A water-based ceramic release agent for RKEF ferronickel smelting submerged arc furnace tapping chain conveyer and a preparation and application method thereof
The water-based ceramic release agent with a SiO₂-Al₂O₃-Fe₂O₃-CaO-MgO multi-component compound system solves the problem of unstable demolding at high temperatures in nickel-iron smelting, realizes efficient automated continuous operation, and improves the production efficiency and mold service life of nickel-iron smelting.
Patent Information
- Application Number
- CN202611398327.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-10
- Publication Date
- 2026-11-20
AI Technical Summary
In existing nickel-iron smelting processes, limestone release agents tend to stick to the mold at high temperatures, resulting in unstable release effects and hindering automated continuous operation. Furthermore, the high cost makes it impossible to meet the high-temperature casting requirements of the iron chain plate machine at the RKEF nickel-iron smelting submerged arc furnace.
A water-based ceramic release agent using a SiO₂-Al₂O₃-Fe₂O₃-CaO-MgO multi-component compound system, by controlling particle size and density and adding suspending stabilizers and dispersants, forms a stable ceramic isolation layer at high temperatures, achieving rapid sintering and high adhesion, suitable for continuous spraying operations.
A dense ceramic isolation layer is formed at 1430–1480℃, preventing nickel-iron from adhering to the mold. The demolding rate is over 99%, and the spraying adhesion rate is as high as 95%, reducing manual labor intensity, improving casting efficiency, and extending mold life.
Smart Images

Figure CN123128433A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of refractory materials and metallurgical auxiliary materials technology, specifically relating to a water-based ceramic release agent for the iron chain plate machine of the RKEF nickel-iron smelting submerged arc furnace, as well as the preparation method and application method of the release agent. Background Technology
[0002] The rotary kiln electric arc furnace (RKEF) process is currently the mainstream process worldwide for producing nickel-iron alloys from laterite nickel ore. The smelting temperature inside the RKEF reaches 1450–1600℃. Molten nickel-iron flows through the tap into the tundish, and then is distributed to the casting molds on the chain conveyor for continuous casting. To prevent chemical adhesion and sintering between the high-temperature molten nickel-iron and the molds, a release agent must be sprayed onto the inner surface of the molds before casting.
[0003] Currently, nickel-iron smelting enterprises generally use limestone mixed with water as a release agent. This technology has the following prominent problems: (1) The concentration and density of limestone slurry are difficult to control precisely, the slurry quality fluctuates greatly, the release effect is unstable, and nickel-iron blocks often stick to the mold, requiring manual removal, which seriously reduces casting efficiency; (2) A single limestone system is prone to over-sintering or insufficient sintering at high temperatures of 1430-1480℃, and the residue adheres to the mold surface, resulting in a short mold cleaning cycle and frequent shutdowns for cleaning; (3) The consumption of limestone is large, and the cost is high; (4) The manual batching and manual spraying methods are outdated and cannot achieve automated continuous operation.
[0004] For the non-ferrous metal die-casting industry, several water-based release agent patents have been reported. For example, CN118808542A discloses a silicon oxynitride ceramic coating release agent suitable for low-melting-point metals such as aluminum and tin, but unable to withstand the ultra-high temperatures of molten nickel-iron. Another release agent for casting refractory materials is mainly composed of silicon carbide and polyvinyl alcohol, primarily used to prevent sand from sticking to sand molds, which is incompatible with the continuous spraying release requirements of chain conveyor casting molds. Currently, there is no systematic technical solution, domestically or internationally, specifically for water-based ceramic release agents for RKEF nickel-iron smelting submerged arc furnace iron chain conveyors.
