A sand box using method applied to machine tool casting production

By using external positioning lugs and locally reinforced chilled sand in the casting production of large machine tool parts, the problems of positioning failure and insufficient cooling caused by mismatched sand box dimensions were solved, achieving precise box closing and efficient cooling of castings, and avoiding leakage and dimensional deviations.

CN123128449APending Publication Date: 2026-11-20TONGYU HEAVY IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611580393.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In the production of large machine tool castings, the use of sand boxes with mismatched dimensions can lead to misalignment of the mating surfaces, insufficient support of the molding sand, lack of positioning reference, leakage and fire during pouring, and conventional sand filling methods cannot meet the needs of local structural support and cooling, resulting in dimensional deviations and structural defects in the castings.

Method used

External positioning ear plates are fixed to the outer walls of the cover box and bottom box of different sizes. The positioning pin holes are calibrated by a three-dimensional scribing instrument. The suspended misalignment area is filled with locally reinforced chilled sand and solidified to form a suspended reinforced retaining wall. When closing the box, ceramic fiber rope and refractory mud strips are used for sealing.

Benefits of technology

The positioning reference of the irregular sand box was re-established, providing structural support and cooling capacity, preventing leakage and fire, and ensuring the dimensional accuracy and microstructure quality of the castings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128449A_ABST
    Figure CN123128449A_ABST
Patent Text Reader

Abstract

The application relates to the technical field of casting processes, and discloses a sand box using method applied to casting production of machine tool castings. In view of the positioning failure and fire running problems caused by the jointing of special-shaped sand boxes, the application fixes external positioning ear plates on the outer side walls of the size-unmatched cover box and bottom box to rebuild the jointing datum; the cover box is placed upside down above the bottom box with a pattern preset to form a suspended dislocation area; the local reinforced chilling sand is filled into the area to solidify and form a suspended reinforced retaining wall; the remaining internal box space is filled with conventional main body furan self-hardening sand to solidify and form a casting cavity; ceramic fiber ropes are laid on the parting surface and the joint, and fire-resistant clay is applied, the external positioning ear plates are used for jointing, and finally, liquid cast iron is poured. The application solves the positioning precision problem of the special-shaped sand box, provides structural support and chilling effect for the local suspended area, blocks the joint gap, and prevents iron liquid overflow and leakage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of casting technology, specifically to a method for using sand boxes in the casting production of machine tool parts. Background Technology

[0002] In the sand casting production of large machine tool castings, complete sets of upper and lower sand molds are typically used for molding and pouring. With the evolution of machine tool models and increasing customization demands, foundry companies often face a shortage of sand molds of specific sizes. To ensure production schedules, in actual production, it is necessary to use idle large or small sand molds that do not perfectly match the dimensions for substitution.

[0003] Using this type of irregularly shaped sand box for assembly molding presents several technological defects. Due to the difference in size between the upper and lower sand boxes, the original positioning pins cannot fit, resulting in a loss of accurate positioning reference during assembly and easily causing misalignment of the machine tool casting. Simultaneously, the difference in size between the upper and lower boxes creates a suspended misalignment area at the joint. Conventional single-filling sand processes are insufficient to provide structural support in this suspended area, making the molding sand prone to settling or falling off under the pressure of molten cast iron and its own weight. Furthermore, the irregular parting surface leads to incomplete sealing between the upper and lower sand boxes, increasing the risk of high-temperature molten iron overflow and fire during the pouring stage. Additionally, the suspended misalignment area corresponds to specific stress points on the machine tool; the thermal conductivity of conventional main molding sand is insufficient to meet the rapid cooling requirements of thicker sections, easily causing localized loose microstructure or shrinkage cavities in the machine tool casting.

[0004] Therefore, this invention proposes a method for using sand boxes in machine tool casting production to address the shortcomings of existing technologies. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this invention provides a method for using sand boxes in machine tool casting production. This method solves the problems in existing large machine tool casting production where mismatched sand boxes of different sizes cause misalignment and suspension of the mating surfaces, leading to insufficient molding sand support, missing positioning references, leakage during pouring, and fire hazards. It also addresses the issue that conventional sand filling methods cannot adequately meet both local structural support and cooling requirements, resulting in casting dimensional deviations and structural defects.

