A big square billet rolling 55sic alloy steel billet pass system and rolling method
By designing a 9-stand rolling mill pass system and hydraulic motor adjustment, the problems of size switching and center segregation during the rolling process of 55SiCr alloy steel were solved, enabling rapid adjustment of small billets and high-quality finished product production.
Patent Information
- Application Number
- CN202611515803.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-20
AI Technical Summary
The existing die system cannot quickly adapt to the production switching of small square billets with different cross sections, which makes 55SiCr alloy steel prone to folding defects and center segregation during the rolling process, making it difficult to meet the quality standards of high-end spring steel.
A pass system comprising nine rolling mills was designed, which uses hydraulic motors to adjust the pass height and inlet rolling guide opening of each pass to achieve rapid and free switching of small billet size, and improves center segregation through large deformation rolling.
It enables rapid adjustment of small billet size and stable control of finished product quality, reduces folding defects and center segregation, and improves the finished product performance and yield of 55SiCr alloy steel.
Smart Images

Figure CN123128323A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of metal rolling technology, and in particular to a roll pass system and rolling method for rolling small square billets of 55SiCr alloy steel from large square billets. Background Technology
[0002] 55SiCr alloy spring steel is widely used in high-end applications such as automotive suspension springs due to its excellent fatigue resistance and hardenability. Its typical production process is: converter smelting → LF furnace refining → continuous casting of large billets → rolling of large billets into small billets → grinding → wire rod rolling (two-stage forming). Because this steel has a high alloy content, center segregation is prone to occur during continuous casting; and when the Cr mass fraction is greater than 0.60%, the rolling width increase significantly. Therefore, a dedicated die system needs to be designed separately, and the die filling degree of each pass must be strictly controlled below 98% to prevent overfilling and surface defects such as folds.
[0003] There are two main methods for turning large billets into smaller ones: one is to use a reversible billet mill for multi-pass reciprocating rolling; the other is to use a continuous rolling mill for continuous billet rolling. Taking a 300 mm × 390 mm large billet as an example, existing rolling processes and pass systems are mostly designed for carbon steel and low alloy steel, and can usually only produce small billets of single specifications such as 140 mm × 140 mm. When directly used for 55SiCr alloy steel, due to its widening characteristics which differ significantly from ordinary steel grades, the measured maximum pass filling degree can reach over 99%, which easily leads to folding defects due to overfilling, seriously affecting the quality of the finished product.
[0004] Furthermore, the dimensions of the heating furnace and its internal billet load-bearing beams in the downstream wire rod workshop are fixed, making it difficult to freely adjust the billet length. For example, the maximum allowable billet length in a certain wire rod workshop heating furnace is 16.0 m. (Based on the density of 55SiCr being 7.64 g / cm³...) 3 Calculations show that the theoretical weight of a 140mm×140mm square billet at this length is approximately 2.395 t. However, since this steel grade requires two heating, rolling, and grinding processes, the overall yield typically fluctuates between 86% and 92%, and the actual weight of the finished coil is only 2.060-2.203 t, making it difficult to consistently meet the ordering requirement of a coil weight of not less than 2.1 t.
[0005] In summary, the existing technology has the following main shortcomings: Poor flexibility in specification switching: The existing die system cannot quickly adapt to the production switching of small square billets with different cross-sections. When the customer's coil weight requirement varies within the range of 2.1-2.5 t, it is difficult to compensate for the coil weight deviation caused by yield fluctuations by adjusting the billet cross-sectional dimensions; High difficulty in quality control: There is a lack of dedicated die design for the characteristics of 55SiCr high-alloy steel, making it difficult to accurately control the die filling degree, easily causing folding and aggravating center segregation, making it difficult to simultaneously meet high performance and specific coil weight requirements; Limitations of single-fire forming: Although single-fire forming of small square billets can shorten the process, compared with two-fire forming, the degree and fluctuation of center segregation of elements such as C, Mn, and Cr are more significant, and it is often accompanied by internal defects such as center porosity and shrinkage cavities, making it difficult to meet the quality standards of high-end spring steel. Summary of the Invention
[0006] In view of the problems existing in the prior art, this application provides a roll pass system and rolling method for rolling small square billets of 55SiCr alloy steel from large square billets. It has the ability to quickly and freely adjust the size and can effectively control the center segregation level, avoiding the problem of folding defects caused by the large fill degree of the roll pass when rolling 55SiCr alloy steel, so as to meet the different customers' needs for the performance and coil weight of 55SiCr alloy steel.
[0007] To achieve this objective, the following technical solution is adopted in this application:
[0008] In one aspect, this application provides a pass system for rolling small square billets of 55SiCr alloy steel from large square billets. The pass system comprises nine rolling mills connected in sequence. The nine rolling mills alternate between vertical and horizontal rolling, and are respectively referred to as passes 1 to 9 in the rolling sequence, and are respectively called hole 1, hole 2, hole 3, hole 4, hole 5, hole 6, hole 7, hole 8, and hole 9.
[0009] Holes 1, 3, 5, 7, and 9 are square holes, while holes 2, 4, 6, and 8 are box holes.
