Isolating coating for interface between lost foam white pattern and furan resin sand and preparation method thereof
By introducing phase change microcapsules into the coating, the problems of dense isolation at low temperatures and efficient venting at high temperatures are solved, realizing the time-triggered switching of coating functions and improving the stability of the lost foam casting process and the quality of castings.
Patent Information
- Application Number
- CN202611364247.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-20
AI Technical Summary
In existing lost foam casting technology, the coating cannot achieve dense isolation at low temperatures or efficient venting at high temperatures. This results in a lack of coordination between "acid resistance" and "permeability" in the process, becoming a bottleneck restricting the widespread application of the lost foam-furan resin sand composite process in high-precision large castings.
Phase change microcapsules are introduced into the coating as core functional fillers. During the low-temperature curing stage, they fill the pores between refractory aggregates in solid form to form a dense acid barrier. During the high-temperature casting stage, the core material melts and vaporizes to generate air-permeable channels, thereby realizing the time-triggered switching of the coating function.
It achieves dynamic coordination of the functional requirements of "acid resistance and density" and "high-throughput permeability" without changing the physical structure of the coating, which significantly improves the stability of the lost foam casting process and the surface quality of the castings.
Smart Images

Figure CN123128432A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of lost foam casting technology, and more specifically to an isolation coating for the interface between the lost foam white mold and furan resin sand, and a method for preparing the same. Background Technology
[0002] In the field of lost foam casting, to meet the complex structural requirements of large castings (such as machine tool gantry bases and columns), a composite molding process of "EPS white mold + furan resin self-hardening sand" is often used. In this process, the EPS foam white mold serves as the cavity reference, and its surface needs to be coated with a layer of lost foam coating to isolate the high-temperature molten iron from direct contact with the molding sand and to guide the pyrolysis gas out during pouring. However, during the molding and curing stage, sulfonic acid curing agents (such as p-toluenesulfonic acid aqueous solution, pH 1-3) need to be added to the furan resin sand to achieve room temperature self-hardening. This acidic medium can easily penetrate through the coating pores to the surface of the EPS white mold, catalyzing the breakage of its molecular chains, resulting in softening of the white mold surface, dimensional shrinkage, or local dissolution, with an error of 0.1-1.0 mm. At the same time, the exothermic reaction of resin curing (40-60℃) is close to the glass transition temperature of EPS (85-100℃), further aggravating thermal deformation. Traditional solutions to suppress this corrosion include adding alkaline neutralizing fillers such as MgO and CaCO3 to the coating in an attempt to consume the acid through chemical neutralization. However, this method generates water and CO2, which can form bubbles in the coating, compromising its density and reducing its high-temperature strength. Alternatively, increasing the coating thickness to 3-5 mm can delay the diffusion of the acid, but this makes it difficult for EPS pyrolysis gases (such as styrene, CO, and CH4) to escape during casting, increasing the porosity defect rate of the casting by 2-4 times. Furthermore, the coating is prone to cracking and peeling during handling and sand filling. Another technical solution (such as CN1663707A) incorporates 0.1-1.0% organic short fibers into the coating, utilizing their vaporization at high temperatures to form interconnected micropores to improve air permeability. However, these fibers only play a mechanical crack-resistant role at low temperatures. Due to their low content, they cannot fill the inherent pores of the coating. Instead, they form capillary channels at the fiber-matrix interface, accelerating acid penetration. Their design goal is to "improve cold-state air permeability," which is completely contrary to the actual requirement of "dense acid-resistant coating in cold state."
[0003] The aforementioned traditional technical solutions are all based on the conventional thinking of "static chemical modification" or "single physical thickening," attempting to solve the acid etching problem by permanently changing the coating composition or structure. However, they fail to recognize that acid erosion only occurs during the molding and curing stage (1-3 hours), while the need for high permeability only exists during the casting and vaporization stage (several minutes). There is a clear functional conflict between the two in the temporal dimension. Existing coatings cannot achieve dense isolation at low temperatures or efficient venting at high temperatures, resulting in a lack of synergistic achievement of "acid resistance" and "permeability" in the process. This has become the core bottleneck restricting the widespread application of the lost foam-furan resin sand composite process in high-precision large castings. Summary of the Invention
[0004] To address the problems in the prior art, this application provides an isolation coating for the interface between lost foam casting white mold and furan resin sand, comprising: refractory aggregate and phase change microcapsules; the refractory aggregate comprises zircon powder and quartz powder, wherein the mass ratio of zircon powder to quartz powder is 55:10 to 45:15; the core material of the phase change microcapsules is an organic phase change material with a melting point of 55-65℃, the shell material is a thermosetting resin, the particle size is 5-30μm, and the content of the phase change microcapsules is 15-25% of the mass of the refractory aggregate; the organic phase change material is selected from n-alkanes C 20 -C 35 Specifically, it is one or more of n-eicosane, n-docosane, n-tetracosane, n-hexacosane, n-octacosane, n-trianetracosane, n-dodecane, n-tetracosane, or n-pentadecane; the thermosetting resin is melamine-formaldehyde resin, which is prepared by reacting melamine and formaldehyde at a molar ratio of 1:2.0-3.5, and methanol is added as a co-solvent during the reaction. The shell wall thickness of the melamine-formaldehyde resin is 0.8-1.8 μm, and the crosslinking density in the shell layer is 0.45-0.65 mmol / g.
[0005] Optionally, in one possible implementation of this application, the phase change microcapsules have a particle size D50 of 10-15 μm and a particle size distribution span D90 / D10 ≤ 3.0; the zircon powder has an average particle size of 4.5-5.5 μm and the quartz powder has an average particle size of 3.0-4.0 μm, and both particle size distributions satisfy D95 ≤ 12 μm.