[0006] To achieve the above objectives, the present invention provides the following technical solution: a method for using a sand box in machine tool casting production, comprising the following steps: External positioning ear plates are fixed at corresponding positions on the outer side wall of the cover box (which is larger than the bottom box) and the outer side wall of the bottom box, respectively. The cover box is placed upside down on top of the base box, which is a pre-set machine tool casting pattern. Due to the size difference between the cover box and the base box, a suspended misalignment area is formed. Locally reinforced chilled sand is filled into the suspended misalignment area and solidified to form a suspended reinforced retaining wall. The remaining area of ​​the internal box space formed by the combination of the cover box, the bottom box and the suspended reinforced retaining wall is filled with conventional main body furan self-hardening sand. After solidification, the machine tool casting pattern is pulled out to form a casting cavity. After the mold is removed, ceramic fiber ropes are laid on the parting surface of the bottom box and the joint of the suspended misalignment area and refractory mud strips are applied. The box is then closed by the external positioning ear plate. Liquid cast iron is injected into the casting cavity, and after the casting cools, the mold is opened and the sand is removed.

[0007] The present invention achieves the following technical effects by implementing the above technical solution: Addressing the positioning failure problem caused by the size difference between the upper and lower sand boxes, an external positioning ear plate is fixed to the outer wall of the box to re-establish the box assembly reference; for the suspended misalignment area, locally reinforced chilled sand is used for filling, and the solidified suspended reinforced retaining wall provides boundary and structural support for subsequent main sand filling, while utilizing the characteristics of chilled sand to increase the cooling rate of cast iron in this area; during the box assembly operation, the compression deformation of ceramic fiber rope and the sealing characteristics of refractory clay strips are used to block the gap at the misalignment joint, preventing molten iron leakage.

[0008] Preferably, a 10-20mm thick low-carbon steel plate is fully welded around the outer surface of the top surface of the cover box to increase the height of the box. Using a three-dimensional scribing instrument and referencing the center line of the machine tool casting pattern, the corresponding upper and lower external positioning ear plates are calibrated for coaxiality, and positioning pin holes are drilled. The box closure operation is achieved by inserting a long rod positioning pin into the positioning pin holes. Increasing the cover box height by welding low-carbon steel plates meets the required molding sand thickness at the top of the machine tool casting, and using a three-dimensional scribing instrument for coaxiality calibration ensures the closure accuracy of the irregularly shaped sand box.

[0009] Preferably, before placing the cover box upside down on the bottom box above the pre-set machine tool casting pattern, the bottom box is placed on the molding base plate, the machine tool casting pattern and PT1000 elliptical pouring cup are placed in it, and a metal top column is placed directly below the suspended misalignment area corresponding to the size of the cover box outside the bottom box. Hanging braces are welded downwards at an angle to the inner wall of the low-carbon steel plate, so that the hanging braces extend into the suspended misalignment area. The metal top column provides support for the suspended part to prevent the molding sand from settling. The hanging braces extend into the interior of the suspended misalignment area to improve the structural strength of the sand wall after curing and prevent the sand from falling off during pouring and scouring.

[0010] Preferably, the locally reinforced chilled sand is a mixture of chromite sand, a curing catalyst, and furan resin; The amount of the curing catalyst added is 30-40 wt% of the mass of the furan resin, and the amount of the furan resin added is 1.0-1.5 wt% of the mass of the chromite sand; the curing catalyst is first added to the chromite sand and mixed evenly, and then the furan resin is added and mixed evenly again. The thickness of the locally reinforced chilled sand in the suspended misalignment area is controlled to be 50-80mm, so that the suspension tie rod is completely embedded in the locally reinforced chilled sand and compacted. Chromite sand with a high thermal conductivity is selected as the material to improve the heat dissipation capacity of the suspended part. The proportion of auxiliary materials is controlled to cooperate with the suspension tie rod to improve the tensile strength of the local molding sand.