[0010] Each of the holes 1-9 independently includes:
[0011] The bottom of the groove is a planar structure with a width dimension b. k Corresponding to the side length of the finished square billet;
[0012] The first sidewall and the second sidewall are respectively connected to the two ends of the bottom of the groove and extend outward and upward, and the angle between the first sidewall and the vertical direction is a fixed sidewall angle α.
[0013] And a first fillet and a second fillet, the first fillet connecting the bottom of the groove to the first sidewall, the second fillet connecting the bottom of the groove to the second sidewall, the first fillet and the second fillet having a fixed root arc radius R;
[0014] The slot size B of the hole type k The bottom dimension b of the groove k The sidewall angle α and the groove depth H1 are jointly determined and satisfy the following relationship:
[0015] B k =b k +2H1·tanα;
[0016] The pass system also includes hydraulic motors connected to the nine rolling mills respectively for adjusting the pass height H of the stands.
[0017] This application controls the size of small square billets by adjusting the height of each rolling pass, enabling rapid and free size adjustment, and effectively controlling the center segregation level to meet the different customer requirements for the performance and coil weight of 55SiCr alloy steel. It features low spare parts cost and quick and efficient size adjustment.
[0018] The hydraulic motor with worm gear that adjusts the height H of the hole profile of each frame in this application is controlled by a button.
[0019] As a preferred technical solution of this application, the hole-shaped groove B of holes 1, 2, 3, 4, 5, 6, 7, 8 and 9 is... k The dimensions are as follows: 326.8mm-328.8mm, 378.2mm-380.2mm, 275.6mm-277.6mm, 295.1mm-297.1mm, 232.5mm-234.5mm, 249.7mm-251.7mm, 186.3mm-188.3mm, 203.6mm-205.6mm, and 152.4mm-154.4mm.
[0020] Hole 1 as described in this application has a slot B. k It can be 326.8mm, 327.8mm, 328.8mm, etc., and the hole type slot B of the hole 2. k It can be 378.2mm, 379.2mm, 380.2mm, etc., and the hole type groove B of the hole 3. k It can be 275.6mm, 276.6mm, 277.6mm, etc., and the hole type slot B of the hole 4. k It can be 295.1mm, 296.1mm, 297.1mm, etc., and the hole type slot B of the hole 5. kIt can be 232.5mm, 233.5mm, 234.5mm, etc., and the hole type slot B of the hole 6. k It can be 249.7mm, 250.7mm, 251.7mm, etc., and the hole type groove B of the hole 7. k It can be 186.3mm, 187.3mm, 188.3mm, etc., and the hole type groove B of the hole 8. k It can be 203.6mm, 204.6mm, 205.6mm, etc., and the hole type slot B of the hole 9. k It can be 152.4mm, 153.4mm, 154.4mm, etc., and other unlisted values within the range are also applicable.
[0021] And / or, the bottom dimension b of the slot of holes 1, 2, 3, 4, 5, 6, 7, 8 and 9. k The thicknesses are 303mm-305mm, 351mm-353mm, 244mm-246mm, 271mm-273mm, 207mm-209mm, 225mm-227mm, 166mm-168mm, 185mm-187mm, and 141mm-143mm, respectively.
[0022] The hole 1 described in this application has a groove bottom size b. k The diameter can be 303mm, 304mm, 305mm, etc., and the bottom dimension b of the hole 2 is... k The hole diameter can be 351mm, 352mm, 353mm, etc., and the hole groove bottom size bk of hole 3 can be 244mm, 245mm, 246mm, etc., and the hole groove bottom size b of hole 4... k It can be 271mm, 272mm, 273mm, etc., and the bottom dimension b of the hole 5 is... k The diameter can be 207mm, 208mm, 209mm, etc., and the bottom dimension b of the hole 6 is... k The hole diameter can be 225mm, 226mm, 227mm, etc., and the hole groove bottom size bk of hole 7 can be 166mm, 167mm, 168mm, etc., and the hole groove bottom size b of hole 8... k It can be 185mm, 186mm, 187mm, etc., and the bottom dimension b of the hole 9 is... k It can be 141mm, 142mm, 143mm, etc., and other values not listed within the range are also applicable.
[0023] And / or, the fillet radius R of the groove bottom of holes 1, 2, 3, 4, 5, 6, 7, 8 and 9 are respectively 29mm-31mm, 29mm-31mm, 33mm-35mm, 29mm-31mm, 27mm-29mm, 25mm-27mm, 22mm-24mm, 19mm-21mm and 19mm-21mm.
[0024] The fillet radius R of the groove bottom of hole 1 described in this application can be 29mm, 30mm, 31mm, etc.; the fillet radius R of the groove bottom of hole 2 can be 29mm, 30mm, 31mm, etc.; the fillet radius R of the groove bottom of hole 3 can be 33mm, 34mm, 35mm, etc.; the fillet radius R of the groove bottom of hole 4 can be 29mm, 30mm, 31mm, etc.; the fillet radius R of the groove bottom of hole 5 can be 27mm, 28mm, 29mm, etc.; the fillet radius R of the groove bottom of hole 6 can be 25mm, 26mm, 27mm, etc.; the fillet radius R of the groove bottom of hole 7 can be 22mm, 23mm, 24mm, etc.; the fillet radius R of the groove bottom of hole 8 can be 19mm, 20mm, 21mm, etc.; the fillet radius R of the groove bottom of hole 9 can be 19mm, 20mm, 21mm, etc.; and other values not listed within the numerical range are also applicable.