[0005] Therefore, developing a water-based ceramic release agent with excellent high-temperature sintering isolation properties, high coating adhesion, easy demolding, no contamination of finished nickel-iron products, and suitability for continuous spraying operations is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0006] To address the shortcomings of existing release agents for nickel-iron casting, such as easy sticking to the mold at high temperatures, unstable release effect, and inability to achieve automated continuous operation, this invention provides a water-based ceramic release agent for the iron chain conveyor of an RKEF nickel-iron smelting submerged arc furnace, along with its preparation and application methods. This release agent can rapidly form a uniform ceramic isolation layer during the nickel-iron molten casting process at 1430–1480℃, exhibits controllable sintering behavior, high coating adhesion, thorough demolding, and does not contaminate the finished nickel-iron product.
[0007] The primary technical objective of this invention is to provide a water-based ceramic release agent for use in the iron chain conveyor of an RKEF nickel-iron smelting submerged arc furnace. Addressing the technical shortcomings of existing limestone release agents for nickel-iron casting, which are prone to sticking to the mold at high temperatures and have unstable release effects, this invention provides a water-based ceramic release agent with a SiO2-Al2O3-Fe2O3-CaO-MgO multi-component composite system.
[0008] The release agent is prepared from the following raw materials in parts by weight: 40-60 parts of SiO2; Al2O3 15-40 parts; Fe2O3 3-10 parts; CaO 0.5–3.5 parts; MgO 0.5 to 3.5 parts.
[0009] The apparent powder density of the release agent is 0.8–1.2 g / cm³. 3 The tap density is 1.3–1.8 g / cm³. 3 The particle size range of the release agent is: a passing rate of not less than 85% through a 180-mesh standard sieve. After being mixed with water to form a slurry, the release agent exhibits a spray adhesion rate greater than 95%.
[0010] Further, the release agent is made from the following raw materials in parts by weight: 45-55 parts SiO2, 20-35 parts Al2O3, 5-8 parts Fe2O3, 1.0-2.5 parts CaO, and 1.0-2.5 parts MgO.
[0011] Furthermore, in order to improve the suspension stability and storage uniformity of the release agent slurry, the raw materials also include 0.1 to 2.0 parts of a suspension stabilizer, wherein the suspension stabilizer is selected from one or more of polyvinyl alcohol (PVA), sodium carboxymethyl cellulose (CMC-Na), and sodium polyacrylate (PAAS).
[0012] Furthermore, in order to improve the dispersibility of the powder in water and prevent agglomeration, the raw materials also include 0.05 to 1.5 parts of a dispersant, wherein the dispersant is sodium hexametaphosphate or polyethylene glycol (PEG-4000).
[0013] The design principle of the chemical composition is as follows: SiO2 and Al2O3 constitute the main system with high refractoriness. At high temperatures, they react to form a mullite (3Al2O3·2SiO2) phase, creating a continuous and stable ceramic isolation layer that prevents direct contact between the molten nickel-iron and the mold. The appropriate introduction of MgO adjusts the sintering temperature range of the system, preventing over- or under-burning. Fe2O3 reacts with SiO2 at high temperatures to form a eutectic phase (such as fir olivine 2FeO·SiO2), promoting rapid sintering and densification of the release agent layer in the early stages of casting. CaO, as a slag-forming component regulator, controls the viscosity and melting point of residual slag, preventing excessive adhesion. The five components work synergistically, balancing suspension dispersibility, high-temperature sintering behavior, and release agent isolation effect.
[0014] The second technical objective of this invention is to provide a method for preparing the above-mentioned water-based ceramic release agent, comprising the following steps: S1: Weigh out SiO2, Al2O3, Fe2O3, CaO and MgO powder raw materials according to the ratio, mix them evenly to obtain mixed dry powder.
[0015] S2: Add a suspending stabilizer and / or a dispersant to the mixed dry powder, and continue stirring and mixing for 15 to 30 minutes to obtain a modified mixed powder.
[0016] S3: Add the modified mixed powder and water to a mixing tank at a mass ratio of 1:1.5 to 1:3.0, and stir at a speed of 200 to 600 r / min for 20 to 40 minutes to prepare a uniform water-based ceramic slurry. Preferably, the powder-to-water ratio is 1:1.8 to 1:2.5, the stirring speed is 300 to 500 r / min, and the stirring time is 25 to 35 minutes.
