Production method of multi-specification q355ne wind power steel
By differentially controlling alloying elements and optimizing heating and rolling parameters, the problems of uneven microstructure and performance fluctuation in the production of Q355NE wind power steel have been solved, and the microstructure uniformity and performance stability of multi-specification steel plates have been improved, especially in thin, medium and thick plates.
Patent Information
- Application Number
- CN202611537519.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-20
AI Technical Summary
In the current production process of Q355NE wind power steel, the finished product has uneven microstructure and large performance fluctuations, especially in steel plates of different thicknesses. This is mainly due to the imbalance of microstructure and performance caused by factors such as composition, heating and rolling.
By differentially controlling the content of alloying elements C, Si, Mn, Nb, V, and Ti, and by controlling heating and rolling parameters, including the slab soaking temperature, single-pass reduction rate, and finishing rolling temperature, the deformation amount and quality of each pass are ensured, austenite grains are refined, ferrite nucleation is improved, and the inhomogeneity of steel plate structure is solved.
It has achieved improvements in the uniformity of microstructure and performance stability of steel plates of different thicknesses, increased grain size by more than one grade, improved weldability and low-temperature toughness, and reduced anisotropic performance differences.
Smart Images

Figure REF-OBJ-1790745123439-000001 
Figure REF-OBJ-1790745123439-000002 
Figure REF-OBJ-1790745123439-000003
Abstract
Description
Technical Field
[0001] This invention relates to the field of hot rolling technology, specifically to a method for producing Q355NE wind power steel of multiple specifications. Background Technology
[0002] As a crucial development direction for clean energy, wind power generation continues to expand its installed capacity. Wind turbine towers, as key load-bearing components of wind turbine generators, endure the combined effects of alternating loads, low-temperature environments, and welding processes over extended periods. This places stringent requirements on the low-temperature impact toughness, weldability, strength-toughness balance, and microstructure uniformity of the steel plates used. Currently, the steel used for wind turbine towers in China mainly comprises grades such as Q355NE and Q355D / E, employing a C-Mn composition system. The target microstructure is predominantly ferrite and pearlite, requiring both the guarantee of the base material's mechanical properties and the consideration of the toughness of the weld heat-affected zone.
[0003] Currently, most Q355NE wind power steel production uses a uniform chemical composition ratio, without differentiated control based on the thickness of the finished steel plate, resulting in the drawbacks of a "one-size-fits-all" composition design. For thin steel plates, the cooling rate is fast, and there is a surplus in toughness and strength; however, the cooling rate of the core of medium and thick plates is insufficient, which easily leads to coarsening of the core structure and a decrease in strength and low-temperature toughness. Thick plates are also prone to the formation of bainite structure, which disrupts the stability of the ferrite-pearlite matrix structure, resulting in an imbalance in the microstructure and properties of products with different thicknesses.
[0004] In the billet heating process, traditional production generally adopts a high-temperature heating system of 1200-1250℃. Although this can ensure the solid solution of microalloying elements, the austenite grain boundaries are prone to migration under high temperature conditions. The austenite grains in the billet grow abnormally, and the TiN particles coarsen and lose their function of pinning grain boundaries, resulting in large fluctuations in the original austenite grain size. This structural defect can be inherited to the finished steel plate, causing the problem of uneven grain size.
[0005] In the rolling process, the single-pass reduction rate of traditional rough rolling is generally less than 10%, resulting in insufficient total deformation. The columnar crystal structure inside the continuously cast billet is difficult to fully break down, leading to severe banded structure after rolling. Inclusions such as Mn and S segregate, causing stratification of the steel plate's thickness, transverse, and longitudinal structures, resulting in significant differences in properties across directions and even the formation of localized coarse-grained bands. In finish rolling, the final rolling temperature is mostly controlled between 850 and 900℃. The rolling window is located within the austenite recrystallization range, making it difficult to form sufficient deformation bands within the austenite. The number of ferrite nucleation sites is limited, resulting in insufficient grain uniformity after phase transformation.
[0006] In summary, it is necessary to design a multi-specification Q355NE wind power steel production method to solve the problem of uneven microstructure and large performance fluctuations in the finished Q355NE wind power steel caused by the influence of composition, heating and rolling factors during the actual production process. Summary of the Invention
[0007] The purpose of this invention is to provide a multi-specification Q355NE wind power steel production method to solve the problem that the finished Q355NE wind power steel has uneven structure and large performance fluctuations due to the influence of composition, heating and rolling factors during the actual production process.