[0025] As a preferred technical solution of this application, the shape coefficient ξ of holes 1, 2, 3, 4, 5, 6, 7, 8, and 9 is calculated using the following formula: Where H is the height of the pass and B is the width of the rolled piece.
[0026] This application guarantees that the filling degree ω of the roll pass is less than 98% when rolling a small square billet with a maximum size of 145×145mm, thus avoiding folding defects caused by excessive width of 55SiCr alloy steel.
[0027] Taking a typical 140mm square billet as an example, the filling degree ω of holes 1 to 9 are 91.8%, 95.7%, 94.3%, 95.8%, 92.9%, 94.9%, 95.1%, 94.4%, and 92.7%, respectively.
[0028] Taking a typical 143-size small square billet as an example, the filling degree ω of hole type 1 to hole 9 are 91.8%, 95.7%, 94.3%, 95.6%, 93.5%, 95.4%, 96.2%, 96.1%, and 95.3%, respectively.
[0029] Taking a typical 145-size square billet as an example, the filling degree ω of holes 1 to 9 are 91.8%, 95.7%, 94.1%, 95.9%, 94.4%, 95.8%, 97.0%, 97.4%, and 96.6%, respectively.
[0030] The shape coefficient ξ of holes 3, 5, 7 and 9 is independently 0.99-1.06, for example, it can be 0.99, 1.01, 1.03, 1.05 or 1.06, but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0031] And / or, the shape coefficient ξ of holes 2, 4, 6 and 8 is independently 1.39-1.58, for example, it can be 1.39, 1.44, 1.49, 1.54 or 1.58, etc., but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0032] To ensure rolling stability, the shape factor ξ for square holes (holes 3, 5, 7, and 9) is 0.99-1.06, ensuring that the height and width dimensions of the square holes are basically the same; the shape factor ξ for box holes (holes 2, 4, 6, and 8) is 1.39-1.58, to ensure sufficient stability during the rolling process and to prevent torsional deformation.
[0033] As a preferred technical solution of this application, the bottom dimension bk of the groove of holes 1, 2, 3, 4, 5, 6, 7, 8 and 9 satisfies the relationship between b and the width B of the rolled piece entering the groove. k -B=4-16mm. This application uses corner protection rolling. To prevent corners from cracking due to rolling deformation, the bottom dimension b of the groove is... k The relationship between b and the width B of the rolled piece entering the pass shape satisfies k -B=4-16mm ensures that the corners quickly enter the R-corner protection zone after deformation, preventing corner cracks due to rapid cooling. The fillet radius R at the bottom of the groove satisfies R=(0.09-0.16)×H, where H is the hole height.
[0034] And / or, the sidewall angle α in holes 1-8 is independently 9-15°, for example, it can be 9°, 10°, 11°, 12°, 13°, 14° or 15°, etc., and the sidewall angle α in hole 9 is 5°.
[0035] The side wall angle of holes 1-8 in this application is 9-15°. While ensuring the size of the rolled piece, the cost of using the rolls should also be taken into account. The larger the angle, the lower the roll consumption, and the easier it is for the iron oxide scale to fall off. The more irregular the square or box shape of the rolled piece is, the more appropriate it should be. Hole 9 is the finished hole for the intermediate billet, and it is only necessary to ensure that the square shape is regular.
[0036] As a preferred technical solution of this application, the formula for calculating the deformation of holes 1, 2, 3, 4, 5, 6, 7, 8, and 9 is as follows: , where F is the cross-sectional area of the hole and n is the hole number.
[0037] The formula for calculating the cross-sectional area F of the rolled piece mentioned above in this application is as follows: Where F is the cross-sectional area of the rolled piece, in mm. 2 F1 represents the hole area, which is equal to the sum of the areas of the upper and lower grooves of the hole, in mm. 2 H1 is the depth of the hole groove, in mm; B k H1 and B represent the width of the slot, in mm. K The data comes from the die pattern drawing; s is the roll gap, mm; ψ is the area correction factor, ψ=0.987-1.000. The die depth H1 dimension, holes 1 to 9 can be 60.05mm, 70mm, 60.05mm, 70.2mm, 60mm, 60.2mm, 60mm, 60.2mm, and 60.5mm respectively.
[0038] The deformation of holes 3, 5, 7 and 9 is independently 18.1%-21.7%, for example, it can be 18.1%, 19.1%, 20.1%, 21.1% or 21.7%, etc., but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0039] And / or, the deformation of each of the holes 1, 2, 4, 6, and 8 is independently 11.9%-19.8%, for example, it can be 11.9%, 12.9%, 13.9%, 14.9%, 15.9%, 16.9%, 17.9%, 18.9%, or 19.8%, etc., but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0040] When rolling 55SiCr alloy steel, the segregation caused by continuous casting during steelmaking can lead to the formation of flat, round, or strip-shaped segregation zones in the center of the billet. This can be controlled through rolling recrystallization to improve the symmetry and uniformity of the segregation zones, ensuring that the segregation level at the center of the finished product is ≤1 (GB / T 1979). To achieve this, square holes 3, 5, 7, and 9 are rolled with a large deformation of 18.1-21.7%. Taking a typical 140mm small square billet as an example, the deformation ε of holes 3, 5, 7, and 9 are 19.2%, 19.5%, 21.7%, and 18.5%, respectively; taking a typical 143mm small square billet as an example, the deformation ε of holes 3, 5, 7, and 9 are 19.2%, 18.9%, 20.5%, and 18.5%, respectively; taking a typical 145mm small square billet as an example, the deformation ε of holes 3, 5, 7, and 9 are 18.7%, 19.0%, 20.0%, and 18.1%, respectively.
