A process for the production of aluminium alloy structural sections
By employing a multi-stage homogenization heat treatment process, gradient heating, and differentiated cooling, the problem of independent design in each stage of aluminum alloy profile production was solved, resulting in a significant improvement in the overall mechanical properties of aluminum alloy profiles.
Patent Information
- Application Number
- CN202611251584.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-18
- Publication Date
- 2026-11-20
AI Technical Summary
In the existing aluminum alloy profile production process, the ingot homogenization, cooling and aging treatment are designed independently without systematic coordination, resulting in uneven diffusion, uneven cooling and poor distribution of precipitated phases, which limits the improvement of the profile's comprehensive mechanical properties.
By employing a multi-stage homogenization heat treatment, gradient heating, differentiated quenching, and three-stage aging process, combined with pre-deformation and controllable cooling, the comprehensive mechanical properties of aluminum alloy profiles are improved.
Through multi-stage homogenization heat treatment and differentiated cooling, the precipitates in aluminum alloy profiles exhibit high density, fine size, and uniform distribution, achieving a synergistic superposition of fine grain strengthening, strain strengthening, and precipitate strengthening, significantly improving the comprehensive mechanical properties of the profiles.
Smart Images

Figure CN123128345A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of aluminum alloy processing technology, and specifically to a production process for aluminum alloy industrial profiles. Background Technology
[0002] Aluminum alloy profiles are widely used in aerospace, rail transportation, automobile manufacturing, and building structures due to their high specific strength, excellent corrosion resistance, and good formability. Current engineering demands for lightweighting and high performance are continuously increasing, leading to a trend towards larger, more complex, and thinner-walled industrial aluminum alloy profiles, which places higher demands on the balance between strength and toughness.
[0003] For heat-treatable aluminum alloys such as the 6XXX series (with magnesium and silicon as the main alloying elements, forming the Mg2Si strengthening phase) and the 7XXX series (with zinc as the main alloying element, usually with the addition of magnesium or copper), their final mechanical properties mainly depend on three key aspects: the quality of ingot homogenization treatment, the degree of preservation of solid solution supersaturation, and the effect of aging precipitation strengthening. In traditional manufacturing processes, these three aspects are designed and controlled independently. Homogenization treatment focuses on compositional homogenization, online quenching focuses on cooling rate and deformation control, and aging treatment focuses on temperature and time parameters, lacking a systematic and coordinated design among them. This segmented and isolated process design approach prevents the strengthening potential of each aspect from being fully explored and superimposed, limiting further improvement in the overall mechanical properties of the profiles.
[0004] Specifically, during the homogenization process, under traditional single-stage or two-stage isothermal holding conditions, slow-diffusing elements such as Cu, Zn, and Mn cannot achieve a completely uniform distribution within a finite time. Dendritic segregation and coarse eutectic phase residues cannot be completely eliminated during subsequent extrusion and heat treatment, becoming inherent structural defects that hinder performance improvement. Although multi-stage homogenization has been studied, the temperature and time parameters for each stage are mostly determined empirically, lacking precise control over diffusion kinetics. More importantly, in existing processes, diffusion relies solely on lattice diffusion driven by concentration gradients, which is limited by the lattice self-diffusion activation energy, making it difficult to achieve complete homogenization within industrial aging time.
[0005] In terms of cooling, traditional water-cooling or air-cooling methods cannot achieve differentiated cooling for complex cross-sections with significant differences in wall thickness: thick-walled areas cool slowly, resulting in insufficient supersaturation of the solid solution and reduced subsequent aging strengthening effect; thin-walled areas cool too quickly, leading to excessive residual stress and deformation after quenching. Regarding aging treatment, under a single temperature field-driven precipitation mode, it is difficult to achieve optimal precipitate nucleation density, uniformity of distribution, and crystallographic orientation. Summary of the Invention
[0006] The present invention aims to provide a production process for aluminum alloy industrial profiles, which achieves synergistic strengthening through deformation heat treatment to significantly improve the overall mechanical properties of the profiles.