[0008] To achieve the above objectives, the basic solution provided by this invention is: a method for producing multi-specification Q355NE wind power steel, comprising the following steps: Heating: The slab is heated in a walking beam furnace, and the temperature of the soaking zone is controlled at 1130-1180℃; Rough rolling: During the rolling process, the rolling temperature of each pass, as well as the roll gap value, rolling force, torque and rolling speed of the rolling mill are controlled according to the target steel plate thickness to ensure that the single-pass reduction rate is ≥16% and the total rough rolling reduction rate is ≥70%. After 10 to 16 passes, an intermediate billet with a thickness of 50 to 125 mm is rolled and then sent to the finishing mill. Finishing: The intermediate billet after roughing is sent to the finishing mill and the final rolling temperature is controlled at 810±20℃. After 8 to 10 passes, it is rolled into a steel plate with a thickness of 8 to 80 mm.
[0009] The beneficial effects of the present invention are as follows: (1) The present invention differentiates the content of C, Si, Mn, Nb, V and Ti alloying elements according to three thickness ranges of 8-19mm, 20-49mm and 50-80mm, while strictly controlling the carbon equivalent CEV≤0.42% and the welding crack sensitivity index Pcm≤0.20%; and reduces the carbon and microalloy content of thin steel plates to ensure welding toughness, while appropriately increasing the carbon and manganese content of thick steel plates to compensate for the core strength decay, and reducing the silicon content as the steel plate thickness increases to suppress abnormal precipitation of bainite in the core, taking into account fine grain strengthening, precipitation strengthening and welding performance, and solving the problem of imbalance of structure and performance of steel plates of different thicknesses from the source of composition; (2) By controlling the temperature of the slab soaking section at 1130-1180℃, the present invention ensures sufficient solid solution of microalloying elements while inhibiting abnormal growth of austenite grains; and by adopting a large reduction system with a single-pass reduction rate of ≥16% and a total reduction rate of ≥70% in the rough rolling stage, the columnar crystals of the slab are fully broken up, reducing the banded structure segregation caused by Mn and S inclusions; at the same time, the finishing rolling stage controls the final rolling temperature at 810±20℃, achieving cumulative large deformation in the non-recrystallized austenite region, providing nucleation cores for ferrite phase transformation; thus, the grain size of the final product is stably at grade 9-10, which is more than 1 grade higher than that of the traditional process.
[0010] Option 2, this is the preferred option of the basic option, where the slab composition is adjusted according to the target steel plate thickness, specifically as follows: When the target steel plate thickness is 8–19 mm, the slab composition is as follows: C content is 0.085–0.115%, Si content is 0.30–0.40 wt%, Mn content is 1.20–1.30 wt%, Nb content is 0.018–0.03%, and Ti content is 0.01–0.02%. When the target steel plate thickness is 20–49 mm, the slab composition is as follows: C content is 0.11–0.14%, Si content is 0.25–0.35 wt%, Mn content is 1.40–1.50 wt%, Nb content is 0.025–0.035%, V content is 0.015–0.025%, and Ti content is 0.015–0.02%. When the target steel plate thickness is 50-80mm, the slab composition is as follows: C content is 0.12-0.15%, Si content is 0.10-0.20wt%, Mn content is 1.45-1.55wt%, Nb content is 0.025-0.035%, V content is 0.015-0.025%, and Ti content is 0.015-0.02%.
[0011] For thin, medium, and thick plates, carbon, silicon, manganese, Nb, V, and Ti microalloying systems are matched respectively, taking into account the requirements of precipitation strengthening, solid solution strengthening, fine grain strengthening, and weldability.
[0012] Option 3, an optimized version of Option 2, involves the following steps in the roughing process: when the target steel plate thickness is 8–19 mm, the initial rolling temperature for the first to sixteenth passes is 1023–1137 °C, the roll gap for the first to sixteenth passes is 54–230 mm, the rolling force for the first to sixteenth passes is 10420–34513 KN, the torque for the first to sixteenth passes is 439–3226 rap / min, and the rolling speed for the first to sixteenth passes is 1.5–1.7 m / s. For thin steel plates of 8–19 mm, ensuring the deformation amount in each pass and refining the austenite grains through repeated recrystallization, deformation, and recrystallization cycles improves the inhomogeneity of the original slab microstructure.
