Large aperture thin wall shell shell mold layer coating hanging drying method and application

By setting a modified polyvinyl alcohol sacrificial layer and a six-layer gradient coating process in the through holes of the large-diameter thin-walled shell wax mold, the problem of through hole blockage caused by wax accumulation was solved, achieving high-precision and high-strength preparation of the shell mold and ensuring the quality of the casting.

CN123128445APending Publication Date: 2026-11-20XUANCHENG CHIEFTECH METAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611420625.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-14
Publication Date
2026-11-20

Smart Images

  • Figure CN123128445A_ABST
    Figure CN123128445A_ABST
Patent Text Reader

Abstract

The application discloses a large-aperture thin-wall shell shell mold layering coating and drying method and application, comprising the following steps: S1 wax mold pretreatment: the wax mold group is cleaned by using a cleaning agent with a pH value of 4-6, the cleaning time is 15-30 seconds, and then the surface moisture is blown dry by compressed air; the application sets a modified polyvinyl alcohol sacrificial layer on the inner wall of the shell mold through hole, the sacrificial layer is dissolved by high-temperature and high-pressure steam in the wax removal process and is discharged with the wax removal liquid, so that a compensation gap is formed between the inner wall of the shell mold through hole and the wax mold; the gap becomes a reserved expansion allowance of the inner wall of the shell mold through hole after baking, effectively compensates the thermal expansion of the shell mold, avoids the through hole from being reduced in diameter, deformed and cracked, and significantly improves the through hole diameter precision and roundness of the large-aperture thin-wall shell casting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of investment casting technology, and in particular to a method and application for layered coating and drying of large-diameter thin-walled shell molds. Background Technology

[0002] Investment casting is the main forming process for producing complex thin-walled castings such as aero-engine casings, gas turbine shells, and spacecraft structural components. The quality of the shell mold (mold) preparation directly affects the dimensional accuracy, surface quality, and yield of the castings.

[0003] Large-aperture thin-walled shells present unique technical challenges in shell mold preparation due to their large through-hole or blind-hole structures. Current shell-making processes typically employ multi-layer coating, where a wax mold is sequentially immersed in a silica sol-based refractory slurry, sprinkled with sand, and dried layer by layer to form a ceramic shell of a certain thickness. However, during the coating process, the slurry easily accumulates on the inner walls and edges of the through-holes. This accumulation intensifies with each coating layer, significantly reducing the effective diameter of the through-holes and even causing complete blockage. This not only affects the smooth removal of wax during the subsequent dewaxing process—where the wax melts and vaporizes at high temperatures, and if the liquid or gas cannot be removed promptly, the shell will crack, forming microcracks—but also directly leads to the casting failing to form or developing shrinkage defects due to poor heat dissipation after forming. Summary of the Invention