[0017] S4: Pass the water-based ceramic slurry through a 100-mesh sieve to remove large particulate impurities, thus obtaining the finished release agent slurry. The solid content of the obtained slurry is approximately 30% to 45%.
[0018] The third technical objective of this invention is to provide a method for applying the above-mentioned water-based ceramic release agent, wherein the release agent is applied to the iron chain conveyor of the RKEF nickel-iron smelting submerged arc furnace, specifically including the following steps: A1: The prepared water-based ceramic release agent slurry is sprayed onto the inner surface of the casting mold of the chain conveyor, with a spraying thickness of 0.3 to 1.5 mm, preferably 0.5 to 1.0 mm.
[0019] A2: After spraying, wait 30 to 60 seconds for the coating to level naturally and dry initially. Then, pour the molten nickel-iron from the electric arc furnace (temperature 1430 to 1480°C) into the mold for casting.
[0020] A3: After the nickel-iron melt solidifies (usually after cooling for 3 to 8 minutes), the mold is turned over or vibrated, and the nickel-iron block is automatically demolded. The release agent coating remaining on the mold surface is loose and flaky, which is easy to remove or cover before the next spraying.
[0021] Optimal spraying process parameters: compressed air pressure 0.4–0.7 MPa, distance between spray gun and inner surface of mold 20–40 cm, spraying angle 70°–90°. Spraying operation should be carried out 5–15 minutes before tapping.
[0022] The technical solution provided by this invention has the following beneficial effects: (1) The water-based ceramic release agent of the present invention adopts a multi-component compound system of SiO2-Al2O3-Fe2O3-CaO-MgO. At the casting temperature of nickel-iron melt of 1430~1480℃, it can quickly form a dense ceramic isolation layer with mullite as the main crystalline phase, effectively preventing the chemical adhesion and mechanical adhesion between nickel-iron and the mold. The release rate can reach more than 99%, and completely solve the problem of sticking to the mold.
[0023] (2) By strictly controlling the particle size (180 mesh passing rate ≥85%) and apparent density / tapered density of the release agent, combined with the addition of suspension stabilizer and dispersant, the prepared slurry has the characteristics of high stirring suspension rate and low particle settling rate (settling rate <5% after standing for 2 hours), and the spraying adhesion rate is as high as 95% or more, with uniform coating and no peeling.
[0024] (3) The release agent of the present invention does not contain phosphorus, sulfur and other elements that are harmful to the quality of nickel iron, does not contaminate the finished nickel iron product, and the residue after demolding is easy to clean, and the service life of the mold is extended by more than 30%.
[0025] (4) The preparation method of the present invention is simple and easy to industrialize; the application method is simple and can realize continuous spraying operation, greatly reduce the intensity of manual labor and improve casting efficiency.
[0026] (5) This invention is specifically designed for the harsh working conditions of the iron chain plate machine for RKEF nickel-iron smelting submerged arc furnace, filling the technological gap in this sub-field both domestically and internationally. Attached Figure Description
[0027] Figure 1 This is a flow chart illustrating the preparation process of the water-based ceramic release agent of this invention. Detailed Implementation
[0028] The present invention will now be clearly and completely described through specific embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention. Example 1
[0029] This embodiment provides a water-based ceramic release agent for the iron chain plate machine of the RKEF nickel-iron smelting submerged arc furnace, which is made from the following raw materials in parts by weight: 50 parts SiO2, 30 parts Al2O3, 8 parts Fe2O3, 2.0 parts CaO, and 2.0 parts MgO.
[0030] The apparent powder density of the release agent described in this embodiment is 1.0 g / cm³. 3 The tap density is 1.5 g / cm³. 3 The pass rate for 180 mesh is 92%.