[0011] Preferably, during the process of filling and curing the locally reinforced chilled sand into the suspended misalignment area, the curing method is as follows: hot air at a temperature of 60-80℃ is continuously blown into the sand layer in the suspended misalignment area for 10-20 minutes to accelerate dehydration, cross-linking, and curing. The introduction of hot air accelerates the cross-linking and curing process of the furan resin in the suspended misalignment area, enabling the suspended reinforced retaining wall to quickly reach a strength capable of withstanding subsequent lateral extrusion pressure.

[0012] Preferably, the raw materials for mixing the conventional bulk furan self-hardening sand include natural quartz sand, a curing catalyst, and furan resin; The curing catalyst is added at 25-35 wt% of the mass of the furan resin, and the furan resin is added at 0.8-1.2 wt% of the mass of the natural quartz sand. The curing catalyst is first added to the natural quartz sand and mixed thoroughly, then the furan resin is added and mixed thoroughly again. Using natural quartz sand as the raw sand, while meeting the requirements for mold cavity collapsibility and permeability, controls the cost of auxiliary materials.

[0013] Preferably, the remaining area of ​​the internal box space formed by the combination of the cover box, the bottom box, and the suspended reinforced retaining wall is filled with conventional bulk furan self-hardening sand, and a temperature measuring hole is reserved on the cover box. After curing, the machine tool casting pattern is pulled out for demolding. During the process of forming the casting cavity, the curing time of the conventional bulk furan self-hardening sand at room temperature is controlled to be 30-60 minutes. Reasonable control of the curing time ensures that the overall molding sand strength reaches the operational requirements for stable demolding.

[0014] Preferably, a ring of ceramic fiber rope with a diameter of 15-20 mm is laid at the parting surface of the bottom box and the joint of the suspended misalignment area after demolding, and a refractory clay strip with a thickness of 3-8 mm is applied to the ceramic fiber rope. The flexibility of the ceramic fiber rope and the plasticity of the refractory clay strip are used to fill the structural gaps caused by the irregular parting surface.

[0015] Preferably, after the enclosure is closed using the external positioning ear plates, refractory mortar is used to seal the external joints. The internal layer of ceramic fiber rope and refractory mortar strips, combined with the external mortar sealing, forms a double seal, preventing leakage at the joints.

[0016] Preferably, the process of injecting liquid cast iron into the casting cavity, and then opening the mold and removing sand after cooling includes: placing a weight of 40-60T on top of the cover box; Liquid cast iron at a temperature of 1300-1350℃ is injected into the casting cavity; after pouring, it is kept at this temperature for 5-7 days. When the internal temperature, measured through the pre-reserved temperature measuring hole in the cover box, drops to 250-300℃, the box is opened and the sand is removed. A large-tonnage weight is placed to overcome the lifting force during pouring. By using temperature measuring holes to monitor the internal temperature of the mold, the sand is removed when the temperature drops to below 250-300℃, thus reducing the risk of thermal deformation of the machine tool castings caused by rapid cooling after removal from the mold.

[0017] This invention provides a method for using a sand box in machine tool casting production. It has the following beneficial effects: 1. This invention re-establishes the positioning benchmark for irregularly shaped sand boxes by fixing external positioning ear plates to the outer walls of the cover and bottom boxes of different sizes, and drilling positioning pin holes with the assistance of a three-dimensional scribing instrument. This feature solves the technical problem that the original pin sleeves cannot be matched due to the use of unused sand boxes, ensures the fitting accuracy of the upper and lower sand boxes, and avoids dimensional deviations in machine tool castings caused by misaligned boxes.

[0018] 2. This invention addresses the suspended misalignment areas caused by differences in sand box dimensions by using locally reinforced chilled sand for filling and combining it with hot air to accelerate curing, forming a suspended reinforced retaining wall with supporting capabilities. This retaining wall, combined with metal top columns and suspension braces, provides boundary and structural support for subsequent conventional main sand filling, preventing the molding sand from settling and falling off; at the same time, the high thermal conductivity of the chilled sand accelerates the heat dissipation rate in the local area, meeting the cooling requirements of specific parts of the machine tool.