[0004] To address the shortcomings of existing technologies, this invention provides the following technical solution: On the one hand, a method for layering and drying a large-aperture thin-walled shell mold is provided, including the following steps: S1 Wax Model Pretreatment: Clean the wax model assembly with a cleaning agent with a pH value of 4-6 for 15-30 seconds, and then dry the surface moisture with compressed air. S2 Sacrificial Layer Forming: Inject the modified polyvinyl alcohol film-forming agent solution into the inner cavity of the shell through hole, let it stand for 2-4 seconds, and then blow out the excess solution to form a sacrificial layer with a thickness of 0.2-0.5 mm on the inner wall of the through hole. After drying, the resulting sacrificial layer does not dissolve or swell under the condition of surface slurry coating, but can dissolve or decompose under dewaxing conditions; dry at a temperature of 25±2℃ and a humidity of 40±5% for 5-10 minutes. S3 Surface Coating and Type Casting Blowing: Immerse the wax model processed in step S2 into the surface slurry at an angle of 30-45° for 10-15 seconds. The surface slurry covers the outer layer of the sacrificial layer. After removal, use compressed air to blow slurry at specific points on the type casting area to eliminate air bubbles and remove excess slurry. S4 Through-hole Protection Treatment: After the surface layer is sanded and dried, the through-holes of the shell are pre-wetted with silica sol for 2-3 seconds, and then the second layer is applied. S5 Six-Layer Coating: Apply, sand, and dry the first to sixth layers sequentially according to the following parameters: First layer: Slurry concentration 40-50 seconds (4# cup), sprinkle with 100-120 mesh zircon sand, dry for 6 hours at 23±1℃ and 80±5% humidity; Second layer: Slurry concentration 25-32 seconds (5# cup), sprinkle with 60-mesh Malaysian sand, dry for 4 hours, temperature 23±1℃, humidity 80±5%; Third layer: Slurry concentration 15-23 seconds (5# cup), sprinkle with 35-mesh Malaysian sand, dry for 4 hours at 23±1℃ and 45±5% humidity; Fourth layer: Slurry concentration 9-13 seconds (5# cup), sprinkle with 22-mesh Malaysian sand, dry for 4 hours at 23±1℃ and 45±5% humidity; Fifth layer: Slurry concentration 8-11 seconds (5# cup), sprinkle with 22-mesh Malaysian sand, dry for 4 hours at 23±1℃ and 45±5% humidity; Sixth layer: Slurry concentration 6-8 seconds (5# cup), no sand sprinkling, drying for more than 10 hours, temperature 23±1℃, humidity 45±5%; The slurry includes silica sol binder and refractory powder; wherein, the refractory powder of the first layer of slurry is zirconium powder, and the refractory powder of the second to sixth layers of slurry is mullite powder; the pH value of each layer of slurry is controlled between 9.2 and 10.6. S6 No Slurry Accumulation Control: After each layer of coating is applied, the slurry is suspended and controlled until it no longer drips continuously. Then, sand is sprinkled. After sprinkling the sand, compressed air is used to blow away the slurry accumulation and loose sand in the duct area. S7 Dewaxing and Sacrificial Layer Removal: After all six layers of coating and drying are completed, the module is placed in a dewaxing kettle for dewaxing. High-temperature and high-pressure water vapor in the dewaxing kettle penetrates through the shell mold pores and contacts the sacrificial layer. The sacrificial layer dissolves or decomposes and is discharged with the dewaxing liquid, forming a compensation gap between the inner wall of the shell mold through hole and the wax mold. This gap becomes the reserved expansion margin of the inner wall of the shell mold through hole after firing.

[0005] As an improvement to the above technical solution, in step S2, the modified polyvinyl alcohol film-forming agent is cross-linked modified polyvinyl alcohol, the concentration of the modified polyvinyl alcohol film-forming agent solution is 8-12 wt%, and the cross-linking agent is one or more of borax, boric acid, or glutaraldehyde.

[0006] As an improvement to the above technical solution, the drying conditions for the sacrificial layer in step S2 are: temperature 25±2℃, humidity 40±5%, and time 5-10 minutes.

[0007] As an improvement to the above technical solution, the compressed air pressure used to blow out the excess solution in step S2 is 0.1-0.3MPa, the blowing direction is unidirectional blowing from one end of the through hole to the other end, and the blowing time is 2-5 seconds.

[0008] As an improvement to the above technical solution, the process parameters for the dewaxing process in step S7 are: temperature 150-180℃, pressure 0.6-0.8MPa, and dewaxing time 8-15 minutes.

[0009] As an improvement to the above technical solution, the pre-wetting treatment of the through holes in step S4 is only performed before the second layer of coating.

[0010] As an improvement to the above technical solution, the no-slurry control in step S6 also includes: the standing time from the topcoat to the sand spreading is 30-60 seconds.

[0011] On the other hand, the application of the aforementioned method for layered coating and drying of large-aperture thin-walled shell molds is provided.