[0031] The preparation method of the water-based ceramic release agent for the iron chain conveyor of the RKEF nickel-iron smelting submerged arc furnace is as follows: S1: Weigh out SiO2, Al2O3, Fe2O3, CaO and MgO powder raw materials according to the above ratio, mix them evenly to obtain mixed dry powder.
[0032] S2: Add 0.5 parts of sodium carboxymethyl cellulose (CMC-Na) as a suspension stabilizer and 0.2 parts of sodium hexametaphosphate as a dispersant to the mixed dry powder, and continue stirring and mixing for 20 minutes to obtain the modified mixed powder.
[0033] S3: Add the modified mixed powder and water to a mixing tank at a powder-to-water mass ratio of 1:2.0, and stir at 400 r / min for 30 minutes to prepare a uniform water-based ceramic slurry.
[0034] S4: Pass the water-based ceramic slurry through a 100-mesh sieve to remove large particulate impurities, thus obtaining the finished release agent slurry. The density of the obtained slurry is 1.35 g / cm³. 3 .
[0035] The application method of the water-based ceramic release agent prepared for the iron chain conveyor of the RKEF nickel-iron smelting submerged arc furnace is as follows: A1: Spray the prepared release agent slurry onto the inner surface of the chain plate machine casting mold with a spray thickness of 0.8 mm, compressed air pressure of 0.5 MPa, a distance of 30 cm between the spray gun and the inner surface of the mold, and a spray angle of 90°. Complete the spraying 10 minutes before tapping the iron.
[0036] A2: After spraying, wait 45 seconds for the coating to level naturally and dry initially, then pour molten nickel-iron at 1450℃ into the mold for casting.
[0037] A3: After the nickel-iron melt solidifies and cools for 5 minutes, the mold is flipped over, and the nickel-iron block is automatically demolded.
[0038] Testing showed that the release agent slurry obtained in this embodiment had a spray adhesion rate of 96%, a settling rate of <5% after standing for 2 hours, and a release rate of >99%. After 8 hours of continuous use, no mold cleaning was required, no iron adhered to the mold surface, the release agent coating was uniformly sintered, and peeled off in flakes. No residual release agent was detected in the finished nickel-iron product. Example 2
[0039] This embodiment provides a water-based ceramic release agent for use in the iron chain conveyor of an RKEF nickel-iron smelting submerged arc furnace, which is made from the following raw materials in parts by weight: 55 parts SiO2, 25 parts Al2O3, 6 parts Fe2O3, 1.5 parts CaO, and 1.5 parts MgO.
[0040] The apparent powder density of the release agent described in this embodiment is 0.95 g / cm³. 3 The tap density is 1.45 g / cm³. 3 The 180-mesh pass rate is 90%.
[0041] The preparation method of the water-based ceramic release agent for the iron chain conveyor of the RKEF nickel-iron smelting submerged arc furnace is as follows: S1: Weigh out SiO2, Al2O3, Fe2O3, CaO and MgO powder raw materials according to the above ratio, mix them evenly to obtain mixed dry powder.
[0042] S2: Add 0.8 parts of polyvinyl alcohol (PVA) suspension stabilizer and 0.3 parts of polyethylene glycol-4000 dispersant to the mixed dry powder, and continue stirring and mixing for 18 minutes to obtain modified mixed powder.
[0043] S3: Add the modified mixed powder and water to a mixing tank at a powder-to-water mass ratio of 1:2.2, and stir at 350 r / min for 35 minutes to prepare a uniform water-based ceramic slurry.
[0044] S4: Pass the water-based ceramic slurry through a 100-mesh sieve to remove large particulate impurities, and the finished release agent slurry is obtained.
[0045] The application method of the water-based ceramic release agent prepared for the iron chain conveyor of the RKEF nickel-iron smelting submerged arc furnace is as follows: A1: Spray the prepared release agent slurry onto the inner surface of the chain plate machine casting mold with a spray thickness of 0.6 mm, compressed air pressure of 0.5 MPa, a distance of 30 cm between the spray gun and the inner surface of the mold, and a spray angle of 80°. Complete the spraying 12 minutes before tapping the iron.