[0007] To achieve the above objectives, this application provides the following technical solution: A manufacturing process for aluminum alloy industrial profiles includes the following steps: S1. Homogenization heat treatment: The aluminum alloy ingot is subjected to the first stage of homogenization, the second stage of homogenization, intermediate cooling and pre-deformation, the third stage of homogenization and final cooling in sequence. The process involves the following steps: the first homogenization stage involves heating the ingot to 420–450 °C at a rate of 20–40 °C / h and holding it at that temperature for 2–4 h; the second homogenization stage involves heating the ingot to 460–490 °C at a rate of 15–30 °C / h and holding it at that temperature for 4–6 h; the intermediate cooling and pre-deformation stage involves cooling the ingot to 200–250 °C at a rate of 40–60 °C / h, and applying a 0.5%–1.5% compression pre-deformation at this temperature; the third homogenization stage involves heating the ingot to 530–560 °C at a rate of 20–40 °C / h and holding it at that temperature for 4–8 h; and the final cooling stage involves cooling the ingot to room temperature at a rate of 50–80 °C / h. S2, Gradient heating: The ingot after S1 homogenization treatment is subjected to gradient heating to the extrusion temperature; S3, Extrusion molding: The ingot heated by gradient S2 is extruded to obtain an aluminum alloy profile with a predetermined cross-sectional shape; S4. Quenching: The profile after extrusion in step S3 is quenched online; the profile has a length direction along the extrusion direction and a cross-sectional direction perpendicular to the extrusion direction; the online quenching is set with multiple quenching sections along the length direction of the profile, and different cooling intensities are set according to the wall thickness difference of the profile cross-section within the same quenching section. S5. Stretch straightening: Stretch straightening is performed on the profiles after S4 quenching.
[0008] As a preferred embodiment, for thick-walled regions with a wall thickness ≥ 5 mm in the profile cross-section, the cooling rate is 20–35 ℃ / s; for medium-thickness regions with a wall thickness of 2–5 mm in the profile cross-section, the cooling rate is 10–20 ℃ / s; and for thin-walled regions with a wall thickness ≤ 2 mm in the profile cross-section, the cooling rate is 5–10 ℃ / s.
[0009] In some embodiments, the temperature difference between different parts of the profile cross section at the end of quenching does not exceed 30°C.
[0010] Furthermore, in step S1, the pre-deformation is achieved by applying axial compression to the ingot using a hydraulic press, and the ingot temperature is maintained at 200–250 °C during the pre-deformation process.
[0011] As a preferred embodiment, the aluminum alloy is a 6XXX series aluminum alloy containing Zn or a 7XXX series aluminum alloy.
[0012] In the optimized version, in step S1, the compression pre-deformation amount is 0.5% to 1.5% of the ingot length.
[0013] As a preferred embodiment, in step S4, the cross-sectional differential cooling is achieved by setting an independent control valve on the cooling medium nozzle of the quenching device, and adjusting the cooling medium flow rate and pressure of each nozzle according to the wall thickness distribution of the profile cross-section.
[0014] As a preferred embodiment, in step S5, the stretching amount of the stretching straightening is 0.5% to 2.0%.
[0015] As a preferred embodiment, the process also includes step S6, which involves subjecting the profile after stretching and straightening in step S5 to a three-stage aging treatment; the three-stage aging treatment includes, in sequence: First-stage aging treatment: heat preservation at 60-90℃ for 4-8 hours, while applying mechanical vibration with a frequency of 20-50 Hz and an amplitude of 0.1-0.5 mm; Second-stage aging treatment: keep at 120-160℃ for 6-12 hours, while applying uniaxial tensile stress of 50-100 MPa; Third-level aging treatment: Keep at 170-200℃ for 4-10 hours without applying external force.
[0016] Working principle and beneficial effects of the present invention: The aluminum alloy profiles prepared by this invention exhibit high-density, fine, and uniformly distributed precipitates, which also possess a preferred orientation along specific crystal planes. The microstructure contains coherent or semi-coherent interface structures between dislocations and precipitates, achieving a synergistic superposition of grain refinement strengthening, strain strengthening, and precipitate strengthening. Attached Figure Description
[0017] Figure 1 A process flow diagram was generated for this application. Detailed Implementation
[0018] The following detailed description illustrates the specific implementation method: Example 1: Taking 6XXX series Zn-containing aluminum alloy as an example, the chemical composition of the ingot is: Zn 1.2wt%, Mg 1.0wt%, Si 0.8wt%, Cu 0.5wt%, with the balance being Al and unavoidable impurities.