[0012] The beneficial effects of this invention are: A modified polyvinyl alcohol sacrificial layer is provided on the inner wall of the shell mold through hole. This sacrificial layer is dissolved by high temperature and high pressure water vapor during the dewaxing process and discharged with the dewaxing liquid, thereby forming a compensation gap between the inner wall of the shell mold through hole and the wax pattern. After firing, this gap becomes the reserved expansion allowance of the inner wall of the shell mold through hole, effectively compensating for the thermal expansion of the shell mold, avoiding through hole shrinkage, deformation and cracking, and significantly improving the through hole diameter accuracy and roundness of large-diameter thin-walled shell castings. Cross-linked modified polyvinyl alcohol is used as a film-forming agent. The sacrificial layer obtained after drying does not dissolve or swell under the conditions of topcoat slurry coating, thus avoiding damage to the sacrificial layer and contamination of the slurry by the topcoat slurry. At the same time, the sacrificial layer can still dissolve or decompose under dewaxing conditions, achieving the dual effect of "stable existence during coating and reliable removal during dewaxing", ensuring the stable formation of the compensation gap. A six-layer gradient coating process is employed, with the top layer using fine-grained zircon sand, and the second to sixth layers using mullite powder with progressively coarser layers. This ensures that the shell mold achieves high green and post-firing strength while maintaining low surface roughness. Example data shows that the flexural strength after firing can reach 15.2-16.2 MPa. By using methods such as slurry control after each coating layer, surface layer settling, and compressed air purging at specific points after sand application to remove slurry and loose sand from the ducts, the blockage of through holes and excessive thickness of local shell molds are avoided, further ensuring the dimensional accuracy of through holes and the uniformity of shell molds. After the surface layer is sanded and dried, silica sol is used to pre-wet the shell through holes, which improves the adhesion of the second layer of slurry to the through holes, increases the interlayer bonding force, and reduces the probability of shell mold delamination and peeling at the through holes. Attached Figure Description

[0013] Figure 1 This is a schematic diagram of the process of the present invention. Detailed Implementation

[0014] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0015] Example 1

[0016] This embodiment provides a layered coating and drying method for a large-aperture thin-walled shell mold, used to prepare a ceramic shell. The shell has a through-hole design with an aperture D=25mm and a wall thickness T=3mm. S1 wax model pretreatment: Clean the wax model with a cleaning agent with a pH value of 4-6 for 15 seconds, and then dry the surface moisture with compressed air. S2 sacrificial layer forming: A modified polyvinyl alcohol film-forming agent solution with a concentration of 8 wt% (modified by borax crosslinking, with the crosslinking agent amount being 3.0 wt% of the PVA mass) was injected into the inner cavity of the shell through hole. After standing for 2 seconds, the excess solution was blown out, so that a sacrificial layer with a thickness of 0.5 mm was formed on the inner wall of the through hole. Compressed air pressure of 0.1 MPa was used to blow the through hole unidirectionally from one end to the other for 5 seconds. The through hole was dried for 10 minutes at a temperature of 23℃ and a humidity of 40%. The sacrificial layer obtained after drying did not dissolve or swell under the condition of surface slurry coating, but could dissolve under the condition of dewaxing. S3 surface coating and lettering blowing: The wax model processed in step S2 is immersed in the surface slurry at a 30° angle for 15 seconds, with the surface slurry covering the outer layer of the sacrificial layer. After removal, compressed air at a pressure of 0.2 MPa is used to blow slurry at specific points on the casting area to eliminate air bubbles and remove excess slurry. The surface slurry includes silica sol binder and refractory powder, with the refractory powder being zirconium powder. S4 through-hole protection treatment: After sprinkling 100-120 mesh zircon sand on the surface, it is dried for 6 hours at a temperature of 23℃ and a humidity of 80%. After drying, the shell through holes are pre-wetted with silica sol for 3 seconds, and then the second coating is applied. S5 six-layer coating: Complete the coating, sanding, and drying of the first through sixth layers in sequence according to the following parameters: First layer: Slurry concentration 40 seconds (4# cup), sprinkle with 100-mesh zircon sand, dry for 6 hours at 23℃ and 80% humidity; Second layer: Slurry concentration 25 seconds (5# cup), sprinkle with 60-mesh Malaysian sand, dry for 4 hours at 23℃ and 80% humidity; Third layer: slurry concentration 15 seconds (5# cup), sprinkle with 35-mesh Malaysian sand, dry for 4 hours at 23℃ and 45% humidity; Fourth layer: Slurry concentration 9 seconds (5# cup), sprinkle with 22-mesh Malaysian sand, dry for 4 hours at 23℃ and 45% humidity; Fifth layer: Slurry concentration 8 seconds (5# cup), sprinkle with 22-mesh Malaysian sand, dry for 4 hours at 23℃ and 45% humidity; Sixth layer: slurry concentration 6 seconds (5# cup), no sand sprinkling, drying for 10 hours at 23℃ and 45% humidity; The slurry comprises a silica sol binder and refractory powder. The first layer of the slurry uses zirconium powder as the refractory powder, while the second to sixth layers use mullite powder. The pH value of each layer of the slurry is controlled between 9.2 and 10.6. S6 No Slurry Accumulation Control: After each layer is applied, the slurry is suspended and controlled until it no longer drips continuously before sand is sprinkled. The settling time from the top layer application to the sand sprinkling is 30 seconds. After sand sprinkling, compressed air is used to blow away the slurry and loose sand in the duct area. S7 Dewaxing and Sacrificial Layer Removal: After all six layers of coating and drying are completed, the module is placed in a dewaxing kettle and dewaxed for 15 minutes at a temperature of 150℃ and a pressure of 0.8MPa. High-temperature and high-pressure water vapor in the dewaxing kettle permeates through the shell mold pores and contacts the sacrificial layer. The sacrificial layer dissolves and is discharged with the dewaxing liquid, forming a compensation gap between the inner wall of the shell mold through hole and the wax mold. This gap becomes the reserved expansion margin of the inner wall of the shell mold through hole after firing.