[0041] Secondly, this application provides a rolling method for rolling small square billets of 55SiCr alloy steel from large square billets. The rolling method for rolling small square billets of 55SiCr alloy steel from large square billets adopts the rolling system described in the first aspect, and the rolling method includes the following steps:
[0042] Large square billets are rolled sequentially through holes 1 to 9 into small square billets; wherein, during the rolling process, the specifications of the resulting small square billets are switched by adjusting the rolling speed and hole height of each pass and adjusting the opening degree of the inlet rolling guide.
[0043] The rolling method for rolling 55SiCr alloy steel small square billets provided in this application can achieve rapid and free switching between small square billet sizes of 140-145mm simply by adjusting the height H of the pass profiles on each stand, thereby controlling the weight of the finished coil.
[0044] In the rolling method for rolling 55SiCr alloy steel small square billets from large square billets described in this application, the specific method for adjusting the opening degree of the inlet rolling guide is as follows: according to the actual pass height H of each pass, adjust the guide symmetrically and ensure that its center coincides with the pass center. After locking, re-measure the opening degree and centering. During trial rolling, observe the bite, deviation, torsion and scratches, and then make fine adjustments until the rolling is stable.
[0045] Before rolling, the large square billet is first sent to a heating furnace for heating, and the heating temperature should be greater than 1150℃ and the initial rolling temperature should be greater than 1000℃.
[0046] When switching from producing 140mm small square billets to 143mm small square billets, rolling should be stopped, the roll pass height and rolling speed of the mill should be reset, and the opening of the inlet rolling guides should be adjusted. After completing the above work, the mill should be restarted. The above steps should be repeated when switching from producing 143mm small square billets to 145mm small square billets. The billet size switching should be organized in order from smallest to largest or from largest to smallest to maintain production stability.
[0047] As a preferred technical solution of this application, the size of the large square billet is 300-320mm×380-400mm, for example, it can be 300×380mm, 320mm×400mm, 320mm×380mm, 300mm×400mm or 310mm×390mm, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0048] And / or, the size of the small square billet is 140-145mm×140-145mm, for example, it can be 140mm×140mm, 145mm×145mm, 140mm×145mm, 145mm×140mm or 142mm×143mm, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0049] When the size of the small square billet described in this application is 140mm×140mm, the hole height H of holes 1 to 9 are 345mm, 230mm, 260mm, 200mm, 210mm, 160mm, 168mm, 129mm, and 142.5mm respectively.
[0050] And / or, when the size of the small square billet is 143mm×143mm, the hole height H of holes 1 to 9 is 345mm, 230mm, 260mm, 202mm, 212mm, 163mm, 173mm, 134mm, and 146.0mm respectively; when the size of the small square billet is 145mm×145mm, the hole height H of holes 1 to 9 is 345mm, 230mm, 262mm, 204mm, 213mm, 165mm, 176mm, 136mm, and 148.5mm respectively.
[0051] As a preferred technical solution of this application, the formula for calculating the pass filling degree ω of each pass in the rolling process is: ω=B / B k Where B is the width of the rolled piece, B k This refers to the size of the slot.
[0052] As a preferred technical solution of this application, the calculation formula for the rolling speed of each pass in the rolling process is as follows: , where V n-1 V is the rolling speed of the previous rolling mill. n μ represents the rolling speed of the current stand rolling mill. n This represents the elongation coefficient of the current stand rolling mill.
[0053] As a preferred technical solution of this application, the formula for calculating the elongation coefficient μ of each pass in the rolling process is as follows: , of which F n F represents the cross-sectional area of the rolled piece for the current die type. n+1 This represents the cross-sectional area of the rolled piece for the next pass.
[0054] Compared with existing technical solutions, this application has at least the following beneficial effects:
[0055] (1) The roll pass system for rolling 55SiCr alloy steel small square billets from large square billets provided in this application can continuously roll out small square billets of various billet shapes using a single roll pass system. The spare parts cost is low, and the specification change is simple and efficient.
[0056] (2) The die-cutting method for rolling 55SiCr alloy steel small square billets from large square billets provided in this application can achieve rapid specification switching within the range of 140-145mm×140-145mm, meet the customer's requirements for coil weight, and improve the center segregation of chemical elements by rolling the large deformation of the square die during the rolling process of small square billets through two-fired forming, ensuring that the center segregation level of the finished product is ≤1 grade (GB / T 1979), reducing the breakage in the spring manufacturing process, improving the strength and toughness of 55SiCr alloy steel wire, and making the spring products have good market competitiveness. Attached Figure Description
[0057] Figure 1 This is a layout diagram of the roll pass system for rolling 55SiCr alloy steel into small square billets from large square billets, as provided in this application.
