A method for improving the uniformity of the properties of the edge and center structure of magnesium-lithium alloy rods
By combining extrusion and room temperature rotary forging processes with single-pass first and last deformation feeding and water cooling treatment, the problem of uneven microstructure and properties between the edge and center of magnesium-lithium alloy bars was solved, achieving uniformity across the entire cross section and improving the mechanical properties and service reliability of the bars.
Patent Information
- Application Number
- CN202610907246.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-23
- Publication Date
- 2026-11-20
AI Technical Summary
The existing rotary forging process results in significant differences in the microstructure and properties between the edge and center of magnesium-lithium alloy bars, affecting the service reliability and processing stability of the bars, and there is a lack of effective process solutions.
A single-pass, end-to-end deformation feeding and intermediate water cooling rotary forging method is adopted, combined with extrusion and room temperature rotary forging processes. By controlling the deformation amount and temperature, the uniformity of the microstructure and properties of the magnesium-lithium alloy rods at the edges and center is achieved.
It achieves uniform microstructure and properties across the entire cross-section of magnesium-lithium alloy rods, improves the overall mechanical properties and service stability of the rods, simplifies the manufacturing process, and is suitable for high-plasticity lightweight structural components.
Smart Images

Figure CN123128352A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal material processing technology, and in particular to a method for improving the uniformity of microstructure properties at the edges and center of magnesium-lithium alloy rods. Background Technology
[0002] Magnesium-lithium alloys possess advantages such as low density, high specific strength, and good specific stiffness, making them promising candidates for lightweight applications in aerospace, rail transportation, and other fields. For bar-type components, in addition to requiring high strength and ductility, it is also essential to ensure high consistency in microstructure and properties across different locations on the cross-section to guarantee the component's synergistic load-bearing capacity and dimensional stability during service.
[0003] Rotary forging, as an efficient bar plastic forming process, can refine the microstructure and improve mechanical properties through radial high-frequency loading, and is currently widely used in the bar processing field. However, existing rotary forging processes mostly adopt conventional unidirectional continuous feeding methods, which causes the surface area of the bar to preferentially bear larger plastic deformation, while the deformation of the central area lags behind. This easily leads to obvious microstructure and property gradients in the cross-sectional direction, manifested as significant differences in grain size, deformed microstructure, and mechanical properties between the edge and the center, thus affecting the overall service reliability and subsequent processing stability of the bar.
[0004] Currently, research on improving the performance of magnesium-lithium alloys focuses primarily on alloying design. However, effective process solutions are lacking for addressing the radial microstructure and properties inhomogeneity caused by insufficient coordination between edge and center deformation during bar forging. Therefore, achieving uniform microstructure and properties across the entire cross-section of the bar through the design of composite deformation paths and forging feed methods is a pressing technical problem to be solved in this field. Summary of the Invention
[0005] The purpose of this invention is to provide a method for improving the uniformity of the microstructure and properties of magnesium-lithium alloy bars at the edges and center. By using a rotary forging method with single-pass first-and-last deformation feeding and intermediate water cooling, the uniformity of the bar's microstructure and properties is achieved, thereby solving the problems mentioned in the background art and producing magnesium-lithium alloy bars with uniform properties, high yield strength ratio, and high plasticity.
[0006] To achieve the above objectives, the present invention provides a method for improving the uniformity of microstructure properties at the edge and center of magnesium-lithium alloy rods, comprising the following steps: S1. Preparation of magnesium-lithium alloy ingots; S2. After heat treatment, the magnesium-lithium alloy ingot obtained in step S1 is extruded to obtain magnesium-lithium alloy extruded bars. S3. The extruded bar obtained in step S2 is subjected to multi-pass room temperature rotary forging deformation. Each pass is fed in by first and last deformation, and water cooling is performed after the pass is completed to finally obtain a magnesium-lithium alloy bar with uniform microstructure and properties at the edge and center.
[0007] Preferably, in step S1, the magnesium-lithium alloy ingot is a magnesium-lithium alloy containing Zn and Er.