[0013] Option 4, an optimized version of Option 2, involves the following steps in the roughing process: when the target steel plate thickness is 20–49 mm, the initial rolling temperature for the first to sixteenth passes is 979–1098 °C, the roll gap for the first to sixteenth passes is 70–305 mm, the rolling force for the first to sixteenth passes is 14788–33089 KN, the torque for the first to sixteenth passes is 1063–3192 rap / min, and the rolling speed for the first to sixteenth passes is 1.5–1.8 m / s. For medium-thickness finished products of 20–49 mm, reducing the initial rolling temperature to 979 °C can reduce surface oxidation and burn-off, improving surface quality and plate shape.
[0014] Option 5, an optimal choice of Option 2, involves the following steps in the roughing process: for a target steel plate thickness of 50–80 mm, the initial rolling temperature for passes 1 through 16 is 1028–1098 °C, the roll gap for passes 1 through 16 is 115–310 mm, the rolling force for passes 1 through 16 is 17362–32652 KN, the torque for passes 1 through 16 is 967–3154 rap / min, and the rolling speed for passes 1 through 16 is 1.5–1.7 m / s. For finished products with a thickness of 50–80 mm, the overall initial rolling temperature is relatively high, which compensates for the slow heat dissipation of thick billets and the need to maintain core temperature. Simultaneously, the increased rolling force ensures sufficient pass reduction, achieving a total roughing reduction rate of ≥70%, and preventing substandard core impact energy in thick plates.
[0015] Option 6, which is a preferred option of Option 2, involves the following steps: In the finishing rolling process, when the target steel plate thickness is 8–19 mm, the initial rolling temperature for the first to tenth passes is 726–1039 °C, the roll gap for the first to sixth passes is 9–50 mm, the rolling force for the first to sixth passes is 24525–39769 KN, the bending roll force for the first to sixth passes is 2000–3328 KN, the rolling speed for the first to sixth passes is 2–3.5 m / s, and the torque for the first to sixth passes is 543–2822 rap / min.
[0016] Option 7, a preferred option of Option 2, involves the following steps in the finishing rolling process: when the target steel plate thickness is 20–49 mm, the initial rolling temperature for the first to tenth passes is 762–885 °C, the roll gap for the first to sixth passes is 29–115 mm, the rolling force for the first to sixth passes is 21235–40323 KN, the bending force for the first to sixth passes is 2000–3361 KN, the rolling speed for the first to sixth passes is 1.5–3 m / s, and the torque for the first to sixth passes is 953–2760 rap / min. For medium-thickness finished products of 20–49 mm, increasing the roll gap and reducing the rolling speed in the finishing rolling stage can prevent loss of shape control during rolling.
[0017] Option 8, an optimized version of Option 2, involves the following steps in the finishing rolling process: when the target steel plate thickness is 50–80 mm, the initial rolling temperature for the first to tenth passes is 741–815 °C, the roll gap for the first to sixth passes is 54–110 mm, the rolling force for the first to sixth passes is 34028–47294 KN, the bending roll force for the first to sixth passes is 2533–3271 KN, the rolling speed for the first to sixth passes is 1.5–2.5 m / s, and the torque for the first to sixth passes is 2046–3409 rap / min. For 50–80 mm thick plates, the rolling speed is further reduced in the finishing rolling stage to avoid shape defects and mill impact caused by high-speed rolling of thick plates. Detailed Implementation
[0018] The present invention will be further described in detail below through specific embodiments: Example 1
[0019] A method for producing multi-specification Q355NE wind power steel includes the following steps: Heating: The slab is heated in a walking beam furnace, and the temperature of the soaking zone is controlled at 1130-1180℃; the slab contains 0.085-0.115% C, 0.30-0.40 wt% Si, 1.20-1.30 wt% Mn, 0.018-0.03% Nb, and 0.01-0.02% Ti. Rough rolling: The heated slab is rolled into an intermediate slab with a thickness of 50 mm through seven rough rolling passes. The starting temperature, roll gap, rolling force, torque and rolling speed of the first to tenth passes are shown in Table 1-1. Table 1-1: Summary of rolling parameters in the roughing stage of Example 1
[0020] Finishing rolling: The intermediate billet after roughing is fed into the finishing mill and rolled into a steel plate with a thickness of 10mm through eight passes; the initial rolling temperature, roll gap value, rolling force, bending roll force, rolling speed and torque for the first to eighth passes are shown in Table 1-2: Table 1-2: Summary of rolling parameters in the finishing stage of Example 1
[0021] Example 2