[0019] S1. Pre-deformation coupled multi-segment stepped homogenization heat treatment: First stage homogenization: Heat to 435℃ at a heating rate of 30℃ / h and hold for 3h; Second stage homogenization: Heat to 475℃ at a heating rate of 20℃ / h and hold for 5h; Intermediate cooling and pre-deformation: The temperature is reduced to 220℃ at a cooling rate of 50℃ / h, and axial compression pre-deformation is applied to the ingot using a hydraulic press. The pre-deformation amount is 1.0% of the ingot length. The third stage of homogenization: the temperature is increased to 545℃ at a heating rate of 30℃ / h and held for 6h; Final cooling: Cooling to room temperature at a cooling rate of 65℃ / h.
[0020] S2. Gradient heating: The ingot, after being homogenized by S1, is gradually heated to the extrusion temperature.
[0021] S3. Extrusion molding: The ingot heated by gradient S2 is extruded to obtain an aluminum alloy profile with a predetermined cross-sectional shape.
[0022] S4. Controllable quenching stress field, constructive cross-section differential online quenching: Thick-walled areas with a wall thickness ≥ 5 mm in the profile section are cooled by strong water mist at a rate of 28℃ / s. Medium wall thickness areas with a wall thickness of 2-5 mm are cooled by air mist at a rate of 15℃ / s. Thin-walled areas with a wall thickness of ≤2mm are cooled by air at a rate of 8℃ / s. The temperature difference between different parts of the cross section at the end of quenching is 25℃.
[0023] S5. Stretch straightening: Stretch amount is 1.2%.
[0024] S6. Level 3 Time-Constraint Processing: First-level aging: heat preservation at 75℃ for 6 hours, while applying mechanical vibration with a frequency of 35Hz and an amplitude of 0.3mm; Second-stage aging: heat preservation at 140℃ for 9 hours, while applying uniaxial tensile stress of 75MPa; Level 3 aging: Keep warm at 185℃ for 7 hours without applying any external force.
[0025] Testing showed that the aluminum alloy profile prepared in Example 1 had a tensile strength of 425 MPa, a yield strength of 390 MPa, and an elongation after fracture of 10.5%.
[0026] Example 2: Taking 7XXX series aluminum alloy as an example, the chemical composition of the ingot is: Zn 1.8wt%, Mg 1.3wt%, Si 0.5wt%, Cu 0.6wt%, with the balance being Al and unavoidable impurities.
[0027] S1. Pre-deformation coupled multi-segment stepped homogenization heat treatment: First stage homogenization: Heat to 440℃ at a heating rate of 25℃ / h and hold for 3.5h; Second stage homogenization: Heat to 485℃ at a heating rate of 25℃ / h and hold for 5.5h; Intermediate cooling and pre-deformation: The temperature is reduced to 235℃ at a cooling rate of 45℃ / h, and axial compression pre-deformation is applied to the ingot using a hydraulic press. The pre-deformation amount is 1.3% of the ingot length. The third stage of homogenization: the temperature is increased to 555℃ at a heating rate of 35℃ / h and held for 7h. Final cooling: Cooling to room temperature at a rate of 70℃ / h.
[0028] Steps S2-S5 are the same as in Example 1.
[0029] S6. Level 3 Time-Constraint Processing: First-level aging: Keep at 80℃ for 5 hours, while applying mechanical vibration with a frequency of 40Hz and an amplitude of 0.25mm; Second-stage aging: heat preservation at 150℃ for 8 hours, while applying uniaxial tensile stress of 85MPa; Level 3 aging: Keep warm at 190℃ for 6 hours without applying any external force.
[0030] Testing showed that the aluminum alloy profile prepared in this embodiment had a tensile strength of 550 MPa, a yield strength of 510 MPa, and an elongation after fracture of 9.0%.
[0031] Comparative Example 1: Traditional single-stage homogenization (545℃×8h) + traditional water-cooled quenching + traditional single-stage aging (175℃×8h) was adopted, and the other conditions were the same as those in Example 1 (the traditional water-cooled quenching specifically refers to: immersing the extruded high-temperature profile directly into a room temperature water bath for overall immersion quenching, or using a high-pressure water curtain to spray the entire cross section of the profile indiscriminately).