[0019] 3. This invention lays ceramic fiber ropes and refractory mortar strips at the internal joints of the bottom box parting surface and the suspended misalignment area, and applies refractory mortar to the external joints after the box is assembled. Utilizing the flexible deformation of the ceramic fiber ropes under pressure and the filling properties of the refractory mortar, the irregular structural gaps generated at the joints of the shaped sand box are sealed, preventing the overflow and leakage of high-temperature molten cast iron during the pouring stage. Attached Figure Description

[0020] Figure 1 This is a graph showing the change of the DSC isothermal curing heat flux rate over time according to the present invention. Figure 2 This is a graph showing the evolution of the compressive strength of the molding sand of the present invention over time; Figure 3 This is a diagram showing the shear load-displacement curve of the suspended sand block according to the present invention. Figure 4 This is the high-temperature static pressure penetration back-side temperature response curve of the present invention. Detailed Implementation

[0021] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0022] Example 1:

[0023] This embodiment provides a method for using sand boxes in machine tool casting production, including the following steps: The sand box was modified and a positioning benchmark was established. A large, unused sand box, larger than the base box, was selected as the cover box. A 15mm thick Q235 low-carbon steel plate was fully welded around the outer surface of its top to increase the height of the box, and the weld slag was cleaned. Due to the size difference between the upper and lower sand boxes, the original pin sleeves could not fit. External positioning ear plates were welded at corresponding positions on the outer wall of the base box and the outer wall of the modified cover box. Using a 3D scribing instrument with the center line of the machine tool casting pattern as a benchmark, the coaxiality of the upper and lower external positioning ear plates was calibrated, and positioning pin holes were drilled.

[0024] Arrange the base box and construct its internal support. Place the base box on the molding base plate, and put in the machine tool casting pattern and the PT1000 elliptical pouring cup (i.e., the elliptical pouring cup with a built-in temperature sensor). Place a metal top column directly below the overhanging part of the base box corresponding to the overhanging part of the cover box. Invert the raised cover box and place it above the base box and the metal top column. Weld 10mm diameter round steel bars diagonally downwards to the inner wall of the raised steel plate of the cover box as suspension tie bars. The suspension tie bars extend into the overhanging misalignment area caused by the size difference, forming an internal stress-bearing skeleton.

[0025] Localized reinforcement sand filling and hot air intervention were implemented. Locally reinforced chilled sand was prepared using a sand mixer: first, 35 wt% of a curing catalyst (based on the resin mass) was added to the chromite sand and mixed thoroughly; then, 1.2 wt% of furan resin (based on the original sand mass) was added and mixed thoroughly. This locally reinforced chilled sand was then focused on filling the suspended misalignment area above the metal top column and around the suspension tie rods, with a thickness controlled at 60 mm and compacted to ensure the suspension tie rods were completely embedded in the sand. The hot air generator was then turned on, and hot air at 70°C was continuously blown into the sand layer in the suspended misalignment area for 15 minutes to accelerate the dehydration, cross-linking, and curing of the furan resin, forming a self-supporting suspended reinforced retaining wall.

[0026] Fill the remaining internal cavity of the combined sand box with conventional main body furan self-hardening sand (the mixing order is: first add 30wt% of the curing catalyst to the natural quartz sand and mix well, then add 1.0wt% of the furan resin to the original sand and mix well), pound and level it. Demold after the integral molding sand has cured at room temperature for 40 minutes.

[0027] The process involves assembling the sand box and applying multiple seals. A 15mm diameter ceramic fiber rope is laid around the parting surface and joints of the suspended misalignment area of ​​the bottom box after demolding, and a 5mm thick layer of refractory mortar is applied. The top box is then lifted, and a long rod is inserted into the positioning pin holes of the upper and lower external positioning ear plates to achieve precise assembly of the irregularly shaped sand box. After assembly, refractory mortar is applied again to seal the external joints.

[0028] A 50-ton pressure iron was placed on top of the mold box to press it down. Liquid cast iron at 1320℃ was poured into the mold cavity through a PT1000 elliptical pouring cup, with a total pouring weight of 13.4 tons. After pouring, the mold was kept at the required temperature for 6 days. When the internal temperature was measured to be below 300℃ through the temperature measuring hole, the mold box was opened and the sand was removed.