[0058] Figures 2-10 This is a diagram of the hole type system (holes 1-9) for rolling 55SiCr alloy steel into small square billets from large square billets, as provided in Embodiment 1 of this application.
[0059] Figure 11 This is a sample image of a 140mm×140mm 55SiCr alloy steel small square billet, as provided in Example 1 of this application, for low-magnification acid leaching test. The left side is random sample 1, and the right side is random sample 2. Detailed Implementation
[0060] To facilitate understanding of this application, the following embodiments are provided. Those skilled in the art should understand that these embodiments are merely illustrative and should not be construed as limiting the scope of this application.
[0061] It should be clarified that any use of the process provided in the embodiments of this application or any substitution or change of conventional data falls within the protection and disclosure scope of this application.
[0062] Example 1
[0063] This embodiment provides a pass system and method for rolling a 300mm×390mm large square billet into a 140mm×140mm 55SiCr alloy steel small square billet. The pass system includes nine rolling mills connected in sequence. The nine rolling mills alternate between vertical and horizontal rolling, and are numbered from the first to the ninth pass according to the rolling sequence, and are respectively called hole 1, hole 2, hole 3, hole 4, hole 5, hole 6, hole 7, hole 8, and hole 9.
[0064] Holes 1, 3, 5, 7, and 9 are square holes, while holes 2, 4, 6, and 8 are box holes.
[0065] Each of the holes 1-9 independently includes:
[0066] The bottom of the groove is a planar structure with a width dimension b. k Corresponding to the side length of the finished square billet;
[0067] The first sidewall and the second sidewall are respectively connected to the two ends of the bottom of the groove and extend outward and upward, and the angle between the first sidewall and the vertical direction is a fixed sidewall angle α.
[0068] And a first fillet and a second fillet, the first fillet connecting the bottom of the groove to the first sidewall, the second fillet connecting the bottom of the groove to the second sidewall, the first fillet and the second fillet having a fixed root arc radius R;
[0069] The slot size B of the hole type k The bottom dimension b of the groove k The sidewall angle α and the groove depth H1 are jointly determined and satisfy the following relationship:
[0070] B k =b k +2H1·tanα;
[0071] The pass system also includes hydraulic motors connected to the nine rolling mills respectively for adjusting the pass height H of the stands;
[0072] The sidewall angle α of holes 1-8 is 15°, and the sidewall angle α of hole 9 is 5°;
[0073] The slot B of holes 1, 2, 3, 4, 5, 6, 7, 8 and 9 k The dimensions are 327.8mm, 379.2mm, 276.6mm, 296.1mm, 233.5mm, 250.7mm, 187.3mm, 204.6mm, and 153.4mm, respectively.
[0074] The bottom dimension b of the groove of holes 1, 2, 3, 4, 5, 6, 7, 8 and 9 k The thicknesses are 304mm, 352mm, 245mm, 272mm, 208mm, 226mm, 167mm, 186mm, and 142mm, respectively.
[0075] The fillet radius R of the groove bottom of holes 1, 2, 3, 4, 5, 6, 7, 8 and 9 are 30mm, 30mm, 34mm, 30mm, 28mm, 26mm, 23mm, 20mm and 20mm respectively.
[0076] The shape factor ξ of holes 3, 5, 7 and 9 is 1.02, and the shape factor ξ of holes 2, 4, 6 and 8 is 1.48.
[0077] The filling degree ω of the holes 1 to 9 are 91.8%, 95.7%, 94.3%, 95.8%, 92.9%, 94.9%, 95.1%, 94.4%, and 92.7%, respectively.
[0078] The deformation amounts of holes 3, 5, 7, and 9 are 18.1%, 19.2%, 20.0%, and 21.7%, respectively, while the deformation amounts of holes 1, 2, 4, 6, and 8 are 11.9%, 19.8%, 16.4%, 16.9%, and 16.2%, respectively.
[0079] Holes 1-9 adopt a universal design, and there is no need to change the hole type. The size of the small billet can be freely switched by simply adjusting the height H of the hole type of each frame through the hydraulic motor.
[0080] The rolling method employs the aforementioned pass system and includes: rolling a 300mm × 390mm large square billet sequentially through passes 1 to 9 into a 140mm × 140mm small square billet. The height H and rolling speed V of each pass are shown in Table 1.
[0081]
[0082] The results of the low-magnification acid leaching test (a mixed solution of 4% nitric acid and alcohol by volume) of the finished small square billet obtained in this embodiment are shown in the figure below. Figure 11 The left side is random sample 1, and the right side is random sample 2; the test method is YB / T 4413-2014 Metallographic evaluation method for center segregation of high carbon steel wire rod; the test results are: the segregation level of random sample 1 is close to 0, and the segregation level of random sample 2 is < 1.
[0083] Example 2
[0084] This embodiment provides a pass system and method for rolling a 300mm×390mm large square billet into a 143mm×143mm 55SiCr alloy steel small square billet. The pass system includes nine rolling mills connected in sequence. The nine rolling mills alternate between vertical and horizontal rolling, and are numbered from the first to the ninth pass according to the rolling sequence, and are respectively called hole 1, hole 2, hole 3, hole 4, hole 5, hole 6, hole 7, hole 8, and hole 9.
