip. This strip is then galvanized to obtain duplex steel. Furthermore, no edge cracks are generated during the cold rolling process, resulting in a high-strength duplex steel product that meets quality standards.

[0090] Tests showed that the yield strength of the duplex steel prepared in Example 3 was 469 MPa, the tensile strength was 790 MPa, and the elongation was 26%.

[0091] Comparative Example 1 Compared to Example 1, the laminar cooling steps were changed.

[0092] In Comparative Example 1, three sets of edge shielding devices were used during the laminar flow cooling process, and the other steps were the same as in Example 1, resulting in the preparation of dual-phase steel.

[0093] The edge microstructure of the cooled, finished strip consists of bainite, martensite, and ferrite, exhibiting martensitic structure. During cold rolling, edge cracks occur on the outer 40m of the hot-rolled coil, requiring rewinding and repair to remove the cracked portion. Testing showed that the yield strength of the duplex steel obtained in Comparative Example 1 was 460 MPa, the tensile strength was 788 MPa, and the elongation was 24%. It should be noted that the total length of the hot-rolled coil was 800m; assuming 50% of the coils require the removal of the outer 40m, the yield loss is 2.5% (the same applies below).

[0094] Comparative Example 2 Compared to Example 1, the winding temperature was changed.

[0095] In Comparative Example 2, the winding temperature was 620°C, and the other steps were the same as in Example 1, resulting in the preparation of duplex steel.

[0096] The edge structure of the finished strip after cooling contains martensite; edge cracks occur during cold rolling; according to the test, the yield strength of the duplex steel prepared in Comparative Example 2 is 445 MPa, the tensile strength is 785 MPa, and the elongation is 20%.

[0097] Comparative Example 3 Compared to Example 1, the exit temperature of the finishing mill was changed.

[0098] In Comparative Example 3, the exit temperature of the finishing mill was 915°C, and the other steps were the same as in Example 1, resulting in the preparation of duplex steel.

[0099] After cooling, the grains on the edge of the finished strip are coarse, and edge cracks occur during cold rolling. According to the test, the yield strength of the duplex steel prepared in Comparative Example 3 is 442 MPa, the tensile strength is 782 MPa, and the elongation is 20%.

[0100] Comparative Example 4 Compared to Example 1, ultra-fast cooling is not performed; only laminar flow cooling is used.

[0101] In Comparative Example 4, laminar cooling adopted a front-end centralized cooling mode and did not use side shielding. Other steps were the same as in Example 1, and dual-phase steel was obtained.

[0102] Edge cracks occurred during the cold rolling process; tests showed that the yield strength of the duplex steel prepared in Comparative Example 4 was 450 MPa, the tensile strength was 780 MPa, and the elongation was 19%.

[0103] See Figure 1 and Figure 2 Furthermore, in conjunction with Examples 1-3 and Comparative Examples 1-4, it can be seen that the present invention, by combining ultra-fast cooling with front-end concentrated laminar flow cooling without using edge shielding, and simultaneously using a coiling temperature of 500-560°C and natural stacking cooling treatment, can enable the edge of the finished rolled strip to obtain a fine and uniform bainite and ferrite multiphase structure, and the edge structure does not contain martensite, fundamentally suppressing the generation of cold rolling edge cracks. This shows that the method of the present invention can effectively control cold rolling edge cracks in dual-phase steel, and improve production efficiency and yield.

[0104] In Comparative Example 1, after edge shielding, the edge temperature increased. Due to the low austenitic transformation temperature of high-strength duplex steel, the residual austenite at the edge, after coiling, is cooled more rapidly because the outer coil is in full contact with the saddle and air, while the inner coil is in contact with the mandrel and air. Furthermore, the outer coil cools faster than the inner coil after uncoiling, resulting in a larger quantity of relatively coarse martensite. This coarse martensite forms a phase interface with ferrite. During cold rolling, crack initiation easily occurs at this ferrite / martensite interface between the inner and outer coils of the hot-rolled steel coil, leading to edge cracking. The outer coil contains more martensite, making it more prone to edge cracking.

[0105] This invention does not employ edge shielding and uses a lower coiling temperature, which allows the austenitic structure at the edge of the strip to undergo sufficient ferrite and bainite phase transformation during laminar cooling, while refining the ferrite and bainite grains. The intragranular precipitates of ferrite at low temperatures increase the strength of the ferrite grains, further reducing the strength difference between ferrite and bainite, making it easier for the two to deform in tandem without generating crack initiation, thereby effectively avoiding the aforementioned edge cracking problem.