[0017] Example 2

[0018] This embodiment provides a layered coating and drying method for a large-aperture thin-walled shell mold, used to prepare a ceramic shell. The shell has a through-hole design with an aperture D=30mm and a wall thickness T=4mm. S1 wax model pretreatment: Clean the wax model with a cleaning agent with a pH value of 4-6 for 15 seconds, and then dry the surface moisture with compressed air. S2 sacrificial layer forming: A 12wt% modified polyvinyl alcohol film-forming agent solution (modified with glutaraldehyde, the crosslinking agent amount being 1.75wt% of the PVA mass) was injected into the inner cavity of the shell through-hole. After standing for 2 seconds, excess solution was blown out, forming a 0.2mm thick sacrificial layer on the inner wall of the through-hole. Compressed air at a pressure of 0.3MPa was used to blow the through-hole unidirectionally from one end to the other for 2 seconds to remove excess solution and clear the channel. The solution was dried at 27℃ and 45% humidity for 5 minutes. The resulting sacrificial layer did not dissolve or swell under the surface coating slurry conditions, but it could dissolve under dewaxing conditions. S3 surface coating and lettering blowing: The wax model processed in step S2 is immersed in the surface slurry at a 30° angle for 10 seconds, with the surface slurry covering the outer layer of the sacrificial layer. After removal, compressed air at a pressure of 0.5 MPa is used to blow slurry at specific points on the casting area to eliminate air bubbles and remove excess slurry. The surface slurry includes silica sol binder and refractory powder, with the refractory powder being zirconium powder. S4 through-hole protection treatment: After sprinkling 120-mesh zircon sand on the surface, it is dried for 6 hours at a temperature of 23℃ and a humidity of 80%. After drying, the shell through holes are pre-wetted with silica sol for 2 seconds, and then the second coating is applied. S5 six-layer coating: Complete the coating, sanding, and drying of the first through sixth layers in sequence according to the following parameters: First layer: slurry concentration 50 seconds (4# cup), sprinkle with 120 mesh zircon sand, dry for 6 hours, temperature 23℃, humidity 80%, pH value 9.2; Second layer: slurry concentration 32 seconds (5# cup), sprinkle with 60-mesh Malaysian sand, dry for 4 hours at 23℃, humidity 80%, pH 9.2; Third layer: slurry concentration 23 seconds (5# cup), sprinkle with 35-mesh Malaysian sand, dry for 4 hours at 23℃, humidity 45%, pH 9.2; Fourth layer: slurry concentration 13 seconds (5# cup), sprinkle with 22-mesh Malaysian sand, dry for 4 hours at 23℃, humidity 45%, pH 9.2; Fifth layer: slurry concentration 11 seconds (5# cup), sprinkle with 22-mesh Malaysian sand, dry for 4 hours at 23℃, humidity 45%, pH 9.2; Sixth layer: slurry concentration 8 seconds (5# cup), no sand sprinkling, drying for 12 hours, temperature 23℃, humidity 45%, pH value 9.2; The slurry includes silica sol binder and refractory powder. The refractory powder of the first layer of slurry is zirconium powder, and the refractory powder of the second to sixth layers of slurry is mullite powder. The pH value of each layer of slurry is controlled between 9.2 and 10.6. S6 No Slurry Accumulation Control: After each layer is applied, the slurry is suspended and controlled until it no longer drips continuously before sand is sprinkled. The settling time from the top layer application to the sand sprinkling is 30 seconds. After sand sprinkling, compressed air is used to blow away the slurry and loose sand in the duct area. S7 Dewaxing and Sacrificial Layer Removal: After all six layers of coating and drying are completed, the module is placed in a dewaxing kettle and dewaxed for 8 minutes at a temperature of 180℃ and a pressure of 0.6MPa. High-temperature and high-pressure water vapor in the dewaxing kettle permeates through the shell mold pores and contacts the sacrificial layer. The sacrificial layer dissolves and is discharged with the dewaxing liquid, forming a compensation gap between the inner wall of the shell mold through hole and the wax mold. This gap becomes the reserved expansion margin of the inner wall of the shell mold through hole after firing. Example 3