[0085] Each of the holes 1-9 independently includes:
[0086] The bottom of the groove is a planar structure with a width dimension b. k Corresponding to the side length of the finished square billet;
[0087] The first sidewall and the second sidewall are respectively connected to the two ends of the bottom of the groove and extend outward and upward, and the angle between the first sidewall and the vertical direction is a fixed sidewall angle α.
[0088] And a first fillet and a second fillet, the first fillet connecting the bottom of the groove to the first sidewall, the second fillet connecting the bottom of the groove to the second sidewall, the first fillet and the second fillet having a fixed root arc radius R;
[0089] The slot size B of the hole type k The bottom dimension b of the groove k The sidewall angle α and the groove depth H1 are jointly determined and satisfy the following relationship:
[0090] B k =b k +2H1·tanα;
[0091] The pass system also includes hydraulic motors connected to the nine rolling mills respectively for adjusting the pass height H of the stands;
[0092] The sidewall angle α of holes 1-8 is 9°, and the sidewall angle α of hole 9 is 5°;
[0093] The slot B of holes 1, 2, 3, 4, 5, 6, 7, 8 and 9 k The dimensions are 327.8mm, 379.2mm, 276.6mm, 296.1mm, 233.5mm, 250.7mm, 187.3mm, 204.6mm, and 153.4mm, respectively.
[0094] The bottom dimension b of the groove of holes 1, 2, 3, 4, 5, 6, 7, 8 and 9 k The thicknesses are 304mm, 352mm, 245mm, 272mm, 208mm, 226mm, 167mm, 186mm, and 142mm, respectively.
[0095] The fillet radius R of the groove bottom of holes 1, 2, 3, 4, 5, 6, 7, 8 and 9 are 30mm, 30mm, 34mm, 30mm, 28mm, 26mm, 23mm, 20mm and 20mm respectively.
[0096] The shape factor ξ of holes 3, 5, 7 and 9 is 1.02, and the shape factor ξ of holes 2, 4, 6 and 8 is 1.48.
[0097] The filling degree ω of the holes 1 to 9 are 91.8%, 95.7%, 94.3%, 95.6%, 93.5%, 95.4%, 96.2%, 96.1%, and 95.3%, respectively.
[0098] The deformation amounts of holes 3, 5, 7, and 9 are 18.1%, 19.2%, 20.0%, and 21.7%, respectively, while the deformation amounts of holes 1, 2, 4, 6, and 8 are 11.9%, 19.8%, 15.4%, 16.9%, and 16%, respectively.
[0099] Holes 1-9 adopt a universal design, and there is no need to change the hole type. The size of the small billet can be freely switched by simply adjusting the height H of the hole type of each frame through the hydraulic motor.
[0100] The rolling method employs the aforementioned pass system and includes: rolling a 300mm × 390mm large square billet sequentially through passes 1 to 9 into a 143mm × 143mm small square billet. The height H and rolling speed V of each pass are shown in Table 2.
[0101]
[0102] Example 3
[0103] This embodiment provides a pass system and method for rolling a 300mm×390mm large square billet into a 145mm×145mm 55SiCr alloy steel small square billet. The pass system includes nine rolling mills connected in sequence. The nine rolling mills alternate between vertical and horizontal rolling, and are numbered from the first to the ninth pass according to the rolling sequence, and are respectively called hole 1, hole 2, hole 3, hole 4, hole 5, hole 6, hole 7, hole 8, and hole 9.
[0104] Holes 1, 3, 5, 7, and 9 are square holes, while holes 2, 4, 6, and 8 are box holes.
[0105] Each of the holes 1-9 independently includes:
[0106] The bottom of the groove is a planar structure with a width dimension b. k Corresponding to the side length of the finished square billet;
[0107] The first sidewall and the second sidewall are respectively connected to the two ends of the bottom of the groove and extend outward and upward, and the angle between the first sidewall and the vertical direction is a fixed sidewall angle α.
[0108] And a first fillet and a second fillet, the first fillet connecting the bottom of the groove to the first sidewall, the second fillet connecting the bottom of the groove to the second sidewall, the first fillet and the second fillet having a fixed root arc radius R;
[0109] The slot size B of the hole type k The bottom dimension b of the groove k The sidewall angle α and the groove depth H1 are jointly determined and satisfy the following relationship:
[0110] B k =b k +2H1·tanα;
[0111] The pass system also includes hydraulic motors connected to the nine rolling mills respectively for adjusting the pass height H of the stands;
[0112] The sidewall angle α of holes 1-8 is 13°, and the sidewall angle α of hole 9 is 5°;
[0113] The slot B of holes 1, 2, 3, 4, 5, 6, 7, 8 and 9 k The dimensions are 327.8mm, 379.2mm, 276.6mm, 296.1mm, 233.5mm, 250.7mm, 187.3mm, 204.6mm, and 153.4mm, respectively.
[0114] The bottom dimension b of the groove of holes 1, 2, 3, 4, 5, 6, 7, 8 and 9 k The thicknesses are 304mm, 352mm, 245mm, 272mm, 208mm, 226mm, 167mm, 186mm, and 142mm, respectively.