[0006] Optionally, in one possible implementation of this application, the isolation coating further comprises an alkaline silica sol as a high-temperature binder, having a SiO2 content of 29-31% and a pH of 9.2-9.8; the alkaline silica sol has a particle diameter of 5-15 nm and a SiO2 to water molar ratio of 1:8-1:12; the isolation coating has a solid content of 58-62% and a Baume degree of 65-70°Bé; and the dry film thickness of the isolation coating is 1.8-2.5 mm.
[0007] Optionally, in one possible implementation of this application, the isolation coating is used in the lost foam and furan resin self-hardening sand composite molding process, wherein the curing agent of the furan resin sand is one or more of p-toluenesulfonic acid, naphthalenesulfonic acid formaldehyde condensate or benzenesulfonic acid, and its pH is 1.5-2.5; the white mold is expandable polystyrene (EPS), with a density of 18-22 g / L and a particle size of 0.3-0.8 mm.
[0008] Furthermore, this application also provides a method for preparing an isolation coating for the interface between lost foam casting white mold and furan resin sand, comprising the following steps:
[0009] Add the phase change microcapsules to the mixture of refractory aggregate, liquid medium and additives at a speed of 300-500 rpm and stir for 5-10 minutes.
[0010] The core material of the phase change microcapsules is an organic phase change material with a melting point of 55-65℃, the shell material is a thermosetting resin, the particle size is 5-30μm, and the content of the phase change microcapsules is 15-25% of the mass of the refractory aggregate; the liquid medium is water, the amount of which makes the final coating solid content 55-65%; the additives include alkaline silica sol, polyvinyl alcohol PVA1788, sodium carboxymethyl cellulose CMC, sodium bentonite and alkylphenol polyoxyethylene ether OP10, and their addition order is: sodium bentonite, alkaline silica sol, PVA1788, CMC, OP10;
[0011] The sodium-based bentonite is pre-hydrated and swollen in 1 / 3 of the total water volume for 30-40 minutes before being added, and the hydration temperature is 20-25℃.
[0012] Before adding the phase change microcapsules, the mixture is dispersed at high speed of 1500-2000 rpm for 20-30 minutes to form a homogeneous paste system with a viscosity of 8000-15000 mPa·s.
[0013] After the phase change microcapsules are added, the stirring speed is 350-450 rpm and the stirring time is 6-9 minutes. The system is allowed to stand for 12-14 minutes for natural defoaming, or vacuum defoaming is performed at 0.08-0.09 MPa for 5-7 minutes.
[0014] Compared with the prior art, the technical solution of this application has the following beneficial effects:
[0015] By applying the technical solution of this application, phase change microcapsules, comprising 15-25% of the refractory aggregate mass, are introduced into the refractory aggregate. The core material is an organic phase change material with a melting point of 55-65℃, and the shell material is a thermosetting resin with a particle size controlled at 5-30μm. This achieves a time-sequential intelligent response to the coating's function: Under the low-temperature conditions of the molding and curing stage, the phase change microcapsules remain solid, effectively filling the coating pores to form a dense structure and blocking the corrosion and penetration of the sulfonic acid curing agent in the furan resin sand onto the white mold. Under the high-temperature environment of the casting and gasification stage, the core material melts and rapidly gasifies, while the thermosetting resin shell undergoes thermal degradation, generating interconnected air channels in situ. This significantly improves the coating's gas permeability, thus dynamically coordinating the seemingly contradictory functional requirements of "acid resistance and density" and "high-throughput permeability" without altering the coating's physical structure. This synergistic mechanism avoids the complexity of traditional coating processes that require multi-layer structures or additive formulations to achieve functional switching, significantly improving the stability of the lost foam casting process and the surface quality of the castings. Attached Figure Description
[0016] Figure 1 This is a schematic flowchart illustrating a method for preparing an isolation coating at the interface between the lost foam casting white mold and furan resin sand, as described in an embodiment of this application. Detailed Implementation
[0017] The technical solutions of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of the embodiments. The components of this application described and shown in the accompanying drawings can generally be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of this application provided in the accompanying drawings is not intended to limit the scope of the claimed application, but merely represents selected embodiments of this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without inventive effort are within the scope of protection of this application. It should be noted that similar reference numerals and letters in the following drawings indicate similar items; therefore, once an item is defined in one drawing, it does not need to be further defined and explained in subsequent drawings. Furthermore, in the description of this application, the terms "first," "second," etc., are used only to distinguish descriptions and should not be construed as indicating or implying relative importance.
[0018] In the field of lost foam casting, to meet the complex structural requirements of large castings (such as machine tool gantry bases and columns), a composite molding process of "EPS white mold + furan resin self-hardening sand" is often used. In this process, the EPS foam white mold serves as the cavity reference, and its surface needs to be coated with an isolation coating to prevent direct contact between the high-temperature molten iron and the molding sand, and to guide the pyrolysis gas to escape during pouring. However, this composite process has two time-separate and functionally mutually exclusive process requirements: First, during the molding and curing stage (1-3 hours, ambient temperature not higher than 60℃), the sulfonic acid curing agent (pH 1-3) in the furan resin sand will penetrate through the coating pores to the surface of the EPS white mold, catalyzing the breakage of its molecular chains, resulting in softening, dimensional shrinkage, or local dissolution of the white mold surface, with dimensional errors reaching 0.1-1.0mm. At this time, the coating is required to be dense and acid-resistant. Second, during the casting and vaporization stage (several minutes, temperature not lower than 300℃), the gases (such as styrene, carbon monoxide, and methane) generated by the pyrolysis of the EPS white mold need to escape smoothly. At this time, the coating is required to be highly permeable and capable of venting. Existing technologies consistently treat coatings as a "static functional body," attempting to solve the problem through permanent chemical modification (such as adding alkaline neutralizing fillers like MgO and CaCO3) or simple physical thickening (such as increasing the coating thickness to 3-5 mm). The former generates water and carbon dioxide during the neutralization reaction, forming bubbles in the coating and compromising its density; the latter hinders the escape of pyrolysis gases, increasing the porosity defect rate of castings by 2-4 times. Another technical solution (such as CN1663707A) incorporates short organic fibers into the coating to improve permeability, but its low fiber content and high aspect ratio not only fail to seal the coating pores but also create acid penetration channels at low temperatures. None of the above solutions can simultaneously meet the requirements of "low-temperature density and acid resistance" and "high-temperature high-throughput permeability," becoming the core bottleneck restricting the widespread application of the lost foam-furan resin sand composite process in high-precision large castings.