[0046] A2: After spraying, wait 40 seconds for the coating to level naturally and dry initially, then pour molten nickel-iron at 1470℃ into the mold for casting.
[0047] A3: After the nickel-iron melt solidifies and cools for 4 minutes, the mold is flipped over, and the nickel-iron block is automatically demolded.
[0048] Testing showed that the release agent slurry obtained in this embodiment had a spray adhesion rate of 97%, a settling rate of <5% after standing for 2 hours, and a release rate of >99%. No sticking occurred after 12 hours of continuous production, demonstrating excellent release performance. Example 3
[0049] This embodiment provides a water-based ceramic release agent for use in the iron chain conveyor of the RKEF nickel-iron smelting submerged arc furnace, which is made from the following raw materials in parts by weight: 45 parts SiO2, 35 parts Al2O3, 7 parts Fe2O3, 2.5 parts CaO, and 2.5 parts MgO.
[0050] The apparent powder density of the release agent described in this embodiment is 1.1 g / cm³. 3 The tap density is 1.6 g / cm³. 3 The pass rate for 180 mesh is 88%.
[0051] The preparation method of the water-based ceramic release agent for the iron chain conveyor of the RKEF nickel-iron smelting submerged arc furnace is as follows: S1: Weigh out SiO2, Al2O3, Fe2O3, CaO and MgO powder raw materials according to the above ratio, mix them evenly to obtain mixed dry powder.
[0052] S2: Add 1.0 part of sodium polyacrylate (PAAS) suspension stabilizer to the mixed dry powder, and continue stirring and mixing for 25 minutes to obtain the modified mixed powder.
[0053] S3: Add the modified mixed powder and water to a mixing tank at a powder-to-water mass ratio of 1:1.8, and stir at 450 r / min for 25 minutes to prepare a uniform water-based ceramic slurry.
[0054] S4: Pass the water-based ceramic slurry through a 100-mesh sieve to remove large particulate impurities, and the finished release agent slurry is obtained.
[0055] The application method of the water-based ceramic release agent prepared for the iron chain conveyor of the RKEF nickel-iron smelting submerged arc furnace is as follows: A1: Spray the prepared release agent slurry onto the inner surface of the chain plate machine casting mold with a spray thickness of 1.0 mm, compressed air pressure of 0.6 MPa, a distance of 25 cm between the spray gun and the inner surface of the mold, a spray angle of 90°, and complete the spraying 8 minutes before tapping the iron.
[0056] A2: After spraying, wait 50 seconds for the coating to level naturally and dry initially, then pour molten nickel-iron at 1440℃ into the mold for casting.
[0057] A3: After the nickel-iron melt solidifies and cools for 6 minutes, the mold is flipped over, and the nickel-iron block is automatically demolded.
[0058] Testing showed that the release agent slurry obtained in this embodiment had a spray adhesion rate of 95.5%, a settling rate of <5% after standing for 2 hours, and a release rate of >99%. The mold cleaning cycle was extended from once every 2 hours to once every 8 hours, and the demolding was satisfactory. Comparative Example 1
[0059] This comparative example provides a release agent slurry formulated with industrial-grade limestone powder.
[0060] It is prepared from the following raw materials in parts by weight: 100 parts of industrial grade limestone powder (CaO content ≥ 52%), mixed with water to form a slurry with a density of 1.25 g / cm³. 3 .
[0061] Its preparation method is as follows: Industrial-grade limestone powder and water are added to a mixing tank in a certain proportion and stirred until evenly mixed to obtain limestone slurry.
[0062] Its application method is as follows: The prepared limestone slurry was sprayed onto the inner surface of the same chain plate machine casting mold, with a spray thickness of about 0.8 mm. The spraying was completed 10 minutes before tapping the iron, and then molten nickel-iron at a temperature of 1450℃ was poured into the mold for casting.