[0029] Example 2:

[0030] This embodiment provides a method for using sand boxes in machine tool casting production, including the following steps: A 10mm thick low-carbon steel plate is welded to the top surface of the mold box. The upper and lower external positioning ear plates are aligned for coaxiality and drilled. Metal top columns are placed around the bottom mold box. The mold box is inverted, and 8mm diameter suspension braces are welded to the inner wall of the mold box, extending to the suspended misalignment area. Locally reinforced chilled sand is prepared (first adding 30wt% curing catalyst by weight of resin, then adding 1.0wt% furan resin by weight of raw sand). This mixture is filled into the suspended misalignment area to a thickness of 50mm and compacted. Hot air at 60℃ is continuously blown through for 10 minutes. The remaining cavity is filled with conventional main body furan self-hardening sand (first adding 25wt% curing catalyst by weight of resin, then adding 0.8wt% furan resin by weight of raw sand). After curing for 30 minutes, the mold is removed. A 15mm diameter ceramic fiber rope is laid at the joint and a 3mm thick refractory mortar strip is applied. The mold box is closed using the external positioning ear plates, and the external refractory mortar is applied to the joints. A 40-ton pressure iron was placed in the mold for pressing. Liquid cast iron at a temperature of 1300℃ was injected into the cavity and kept at this temperature for 5 days. When the internal temperature dropped to 250℃, the mold was opened and the sand was removed.

[0031] Example 3:

[0032] This embodiment provides a method for using sand boxes in machine tool casting production, including the following steps: A 20mm thick low-carbon steel plate is welded to the top surface of the mold box. The upper and lower external positioning ear plates are aligned for coaxiality and drilled. Metal top columns are placed around the bottom mold box. The mold box is inverted, and 12mm diameter suspension braces are welded to the inner wall of the mold box, extending to the suspended misalignment area. Locally reinforced chilled sand is prepared (first adding 40wt% curing catalyst by weight of resin, then adding 1.5wt% furan resin by weight of raw sand). This mixture is filled into the suspended misalignment area to a thickness of 80mm and compacted. Hot air at 80℃ is continuously blown through for 20 minutes. The remaining cavity is filled with conventional main body furan self-hardening sand (first adding 35wt% curing catalyst by weight of resin, then adding 1.2wt% furan resin by weight of raw sand). After curing for 60 minutes, the mold is removed. A 20mm diameter ceramic fiber rope is laid at the joint, and an 8mm thick refractory mortar strip is applied. The mold box is closed using the external positioning ear plates, and the external refractory mortar is applied to the joints. A 60-ton pressure iron was placed in the mold for pressing. Liquid cast iron at a temperature of 1350℃ was injected into the cavity and kept at this temperature for 7 days. When the internal temperature dropped to 280℃, the mold was opened and the sand was removed.

[0033] Comparative Example 1: Compared to Example 1, the difference lies in the omission of the step of welding a 10mm diameter round steel bar diagonally downwards to the inner wall of the cover box as a suspension tie, thus eliminating the internal load-bearing framework within the suspended misalignment area. Everything else remains the same.

[0034] Comparative Example 2: Compared to Example 1, the difference lies in the elimination of the localized reinforcing sand filling and hot air intervention steps. Specifically, the suspended misalignment area does not use locally reinforcing chilled sand containing chromite sand, nor does it use continuous 70°C hot air blowing. Instead, it is uniformly filled with conventional main body furan self-hardening sand along with the remaining cavity and allowed to cure naturally at room temperature. All other aspects remain the same.

[0035] Comparative Example 3: Compared to Example 1, the difference lies in the elimination of the step of welding external positioning ear plates at corresponding positions on the outer wall of the bottom box and the outer wall of the modified cover box. During box assembly, alignment and fastening are achieved solely through visual inspection by the crane operator and manual stringing. Everything else remains the same.

[0036] Comparative Example 4: Compared to Example 1, the difference is that the step of laying ceramic fiber ropes and applying refractory mortar strips at the joints of the parting surface and the suspended misalignment area before closing the mold is omitted. The mold is closed directly, and refractory mortar is only applied to the external joints after closing the mold. Everything else is the same.