[0022] A method for producing multi-specification Q355NE wind power steel, the steps of which are the same as those in Example 1, the difference being: Rough rolling: The heated slab is rolled into an intermediate slab with a thickness of 60 mm through seven rough rolling passes. The starting temperature, roll gap, rolling force, torque and rolling speed of the first to tenth passes are shown in Table 2-1. Table 2-1: Summary of rolling parameters in the roughing stage of Example 2
[0023] Finishing rolling: The intermediate billet after roughing is fed into the finishing mill and rolled into a steel plate with a thickness of 12mm through eight passes; the starting temperature, roll gap, rolling force, bending roll force, rolling speed and torque of the first to eighth passes are shown in Table 2-2: Table 2-2: Summary of rolling parameters in the finishing stage of Example 2
[0024] Example 3
[0025] A method for producing multi-specification Q355NE wind power steel, the steps of which are the same as those in Example 1, the difference being: Rough rolling: The heated slab is rolled into an intermediate slab with a thickness of 60 mm through seven rough rolling passes. The starting temperature, roll gap, rolling force, torque and rolling speed of the first to tenth passes are shown in Table 3-1. Table 3-1: Summary of rolling parameters in the roughing stage of Example 3
[0026] Finishing rolling: The intermediate billet after roughing is fed into the finishing mill and rolled into a steel plate with a thickness of 15mm through eight passes; the initial rolling temperature, roll gap value, rolling force, bending roll force, rolling speed and torque for the first to eighth passes are shown in Table 3-2: Table 3-2: Summary of rolling parameters in the finishing stage of Example 3
[0027] Example 4
[0028] A method for producing multi-specification Q355NE wind power steel, the steps of which are the same as those in Example 1, the difference being: Heating: The slab is heated in a walking beam furnace, and the temperature of the soaking zone is controlled at 1130-1180℃; the slab contains 0.11-0.14% C, 0.25-0.35 wt% Si, 1.40-1.50 wt% Mn, 0.025-0.035% Nb, 0.015-0.025% V, and 0.015-0.02% Ti. Rough rolling: The heated slab is rolled into an intermediate slab with a thickness of 70 mm through seven rough rolling passes. The rolling temperature, roll gap, rolling force, torque and rolling speed of the first to tenth passes are shown in Table 4-1. Table 4-1: Summary of rolling parameters in the roughing stage of Example 4
[0029] Finishing rolling: The intermediate billet after roughing is fed into the finishing mill and rolled into a steel plate with a thickness of 20mm through eight passes; the initial rolling temperature, roll gap value, rolling force, bending roll force, rolling speed and torque for the first to eighth passes are shown in Table 4-2: Table 4-2: Summary of rolling parameters in the finishing stage of Example 4
[0030] Example 5
[0031] A method for producing Q355NE wind power steel of multiple specifications, the steps of which are the same as those in Example 4, the difference being: Rough rolling: The heated slab is rolled into an intermediate slab with a thickness of 90 mm through seven rough rolling passes. The starting temperature, roll gap, rolling force, torque and rolling speed of the first to tenth passes are shown in Table 5-1. Table 5-1: Summary of rolling parameters in the roughing stage of Example 5
[0032] Finishing rolling: The intermediate billet after roughing is fed into the finishing mill and rolled into a steel plate with a thickness of 30mm through eight passes; the starting temperature, roll gap, rolling force, bending roll force, rolling speed and torque of the first to eighth passes are shown in Table 5-2: Table 5-2: Summary of rolling parameters in the finishing stage of Example 5
[0033] Example 6
[0034] A method for producing Q355NE wind power steel of multiple specifications, the steps of which are the same as those in Example 4, the difference being: Rough rolling: The heated slab is rolled into an intermediate slab with a thickness of 120 mm through eight rough rolling passes. The starting temperature, roll gap, rolling force, torque and rolling speed of the first to tenth passes are shown in Table 6-1. Table 6-1: Summary of rolling parameters in the roughing stage of Example 6
[0035] Finishing: The intermediate billet after roughing is fed into the finishing mill and rolled into a steel plate with a thickness of 49mm through eight passes; the starting temperature, roll gap, rolling force, bending roll force, rolling speed and torque of the first to eighth passes are shown in Table 6-2. Table 6-2: Summary of rolling parameters in the finishing stage of Example 6
[0036] Example 7