[0032] Comparative Example 2: Based on Example 1, the intermediate pre-deformation step in S1 was omitted. The temperature was increased to 435°C at a heating rate of 30°C / h and held for 3 hours. Then, the temperature was increased to 475°C at a heating rate of 20°C / h and held for 5 hours. After the second homogenization was completed, the temperature was decreased to 220°C at a cooling rate of 50°C / h. At this temperature, only a short period of heat homogenization was performed (holding for 30 minutes), but no compression pre-deformation was applied. Then, the temperature was directly increased to the third homogenization temperature at a heating rate of 30°C / h. The temperature was increased to 545°C and held for 6 hours. Then, the temperature was decreased to room temperature at a cooling rate of 65°C / h. The remaining conditions were the same as in Example 1.
[0033] Comparative Example 3: Based on Example 1, the cross-sectional differential cooling in S4 (i.e., uniform water cooling) was removed, and the remaining conditions were the same as in Example 1.
[0034] Comparative Example 4: Based on Example 1, mechanical vibration and uniaxial tensile stress in S6 were eliminated (i.e., conventional three-stage aging was adopted: 75℃×6 h→140℃×9 h→185℃×7 h, with no vibration and no stress), and the remaining conditions were the same as in Example 1.
[0035] Comparative Example 5: Based on Example 1, the following adjustments were made: S1 is the same as in Example 1; S4 eliminates the cross-sectional differential cooling and adopts uniform water quenching (specifically: the entire cross-section of the profile is subjected to non-differentiated full-coverage spray cooling at a rate of 15℃ / s, without distinguishing between thick-walled and thin-walled areas); S6 eliminates mechanical vibration and uniaxial tensile stress and adopts conventional three-stage aging: 75℃×6h→140℃×9h→185℃×7h, without applying vibration or stress; the remaining conditions are the same as in Example 1.
[0036] Comparative Example 6: Based on Example 1, the following adjustments were made: S1 omits the intermediate pre-deformation step and adopts the conventional three-stage homogenization (the specific process is the same as S1 in Comparative Example 2). S4 is the same as Example 1 (including cross-sectional differential quenching); S6 eliminates mechanical vibration and uniaxial tensile stress, and adopts conventional three-stage aging: 75℃×6h→140℃×9h→185℃×7h, without applying vibration or stress; the remaining conditions are the same as in Example 1.
[0037] Comparative Example 7: Based on Example 1, the following adjustments were made: S1 omits the intermediate pre-deformation step and adopts the conventional three-stage homogenization (the specific process is the same as S1 in Comparative Example 2). S4 eliminates cross-sectional differential cooling and adopts uniform water quenching (cooling rate 15℃ / s). S6 is the same as Example 1 (including mechanical vibration and uniaxial tensile stress). The remaining conditions are the same as in Example 1.
[0038] Comparative Example 8: S1 Homogenization: Traditional single-stage homogenization was adopted, with the temperature increased to 545℃ at 30℃ / h and held for 8h (same as Comparative Example 1), without intermediate pre-deformation; S2 gradient heating: Same as in Example 1; S3 extrusion molding: Same as Example 1; S4 online quenching: adopts traditional water-cooled quenching (same as comparative example 1), with no cross-sectional difference control; S5 Solution Treatment: The extruded profile is solution treated at 530℃ for 2 hours, followed by water quenching to room temperature; S6 pre-aging: Pre-aging treatment at 100℃ for 4 hours; S7 Pre-deformation: Apply 3% room temperature tensile pre-deformation to the pre-aged profile.
[0039] S8 dual-stage aging: Stage 1 aging at 120℃ for 30 minutes, Stage 2 aging at 170℃ for 30 minutes; The other unmentioned conditions are the same as in Example 1.
[0040] The mechanical performance test results are shown in the table below:
[0041] Comparative Example 8 uses solution quenching followed by room temperature pre-deformation (requiring separate solution treatment and pre-deformation processes). In contrast, the S1 solution of this invention embeds pre-deformation into the homogenization intermediate stage (requiring no additional process). While achieving the same performance level (395 MPa), it eliminates the separate solution treatment and pre-deformation processes, simplifying the process, reducing energy consumption, improving efficiency, and avoiding the adverse effects of pre-deformation after solution treatment on the dimensional accuracy of the profile. Furthermore, the complete solution in Example 1 further enhances the performance to 425 MPa.
[0042] When Comparative Example 3 already achieved a performance level comparable to Comparative Example 8 (395 MPa), the addition of S4 section-differentiated quenching further boosted the tensile strength to 425 MPa, an increase of 30 MPa. This demonstrates that the role of S4 is not only to control residual stress, but also to create a controllable residual stress field and transfer it across processes to stage S6, where it superimposes with the applied stress, producing an additional strengthening effect. Without S4, even with both S1 and S6 present, the performance can only reach a level comparable to existing technologies.