[0008] Preferably, in step S1, the specific operation for preparing the magnesium-lithium alloy ingot is as follows: pure magnesium ingot, pure zinc ingot, magnesium-lithium master alloy and magnesium-erbium master alloy are placed in a vacuum furnace and melted at 710℃-720℃ under a protective atmosphere. After complete melting, the mixture is stirred evenly, the surface slag is removed, and after standing, it is poured into a mold and cooled to obtain the magnesium-lithium alloy ingot.
[0009] Preferably, in step S2, the specific operation of heat treatment is as follows: after removing the surface oxide scale or contamination layer from the magnesium-lithium alloy ingot obtained in step S1, it is placed in a heating furnace for preheating. The preheating temperature is 130℃-280℃, and the holding time is 0.5-1.5h.
[0010] Preferably, in step S2, the specific parameters of the extrusion molding process are: extrusion ratio of 18:1-28:1, extrusion speed of 0.5-2 mm / s, and extrusion temperature of 130℃-280℃.
[0011] Preferably, in step S3, 3-12 passes of rotary forging are performed, with a radial reduction of 0.2-0.6 mm in each pass.
[0012] Preferably, in step S3, each pass of rotary forging covers the entire length of the bar.
[0013] Preferably, in step S3, the deformation amount of rotary forging is 30%-60%.
[0014] This invention employs a synergistic process of extrusion and room temperature rotary forging, achieving significant synergistic effects. Extrusion first involves hot deformation of the ingot within a temperature range of 130℃-280℃, resulting in extruded bars with a preliminary refined microstructure and a certain texture orientation. This reduces the deformation resistance of subsequent room temperature rotary forging. Room temperature rotary forging then performs progressive deformation based on this, utilizing the high dislocation density of the extruded microstructure to promote uniform deformation transmission from the surface to the center, avoiding the inherent lag of edge deformation and center deformation in a single rotary forging process. Furthermore, this invention uses a method of "deformation at the beginning and end of each pass + water cooling after each pass" in the rotary forging process, achieving synergy in deformation uniformity and thermal control. The alternating feeding at the beginning and end of each pass eliminates the axial cumulative deformation bias caused by unidirectional continuous feeding, ensuring that the deformation force is evenly distributed along the entire length and cross-section of the bar. Immediate water cooling after each pass eliminates the heat accumulation between passes caused by the heat generated by plastic deformation, ensuring that each pass is carried out under constant room temperature conditions. The combination of these two factors makes multi-pass rotary forging a stable cycle of "uniform deformation - rapid recovery - uniform deformation again", ensuring that the evolution of the microstructure at the edge and center is synchronized.
[0015] Furthermore, this invention controls the radial reduction per pass to 0.2-0.6 mm, ensuring that the strain in each pass is within the optimal window for room temperature plastic forming of the material, avoiding excessive work hardening of the surface layer that hinders the inward transmission of deformation; the total deformation reaches 30%-60%, ensuring sufficient cumulative strain in the core, allowing the deformation effect to gradually penetrate from the surface to the center, ultimately achieving uniform deformation across the entire cross-section. Simultaneously, this invention employs a magnesium-lithium alloy containing Zn and Er, forming a composition-process synergy with the aforementioned process. Zn has a solid solution strengthening effect and promotes dynamic recrystallization during deformation, resulting in more uniform microstructure refinement during rotary forging; Er forms fine, dispersed precipitates, pinning grain boundaries and inhibiting abnormal grain growth. Especially in multi-pass room temperature rotary forging, the addition of Er effectively prevents local grain coarsening, ensuring the synchronicity of microstructure refinement at the edges and center.
[0016] Therefore, the method for improving the uniformity of microstructure properties at the edge and center of magnesium-lithium alloy rods provided by the present invention has the following beneficial effects: (1) The present invention introduces controllable plastic deformation on the basis of extrusion preformed structure through the composite deformation path of "extrusion-room temperature rotary forging", which is beneficial to refine the structure and improve the uniformity of the structure.