[0106] The aforementioned method for controlling edge cracking in duplex steel rolling and the resulting duplex steel employ a front-end centralized cooling mode without edge shielding during laminar flow cooling. This allows the finished strip to complete its main temperature drop and rapidly pass through the phase transformation zone before cooling, effectively shortening the difference in residence time between the edge and center of the finished strip in the high-temperature zone. This significantly reduces the microstructure differences between the edge and center caused by alloy element segregation and uneven cooling, thereby refining the grains and improving the ability to generate crack initiation and prevent crack propagation. Simultaneously, the coiling temperature of 500~560℃ allows the edge of the finished strip to generate a fine-grained bainite and ferrite multiphase microstructure at a relatively fast cooling rate. This multiphase microstructure has strong coordinating deformation capabilities, fundamentally improving the microstructure uniformity at the edge. The process effectively suppresses edge cracking during subsequent cold rolling, avoiding the cold rolling edge cracking problems caused by increased martensite ratio and grain coarsening due to higher edge temperatures and faster cooling rates of the inner and outer rings of the coil after coiling, which are common in traditional edge shielding processes. Furthermore, by subjecting the hot-rolled strip to stacking cooling treatment after coiling, the process promotes the full diffusion and escape of hydrogen in the steel and the uniform release of residual stress, further reducing edge crack sensitivity. Simultaneously, by optimizing the chemical composition of the billet, adding Nb and Ti microalloying elements to the C-Si-Mn-Cr system while controlling the content of impurity elements such as S and P, the resulting dual-phase steel possesses excellent comprehensive mechanical properties, combining high strength and good formability, meeting the requirements for a balance between strength and formability in automotive steel and other applications.

[0107] The method of this invention is simple and easy to operate. The edge crack repair rate of cold-rolled high-strength duplex steel can be reduced from 50% to 0%, avoiding the repair process of trimming or cutting off the length of the edge crack. This increases the production efficiency of the cold rolling mill by 20%, saves 50 yuan / ton in repair process costs, and improves the overall yield by 2.5%. The entire process is simple and efficient, requiring no additional edge trimming or complex edge heating devices. It effectively reduces production costs while ensuring product quality and has good prospects for industrial application.

[0108] The above technical solutions of the present invention are merely preferred embodiments of the present invention and do not limit the patent scope of the present invention. All equivalent structural transformations made under the technical concept of the present invention using the contents of the present invention specification and drawings, or direct / indirect applications in other related technical fields, are included in the patent protection scope of the present invention.

Claims

1. A method for controlling edge cracking during the rolling of duplex steel, characterized in that, Includes the following steps: S1: Provide a steel billet, the chemical composition of which, by mass fraction, comprises: C 0.08~0.13%, Si 0.2~0.8%, Mn 1.8~2.2%, Als 0.025~0.060%, Nb 0.01~0.05%, Ti 0.015~0.04%, Cr 0.1~0.7%, S≤0.010%, P≤0.020%, with the balance being Fe and unavoidable impurities; S2: The steel billet is heated to 1200~1280℃ and held at that temperature, and then rough and finish rolled to obtain a finish rolled strip; S3: Cool the finished strip, the cooling includes ultra-fast cooling and laminar flow cooling. The laminar flow cooling adopts a front-end centralized cooling mode, and no edge shielding is used during the laminar flow cooling process. Then, the strip is coiled. The coiling temperature is 500~560℃ to obtain hot-rolled strip steel. S4: The hot-rolled strip steel after coiling is subjected to a stacking cooling treatment to room temperature, followed by pickling and cold rolling to obtain cold-rolled strip steel, which is then galvanized to obtain the duplex steel.

2. The method for controlling edge cracking during rolling of duplex steel according to claim 1, characterized in that, The thickness of the steel billet is 230~240mm; The total heating time for the steel billet is 160~320min; The heating rate of the steel billet is 4.8~9.8℃ / min; The heat preservation time is 30-70 minutes.

3. The method for controlling edge cracking during rolling of duplex steel according to claim 1, characterized in that, The roughing process consists of 5 to 7 passes. The temperature of the intermediate billet at the exit of the roughing mill is 1070~1120℃.

4. The method for controlling edge cracking during rolling of duplex steel according to claim 1, characterized in that, The inlet temperature of the finishing mill is 1020~1090℃; The exit temperature of the finishing mill is 860~890℃.

5. The method for controlling edge cracking during rolling of duplex steel according to claim 1, characterized in that, The microstructure of the edge of the cooled finished strip includes bainite and ferrite; The volume fraction of bainite is 60-80%.

6. The method for controlling edge cracking during rolling of duplex steel according to claim 1, characterized in that, The thickness of the hot-rolled strip is 2.0~6.0 mm; The ultra-fast cooling rate is 60~110℃ / s; The laminar flow cooling rate is 10~20℃ / s.

7. The method for controlling edge cracking during rolling of duplex steel according to claim 1, characterized in that, The reduction rate of the cold rolling is 45-60%; The thickness of the cold-rolled strip is 1.0~2.5mm.

8. The method for controlling edge cracking during rolling of duplex steel according to claim 1, characterized in that, The stacking cooling method includes: naturally stacking the coiled hot-rolled strip steel in a steel coil warehouse and cooling it to room temperature; During the stack cooling process, forced air blowing and / or water cooling are prohibited for accelerated cooling.

9. A dual-phase steel, characterized in that, The method for controlling edge cracking during rolling of duplex steel according to any one of claims 1 to 8 is used to prepare the steel.

10. The duplex steel according to claim 9, characterized in that, The yield strength of the duplex steel is 440~500MPa, the tensile strength is 780~840MPa, and the elongation is 22~30%.