A method for casting a large appliance component

By combining multi-hole injection molds and bottom-pouring casting with stepped normalizing and vacuum pretreatment, the problems of uneven density of hot-melt metal and high cost of normalizing equipment in the casting of large electrical components have been solved, thereby improving the uniformity and performance of castings and reducing production costs.

CN123128446APending Publication Date: 2026-11-20ZHENJIANG ZHAOXIN ENERGY EQUIPMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611251741.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-18
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Large electrical components suffer from uneven density of hot-melt metal and differences in strength between different parts after cooling during the casting process. Furthermore, normalizing requires large equipment, which is costly.

Method used

The process employs a multi-hole injection mold and bottom-injection casting, combined with stepped normalizing and vacuum pretreatment. By setting multiple injection holes in the mold and using bottom-injection casting, the non-uniformity of the hot-melt metal density is reduced. Vacuum pretreatment reduces bubble defects, and stepped heating and multiple normalizing are used to improve material properties.

Benefits of technology

It achieves uniform distribution of hot-melt metal within the mold, reduces porosity defects, improves the strength and low-temperature impact toughness of castings, and reduces production costs and equipment requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128446A_ABST
    Figure CN123128446A_ABST
Patent Text Reader

Abstract

The present application relates to the field of large electric appliance component preparation forming, and specifically discloses a large electric appliance component casting forming method, mainly comprising the following steps: making a multi-injection hole mold, cleaning the mold, closing the mold, preheating, injecting hot molten metal in a bottom injection mode and pressure maintaining, cooling, demolding, cleaning surface oxides and re-enclosing the mold, normalizing operation, natural cooling, surface testing and flaw detection, by setting multiple injection hole molds and using a bottom injection method for casting, the castings will not have physical properties of different parts due to single injection hole injection of hot molten metal density in a ladder type distribution, the castings after cooling and forming are re-enclosed in the mold for normalizing operation, which can save the cost of purchasing a trolley furnace and other devices, and does not need additional transfer operation, and is more time-saving and labor-saving.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of large electrical component fabrication and molding, and specifically to a method for casting and molding large electrical components. Background Technology

[0002] In power systems, large electrical components are an inevitable part of the architecture, such as stators and rotors of large motors, large electrical cabinet assemblies, etc. Although these structures are simple, their large size makes them more difficult to manufacture than smaller electrical components.

[0003] Currently, most large electrical components on the market are manufactured using casting. This method allows for one-time molding, resulting in better physical properties compared to welding and assembly. However, the one-time molding of large electrical components inevitably presents various problems compared to the manufacturing of smaller components. For example: 1. Due to their large size, the pressure of the molten metal in different parts of the mold is inconsistent during casting, leading to differences in strength after cooling. 2. After casting, normalizing is generally performed to improve the performance of the casting. Normalizing involves heating the metal casting to 30-50°C above the critical temperature, holding it at that temperature for a period of time, and then allowing it to cool naturally. This refines the grains, making the microstructure more uniform and improving the strength and hardness of the casting. Because large castings are large, custom-made large normalizing equipment, such as bogie hearth furnaces, is required, thus increasing production costs. Summary of the Invention

[0004] The present invention addresses the technical problems mentioned in the background section and proposes the following technical solutions: A method for casting and molding large electrical components includes the following steps: S1. Based on the structural design of large electrical components, molds are manufactured, and multiple injection holes are set around the molds. The molds are provided with riser structures. S2. Clean the mold, then close the mold and preheat the mold to raise the internal temperature to 500℃. S3. Inject hot molten metal into the mold. The pouring method is bottom pouring. After the injection is completed, maintain the pressure for 3-5 days. After the molten metal has initially cooled and solidified in the mold cavity, gradually reduce the pressure. After cooling and solidification, use tools such as hydraulic hammers to remove the sand adhering to the gate and the surface of the casting, and then demold. S4. Clean the surface of the casting after demolding to remove the oxides on the surface. Then put it back into the mold for normalizing. Continuously heat the mold until it reaches 900℃ and hold it at that temperature for 5-6 hours. S5. After the heat preservation is completed, open the mold and expose the casting to the air to allow it to cool naturally to room temperature. S6. Use instruments to test the dimensions and smoothness of the metal casting surface, and use ultrasonic testing to detect flaws on the casting surface.