[0019] This embodiment provides a layered coating and drying method for a large-aperture thin-walled shell mold, used to prepare a ceramic shell. The shell has a through-hole design with an aperture D=30mm and a wall thickness T=4mm. S1 wax model pretreatment: Clean the wax model with a cleaning agent with a pH value of 4-6 for 30 seconds, and then dry the surface moisture with compressed air. S2 sacrificial layer forming: A 10wt% modified polyvinyl alcohol film-forming agent solution (modified by cross-linking of borax and glutaraldehyde, with the total amount of cross-linking agent being 1.0wt% of the PVA mass) was injected into the inner cavity of the shell through-hole. After standing for 3 seconds, excess solution was blown out, forming a sacrificial layer with a thickness of 0.35mm on the inner wall of the through-hole. Compressed air at a pressure of 0.2MPa was used to blow the through-hole unidirectionally from one end to the other for 3.5 seconds to remove excess solution and clear the channel. The solution was dried at 25℃ and 40% humidity for 7.5 minutes. The resulting sacrificial layer did not dissolve or swell under the conditions of surface coating slurry, but it could dissolve under dewaxing conditions.

[0020] S3 surface coating and lettering blowing: The wax model processed in step S2 is immersed in the surface slurry at a 37° angle for 12 seconds, with the surface slurry covering the outer layer of the sacrificial layer. After removal, compressed air at a pressure of 0.35 MPa is used to blow slurry at specific points on the casting area to eliminate air bubbles and remove excess slurry. The surface slurry consists of silica sol binder and refractory powder, with zirconium powder as the refractory powder. The slurry concentration is 45 seconds (cup #4), and the pH value is 10.0. S4 through-hole protection treatment: After sprinkling 110-mesh zircon sand on the surface, it is dried for 6 hours at a temperature of 23℃ and a humidity of 80%. After drying, the shell through holes are pre-wetted with silica sol for 2.5 seconds, and then the second coating is applied.

[0021] S5 six-layer coating: Complete the coating, sanding, and drying of the first through sixth layers in sequence according to the following parameters: First layer: slurry concentration 45 seconds (cup #4), sprinkle with 110 mesh zircon sand, dry for 6 hours at 23℃, humidity 80%, pH 10.0; Second layer: slurry concentration 28 seconds (5# cup), sprinkle with 60-mesh Malaysian sand, dry for 4 hours at 23℃, humidity 80%, pH 10.0; Third layer: slurry concentration 19 seconds (5# cup), sprinkle with 35-mesh Malaysian sand, dry for 4 hours at 23℃, humidity 45%, pH 10.0; Fourth layer: slurry concentration 11 seconds (5# cup), sprinkle with 22-mesh Malaysian sand, dry for 4 hours at 23℃, humidity 45%, pH 10.0; Fifth layer: slurry concentration 9.5 seconds (5# cup), sprinkle with 22-mesh Malaysian sand, dry for 4 hours at 23℃, humidity 45%, pH 10.0; Sixth layer: slurry concentration 7 seconds (5# cup), no sand sprinkling, drying for 11 hours, temperature 23℃, humidity 45%, pH value 10.0; The slurry is composed of silica sol binder and refractory powder; wherein, the refractory powder of the first layer of slurry is zirconium powder, and the refractory powder of the second to sixth layers of slurry is mullite powder; the pH value of each layer of slurry is controlled between 9.2 and 10.6. S6 No Slurry Accumulation Control: After each layer is applied, the slurry is suspended and controlled until it stops dripping continuously before sand is applied. The settling time from the top layer application to the sand application is 45 seconds. After sand application, compressed air is used to blow away accumulated slurry and loose sand from the duct area.