[0037] A method for producing multi-specification Q355NE wind power steel, the steps of which are the same as those in Example 1, the difference being: Heating: The slab is heated in a walking beam furnace, and the temperature of the soaking zone is controlled at 1130-1180℃; the slab contains 0.12-0.15% C, 0.10-0.20 wt% Si, 1.45-1.55 wt% Mn, 0.025-0.035% Nb, 0.015-0.025% V, and 0.015-0.02% Ti. Rough rolling: The heated slab is rolled into an intermediate slab with a thickness of 115 mm through seven rough rolling passes. The starting temperature, roll gap, rolling force, torque and rolling speed of the first to tenth passes are shown in Table 7-1. Table 7-1: Summary of rolling parameters in the roughing stage of Example 7
[0038] Finishing: The intermediate billet after roughing is fed into the finishing mill and rolled into a steel plate with a thickness of 50 mm through eight passes; the initial rolling temperature, roll gap, rolling force, bending roll force, rolling speed and torque for the first to eighth passes are shown in Table 7-2: Table 7-2: Summary of rolling parameters in the finishing stage of Example 7
[0039] Example 8
[0040] A method for producing multi-specification Q355NE wind power steel, the steps of which are all the same as those in Example 7, the difference being: Rough rolling: The heated slab is rolled into an intermediate slab with a thickness of 123 mm through seven rough rolling passes. The starting temperature, roll gap, rolling force, torque and rolling speed of the first to tenth passes are shown in Table 8-1. Table 8-1: Summary of rolling parameters in the roughing stage of Example 8
[0041] Finishing rolling: The intermediate billet after roughing is fed into the finishing mill and rolled into a steel plate with a thickness of 60mm through eight passes; the initial rolling temperature, roll gap value, rolling force, bending roll force, rolling speed and torque for the first to eighth passes are shown in Table 8-2: Table 8-2: Summary of rolling parameters in the finishing stage of Example 8
[0042] The steel plates obtained in the above embodiments were subjected to performance testing, and the test results are shown in Table 9: Table 9: Summary Table of Steel Plate Performance Test Results
[0043] In summary, the steel plates with a thickness of 8–19 mm obtained through Examples 1, 2, and 3 all exhibit tensile strengths of 565–581 MPa, yield strengths of 422–442 MPa, and elongations of ≥26%. Among these, the 15 mm thick steel plate obtained in Example 3 has a tensile strength of 581 MPa, a yield strength of 442 MPa, and impact energy at -40℃ reaching 201 J, 210 J, and 190 J, respectively, all of which are superior to the steel plates obtained through Examples 1 and 2. Similarly, the steel plates with a thickness of 20–49 mm obtained through Examples 4, 5, and 6 all exhibit tensile strengths of 569–585 MPa, yield strengths of 420–430 MPa, and elongations of ≥26%. The 30mm thick steel plate obtained in Example 5 has a tensile strength of 582MPa, a yield strength of 430MPa, and impact energy at -40℃ of 238J, 210J, and 196J, respectively. Its plasticity and low-temperature impact toughness are superior to the steel plates obtained in Examples 4 and 6. The 50-80mm thick steel plates obtained in Examples 7 and 8 have tensile strengths of 555-560MPa, yield strengths of 418-425MPa, and elongations of ≥26%. Among them, the 500mm thick steel plate obtained in Example 7 has a tensile strength of 559MPa, a yield strength of 418MPa, and impact energy at -40℃ of 150J, 170J, and 145J, respectively. Its performance is superior to the steel plate obtained in Example 8.
[0044] The above descriptions are merely embodiments of the present invention, and common knowledge regarding specific structures and characteristics is not elaborated upon here. It should be noted that those skilled in the art can make various modifications and improvements without departing from the structure of the present invention, and these should also be considered within the scope of protection of the present invention. These modifications and improvements will not affect the effectiveness of the present invention or the practicality of the patent. The scope of protection claimed in this application should be determined by the content of its claims, and the specific embodiments described in the specification can be used to interpret the content of the claims.
Claims
1. A method for producing multi-specification Q355NE wind power steel, characterized in that, Includes the following steps: Heating: The slab is heated in a walking beam furnace, and the temperature of the soaking zone is controlled at 1130-1180℃; Rough rolling: During the rolling process, the rolling temperature of each pass, as well as the roll gap value, rolling force, torque and rolling speed of the rolling mill are controlled according to the target steel plate thickness to ensure that the single-pass reduction rate is ≥16% and the total rough rolling reduction rate is ≥70%. After 10 to 16 passes, an intermediate billet with a thickness of 50 to 125 mm is rolled and then sent to the finishing mill. Finishing: The intermediate billet after roughing is sent to the finishing mill and the final rolling temperature is controlled at 810±20℃. After 8 to 10 passes, it is rolled into a steel plate with a thickness of 8 to 80 mm.