[0005] Preferably, the large electrical component mold can be manufactured modularly and assembled by splicing. When in use, it can be assembled by splicing. When storing and transporting, the mold can be disassembled into small volume modules for storage and transport. Preferably, in step S4, the process of continuously heating the mold can be carried out in a stepped heating manner. In the first stage, the temperature is raised to 300°C and held for 1 hour. In the second stage, the temperature is raised to 600°C and held for 1 hour. In the third stage, the temperature is raised to 900°C and then held for 5-6 hours. Preferably, the normalizing operation in step S4 is repeated 1-2 times; Preferably, in step S5, after opening the mold, the casting is exposed to the air and can be cooled by setting a high-power fan; Preferably, at least four high-power fans are provided to simultaneously cool the casting from all four sides, ensuring that the cooling rate of the casting remains consistent. Preferably, in step S2, after preheating the mold to 500°C, the air inside the mold is removed by a vacuum device to create a vacuum state inside the mold.

[0006] The beneficial effects of this invention are: 1. By setting multiple injection holes on the mold and using the bottom injection method for casting, compared with a mold with only one injection hole, the hot melt metal distribution after injection in the mold can be more uniform. Especially for large castings, due to their large volume, single-hole injection will inevitably result in the hot melt metal density in the parts far from the injection hole being less than the hot melt metal density around the injection hole. This type of injection mold can solve this problem, so that the casting will not have different physical properties in different parts of the casting due to the stepped distribution of hot melt metal density during the injection process.

[0007] 2. After the casting is demolded, its surface is cleaned first, and then it is sealed in the mold for normalizing. This method replaces the traditional method of gradually putting it into equipment such as a bogie furnace for normalizing. Since large components are large in size, no additional transportation is required, which saves time and effort. There is also no need to purchase additional equipment, resulting in lower costs.

[0008] 3. Compared with the normalizing method in Example 1, which only involves one gradual normalizing process and only one temperature increase, by adding one normalizing process and changing the temperature increase method to a stepped temperature increase, the yield strength of the casting treated by this method is slightly improved, while the low-temperature impact toughness of the material is also greatly improved, making it more adaptable to working environments at low temperatures.

[0009] 4. By using a vacuum device to remove air from the mold, a vacuum state is created inside the mold. Vacuuming the mold in advance can reduce the amount of air mixed in, thus reducing porosity defects caused by air bubbles during the cooling and forming process of the hot molten metal. Attached Figure Description

[0010] Figure 1 This is a flowchart of the present invention. Detailed Implementation

[0011] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.

[0012] In the description of this invention, it should be understood that relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. The connection methods described by the terms "fixed connection" and "fixed arrangement" include, but are not limited to, "welding," "riveting," "adhesion," and "threaded connection." The terms "comprising," "including," or any other variations thereof are intended to cover a non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. The terms “upper,” “lower,” “front,” “back,” “left,” “right,” “top,” “bottom,” “inner,” and “outer,” etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limiting the present invention.

[0013] Example 1 Reference Figure 1 A method for casting and molding large electrical components includes the following steps: S1. Based on the structural design of large electrical components, molds are manufactured, and multiple injection holes are set around the molds, with riser structures set on the molds; S2. Clean the mold, then close the mold and preheat the mold to raise the internal temperature to 500℃. S3. Inject hot molten metal into the mold. The pouring method is bottom pouring. After the injection is completed, maintain the pressure for 3-5 days. After the molten metal has initially cooled and solidified in the mold cavity, gradually reduce the pressure. After cooling and solidification, use tools such as hydraulic hammers to remove the sand adhering to the gate and the surface of the casting, and then demold. S4. Clean the surface of the casting after demolding to remove the oxides on the surface. Then put it back into the mold for normalizing. Continuously heat the mold until it reaches 900℃ and hold it at that temperature for 5-6 hours. S5. After the heat preservation is completed, open the mold and expose the casting to the air to allow it to cool naturally to room temperature. S6. Use instruments to test the dimensions and smoothness of the metal casting surface, and use ultrasonic testing to detect flaws on the casting surface.

[0014] Preferably, large electrical component molds can be manufactured in a modular fashion and assembled by splicing. They can be combined in use and disassembled into smaller modules for storage and transportation.

[0015] In practice, by setting multiple injection holes on the mold and using the bottom injection method for casting, compared to a mold with only one injection hole, the hot melt metal after injection can be distributed more evenly within the mold. This is especially important for large castings, where due to their large volume, single-hole injection will inevitably result in the hot melt metal density in areas far from the injection hole being lower than that around the injection hole. This type of injection mold can solve this problem, preventing the casting from having inconsistent physical properties in different parts due to a stepped distribution of hot melt metal density during the injection process.