[0115] The fillet radius R of the groove bottom of holes 1, 2, 3, 4, 5, 6, 7, 8 and 9 are 30mm, 30mm, 34mm, 30mm, 28mm, 26mm, 23mm, 20mm and 20mm respectively.
[0116] The shape factor ξ of holes 3, 5, 7 and 9 is 1.02, and the shape factor ξ of holes 2, 4, 6 and 8 is 1.48.
[0117] The filling degree ω of the holes 1 to 9 are 91.8%, 95.7%, 94.1%, 95.9%, 94.4%, 95.8%, 97.0%, 97.4%, and 96.6%, respectively.
[0118] The deformation amounts of holes 3, 5, 7, and 9 are 18.1%, 19.2%, 20.0%, and 21.7%, respectively, while the deformation amounts of holes 1, 2, 4, 6, and 8 are 11.9%, 19.8%, 15.2%, 16%, and 15.2%, respectively.
[0119] Holes 1-9 adopt a universal design, and there is no need to change the hole type. The size of the small billet can be freely switched by simply adjusting the height H of the hole type of each frame through the hydraulic motor.
[0120] The rolling method employs the aforementioned pass system and includes: rolling a 300mm×390mm large square billet sequentially through passes 1 to 9 into a 145mm×145mm small square billet. The height H and rolling speed V of each pass are shown in Table 3.
[0121]
[0122] Example 4
[0123] This embodiment provides a die system and method for rolling a 300mm×390mm large square billet into a 140mm×140mm 55SiCr alloy steel small square billet. The only difference between the die system and that in Embodiment 1 is that the filling degree ω of holes 1 to 9 is changed to 99%, and the rest is the same as in Embodiment 1.
[0124] Example 5
[0125] This embodiment provides a die system and method for rolling a 300mm×390mm large square billet into a 140mm×140mm 55SiCr alloy steel small square billet. The only difference between the die system and that in Embodiment 1 is the bottom dimension b of the groove for holes 1, 2, 3, 4, 5, 6, 7, 8, and 9. k The width B of the rolled piece entering the pass is changed to satisfy b. k -B=2mm, and the rest are the same as in Example 1.
[0126] Example 6
[0127] This embodiment provides a die system and method for rolling a 300mm×390mm large square billet into a 140mm×140mm 55SiCr alloy steel small square billet. The only difference between the die system and that in Embodiment 1 is the bottom dimension b of the groove for holes 1, 2, 3, 4, 5, 6, 7, 8, and 9. k The width B of the rolled piece entering the pass is changed to satisfy b. k -B=18mm, and the rest are the same as in Example 1.
[0128] Example 7
[0129] This embodiment provides a die system and method for rolling a 300mm×390mm large square billet into a 140mm×140mm 55SiCr alloy steel small square billet. The only difference between the die system and that in Embodiment 1 is that the deformation of holes 3, 5, 7 and 9 is changed to 15%, while the rest are the same as in Embodiment 1.
[0130] Example 8
[0131] This embodiment provides a die system and method for rolling a 300mm×390mm large square billet into a 140mm×140mm 55SiCr alloy steel small square billet. The only difference between the die system and that in Embodiment 1 is that the deformation of holes 3, 5, 7 and 9 is changed to 25%, while the rest are the same as in Embodiment 1.
[0132] Performance testing
[0133] The examples used the provided 55SiCr alloy steel small square billets to test the deliverable coil weight, finished product center segregation grade, crack ratio, and grinding ratio. The delivery coil weight test method was as follows: the maximum billet length in the downstream workshop was 16.0 meters, and the density was 7.64 g / cm³. 3 The yield rate is calculated as 86%-92%; the center segregation grade of the finished product is based on GB / T 1979; the test method for the center segregation grade of the finished product is YB / T 4413-2014 Metallographic Evaluation Method for Center Segregation of High Carbon Steel Wire Rod; the eddy current testing method is GB / T 30565-2025 General Rules for Eddy Current Testing in Nondestructive Testing.
[0134] The results are shown in Table 4.
[0135]
[0136] As can be seen from Table 4, the roll pass system and rolling method for rolling 55SiCr alloy steel small square billets from large square billets provided in this application can meet the customer's requirement of coil weight ≥2.0t and the center segregation level of finished wire rod ≤1. Furthermore, it can meet the requirement of the number of eddy current inspection points per coil after the increase in coil weight (standard: number of inspection alarm points ≤15 / coil).
[0137] A comprehensive comparison of Examples 1 and 4-8 shows that the 55SiCr alloy spring steel produced using this method can meet various customer requirements regarding coil weight and reduce processing costs for downstream users. The 55SiCr alloy spring steel produced using this method can control the center segregation level of the finished product to ≤1 level, and the number of eddy current testing points per coil to ≤15, ensuring the fatigue resistance and hardenability of the 55SiCr alloy spring steel, and adapting it to the usage requirements of various parts.
[0138] This application illustrates its detailed structural features through the above embodiments, but it is not limited to these detailed structural features, meaning that this application does not necessarily rely on them for implementation. Those skilled in the art should understand that any improvements to this application, equivalent substitutions of selected components, additions of auxiliary components, and selection of specific methods all fall within the protection and disclosure scope of this application.