[0063] Testing revealed that the spray adhesion rate of the release agent slurry obtained in this comparative example was only about 70%. After nickel-iron casting, about 30% of the molds showed severe sticking, requiring manual removal and a production stoppage every 2 hours for cleaning. Comparative Example 2
[0064] This comparative example provides a release agent that does not contain Fe2O3 and MgO, which is prepared from the following raw materials in parts by weight: 55 parts SiO2, 40 parts Al2O3, and 2.0 parts CaO.
[0065] Its preparation method is as follows: S1: Weigh the SiO2, Al2O3 and CaO powder raw materials according to the above ratio, mix them evenly, and obtain mixed dry powder.
[0066] S2: To eliminate the interference of differences in construction performance on the test results, add 0.5 parts of sodium carboxymethyl cellulose (CMC-Na) suspension stabilizer and 0.2 parts of sodium hexametaphosphate dispersant of the same type and amount as in Example 1 to the mixed dry powder, and continue to stir and mix for 20 minutes to obtain the modified mixed powder.
[0067] S3: Add the modified mixed powder and water to a mixing tank at a powder-to-water mass ratio of 1:2.0, and stir at 400 r / min for 30 minutes to prepare a water-based ceramic slurry.
[0068] S4: Pass the water-based ceramic slurry through a 100-mesh sieve to obtain the finished slurry.
[0069] Its application method is as follows: A1: Spray the prepared release agent slurry onto the inner surface of the chain plate machine casting mold, with a spray thickness of 0.8 mm.
[0070] A2: After spraying, wait 45 seconds, then pour the molten nickel-iron at 1450℃ into the mold for casting.
[0071] A3: After the nickel-iron melt solidifies, cool it for 5 minutes, then flip the mold to remove it.
[0072] Testing revealed that the release agent obtained in this comparative example had a slow sintering rate at 1450℃, resulting in a loose coating. After demolding, some nickel and iron remained slightly adhered, with a demolding rate of approximately 85%. Detection and Analysis
[0073] The release agents prepared in Examples 1-3 were compared with those in Comparative Examples 1-2 under the same conditions. The test methods for each performance are as follows: (1) Spraying adhesion rate test: Spray release agent slurry on the inner surface of the casting mold of the chain plate machine. After spraying, weigh the increase in weight of the mold. Calculate the adhesion rate by the ratio of theoretical spraying amount to actual adhesion amount. Each group of tests shall have no less than 5 molds and take the arithmetic mean as the final result.
[0074] (2) Demolding rate detection: The percentage of nickel-iron blocks that automatically demold during continuous casting is counted. The percentage of nickel-iron blocks that automatically demold is taken as the demolding rate, and the number of blocks counted is not less than 100.
[0075] (3) Settling rate test: Let the prepared release agent slurry stand for 2 hours, take the upper layer of slurry to determine the solid content, and calculate the settling rate based on the solid content change rate.
[0076] Table 1 summarizes the formulation composition and main performance data of each embodiment and comparative example.
[0077] Table 1 Comparison of formulation composition and performance between each embodiment and the comparative example
[0078] As shown in Table 1, the release agents of the various embodiments of the present invention are significantly superior to the comparative examples in terms of spray adhesion rate, release rate, slurry suspension stability, and mold cleaning cycle. Comparative Example 1 uses traditional limestone slurry, resulting in low adhesion rate and severe mold sticking; Comparative Example 2's formulation does not contain Fe2O3 and MgO components (its suspension stabilizer, dispersant types and amounts are the same as in Example 1), and its sintering speed at 1450℃ is slow, the coating is loose, and the release rate is only about 85%, proving that the lack of Fe2O3 and MgO is the key factor leading to a significant decrease in release performance. Therefore, the SiO2-Al2O3-Fe2O3-CaO-MgO multi-component composite system of the present invention is significantly superior to the prior art in terms of high-temperature sintering behavior, adhesion rate, and actual release effect.