[0019] To address the aforementioned technical problems, this application provides an isolation coating for the interface between the white mold and furan resin sand in lost foam casting, and a method for preparing such an isolation coating. The core concept of this application lies in introducing a time-gated functional filler centered on "phase change microcapsules" into the coating. During the low-temperature curing stage, the phase change microcapsules physically fill the pores between refractory aggregates in a solid form, forming a dense acid-resistant barrier. During the high-temperature casting stage, the core material melts and vaporizes, accompanied by thermal degradation of the shell material, generating interconnected permeable channels in situ. Thus, without altering the physical structure of the coating, the coating function achieves self-triggered switching according to the process stage, dynamically resolving the functional contradiction between "dense curing" and "permeable casting." The technical solution of this application will be described in detail below with reference to the claims.
[0020] Example 1: In the composite molding process of lost foam casting with white mold and furan resin sand, the acidic medium of the sulfonic acid curing agent in the furan resin sand can penetrate to the surface of the EPS white mold through the coating pores, catalyzing the breakage of the white mold molecular chains, leading to softening, dimensional shrinkage, and even local dissolution of the white mold surface, with dimensional errors reaching 0.1-1.0 mm. Simultaneously, the exothermic curing of the resin (40-60℃) is close to the glass transition temperature of EPS (85-100℃), further exacerbating thermal deformation. Existing methods such as adding alkaline neutralizing fillers, increasing coating thickness, or incorporating organic short fibers all suffer from defects such as "bubbles generated by the neutralization reaction," "difficulty in escaping pyrolysis gases," or "formation of acid penetration channels at low temperatures," failing to achieve both dense isolation at low temperatures and efficient venting at high temperatures. Therefore, a novel isolation coating is needed that can achieve dense acid resistance during the low-temperature curing stage and high-throughput permeability during the high-temperature casting stage.
[0021] To address the aforementioned problems, this embodiment provides an isolation coating for the interface between the lost foam casting white mold and furan resin sand, comprising: refractory aggregate and phase change microcapsules; the refractory aggregate includes zircon powder and quartz powder, wherein the mass ratio of zircon powder to quartz powder is 55:10 to 45:15; the core material of the phase change microcapsules is an organic phase change material with a melting point of 55-65℃, the shell material is a thermosetting resin, the particle size is 5-30μm, and the content of the phase change microcapsules is 15-25% of the mass of the refractory aggregate; the organic phase change material is selected from n-alkanes C 20 -C 35 Specifically, it is one or more of n-eicosane, n-docosane, n-tetracosane, n-hexacosane, n-octacosane, n-trianetracosane, n-dodecane, n-tetracosane, or n-pentadecane; the thermosetting resin is melamine-formaldehyde resin, which is prepared by reacting melamine and formaldehyde at a molar ratio of 1:2.0-3.5, and methanol is added as a co-solvent during the reaction. The shell wall thickness of the melamine-formaldehyde resin is 0.8-1.8 μm, and the crosslinking density in the shell layer is 0.45-0.65 mmol / g.
[0022] Among them, refractory aggregates provide high-temperature skeleton support and acid-resistant dense foundation for the coating. The main crystalline phase of zircon powder is zirconium silicate, with a melting point of about 2550℃. It has a low coefficient of thermal expansion, good thermal conductivity, high chemical stability at high temperatures, and does not easily react with molten metal and furan resin sand. It also has excellent thermal shock resistance and can withstand the severe thermal shock during the pouring of molten iron without cracking. Quartz powder is widely available, inexpensive, has fine particles, and good filling properties. It can fill the gaps between zircon powder particles, improve aggregate gradation, increase bulk density, and reduce coating porosity. The mass ratio of zircon powder to quartz powder is limited to 55:10 to 45:15, so that zircon powder acts as the main component to provide high-temperature refractory and acid resistance, while quartz powder acts as an auxiliary component to improve particle size distribution and dense packing. If the quartz powder content is too high, it will cause a large volume expansion when the β-quartz to α-quartz crystal transformation occurs at 573℃, which can easily lead to high-temperature cracking of the coating. If the quartz powder content is too low, the aggregate filling will be insufficient, the coating porosity will increase, and the dense acid-resistant performance will decrease. The above ratio range achieves a balance between high-temperature strength, low-temperature density, and raw material cost. In practical applications, one or more of the following refractory powders such as corundum powder, mullite powder, and chromite powder can also be selected as refractory aggregates, and this application does not limit this.
[0023] Phase change microcapsules are the core functional filler for achieving sequential switching of coating functions in this application. The core material is an organic phase change material with a melting point of 55–65℃. This melting point range is specifically designed for the temperature control nodes in the casting process: during the molding and solidification stage, the ambient temperature does not exceed 60℃, keeping the core material solid and stably filling the internal pores of the coating to form a dense barrier; during the pouring and vaporization stage, the temperature does not fall below 300℃, causing the core material to melt and rapidly vaporize, releasing the space occupied by the microcapsules and forming in-situ permeable channels. The melting point of 55–65℃ is higher than the upper limit of the solidification stage temperature, ensuring that the core material does not melt prematurely during solidification, and much lower than the pouring stage temperature, ensuring rapid phase change of the core material during pouring. The shell material is a thermosetting resin, which maintains rigidity and integrity at low temperatures, effectively encapsulating and protecting the core material, and undergoes controlled thermal degradation and cracking at high temperatures, releasing the core material in a timely manner. The particle size of the phase change microcapsules is limited to 5–30 μm, which matches the pore size between refractory aggregate particles, enabling them to embed and fill the gaps between aggregates. The content of the phase change microcapsules is limited to 15–25% of the mass of the refractory aggregate. This content ensures that the microcapsules are sufficient to fill the pores of the coating and form a continuous and dense acid barrier, while not weakening the mechanical strength and structural integrity of the coating due to excessive content.