[0017] (2) In the rotary forging process, the present invention adopts the method of first and last deformation feeding in each pass and water cooling after the pass is completed, which avoids the local cumulative deformation bias caused by conventional unidirectional continuous feeding, and makes the deformation distribution of the bar along the axial and radial directions more balanced.
[0018] (3) By controlling the total deformation to 30%-60%, the present invention can effectively reduce the difference in structure and performance gradient between the edge region and the center region of the bar cross section, thereby improving the overall mechanical properties of the bar and enhancing its synergistic load-bearing capacity and service stability.
[0019] (4) The preparation method provided by the present invention has a simple process flow, is easy to implement in industry, and is suitable for the preparation of magnesium-lithium alloy products with high requirements for the uniformity of the bar cross section.
[0020] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description
[0021] Figure 1 The radial metallographic structure and radial hardness distribution diagram of the magnesium-lithium alloy rod prepared in Example 1 of the present invention are shown; wherein, (a) is the metallographic structure of the edge; (b) is the metallographic structure of the core; and (c) is the radial hardness distribution curve. Figure 2 The images show the radial metallographic structure and radial hardness distribution of the magnesium-lithium alloy rod prepared in Example 2 of this invention; wherein, (a) is the metallographic structure of the edge; (b) is the metallographic structure of the core; and (c) is the radial hardness distribution curve. Figure 3 The diagram shows the radial metallographic structure and radial hardness distribution of the magnesium-lithium alloy rod prepared in Comparative Example 1 of this invention; wherein, (a) is the metallographic structure of the edge; (b) is the metallographic structure of the core; and (c) is the radial hardness distribution curve. Figure 4 The radial hardness distribution diagrams are shown for the extruded bars of the present invention after extrusion forming in step S2 but without rotary forging in step S3, and the magnesium-lithium alloy bars prepared in Examples 1, 2, and 1. Detailed Implementation
[0022] The technical solution of the present invention will be further described below with reference to the accompanying drawings and embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention should be considered equivalent substitutions and are included within the protection scope of the present invention. Furthermore, it should be understood that after reading the contents of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims and are all within the protection scope of the present invention.
[0023] In this document, the term "embodiment" means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The term "embodiment" appearing in various places throughout the specification does not necessarily refer to the same embodiment, nor does it specifically limit its independence or connection with other embodiments. In principle, in this application, as long as there are no technical contradictions or conflicts, the technical features mentioned in each embodiment can be combined in any way to form corresponding implementable technical solutions.
[0024] Unless otherwise defined, the technical terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the use of related terms herein is merely for the purpose of describing particular embodiments and is not intended to limit this application.
[0025] Unless otherwise specified, the reagents, instruments, and equipment used in this invention are all commonly used by those skilled in the art, and the testing standards all use national or international standards commonly used in the field, without further explanation.
[0026] In this invention, unless otherwise specified, the numerical ranges involved include the endpoint values of the range and any values between the two endpoint values; the multiple numerical ranges can also be combined to form new preferred ranges. Equivalent substitutions or modifications made by those skilled in the art without departing from the spirit of this invention should fall within the protection scope of this invention.
[0027] The materials, methods, and embodiments described herein are exemplary and should not be construed as limiting unless otherwise stated. The stretching machine used in this embodiment of the invention is model CMT-5105; The metallurgical microscope used in this embodiment of the invention is an OLYMPUS PMG3. In this embodiment of the invention, the vacuum furnace is evacuated to a vacuum level of 2.5 × 10⁻⁶. -1 Pa, then argon gas is added as a protective gas until the entire vacuum furnace is in a protective gas atmosphere for melting.
[0028] Example 1 This embodiment provides a method for improving the uniformity of microstructure properties at the edge and center of magnesium-lithium alloy rods: the specific preparation steps are as follows: S1. Preparation of magnesium-lithium alloy ingots: The magnesium-lithium alloy ingot is composed of the following components by mass percentage: Li: 8%, Zn: 3%, Er: 1.5%, with the balance being Mg and unavoidable impurities, the total impurity content being ≤0.3%.