[0016] After the casting is demolded, its surface is first cleaned, and then it is sealed in the mold for normalizing. This method replaces the traditional method of placing the casting into equipment such as a bogie furnace for normalizing. Since large components are large in size, no additional transportation is required, which saves time and effort. There is also no need to purchase additional equipment, resulting in lower costs.

[0017] Example 2 The difference between this embodiment and embodiment one is that in step S4, the process of continuously heating the mold can be carried out in a stepped heating manner. In the first stage, the temperature is raised to 300°C and held for 1 hour. In the second stage, the temperature is raised to 600°C and held for 1 hour. In the third stage, the temperature is raised to 900°C and then held for 5-6 hours. The normalizing operation is repeated once. Compared to the normalizing method in Example 1, which involves only one gradual normalizing process and a single temperature rise, the changes in casting properties obtained by the method in this example are as follows (taking 10CrNiCu low-alloy cast steel as an example):

[0018] Although the yield strength after one normalizing is already very high, by adding another normalizing step, while maintaining the yield strength slightly increased to 440 MPa, the low-temperature impact toughness of the material is increased from 64J to 246J, making it more adaptable to working environments at low temperatures.

[0019] Example 3 The difference between this embodiment and embodiment one is that in step S5, after opening the mold, the casting is exposed to the air and can be cooled by setting up high-power fans. At least four high-power fans are set up to simultaneously cool the casting around its perimeter, ensuring that the cooling rate of the four sides of the casting is consistent and the temperature drop rate of each part of the casting is uniform. This reduces the thermal stress in each part of the casting, thereby reducing the problem of internal cracks caused by excessive thermal stress, which would reduce the overall strength of the casting.

[0020] Example 4 The difference between this embodiment and embodiment one is that in step S2, after the mold is preheated to 500°C, the air inside the mold is removed by a vacuum device to create a vacuum state inside the mold. Vacuuming the mold in advance can reduce the amount of air mixed in the mold, thus reducing porosity defects caused by air bubbles during the cooling and forming process of the hot melt metal.

Claims

1. A method for casting and molding large electrical components, characterized in that, The following steps are included: S1. Based on the structural design of large electrical components, molds are manufactured, and multiple injection holes are set around the molds. The molds are provided with riser structures. S2. Clean the mold, then close the mold and preheat the mold to raise the internal temperature to 500℃. S3. Inject hot molten metal into the mold. The pouring method is bottom pouring. After the injection is completed, maintain the pressure for 3-5 days. After the molten metal has initially cooled and solidified in the mold cavity, gradually reduce the pressure. After cooling and solidification, use tools such as hydraulic hammers to remove the sand adhering to the gate and the surface of the casting, and then demold. S4. Clean the surface of the casting after demolding to remove the oxides on the surface. Then put it back into the mold for normalizing. Continuously heat the mold until it reaches 900℃ and hold it at that temperature for 5-6 hours. S5. After the heat preservation is completed, open the mold and expose the casting to the air to allow it to cool naturally to room temperature. S6. Use instruments to test the dimensions and smoothness of the metal casting surface, and use ultrasonic testing to detect flaws on the casting surface.

2. The method for casting and molding large electrical components according to claim 1, characterized in that, The large electrical component mold can be manufactured modularly and assembled by splicing. When in use, it can be assembled. When for storage and transportation, the mold can be disassembled into small volume modules for storage and transportation.

3. The method for casting and molding large electrical components according to claim 1, characterized in that, In step S4, the process of continuously heating the mold can be carried out in a stepped heating manner. In the first stage, the temperature is raised to 300°C and held for 1 hour. In the second stage, the temperature is raised to 600°C and held for 1 hour. In the third stage, the temperature is raised to 900°C and then held for 5-6 hours.

4. The method for casting and molding large electrical components according to claim 1, characterized in that, The normalizing operation in step S4 is repeated 1-2 times.

5. The method for casting and molding large electrical components according to claim 1, characterized in that, In step S5, after opening the mold, the casting is exposed to the air and can be cooled by setting a high-power fan.

6. The method for casting and molding large electrical components according to claim 5, characterized in that, At least four high-power fans are installed to simultaneously cool the casting from all four sides, ensuring a consistent cooling rate.

7. The method for casting and molding large electrical components according to claim 1, characterized in that, In step S2, after the mold is preheated to 500°C, the air inside the mold is removed by a vacuum device to create a vacuum inside the mold.