[0024] Organic phase change materials are selected from n-alkanes C 20 -C 35Specifically, it includes one or more of n-eicosane, n-docosane, n-tetracosane, n-hexacosane, n-octacosane, n-triane, n-dodecane, n-tetradecane, or n-pentadecane. n-Alkanes are long-chain saturated hydrocarbons, possessing advantages such as high phase change enthalpy, chemical inertness, non-corrosiveness, no supercooling, and good cycle stability. Furthermore, their melting point increases systematically with increasing carbon chain length. Therefore, by selecting a single n-alkane with a suitable carbon chain length, or by combining multiple n-alkanes, the melting point of the phase change material can be precisely controlled to the target range of 55–65°C, thus accurately matching the temperature windows of the molding and solidification stages and the casting and vaporization stages. In practical applications, other organic phase change materials such as paraffin wax, fatty acids, and polyols can also be selected; this application does not limit the choice of organic phase change materials.
[0025] The thermosetting resin is melamine-formaldehyde resin, which is prepared by reacting melamine and formaldehyde at a molar ratio of 1:2.0–3.5, with methanol added as a co-solvent during the reaction. Melamine-formaldehyde resin exhibits high crosslinking density, good heat resistance, chemical corrosion resistance, and high mechanical strength. It can stably coat the core material at low temperatures, resist the erosion of the acidic environment of furan resin sand, and undergo controlled degradation according to a predetermined pattern at high temperatures. The molar ratio of melamine to formaldehyde is limited to 1:2.0–3.5 to control the degree of crosslinking of the resin: too low a molar ratio results in insufficient crosslinking and insufficient shell strength; too high a molar ratio results in excessively dense crosslinking, an overly brittle shell, and difficulty in achieving controlled degradation at high temperatures. Adding methanol as a co-solvent during the reaction optimizes the uniformity of the reaction between melamine and formaldehyde, avoids localized looseness or premature crosslinking of the resin shell, and ensures stable microcapsule coating efficiency and uniform dispersion in the refractory aggregate. The shell wall thickness of the melamine-formaldehyde resin is limited to 0.8–1.8 μm: if the shell wall is too thin, the mechanical strength is insufficient and it is prone to breakage during stirring and handling; if the shell wall is too thick, it is difficult to degrade in time within the expected temperature window at high temperatures, affecting the formation of air permeable channels. The crosslinking density in the shell layer is limited to 0.45–0.65 mmol / g to control the fracture energy barrier of the resin network at high temperatures, promoting orderly pyrolysis of the shell material within a specific temperature window and forming interconnected microporous channels. In practical applications, other thermosetting resins such as urea-formaldehyde resin, phenolic resin, and polyurethane resin can also be selected as shell materials, and this application does not limit this.
[0026] In this embodiment, the isolation coating achieves a time-triggered switching of coating functions through the physical phase change behavior of phase change microcapsules in the composite molding process of lost foam casting and furan resin sand. During the molding and curing stage (≤60℃), the core material of the phase change microcapsules remains solid, forming a dense and continuous stacked structure in synergy with refractory aggregates (zircon powder and quartz powder). This physically fills the internal pores of the coating, blocking the penetration path of the sulfonic acid curing agent in the furan resin sand, thereby protecting the EPS white mold from chemical corrosion by acidic media. During the casting and vaporization stage (≥300℃), the core material of the phase change microcapsules melts and rapidly vaporizes due to the temperature exceeding the melting point. At the same time, the thermosetting resin shell undergoes thermal degradation and rupture, leaving a network of interconnected micron-sized micropores in situ. This allows the coating to automatically switch from a "closed and dense state" to an "open and permeable state," ensuring the smooth discharge of pyrolysis gases from the white mold.
[0027] This embodiment achieves the sequential synergy of two functions—acid-resistant density and high-flux permeability—in the same coating system by introducing phase change microcapsules into the refractory aggregate. These microcapsules comprise 15–25% of the refractory aggregate by weight, have a core material melting point of 55–65°C, a shell material of thermosetting resin, and a particle size of 5–30 μm. This approach does not rely on chemical neutralization, thickening, or permanent pore structures, avoiding the complexities of traditional coating processes that require multi-layer structures or additive formulations to achieve functional switching. It significantly improves the stability of the lost foam casting process and the surface quality of the castings, effectively reducing dimensional distortion of the white foam and porosity defects in the castings.
[0028] Example 2: Whether phase change microcapsules can fully fill the pores of refractory aggregates at low temperatures and form uniformly connected permeable channels at high temperatures largely depends on the matching relationship between the microcapsule particle size and the aggregate particle size. If the phase change microcapsule particle size is too large or the distribution is too wide, it will be difficult to embed into the aggregate gaps and form a dense acid-resistant isolation layer; if the refractory aggregate particle size is too large or the distribution is too wide, the pores will be uneven, the microcapsules will not be fully filled or the structure will collapse, and the permeable channels will be disordered and the local permeability will be inconsistent after high-temperature vaporization. Therefore, it is necessary to further limit the particle size parameters of the phase change microcapsules and the refractory aggregates to achieve the dual goals of dense acid resistance and uniform permeability.
[0029] Based on Example 1, in this example, the particle size D50 of the phase change microcapsules is 10–15 μm, and the particle size distribution span D90 / D10≤3.0; the average particle size of zircon powder is 4.5–5.5 μm, and the average particle size of quartz powder is 3.0–4.0 μm, and the particle size distribution of both satisfies D95≤12 μm.