[0029] According to the above alloy composition ratio, pure magnesium ingots, pure zinc ingots, magnesium-lithium master alloy, and magnesium-erbium master alloy were selected as raw materials. Under argon protection, the raw materials were placed in a crucible and heated to 720°C in a vacuum furnace until all materials were completely melted, obtaining the alloy melt. During this process, the vacuum was evacuated to 2.5 × 10⁻⁶. -1 Pa; Subsequently, the alloy melt was stirred evenly at 710℃, the surface slag was removed, and it was allowed to stand for 5 minutes. Then it was poured into a stainless steel mold with a diameter of Φ90mm and a length of 300mm. It was naturally cooled in a vacuum furnace and then machined by turning and wire cutting to obtain an ingot with a diameter of Φ80mm.
[0030] S2, Extrusion molding: Remove the oxide scale from the alloy ingot obtained in step S1, place it in a heating furnace and preheat it at 230°C for 1 hour; then extrude the preheated ingot under the conditions of extrusion temperature of 230°C, extrusion ratio of 28:1 and extrusion speed of 0.6 mm / s to obtain extruded bar.
[0031] S3, Room temperature rotary forging deformation: The extruded bar obtained in step S2 was subjected to multi-pass room temperature rotary forging deformation. Each pass employed a head-and-tail deformation feeding method, meaning each rotary forging pass covered the entire length of the bar; first, one end of the bar was deformed, then it was fed to the other end to complete the deformation for that pass. Water cooling was performed immediately after each pass. Initially, six passes of deformation were performed with a radial compression of 0.4 mm, followed by a single pass with a compression of 0.2 mm, for a total of seven rotary forging passes, until the cumulative deformation reached 30%, ultimately yielding a magnesium-lithium alloy bar with a diameter of 13.4 mm.
[0032] The performance of the magnesium-lithium alloy rod obtained in this embodiment was tested, and the results are as follows: yield strength is 186 MPa, tensile strength is 198 MPa, and elongation is 43.4%.
[0033] Figure 1 The radial metallographic structure and hardness distribution of the magnesium-lithium alloy rod are shown. Figure 1 (a) and Figure 1 As shown in (b), both the edge and core of the bar exhibit fine equiaxed grain structures with similar grain sizes and no obvious coarse grains or structural differences; Figure 1 As shown in (c), from the center to the edge of the bar, the hardness value remains within a narrow range of 60.1 HV to 62.2 HV, with a gentle curve and uniform hardness distribution, without a significant hardness gradient between the center and the edge. These results indicate that through the "extrusion + room temperature rotary forging" composite process of this invention, and by employing initial and final deformation feeding and water cooling after each pass, when the cumulative deformation reaches 30%, the microstructure and properties of the bar's edge and center become consistent, achieving uniformity across the entire cross-section.
[0034] Example 2 This embodiment provides a method for improving the uniformity of microstructure properties at the edge and center of magnesium-lithium alloy bars. The preparation steps are basically the same as in Example 1, except for the difference in the cumulative deformation amount during rotary forging in step S3. The specific operation of step S3 is as follows: S3, Room temperature rotary forging deformation: The extruded bar obtained in step S2 was subjected to multi-pass room temperature rotary forging deformation. Each pass employed a head-and-tail deformation feeding method, meaning each rotary forging pass covered the entire length of the bar; first, one end of the bar was deformed, then it was fed to the other end to complete the deformation for that pass. Water cooling was performed immediately after each pass. First, 11 passes of deformation were performed with a radial compression of 0.4 mm, followed by a single pass of deformation with a radial compression of 0.3 mm, for a total of 12 passes of rotary forging, until the cumulative deformation reached 50%, ultimately yielding a magnesium-lithium alloy bar with a diameter of 11.3 mm.
[0035] The magnesium-lithium alloy rods obtained in this embodiment were subjected to performance tests, and the results are as follows: yield strength is 190 MPa, tensile strength is 203 MPa, and elongation is 34.9%.