Claims
1. A roll pass system for rolling small square billets of 55SiCr alloy steel from large square billets, characterized in that, The pass system includes nine rolling mills connected in sequence on the rolls. The nine rolling mills alternate between vertical and horizontal rolling, and are numbered from the first pass to the ninth pass according to the rolling sequence. They are respectively called hole 1, hole 2, hole 3, hole 4, hole 5, hole 6, hole 7, hole 8, and hole 9. Holes 1, 3, 5, 7, and 9 are square holes, while holes 2, 4, 6, and 8 are box holes. Each of the holes 1-9 independently includes: The bottom of the groove is a planar structure with a width dimension b. k Corresponding to the side length of the finished square billet; The first sidewall and the second sidewall are respectively connected to the two ends of the bottom of the groove and extend outward and upward, and the angle between the first sidewall and the vertical direction is a fixed sidewall angle α. And a first fillet and a second fillet, the first fillet connecting the bottom of the groove to the first sidewall, the second fillet connecting the bottom of the groove to the second sidewall, the first fillet and the second fillet having a fixed root arc radius R; The slot size B of the hole type k The bottom dimension b of the groove k The sidewall angle α and the groove depth H1 are jointly determined and satisfy the following relationship: B k =b k +2H1·tanα; The pass system also includes hydraulic motors connected to the nine rolling mills respectively for adjusting the pass height H of the stands.
2. The hole pattern system according to claim 1, characterized in that, The slot B of holes 1, 2, 3, 4, 5, 6, 7, 8 and 9 k The dimensions are as follows: 326.8mm-328.8mm, 378.2mm-380.2mm, 275.6mm-277.6mm, 295.1mm-297.1mm, 232.5mm-234.5mm, 249.7mm-251.7mm, 186.3mm-188.3mm, 203.6mm-205.6mm, and 152.4mm-154.4mm. And / or, the bottom dimension b of the slot of holes 1, 2, 3, 4, 5, 6, 7, 8 and 9. k The following are the thicknesses in order: 303mm-305mm, 351mm-353mm, 244mm-246mm, 271mm-273mm, 207mm-209mm, 225mm-227mm, 166mm-168mm, 185mm-187mm, and 141mm-143mm. And / or, the fillet radius R of the groove bottom of holes 1, 2, 3, 4, 5, 6, 7, 8 and 9 are respectively 29mm-31mm, 29mm-31mm, 33mm-35mm, 29mm-31mm, 27mm-29mm, 25mm-27mm, 22mm-24mm, 19mm-21mm and 19mm-21mm.
3. The hole pattern system according to claim 1 or 2, characterized in that, The formula for calculating the shape factor ξ of holes 1, 2, 3, 4, 5, 6, 7, 8, and 9 is as follows: Where H is the height of the pass and B is the width of the rolled piece; The shape coefficient ξ of holes 3, 5, 7 and 9 is independently 0.99-1.06; And / or, the shape coefficient ξ of holes 2, 4, 6 and 8 is independently 1.39-1.
58.
4. The hole pattern system according to any one of claims 1 to 3, characterized in that, The bottom dimension b of the groove of holes 1, 2, 3, 4, 5, 6, 7, 8 and 9 k The relationship between b and the width B of the rolled piece entering the pass shape satisfies k -B = 4-16mm; And / or, the sidewall angle α in holes 1-8 is independently 9-15°, and the sidewall angle α in hole 9 is 5°.
5. The hole pattern system according to any one of claims 1 to 4, characterized in that, The formula for calculating the deformation of holes 1, 2, 3, 4, 5, 6, 7, 8, and 9 is as follows: Where F is the cross-sectional area of the aperture and n is the aperture number; The deformation of holes 3, 5, 7, and 9 is independently 18.1%-21.7%; And / or, the deformation of each of the holes 1, 2, 4, 6 and 8 is independently 11.9%-19.8%.
6. A rolling method for producing small square billets of 55SiCr alloy steel from large square billets, wherein the rolling method employs the die system described in any one of claims 1 to 5, characterized in that, The rolling method includes the following steps: Large square billets are rolled sequentially through holes 1 to 9 into small square billets; wherein, during the rolling process, the specifications of the resulting small square billets are switched by adjusting the rolling speed and hole height of each pass and adjusting the opening degree of the inlet rolling guide.
7. The rolling method according to any one of claims 6, characterized in that, The dimensions of the large square billet are 300-320mm × 380-400mm; And / or, the dimensions of the small square billet are 140-145mm × 140-145mm.
8. The rolling method according to claim 6 or 7, characterized in that, The formula for calculating the pass filling degree ω in each pass of the rolling process is: ω = B / B k Where B is the width of the rolled piece, B k This refers to the size of the slot; And / or, the pass filling degree ω of each pass in the rolling process is less than 98%.
9. The rolling method according to any one of claims 6 to 8, characterized in that, The formula for calculating the rolling speed of each pass in the rolling process is as follows: , where V n-1 V is the rolling speed of the previous rolling mill. n μ represents the rolling speed of the current stand rolling mill. n This represents the elongation coefficient of the current stand rolling mill.
10. The rolling method according to any one of claims 6 to 9, characterized in that, The formula for calculating the elongation coefficient μ of each pass in the rolling process is as follows: , of which F n F represents the cross-sectional area of the rolled piece for the current die type. n+1 This represents the cross-sectional area of the rolled piece for the next pass.