[0030] Among them, the particle size D50 of the phase change microcapsules refers to the particle size value corresponding to the cumulative particle size distribution reaching 50%, which is limited to 10–15 μm. This ensures that the microcapsule size is highly concentrated within the suitable range of the pores between refractory aggregate particles, ensuring that the microcapsules can uniformly fill the gaps between aggregates at low temperatures and form a dense and leak-proof acid-resistant isolation layer. The particle size distribution span D90 / D10 refers to the ratio of the particle size values corresponding to the cumulative particle size distribution reaching 90% and 10%, which is limited to no more than 3.0. This indicates that the microcapsule particle size distribution is concentrated and the size is uniform, avoiding insufficient local density or disordered air permeability channels caused by excessive particle size dispersion. The average particle size of zircon powder is limited to 4.5–5.5 μm, and the average particle size of quartz powder is limited to 3.0–4.0 μm, meaning the quartz powder is slightly finer than the zircon powder. This allows the quartz powder to fill the spaces between the zircon powder particles, forming a dense particle size distribution. Simultaneously, the particle size distribution of both zircon and quartz powder satisfies D95 ≤ 12 μm, meaning that over 95% of the aggregate particles have a diameter not exceeding 12 μm. This controls the pore size between aggregate particles within a range that precisely matches the particle size of the phase change microcapsules (5–30 μm). The specific values of the above particle size parameters can be adjusted within a given range according to actual working conditions and raw material sources; this application does not impose such limitations.
[0031] In this embodiment, the phase change microcapsule particle size (D50 10–15 μm, D90 / D10 ≤ 3.0) and the refractory aggregate particle size (zircon powder 4.5–5.5 μm, quartz powder 3.0–4.0 μm, D95 ≤ 12 μm) form a precise size match. During the molding and curing stage, the microcapsules can stably embed and completely fill the pores between aggregate particles, constructing a dense, uniform, and acid-resistant barrier structure. During the casting and gasification stage, the microcapsule core material melts upon heating and escapes uniformly, leaving behind a consistent distribution and good connectivity of micropore channels, achieving a sequential functional switch from dense impermeability to high permeability.
[0032] This embodiment avoids problems such as uneven porosity, incomplete microcapsule filling, or structural collapse caused by excessively large particle size or excessively wide distribution by limiting the particle size parameters and distribution width of the phase change microcapsules and refractory aggregates. This ensures that the coating has consistent and reliable acid resistance and density at low temperatures and consistent and stable air permeability at high temperatures. It significantly improves the structural stability and functional reliability of the coating under dual-stage conditions, thereby ensuring the surface quality and process stability of the casting.
[0033] Example 3: After the phase change microcapsules vaporize during the high-temperature casting stage, a microporous network is left in situ. At this point, the structural integrity of the coating depends on the continuous support of the high-temperature binder at high temperatures. If the coating partially collapses or crumbles after the phase change microcapsules vaporize due to binder pyrolysis or insufficient strength, the venting channels will lose their structural support, and the coating will be unable to maintain stable venting performance during the casting stage, and defects such as sand adhesion and sand erosion are likely to occur. Therefore, it is necessary to introduce a high-temperature binder that can form a stable skeleton at high temperatures, and to control the solid content and dry film thickness of the coating accordingly.
[0034] Based on Example 1, in this example, the isolation coating further includes alkaline silica sol as a high-temperature binder, with a SiO2 content of 29–31% and a pH of 9.2–9.8; the alkaline silica sol has a particle diameter of 5–15 nm and a SiO2 to water molar ratio of 1:8–1:12; the isolation coating has a solid content of 58–62% and a Baume degree of 65–70°Bé; and the dry film thickness of the isolation coating is 1.8–2.5 mm.
[0035] In this process, alkaline silica sol is used as a high-temperature binder, with a SiO2 content limited to 29–31% and a pH limited to 9.2–9.8. During the heating process, the silica sol undergoes a dehydration and condensation reaction, forming a dense and stable three-dimensional silica-oxygen network framework. This framework supports and maintains the integrity of the coating structure after the phase change microcapsules vaporize to form a microporous network, preventing local collapse due to insufficient strength after the high-temperature binder pyrolysis. The specific values of SiO2 content and pH synergistically optimize the gelation behavior and refractory properties of the silica sol, ensuring its stable support of the permeable channels during the high-temperature vaporization stage of furan resin sand. The particle diameter of the alkaline silica sol is limited to 5–15 nm, and the molar ratio of SiO2 to water is limited to 1:8–1:12. Nanoscale particles can uniformly fill the microporous network and rapidly form a continuous and dense silica-oxygen framework. Simultaneously, the particle size and molar ratio synergistically control the water evaporation rate and gel shrinkage behavior, preventing framework breakage and pore collapse caused by excessively large particles or excessive water content. In practical applications, other high-temperature adhesives such as ethyl silicate hydrolysate and water glass can also be selected, but this application does not limit the specific adhesives used.
[0036] The solid content of the isolation coating is limited to 58–62%, and the Baumé degree is limited to 65–70°Bé. This is used to control the rheological behavior and drying kinetics of the coating. This concentration range ensures that the coating has appropriate viscosity and surface tension during the coating process, enabling it to uniformly cover the white mold surface without sagging or local accumulation. Simultaneously, it slowly releases moisture during drying, effectively reducing shrinkage stress and preventing cracking or delamination due to excessively rapid drying. The dry film thickness of the isolation coating is limited to 1.8–2.5 mm. This thickness range is sufficient to form a dense acid barrier during the molding and curing stage, and provides sufficient space for the gas channels formed after the phase change microcapsules vaporize during the casting and vaporization stage. This avoids micropore blockage or insufficient channel density due to excessive thickness, and insufficient acid barrier capacity or reduced structural integrity due to insufficient thickness. The specific values of the above solid content, Baumé degree, and dry film thickness can be adjusted within a given range according to the actual coating process and casting dimensions. This application does not limit these values.