[0036] Figure 2 The radial metallographic structure and hardness distribution of the magnesium-lithium alloy rod prepared in this embodiment are shown. Figure 2 (a) and Figure 2 As shown in (b), both the edge and core of the bar exhibit fine equiaxed grain structures, with grain sizes further refined compared to Example 1, and the difference in structure between the core and edge is minimal; Figure 2 As shown in (c), from the center to the edge of the bar, the hardness value remains within a narrow range of 61.6 HV to 64.6 HV. The curve is flatter than that of Example 1, the hardness distribution is more uniform, and the hardness difference between the center and the edge is further reduced. The above results indicate that when the cumulative deformation is increased to 50%, the uniformity of the microstructure and properties between the edge and the center of the bar is further improved, achieving a better overall cross-sectional homogenization effect.
[0037] Comparative Example 1 This comparative example provides a method for preparing magnesium-lithium alloy rods. The preparation steps are basically the same as in Example 1, except that the cumulative deformation amount in step S3 is lower (10%), which illustrates the technical problem of significant differences in microstructure and properties between the edge and center when the deformation amount is insufficient. The specific operation of step S3 is as follows: S3, Room temperature rotary forging deformation: The extruded bar obtained in step S2 was subjected to multi-pass room temperature rotary forging. Each pass was fed in with deformation at both ends, and water cooling was performed immediately after each pass. First, a single-pass deformation with a radial compression of 0.4 mm was performed, followed by a single-pass deformation with a radial compression of 0.3 mm, for a total of two passes of rotary forging, until the cumulative deformation reached 10%, finally obtaining a magnesium-lithium alloy bar with a diameter of 15.3 mm.
[0038] The magnesium-lithium alloy rods obtained in this comparative example were tested for performance, and the results were: yield strength of 173 MPa, tensile strength of 180 MPa, and elongation of 36.0%.
[0039] Figure 3 The radial metallographic structure and hardness distribution of the magnesium-lithium alloy rods prepared in this comparative example are shown. Figure 3 (a) and Figure 3 As shown in (b), the microstructure at the edge of the bar has been significantly refined, while the core microstructure retains the relatively coarse grain morphology of the extruded state. Some grains have only undergone slight fragmentation to form subgrains, and there is a significant difference between the microstructure of the core and the edge. Figure 3 As shown in (c), the hardness value gradually increases from approximately 53.0 HV to approximately 58.6 HV from the center to the edge of the bar, and the curve exhibits a clear sloping gradient, indicating that the properties of the core and the edge are inconsistent. The above results show that when the cumulative deformation is only 10%, the rotary forging deformation is mainly concentrated in the surface area and fails to be effectively transferred to the core, thus failing to achieve uniform microstructure and properties across the entire cross-section of the bar.
[0040] Comparative Example 2 In their article "Ultra-high specific strength of Mg-Li alloy via rotary swaging," published in Volume 36, pp. 7457-7467 of the *Journal of Materials Research and Technology*, Li Silong et al. disclosed a high-strength Mg-4Li alloy with internal and external property gradients that exhibits excellent rotary forging properties. After five rotary forging passes, the edge hardness reached 70 HV, while the core hardness reached 82 HV. Furthermore, the peak hardness in the core became increasingly pronounced with each additional rotary forging pass.
[0041] Comparative Example 3 In their article "Nanocrystallization of the cast AZ31 Mg alloy by low-strain rotary swaging," published in Volume 307, Paper No. 130995 of the journal *Materials Letters*, Chen Xin et al. disclosed a commercially available AZ31 magnesium alloy (Al 3.1%, Zn 0.9%, Mn 0.3% by mass, with the balance being Mg) prepared by rotary forging. After three passes of rotary forging, the hardness of the central region was approximately 80 HV, and the edge hardness was approximately 55 HV. The hardness gradually increased with the number of rotary forging passes, with a greater increase in hardness at the core.
[0042] In addition, the radial hardness test results of the extruded bars of Examples 1-2 and Comparative Example 1 after extrusion forming in step S2 but without rotary forging in step S3, as well as the alloys of Examples 1-2 and Comparative Example 1, are as follows: Figure 4 As shown.