[0022] S7 Dewaxing and Sacrificial Layer Removal: After all six layers of coating and drying are completed, the module is placed in a dewaxing kettle and dewaxed for 11.5 minutes at a temperature of 165℃ and a pressure of 0.7MPa. High-temperature and high-pressure water vapor in the dewaxing kettle permeates through the shell mold pores and contacts the sacrificial layer. The sacrificial layer dissolves and is discharged with the dewaxing liquid, forming a compensation gap between the inner wall of the shell mold through hole and the wax mold. This gap becomes the reserved expansion margin of the inner wall of the shell mold through hole after firing. Comparative Example 1 The difference from Example 1 is that the S2 sacrificial layer forming step is not performed, and the surface slurry is directly applied to the surface of the wax model. The remaining steps are the same as in Example 1.

[0023] Comparative Example 2 The difference from Example 1 is that in step S2, unmodified ordinary polyvinyl alcohol (PVA, concentration 8wt%) is used as the film-forming agent, and no crosslinking agent or hydrophobic modifier is added. The remaining steps are the same as in Example 1.

[0024] Comparative Example 3 The difference from Example 1 is that step S5 is replaced by: preparing a slurry (silica sol + mullite powder, concentration 30 seconds / 5# cup, pH 10.0), repeatedly immersing the module in the slurry and sprinkling it with 22-mesh Malayan sand, drying for 4 hours each time (temperature 23°C, humidity 45%), repeating the operation until the total thickness of the shell mold reaches a thickness equivalent to that of Example 1 (about 6-8 mm), and the remaining steps are the same as in Example 1.

[0025] Comparative Example 4 The difference from Example 1 is that only three coating layers are applied, and the slurry concentration and sand specifications are not precisely controlled according to the six-layer gradient. Step S5 is replaced with: First layer: Slurry concentration 45 seconds (4# cup), sprinkle with 100-mesh zircon sand, dry for 6 hours at 23℃ and 80% humidity; Second layer: Slurry concentration 35 seconds (5# cup), sprinkle with 46-mesh Malaysian sand, dry for 4 hours at 23℃ and 80% humidity; Third layer: slurry concentration 20 seconds (5# cup), no sand sprinkling, dry for 10 hours at 23°C and 45% humidity; the remaining steps are the same as in Example 1.

[0026] Comparative Example 5 The difference from Example 1 is that step S5 is replaced by the following: all 6 layers use the same slurry (silica sol + mullite powder, concentration 25 seconds / 5# cup, pH 10.0), each layer is sprinkled with 60-mesh Malaysian sand, each layer is dried for 4 hours (temperature 23℃, humidity 45%), the 6th layer is dried for more than 10 hours after sprinkling sand, and the remaining steps are the same as in Example 1.

[0027] Performance testing The ceramic shells prepared in Examples 1-3 and Comparative Examples 1-5 were subjected to performance tests. The test samples were all taken from the area including the through holes of the shell. Five samples were randomly selected from each group, and the average value of the test results was taken. The specific methods for each test item are as follows: (1) Bending strength of green blank: The shell mold before dewaxing (green blank) was cut into standard test strips with dimensions of 40 mm × 20 mm × shell mold thickness. The three-point bending method was used for testing, with a span of 30 mm and a loading rate of 0.5 mm / min. (2) Bending strength after firing: The shell mold green billet is fired at 950-1050℃ for 2 hours, cooled in the furnace and cut into the above standard test strips. The three-point bending method is used for testing, and the test conditions are the same as the bending strength of the green billet. (3) Air permeability: Under a fixed pressure difference (ΔP = 100 mmH2O), the volume of gas passing through a unit area shell mold sample per unit time is measured, expressed in cm³. 3 / min means; (4) Porosity: The porosity of the shell mold was determined by Archimedes' displacement method (distilled water as medium) and calculated as the percentage of the volume of open pores to the total volume of the sample. (5) Shell mold surface roughness: The arithmetic mean deviation Ra of the profile is measured at 5 random points on the outer surface of the shell mold using a surface roughness tester, and the average value is taken; The test results of each embodiment and comparative example are summarized in Table 1;