[0037] In this embodiment, after the alkaline silica sol undergoes heating and vaporization of the phase change microcapsules to form a microporous network, it undergoes a dehydration and condensation reaction at high temperature to form a dense and stable three-dimensional silica-oxygen network skeleton. This provides continuous structural support for the air permeability channels and prevents localized coating collapse. The solid content and Baumé degree ensure uniform coating and slow drying, reducing the risk of shrinkage cracking. The dry film thickness balances the acid-resistant density at low temperatures with the air permeability at high temperatures. These three factors work synergistically to maintain structural stability during the functional transition from "dense acid resistance" to "high-flux air permeability."
[0038] This embodiment introduces alkaline silica sol as a high-temperature binder and limits its parameters, while controlling the coating's solid content, Baumé degree, and dry film thickness. This significantly improves the coating's anti-collapse ability and structural integrity during the high-temperature vaporization stage, fundamentally solving the failure risk caused by structural instability between the two functional stages of molding curing and casting vaporization. It also takes into account the adhesion stability of the coating and white mold interface and the overall structural integrity, ensuring the surface quality of the casting and the process yield.
[0039] Example 4: The isolation coating of this application is mainly aimed at the composite molding process of lost foam casting and furan resin self-hardening sand. In this process, the furan resin sand uses a strong acidic sulfonic acid curing agent to achieve room temperature self-hardening. The acidic environment places stringent requirements on the acid resistance of the coating. At the same time, the pyrolysis behavior of the white mold must match the response characteristics of the phase change microcapsules to achieve the functional timing switching of the coating. If the acid resistance design of the coating and the parameters of the white mold are not matched with the specific strong acidic curing agent system and the pyrolysis characteristics of the white mold, the coating will still be difficult to balance protection and permeability in the strong acidic furan resin sand system. Therefore, it is necessary to further limit the curing agent system and white mold parameters applicable to the coating.
[0040] Based on Example 1, in this example, the isolation coating is used in the composite molding process of lost foam and furan resin self-hardening sand. The curing agent of furan resin sand is one or more of p-toluenesulfonic acid, naphthalenesulfonic acid formaldehyde condensate or benzenesulfonic acid, with a pH of 1.5–2.5. The white mold is expandable polystyrene (EPS), with a density of 18–22 g / L and a particle size of 0.3–0.8 mm.
[0041] The curing agent for the furan resin sand is limited to one or more of p-toluenesulfonic acid, naphthalenesulfonic acid formaldehyde condensate, or benzenesulfonic acid, with a pH of 1.5–2.5. This constitutes a strongly acidic curing agent system capable of catalyzing the self-curing of furan resin at room temperature. In the isolation coating of this embodiment, the phase change microcapsules use an organic phase change material with a melting point of 55–65°C as the core material and a thermosetting resin as the shell material. They are uniformly dispersed in the coating at 15–25% of the refractory aggregate mass, ensuring they remain solid during the furan resin sand curing stage. This effectively fills the coating pores and forms a dense hydrophobic barrier, thereby physically preventing the aforementioned strongly acidic curing agent from chemically eroding the lost foam casting white mold. In practical applications, other sulfonic acid curing agents or their mixtures can also be selected as the curing agent; this embodiment does not limit this choice.
[0042] The white mold is limited to expandable polystyrene (EPS) with a density of 18–22 g / L and a particle size of 0.3–0.8 mm. This density and particle size range ensures that the white mold has appropriate structural density and surface stability during the molding and curing stage, which is beneficial for the adhesion of the coating to the surface of the white mold and effectively inhibits the penetration and erosion of the white mold by the acidic curing liquid of furan resin. At the same time, during the casting and vaporization stage, EPS of this specification can release pyrolysis gas at a uniform and controllable rate, which vaporizes synchronously with the organic phase change material core material with a melting point of 55–65°C within a similar temperature window, causing the microcapsule shell to rupture and form a uniformly distributed and well-connected microporous network, realizing the time-sequential switching of coating functions. In practical applications, the white mold can also be made of other foamed plastics (such as copolymer foam materials), and this application does not limit this.
[0043] In this embodiment, during the molding and curing stage, the isolation coating physically fills the pores with solid phase change microcapsules to form a dense hydrophobic barrier, blocking the chemical erosion of the EPS white mold by the strong acid curing agent with a pH of 1.5–2.5. During the casting and vaporization stage, the EPS white mold releases pyrolysis gas at a uniform rate according to the set specifications, which vaporizes synchronously with the phase change microcapsule core material, causing the coating to switch from a dense state to a highly permeable state, promoting the smooth escape of the vaporization products of the white mold, and realizing the intelligent switching between "acid-resistant and dense" and "high-throughput permeability".
[0044] This embodiment limits the application of the coating to a strong acid curing agent system and the density and particle size parameters of the EPS white mold, so that the acid resistance and isolation performance of the coating and the pyrolysis and gasification characteristics of the white mold are synergistically matched. This completely solves the technical contradiction that traditional coatings cannot balance protection and permeability in a strong acid furan resin sand system, and ensures the functional synergy and casting quality consistency of the lost foam-furan resin self-hardening sand composite molding process in the two stages of molding curing and casting gasification.
[0045] Example 5: The shell material of the phase change microcapsules is a thermosetting resin with limited mechanical strength. If high-shear force and high-speed stirring are used during the coating preparation process, the microcapsule shell wall is easily ruptured and the core material leaks, causing the microcapsules to lose their phase change function before coating. Insufficient stirring, on the other hand, will lead to uneven dispersion, agglomeration, or sedimentation of the microcapsules, affecting the consistency of the coating performance. Therefore, a preparation method that can achieve uniform dispersion of the microcapsules while avoiding mechanical damage is needed.