[0043] In summary, deformation heat treatment synergistic strengthening achieves a significant improvement in the overall mechanical properties of profiles.
[0044] The above description is merely a preferred embodiment of this application and does not limit the patent scope of this application. Any equivalent structural transformations made based on the inventive concept of this application and the contents of the specification and drawings of this application, or direct / indirect applications in other related technical fields, are included within the patent protection scope of this application.
Claims
1. A manufacturing process for aluminum alloy industrial profiles, characterized in that, Includes the following steps: S1. Homogenization heat treatment: The aluminum alloy ingot is subjected to the first stage of homogenization, the second stage of homogenization, intermediate cooling and pre-deformation, the third stage of homogenization and final cooling in sequence. The process involves the following steps: the first homogenization stage involves heating to 420–450 °C at a rate of 20–40 °C / h and holding for 2–4 hours; the second homogenization stage involves heating to 460–490 °C at a rate of 15–30 °C / h and holding for 4–6 hours; the intermediate cooling and pre-deformation stage involves cooling to 200–250 °C at a rate of 40–60 °C / h, at which temperature a compression pre-deformation of 0.5%–1.5% is applied to the ingot; the third homogenization stage involves heating to 530–560 °C at a rate of 20–40 °C / h and holding for 4–8 hours; and the final cooling stage involves cooling to room temperature at a rate of 50–80 °C / h. S2, Gradient heating: The ingot after S1 homogenization treatment is subjected to gradient heating to the extrusion temperature; S3, Extrusion molding: The ingot heated by gradient S2 is extruded to obtain an aluminum alloy profile with a predetermined cross-sectional shape; S4. Quenching: The profile after extrusion in step S3 is quenched online; the profile has a length direction along the extrusion direction and a cross-sectional direction perpendicular to the extrusion direction; the online quenching is set with multiple quenching sections along the length direction of the profile, and different cooling intensities are set according to the wall thickness difference of the profile cross-section within the same quenching section. S5. Stretch straightening: Stretch straightening is performed on the profiles after S4 quenching.
2. The production process according to claim 1, characterized in that, For thick-walled areas with a wall thickness ≥ 5 mm in the profile cross-section, the cooling rate is 20–35 ℃ / s; for medium-thickness areas with a wall thickness of 2–5 mm in the profile cross-section, the cooling rate is 10–20 ℃ / s; and for thin-walled areas with a wall thickness ≤ 2 mm in the profile cross-section, the cooling rate is 5–10 ℃ / s.
3. The production process according to claim 2, characterized in that, The temperature difference between different parts of the profile section at the end of quenching shall not exceed 30℃.
4. The production process according to claim 3, characterized in that, In step S1, the pre-deformation is achieved by applying axial compression to the ingot using a hydraulic press, and the ingot temperature is maintained at 200–250 °C during the pre-deformation process.
5. The production process according to claim 4, characterized in that, The aluminum alloy is a 6XXX series aluminum alloy containing Zn or a 7XXX series aluminum alloy.
6. The production process according to claim 5, characterized in that, In step S1, the compression pre-deformation amount is 0.5% to 1.5% of the ingot length.
7. The production process according to any one of claims 1 to 6, characterized in that, In step S4, the cross-sectional differential cooling is achieved by setting independent control valves on the cooling medium nozzles of the quenching device, and adjusting the flow rate and pressure of the cooling medium of each nozzle according to the wall thickness distribution of the profile cross-section.
8. The production process according to claim 7, characterized in that, In step S5, the stretching amount of the stretching straightening is 0.5% to 2.0%.
9. The production process according to claim 8, characterized in that, It also includes step S6, which involves performing a three-stage aging treatment on the profile after stretching and straightening in step S5; the three-stage aging treatment includes, in sequence: First-stage aging treatment: heat preservation at 60-90℃ for 4-8 hours, while applying mechanical vibration with a frequency of 20-50 Hz and an amplitude of 0.1-0.5 mm; Second-stage aging treatment: keep at 120-160℃ for 6-12 hours, while applying uniaxial tensile stress of 50-100 MPa; Third-level aging treatment: Keep at 170-200℃ for 4-10 hours without applying external force.