[0037] Test Example 1: This test example is used to determine the curing kinetics and functional group transformation of the main resin bonding system under different temperature interventions in the embodiments.

[0038] 1. Sample Preparation: Following the proportions in the examples, a certain amount of furan resin and a 65wt% p-toluenesulfonic acid aqueous solution were measured. The curing catalyst was added to the furan resin under a constant temperature water bath environment and mechanically stirred until homogeneous, yielding a mixed test solution. Samples were immediately transferred to the testing equipment. To simulate and compare different operating conditions, the test environment temperatures were set at room temperature (25℃), 60℃, 70℃, and 80℃.

[0039] 2. Differential Scanning Calorimetry (DSC) Test: Isothermal curing kinetics analysis was performed using a differential scanning calorimeter. 5-10 mg of the mixed test solution was weighed and placed in a standard aluminum crucible, which was then sealed and tightened. Under a nitrogen atmosphere at a flow rate of 50 mL / min, the sample was rapidly heated to the set isothermal test temperatures (25℃, 60℃, 70℃, and 80℃) and maintained at this temperature. The heat flow rate over time was recorded, and the peak time of the isothermal exothermic peak was extracted. This time parameter was used to assess the time span required for the system to reach the maximum crosslinking reaction rate.

[0040] 3. Fourier Transform Infrared Spectroscopy (FTIR) Test: The degree of cross-linking reaction was analyzed using a Fourier Transform Infrared Spectrometer equipped with an Attenuated Total Reflectance (ATR) accessory. A small amount of the mixed test solution was coated onto the surface of the ATR crystal and treated at 25℃, 60℃, 70℃, and 80℃ for 15 minutes each. Subsequently, the scanning range was 4000-400 cm⁻¹. -1 4cm resolution -1 Infrared absorption spectra of samples were collected under specific conditions. A 3400 cm⁻¹ depth was selected. -1 The hydroxyl (-OH) stretching vibration peak in the vicinity was used as a characteristic monitoring object. Based on the initial peak area before curing, the area decay rate of this characteristic peak after 15 minutes of treatment was calculated to characterize the conversion rate of hydroxyl groups participating in the polycondensation and dehydration reaction in the system.

[0041] Table 1. Curing kinetics and group transformation parameters of furan resin system under different temperature conditions.

[0042] According to Table 1 and Figure 1 The test data showed that different temperature conditions significantly promoted the crosslinking reaction process of the furan resin system. Figure 1The DSC curves showed that the exothermic peak appeared at 42.6 min under ambient temperature (25℃), while after thermal intervention at 60℃ to 80℃, the time to the isothermal exothermic peak was shortened to 12.4 min to 3.8 min. Combined with the spectral results in Table 1, the hydroxyl conversion rate in the system was 17.8% after 15 min at ambient temperature, while the hydroxyl conversion rate under thermal intervention reached over 69.1% in the same time period. These data indicate that introducing thermal intervention above the conventional operating environment helps overcome the activation energy barrier within the system, accelerating the condensation and dehydration reaction of the furfuryl alcohol unit. This high conversion rate, at the macroscopic level, indicates that it can promote preliminary hardening and cross-linking of the molding sand at the interface in a relatively short time, providing a certain mechanical basis for the subsequent establishment of an early self-supporting structure to resist molten iron lateral pressure.

[0043] Test Example 2: This test case is used to determine the evolution of the early macroscopic mechanical properties of locally reinforced chilled sand under set working conditions.

[0044] 1. The locally enhanced chilled sand in the mixed state of Example 1 and the conventional bulk furan self-hardening sand in Comparative Example 2 were used as experimental subjects.

[0045] 2. Fill the two sets of molding sand into the standard figure-eight tensile test block mold and the cylindrical compressive test block mold with a size of 50mm×50mm respectively, and pound and level them with a pneumatic tamping machine.

[0046] 3. Apply hot air at 70°C to the surface of the sample in the mold of Example 1 for 15 minutes. The end of the blowing is recorded as the initial zero point (0 min) of the mechanical test. The samples in the mold of Comparative Example 2 are kept naturally static at an ambient temperature of 25°C.