[0046] like Figure 1 As shown, this embodiment provides a method for preparing an isolation coating for the interface between the lost foam casting white mold and the furan resin sand, including the following steps:
[0047] S1. Add the phase change microcapsules to the mixture consisting of refractory aggregate, liquid medium and additives at a speed of 300-500 rpm, and stir for 5-10 minutes.
[0048] The core material of the phase change microcapsules is an organic phase change material with a melting point of 55–65℃, the shell material is a thermosetting resin with a particle size of 5–30μm, and the content of the phase change microcapsules is 15–25% of the mass of the refractory aggregate; the liquid medium is water, the amount of which makes the final coating solid content 55–65%; the additives include alkaline silica sol, polyvinyl alcohol PVA1788, sodium carboxymethyl cellulose CMC, sodium bentonite and alkylphenol polyoxyethylene ether OP10, and their addition order is as follows: sodium bentonite, alkaline silica sol, PVA1788, CMC, OP10;
[0049] S2. Sodium-based bentonite is pre-hydrated and swollen in 1 / 3 of the total water volume for 30–40 minutes before being added, with a hydration temperature of 20–25℃.
[0050] S3. Before adding the phase change microcapsules, the mixed system is dispersed at high speed of 1500–2000 rpm for 20–30 minutes to form a homogeneous paste system with a viscosity of 8000–15000 mPa·s.
[0051] S4. After adding the phase change microcapsules, stir at 350–450 rpm for 6–9 minutes, and let the system stand for 12–14 minutes for natural defoaming, or vacuum defoam at 0.08–0.09 MPa for 5–7 minutes.
[0052] The key process control point is adding the phase change microcapsules to the mixing system at a low speed of 300–500 rpm and stirring for 5–10 minutes. Low-speed stirring effectively avoids mechanical damage to the microcapsule shell material from high shear forces, ensuring that the phase change microcapsules maintain structural integrity and prevent core leakage during coating preparation. It also ensures that the microcapsules are uniformly dispersed in the coating matrix without agglomeration or sedimentation. The core material, shell material, particle size, and content of the phase change microcapsules are the same as in Example 1, and their functions will not be repeated.
[0053] Water is used as the liquid medium, and its dosage is controlled to achieve a final coating solids content of 55–65%. Using water as the medium is low-cost and environmentally friendly. Furthermore, this solids content range works synergistically with the physicochemical properties of water to optimize the rheological stability and drying film-forming kinetics of the mixture: during the molding and curing stage, the appropriate solids content ensures uniform dehydration and densification of the coating at low temperatures; during the casting and vaporization stage, after water molecules evaporate upon heating, phase change microcapsules are uniformly dispersed in the coating matrix, forming a controllable microporous network.
[0054] The additives include alkaline silica sol, polyvinyl alcohol (PVA1788), sodium carboxymethyl cellulose (CMC), sodium bentonite, and alkylphenol polyoxyethylene ether (OP10), added in the following order: sodium bentonite, alkaline silica sol, PVA1788, CMC, and OP10. This order of addition follows a clear functional logic: sodium bentonite is first fully hydrated in the liquid medium, constructing a stable three-dimensional suspension network and providing a uniform dispersion basis for subsequent components; alkaline silica sol is then introduced to avoid premature condensation reactions with the polymer binder, ensuring its ability to form a dense ceramic phase at high temperatures; polyvinyl alcohol (PVA1788) and sodium carboxymethyl cellulose (CMC) are added sequentially after the suspension system has stabilized, providing strong room-temperature adhesion and good rheological regulation, respectively, enhancing the structural integrity and crack resistance of the coating during the molding and curing stage; alkylphenol polyoxyethylene ether (OP10), as the last surfactant added, only plays a wetting and dispersing role when the system is basically formed, avoiding damage to the microstructure established in the early stages. In practical applications, the types and order of addition of additives can be adjusted according to the actual formula requirements, and this application does not limit this.
[0055] Sodium-based bentonite is pre-hydrated and swelled in 1 / 3 of the total water volume for 30–40 minutes before addition, at a hydration temperature of 20–25°C. This pre-hydration treatment allows the interlayer structure of sodium-based bentonite to fully absorb water and expand, forming a stable colloidal network. This avoids agglomeration and localized over-thickness caused by rapid water absorption in high-solids content coating systems, thereby significantly improving dispersion uniformity and suspension stability when subsequently added to the main mixing system.
[0056] Before adding the phase change microcapsules, the mixed system is dispersed at high speed of 1500–2000 rpm for 20–30 minutes to form a homogeneous paste system with a viscosity of 8000–15000 mPa·s. This high-speed dispersion is carried out before the addition of microcapsules to fully homogenize the refractory aggregate, liquid medium, and additives, forming a high-viscosity paste matrix. At this point, there are no phase change microcapsules in the system, so no damage to the microcapsules will occur. The high-viscosity paste matrix can effectively restrict the degree of freedom of movement of the phase change microcapsules during subsequent low-speed stirring, buffer the impact of external shear forces on the microcapsule shells, prevent them from breaking due to local hydrodynamic disturbances, and provide a uniform bearing environment for the microcapsules.
[0057] After adding the phase change microcapsules, the stirring speed is 350–450 rpm, and the stirring time is 6–9 minutes. These stirring parameters are further refined: excessive speed or time can easily lead to microcapsule shell rupture, while insufficient speed or time results in uneven dispersion. The parameters of 350–450 rpm and 6–9 minutes ensure uniform dispersion while maximizing the protection of microcapsule integrity. After stirring, the system is allowed to stand for 12–14 minutes for natural defoaming, or vacuum defoamed at 0.08–0.09 MPa for 5–7 minutes. Stirring easily introduces a large number of micron-sized bubbles. If not eliminated in time, these will form penetrating pores during coating drying and curing, weakening its dense acid-resistant ability. Natural defoaming or vacuum defoaming promotes the bubbles to rise, rupture, or escape rapidly, achieving complete removal of the gas phase within the system. This ensures the coating maintains a uniform, dense, and non-porous structure before curing, while preserving the integrity of the phase change microcapsules.