[0028] Table 1 The shell molds of Examples 1-3 exhibit significantly better overall performance than the comparative examples. In terms of five indicators—green bending strength, post-firing bending strength, air permeability, porosity, and shell mold surface roughness—Examples 1-3 demonstrate superior performance. Specifically, the post-firing bending strength of Examples 1-3 is 15.2-16.2 MPa, significantly higher than the 9.0-12.0 MPa of Comparative Examples 2-5; the air permeability of Examples 1-3 is 98-105 cm³. 3 / min, with a porosity of 28-30%, indicates that the use of a modified polyvinyl alcohol sacrificial layer combined with a six-layer gradient coating process ensures both the density of the shell mold and maintains appropriate air permeability. The five overall shell mold indicators of Comparative Example 1 (without sacrificial layer molding) are all slightly lower than those of Example 1. The core difference is still mainly reflected in the dimensional accuracy of the through-hole area and the slurry accumulation, which are not fully reflected in the five columns of indicators in this table. It should be noted that the test samples were taken from the area containing the through-hole. Slurry accumulation in the through-hole area will locally affect the overall test results, hence the slight decrease in the overall indicators of Comparative Example 1. The main function of the sacrificial layer is to form a compensating gap (reserving expansion allowance) after dewaxing. The prevention of slurry accumulation is mainly achieved by the S6 no-slurry control. Therefore, the difference between Comparative Example 1 and Example 1 should be further reflected in the dimensional accuracy of the through-hole of the casting. Comparative Example 2 (unmodified ordinary polyvinyl alcohol) showed a significant decrease in all indicators compared to Example 1. Its flexural strength after calcination decreased to 11.5 MPa, while its air permeability increased to 130 cm³. 3 The porosity increased to 34% and the surface roughness increased to 4.8 μm. This indicates that unmodified polyvinyl alcohol is easily dissolved and contaminated by water in the slurry during the topcoat slurry application process, resulting in poor bonding between the topcoat and the wax mold, which in turn significantly reduces the strength and surface quality of the shell mold. This, in turn, proves the necessity of using cross-linked modified polyvinyl alcohol to form a water-resistant sacrificial layer. The shell mold performance of Comparative Example 3 (single slurry repeated coating), Comparative Example 4 (only 3 coatings), and Comparative Example 5 (6 coatings of the same slurry, all sprinkled with 60-mesh Malaysian sand) was significantly worse than that of the Example. Among them, Comparative Example 4 had the worst performance in all indicators, with a flexural strength of only 9.0 MPa after firing and an air permeability as high as 185 cm³. 3The porosity reached 41% per minute. This is because Comparative Example 4 not only lacked a gradient layered structure but also had only 3 layers and a thin shell mold. The combination of these two factors led to a significant decrease in strength, and a severe deterioration in density and surface quality. If Comparative Example 5, with the same 6 layers but with the same slurry and sand in each layer, is used as a clean control group for the gradient effect, its flexural strength after calcination is 12.0 MPa, significantly lower than the 15.5 MPa of Example 1, indicating that the gradient layered structure alone brings a net gain of approximately 3.5 MPa. Comparative Examples 3 and 5, lacking fine-grained layers or gradient structures, had surface roughnesses of 7.5 μm and 7.0 μm, respectively, further demonstrating that the use of zircon sand layers and a progressively coarser gradient coating process plays an important role in ensuring the surface quality and overall performance of the shell mold.

[0029] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it.