[0043] from Figure 4 It can be seen that under smaller deformation amounts, the radial hardness gradient of the alloy is more obvious: the hardness of the edge is significantly greater than that of the core, and the hardness of the core is not much different from that of the extruded state. However, as the rotary forging deformation reaches more than 30%, the difference between the hardness of the core and the edge gradually narrows. According to the radial microstructure, it can be found that under small deformation amounts, the microstructure of the edge has been refined, but the microstructure of the core still maintains the relatively coarse state of the extruded state, with some grains broken into subgrains. However, as the cumulative deformation of rotary forging reaches 30% or more, the degree of microstructure refinement of the edge and the core gradually becomes consistent, and the microstructure and properties of the bar gradually become more uniform.
[0044] In summary, the preparation method of this invention is simple, the alloy preparation process is short, and the energy consumption requirement is low. The prepared magnesium-lithium alloy has the characteristics of uniform performance and high plasticity, and is suitable for lightweight structural components that require high plasticity and uniform cross-section of the rods. This improves the service safety of the components, provides a new research idea for the development of high-reliability magnesium-lithium alloys, and further broadens their application prospects.
[0045] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the technical solutions of the present invention, and these modifications or equivalent substitutions cannot cause the modified technical solutions to deviate from the spirit and scope of the technical solutions of the present invention.
Claims
1. A method for improving the uniformity of microstructure properties at the edge and center of magnesium-lithium alloy rods, characterized in that, Includes the following steps: S1. Preparation of magnesium-lithium alloy ingots; S2. After heat treatment, the magnesium-lithium alloy ingot obtained in step S1 is extruded to obtain magnesium-lithium alloy extruded bars. S3. The extruded bar obtained in step S2 is subjected to multi-pass room temperature rotary forging deformation. Each pass is fed in by first and last deformation, and water cooling is performed after the pass is completed to finally obtain a magnesium-lithium alloy bar with uniform microstructure and properties at the edge and center.
2. The method for improving the uniformity of microstructure properties at the edge and center of magnesium-lithium alloy rods according to claim 1, characterized in that, In step S1, the magnesium-lithium alloy ingot is a magnesium-lithium alloy containing Zn and Er.
3. The method for improving the uniformity of microstructure properties at the edge and center of magnesium-lithium alloy rods according to claim 1, characterized in that: In step S1, the specific operation for preparing magnesium-lithium alloy ingots is as follows: pure magnesium ingots, pure zinc ingots, magnesium-lithium master alloys and magnesium-erbium master alloys are placed in a vacuum furnace and melted at 710℃-720℃ under a protective atmosphere. After complete melting, the mixture is stirred evenly, surface slag is removed, and after standing, it is poured into a mold and cooled to obtain magnesium-lithium alloy ingots.
4. The method for improving the uniformity of microstructure properties at the edge and center of magnesium-lithium alloy rods according to claim 1, characterized in that: In step S2, the specific operation of heat treatment is as follows: after removing the surface oxide scale or contamination layer from the magnesium-lithium alloy ingot obtained in step S1, it is placed in a heating furnace for preheating. The preheating temperature is 130℃-280℃, and the holding time is 0.5-1.5h.
5. The method for improving the uniformity of microstructure properties at the edge and center of magnesium-lithium alloy rods according to claim 1, characterized in that: In step S2, the specific parameters of the extrusion molding process are: extrusion ratio of 18:1-28:1, extrusion speed of 0.5-2 mm / s, and extrusion temperature of 130℃-280℃.
6. The method for improving the uniformity of microstructure properties at the edge and center of magnesium-lithium alloy rods according to claim 1, characterized in that: In step S3, 3-12 passes of rotary forging are performed, with a radial reduction of 0.2-0.6 mm in each pass.
7. The method for improving the uniformity of microstructure properties at the edge and center of magnesium-lithium alloy rods according to claim 1, characterized in that: In step S3, each pass of rotary forging covers the entire length of the bar.
8. The method for improving the uniformity of microstructure properties at the edge and center of magnesium-lithium alloy rods according to claim 1, characterized in that: In step S3, the deformation amount of rotary forging is 30%-60%.