2. The method for producing multi-specification Q355NE wind power steel according to claim 1, characterized in that, The slab composition is adjusted according to the target steel plate thickness, specifically as follows: When the target steel plate thickness is 8–19 mm, the slab composition is as follows: C content is 0.085–0.115%, Si content is 0.30–0.40 wt%, Mn content is 1.20–1.30 wt%, Nb content is 0.018–0.03%, and Ti content is 0.01–0.02%. When the target steel plate thickness is 20–49 mm, the slab composition is as follows: C content is 0.11–0.14%, Si content is 0.25–0.35 wt%, Mn content is 1.40–1.50 wt%, Nb content is 0.025–0.035%, V content is 0.015–0.025%, and Ti content is 0.015–0.02%. When the target steel plate thickness is 50-80mm, the slab composition is as follows: C content is 0.12-0.15%, Si content is 0.10-0.20wt%, Mn content is 1.45-1.55wt%, Nb content is 0.025-0.035%, V content is 0.015-0.025%, and Ti content is 0.015-0.02%.
3. The method for producing multi-specification Q355NE wind power steel according to claim 2, characterized in that, In the roughing stage, when the target steel plate thickness is 8–19 mm, the initial rolling temperature for the first to sixteenth passes is 1023–1137 °C, the roll gap for the first to sixteenth passes is 54–230 mm, the rolling force for the first to sixteenth passes is 10420–34513 KN, the torque for the first to sixteenth passes is 439–3226 rap / min, and the rolling speed for the first to sixteenth passes is 1.5–1.7 m / s.
4. The method for producing multi-specification Q355NE wind power steel according to claim 2, characterized in that, In the roughing stage, when the target steel plate thickness is 20–49 mm, the initial rolling temperature for the first to sixteenth passes is 979–1098 °C, the roll gap for the first to sixteenth passes is 70–305 mm, the rolling force for the first to sixteenth passes is 14788–33089 KN, the torque for the first to sixteenth passes is 1063–3192 rap / min, and the rolling speed for the first to sixteenth passes is 1.5–1.8 m / s.
5. The method for producing multi-specification Q355NE wind power steel according to claim 2, characterized in that, In the roughing stage, when the target steel plate thickness is 50-80mm, the initial rolling temperature for the first to sixteenth passes is 1028-1098℃, the roll gap for the first to sixteenth passes is 115-310mm, the rolling force for the first to sixteenth passes is 17362-32652KN, the torque for the first to sixteenth passes is 967-3154rap / min, and the rolling speed for the first to sixteenth passes is 1.5-1.7m / s.
6. The method for producing multi-specification Q355NE wind power steel according to claim 2, characterized in that, In the finishing rolling process, when the target steel plate thickness is 8-19 mm, the initial rolling temperature for the first to tenth passes is 726-1039℃, the roll gap for the first to sixth passes is 9-50 mm, the rolling force for the first to sixth passes is 24525-39769 KN, the bending roll force for the first to sixth passes is 2000-3328 KN, the rolling speed for the first to sixth passes is 2-3.5 m / s, and the torque for the first to sixth passes is 543-2822 rap / min.
7. A method for producing multi-specification Q355NE wind power steel according to claim 2, characterized in that, In the finishing rolling process, when the target steel plate thickness is 20-49 mm, the initial rolling temperature for the first to tenth passes is 762-885℃, the roll gap for the first to sixth passes is 29-115 mm, the rolling force for the first to sixth passes is 21235-40323 KN, the bending roll force for the first to sixth passes is 2000-3361 KN, the rolling speed for the first to sixth passes is 1.5-3 m / s, and the torque for the first to sixth passes is 953-2760 rap / min.
8. A method for producing multi-specification Q355NE wind power steel according to claim 2, characterized in that, In the finishing rolling process, when the target steel plate thickness is 50-80mm, the initial rolling temperature for the first to tenth passes is 741-815℃, the roll gap for the first to sixth passes is 54-110mm, the rolling force for the first to sixth passes is 34028-47294KN, the bending roll force for the first to sixth passes is 2533-3271KN, the rolling speed for the first to sixth passes is 1.5-2.5m / s, and the torque for the first to sixth passes is 2046-3409rap / min.