[0058] The preparation method in this embodiment achieves a balance between homogenization of the coating matrix and integrity of the microcapsules through a segmented stirring strategy of "first homogenizing the matrix at high speed, then dispersing the microcapsules at low speed": Before the addition of microcapsules, refractory aggregates, liquid media, and additives are dispersed at high speed to form a high-viscosity homogeneous paste matrix; after the microcapsules are added, they are stirred at low speed to ensure uniform dispersion in the high-viscosity matrix. The high-viscosity matrix restricts the freedom of movement of the microcapsules and buffers shear impact, thereby protecting the microcapsule shell material while achieving uniform dispersion; subsequently, defoaming treatment is used to remove air bubbles, ensuring that the coating is dense and non-porous. The final coating forms a dense acid-resistant barrier during the low-temperature curing stage and achieves high air permeability switching through microcapsule phase change during the high-temperature casting stage.
[0059] The preparation method of this embodiment effectively avoids mechanical damage to the phase change microcapsule shell material caused by high shear force, ensuring the integrity of the microcapsules in coating preparation, drying and subsequent molding processes. It achieves uniform dispersion of microcapsules in the coating matrix without agglomeration or sedimentation, thereby achieving stable filling of the pores between refractory aggregates and constructing a continuous hydrophobic barrier to block the penetration of sulfonic acid curing agent at low temperature. At high temperature, it ensures that the microcapsule shell material degrades completely within the designed temperature range and forms a connected microporous network. It realizes a reliable switch of the coating from a dense and isolated state to a highly permeable and venting state, significantly improving the process stability and coating functional consistency.
[0060] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A separating coating for the interface between lost foam casting white mold and furan resin sand, characterized in that, include: Refractory aggregate and phase change microcapsules; the refractory aggregate includes zircon powder and quartz powder, wherein the mass ratio of zircon powder to quartz powder is 55:10 to 45:15; The core material of the phase change microcapsules is an organic phase change material with a melting point of 55-65℃, the shell material is a thermosetting resin, the particle size is 5-30μm, and the content of the phase change microcapsules is 15-25% of the mass of the refractory aggregate; The organic phase change material is selected from n-alkane C. 20 -C 35 Specifically, it is one or more of n-eicosane, n-docosane, n-tetracosane, n-hexacosane, n-octacosane, n-triane, n-dodecane, n-tetracosane, or n-pentadecane; The thermosetting resin is melamine-formaldehyde resin, which is prepared by reacting melamine and formaldehyde at a molar ratio of 1:2.0-3.5, with methanol added as a co-solvent during the reaction. The shell wall thickness of the melamine-formaldehyde resin is 0.8-1.8 μm, and the crosslinking density in the shell layer is 0.45-0.65 mmol / g.
2. The isolation coating for the interface between the lost foam casting white mold and the furan resin sand according to claim 1, characterized in that, The phase change microcapsules have a particle size D50 of 10-15 μm and a particle size distribution span D90 / D10 ≤ 3.0; the zircon powder has an average particle size of 4.5-5.5 μm and the quartz powder has an average particle size of 3.0-4.0 μm, and both of their particle size distributions satisfy D95 ≤ 12 μm.
3. The isolation coating for the interface between the lost foam casting white mold and the furan resin sand according to claim 1, characterized in that, The isolation coating also includes alkaline silica sol as a high-temperature binder, with a SiO2 content of 29-31% and a pH of 9.2-9.8; the alkaline silica sol has a particle diameter of 5-15 nm and a SiO2 to water molar ratio of 1:8-1:12; the isolation coating has a solid content of 58-62% and a Baume degree of 65-70°Bé; the dry film thickness of the isolation coating is 1.8-2.5 mm.
4. The isolation coating for the interface between the lost foam casting white mold and the furan resin sand according to claim 1, characterized in that, The isolation coating is used in the composite molding process of lost foam casting and furan resin self-hardening sand. The curing agent of furan resin sand is one or more of p-toluenesulfonic acid, naphthalenesulfonic acid formaldehyde condensate or benzenesulfonic acid, with a pH of 1.5-2.
5. The white mold is expandable polystyrene (EPS), with a density of 18-22 g / L and a particle size of 0.3-0.8 mm.
5. A method for preparing an isolation coating for the interface between lost foam casting white mold and furan resin sand, characterized in that, Includes the following steps: Add the phase change microcapsules to the mixture of refractory aggregate, liquid medium and additives at a speed of 300-500 rpm and stir for 5-10 minutes. The core material of the phase change microcapsules is an organic phase change material with a melting point of 55-65℃, the shell material is a thermosetting resin, the particle size is 5-30μm, and the content of the phase change microcapsules is 15-25% of the mass of the refractory aggregate; the liquid medium is water, the amount of which makes the final coating solid content 55-65%; the additives include alkaline silica sol, polyvinyl alcohol PVA1788, sodium carboxymethyl cellulose CMC, sodium bentonite and alkylphenol polyoxyethylene ether OP10, and their addition order is: sodium bentonite, alkaline silica sol, PVA1788, CMC, OP10; The sodium-based bentonite is pre-hydrated and swollen in 1 / 3 of the total water volume for 30-40 minutes before being added, and the hydration temperature is 20-25℃. Before adding the phase change microcapsules, the mixture is dispersed at high speed of 1500-2000 rpm for 20-30 minutes to form a homogeneous paste system with a viscosity of 8000-15000 mPa·s. After the phase change microcapsules are added, the stirring speed is 350-450 rpm and the stirring time is 6-9 minutes. The system is allowed to stand for 12-14 minutes for natural defoaming, or vacuum defoaming is performed at 0.08-0.09 MPa for 5-7 minutes.
Citation Information
Patent Citations
Improved water based coating for lost foam
CN1663707A