[0079] The water-based ceramic release agent and its preparation and application methods provided by this invention can be widely applied in RKEF nickel-iron smelting enterprises, especially suitable for chain-type continuous casting systems. By matching with automatic spraying equipment, the nickel-iron casting process can be upgraded to be intelligent and green, resulting in good economic and social benefits.
[0080] The above description is merely a specific embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural or procedural transformations made using the content of the present invention specification, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.
Claims
1. A water-based ceramic release agent for use in the iron chain conveyor of an RKEF nickel-iron smelting submerged arc furnace, characterized in that, It is prepared from the following raw materials in parts by weight: 40-60 parts of SiO2; Al2O3 15-40 parts; Fe2O3 3-10 parts; CaO 0.5–3.5 parts; MgO 0.5 to 3.5 parts.
2. The water-based ceramic release agent according to claim 1, characterized in that, It is prepared from the following raw materials in parts by weight: 45-55 parts SiO2, 20-35 parts Al2O3, 5-8 parts Fe2O3, 1.0-2.5 parts CaO, and 1.0-2.5 parts MgO.
3. The water-based ceramic release agent according to claim 1, characterized in that, The apparent powder density of the release agent is 0.8–1.2 g / cm³. 3 The tap density is 1.3–1.8 g / cm³. 3 The particle size range of the release agent is such that the passing rate through a 180-mesh standard sieve is not less than 85%.
4. The water-based ceramic release agent according to claim 1, characterized in that, The raw materials also include 0.1 to 2.0 parts of a suspension stabilizer, which is selected from one or more of polyvinyl alcohol, sodium carboxymethyl cellulose, and sodium polyacrylate.
5. The water-based ceramic release agent according to claim 1, characterized in that, The raw materials also include 0.05 to 1.5 parts of a dispersant, which is sodium hexametaphosphate or polyethylene glycol.
6. A method for preparing a water-based ceramic release agent as described in any one of claims 1 to 5, characterized in that, Includes the following steps: S1: Weigh out SiO2, Al2O3, Fe2O3, CaO and MgO powder raw materials according to the ratio, mix them evenly to obtain mixed dry powder; S2: Add a suspending stabilizer and / or dispersant to the mixed dry powder, and continue stirring and mixing for 15 to 30 minutes to obtain a modified mixed powder; S3: Add the modified mixed powder and water to a mixing tank at a mass ratio of 1:1.5 to 1:3.0, and stir at a speed of 200 to 600 r / min for 20 to 40 minutes to prepare a uniform water-based ceramic slurry; S4: Pass the water-based ceramic slurry through a 100-mesh sieve to remove large particulate impurities, and the finished release agent slurry is obtained.
7. The preparation method according to claim 6, characterized in that, The modified mixed powder described in S3 has a mass ratio of 1:1.8 to 1:2.5 to water, a stirring speed of 300 to 500 r / min, and a stirring time of 25 to 35 minutes.
8. A method for applying the water-based ceramic release agent as described in any one of claims 1 to 5, characterized in that, Includes the following steps: A1: The prepared water-based ceramic release agent slurry is sprayed onto the inner surface of the casting mold of the chain conveyor, with a spraying thickness of 0.3 to 1.5 mm; A2: After spraying, wait 30 to 60 seconds for the coating to flow naturally and dry initially, then pour the molten nickel-iron at a temperature of 1430 to 1480°C into the mold for casting. A3: After the nickel-iron melt solidifies, the nickel-iron block will automatically demold.
9. The application method according to claim 8, characterized in that, The coating thickness described in A1 is 0.5–1.0 mm, the compressed air pressure is 0.4–0.7 MPa, and the distance between the spray gun and the inner surface of the mold is 20–40 cm.
10. The application method according to claim 8, characterized in that, The spraying described in A1 is carried out 5 to 15 minutes before tapping.
Citation Information
Patent Citations
Nonferrous metal release agent based on silicon oxynitride ceramic coating and preparation method
CN118808542A