Claims

1. A method for layered coating and drying of a large-aperture thin-walled shell mold, characterized in that: Includes the following steps: S1 Wax Model Pretreatment: Clean the wax model assembly with a cleaning agent with a pH value of 4-6 for 15-30 seconds, and then dry the surface moisture with compressed air; S2 Sacrificial Layer Forming: Inject the modified polyvinyl alcohol film-forming agent solution into the inner cavity of the shell through hole, let it stand for 2-4 seconds, and then blow out the excess solution to form a sacrificial layer with a thickness of 0.2-0.5 mm on the inner wall of the through hole. After drying, the resulting sacrificial layer does not dissolve or swell under the condition of surface slurry coating, but can dissolve or decompose under dewaxing conditions; dry at a temperature of 25±2℃ and a humidity of 40±5% for 5-10 minutes. S3 Surface Coating and Type Casting Blowing: Immerse the wax model processed in step S2 into the surface slurry at an angle of 30-45° for 10-15 seconds. The surface slurry covers the outer layer of the sacrificial layer. After removal, use compressed air to blow slurry at specific points on the type casting area to eliminate air bubbles and remove excess slurry. S4 Through-hole Protection Treatment: After the surface layer is sanded and dried, the through-holes of the shell are pre-wetted with silica sol for 2-3 seconds, and then the second layer is applied. S5 Six-Layer Coating: Apply, sand, and dry the first to sixth layers sequentially according to the following parameters: First layer: Slurry concentration 40-50 seconds (4# cup), sprinkle with 100-120 mesh zircon sand, dry for 6 hours at 23±1℃ and 80±5% humidity; Second layer: Slurry concentration 25-32 seconds (5# cup), sprinkle with 60-mesh Malaysian sand, dry for 4 hours, temperature 23±1℃, humidity 80±5%; Third layer: Slurry concentration 15-23 seconds (5# cup), sprinkle with 35-mesh Malaysian sand, dry for 4 hours at 23±1℃ and 45±5% humidity; Fourth layer: Slurry concentration 9-13 seconds (5# cup), sprinkle with 22-mesh Malaysian sand, dry for 4 hours at 23±1℃ and 45±5% humidity; Fifth layer: Slurry concentration 8-11 seconds (5# cup), sprinkle with 22-mesh Malaysian sand, dry for 4 hours at 23±1℃ and 45±5% humidity; Sixth layer: Slurry concentration 6-8 seconds (5# cup), no sand sprinkling, drying for more than 10 hours, temperature 23±1℃, humidity 45±5%; The slurry comprises silica sol binder and refractory powder; wherein, the refractory powder of the first layer of slurry is zirconium powder, and the refractory powder of the second to sixth layers of slurry is mullite powder, and the pH value of each layer of slurry is controlled between 9.2 and 10.

6. S6 No Slurry Accumulation Control: After each layer of coating is applied, the slurry is suspended and controlled until it no longer drips continuously. Then, sand is sprinkled. After sprinkling the sand, compressed air is used to blow away the slurry accumulation and loose sand in the duct area. S7 Dewaxing and Sacrificial Layer Removal: After all six layers of coating and drying are completed, the module is placed in a dewaxing kettle for dewaxing. High-temperature and high-pressure water vapor in the dewaxing kettle penetrates through the shell mold pores and contacts the sacrificial layer. The sacrificial layer dissolves or decomposes and is discharged with the dewaxing liquid, forming a compensation gap between the inner wall of the shell mold through hole and the wax mold. This gap becomes the reserved expansion margin of the inner wall of the shell mold through hole after firing.

2. The method for layered coating and drying of a large-aperture thin-walled shell mold according to claim 1, characterized in that: In step S2, the modified polyvinyl alcohol film-forming agent is cross-linked modified polyvinyl alcohol, the concentration of the modified polyvinyl alcohol film-forming agent solution is 8-12 wt%, and the cross-linking agent is one or more of borax, boric acid, or glutaraldehyde.

3. The method for layered coating and drying of a large-aperture thin-walled shell mold according to claim 1, characterized in that: In step S2, the drying conditions for the sacrificial layer are: temperature 25±2℃, humidity 40±5%, and time 5-10 minutes.

4. The method for layered coating and drying of a large-aperture thin-walled shell mold according to claim 1, characterized in that: In step S2, the compressed air pressure used to blow out the excess solution is 0.1-0.3 MPa, the blowing direction is unidirectional blowing from one end of the through hole to the other end, and the blowing time is 2-5 seconds.

5. The method for layered coating and drying of a large-aperture thin-walled shell mold according to claim 1, characterized in that: The process parameters for the dewaxing process in step S7 are: temperature 150-180℃, pressure 0.6-0.8MPa, and dewaxing time 8-15 minutes.

6. The method for layered coating and drying of a large-aperture thin-walled shell mold according to claim 1, characterized in that: In step S4, the pre-wetting treatment of the through holes is performed only before the second layer of coating.

7. The method for layered coating and drying of a large-aperture thin-walled shell mold according to claim 1, characterized in that: Step S6, which also includes the control of no slurry accumulation, is to allow the surface layer to stand for 30-60 seconds after application and before sanding.