[0047] 4. Using an intelligent sand strength testing machine, the room temperature tensile strength of two groups of figure-eight shaped specimens was tested at five time points: 0 min, 15 min, 30 min, 60 min, and 120 min. The room temperature compressive strength of the cylindrical specimens was also tested. The peak load at which the specimen fractured or crushed was recorded during the test. Five parallel specimens were prepared for each group at each test point, and the arithmetic mean was taken after removing extreme values ​​as the single-point data.

[0048] Table 2. Evolution of macroscopic mechanical properties of molding sand over time under different working conditions.

[0049] According to Table 2 and Figure 2The macroscopic mechanical properties of molding sand under different mix proportions and working conditions showed varying changes over time. Example 1 group exhibited a tensile strength of 0.41 MPa and a compressive strength of 1.15 MPa at the end of the hot air intervention, and both mechanical properties continued to increase during the subsequent static settling period. Comparative Example 2 group was in a lower strength range initially, with a tensile strength of 0.08 MPa and a compressive strength of 0.21 MPa at the 15-minute mark. Considering the material's heat transfer characteristics, the thermal intervention treatment combined with chromite aggregate helps to promote the formation of bonded bridging structures in the early stages of curing. This mechanical evolution process indicates that thermodynamic intervention can pre-establish a solid retaining wall with initial load-bearing capacity in the suspended misalignment area, providing preliminary mechanical conditions for shortening the overall demolding waiting time and resisting subsequent molten metal lateral pressure.

[0050] Test Example 3: This test case is used to determine the ultimate shear bearing capacity of a solidified sand structure in a suspended misalignment zone under lateral stress conditions.

[0051] 1. The structural units containing the cover box heightening steel plate and the solidified sand body in the suspended misalignment area prepared in Examples 1 to 3 and Comparative Example 1 were used as experimental objects. The basic size of the sample was 300mm × 300mm, and the interface bonding state and the internal skeleton embedding state were kept unchanged.

[0052] 2. Rigidly clamp the steel plate portion of the sample onto the fixed base of the hydraulic servo universal testing machine, so that the cured sand block is in a cantilever state. Install a rigid pressure plate on the side of the sand block (parallel to the contact interface), with the center of action of the pressure plate corresponding to the geometric center of the sand block.

[0053] 3. Apply a quasi-static displacement load to the push plate through the actuating cylinder of the testing machine. The loading rate is set to 2.0 mm / min to simulate the lateral shear thrust generated by the liquid metal on the suspended sand block during the rising process in the cavity.

[0054] 4. During the loading process, simultaneously record the data from the displacement and force sensors of the testing machine. Observe the crack initiation and macroscopic fracture and peeling phenomena on the sand surface. Extract the ultimate shear load values ​​when each group of specimens experiences overall slippage or structural failure, and collect the corresponding load-displacement history curves.

[0055] Table 3. Shear limit load and failure displacement parameters of suspended sand block structures under lateral loading.

[0056] According to Table 3 and Figure 3The embodiment group with built-in metal suspension braces and the comparative example group without such a frame exhibited different load-bearing behaviors under lateral shear thrust. The specimen in Comparative Example 1 underwent macroscopic fracture at a load of 4.15 kN and a displacement of 1.36 mm, with the load curve showing brittle fracture characteristics, and the sand block detached entirely from the steel plate. The ultimate shear loads of Examples 1 to 3 ranged from 37.81 kN to 55.49 kN. During the load-displacement process, after local cracks appeared in the sand body, the load values ​​still showed a sustained or slowly decreasing trend, indicating a progressive failure mode. The test data show that pre-embedding the metal structural component within the suspended misaligned sand body helps establish cross-interface constraint relationships, to some extent changing the working mode of the frameless sand block relying solely on the resin adhesive film to bear the interfacial shear stress. This internal rigid structure bears part of the external thrust distribution, delaying the overall slippage of the suspended sand block and improving the mechanical limit of the component under eccentric static pressure.

[0057] Test Example 4: This test case is used to determine the relative dimensional accuracy of a large-span irregularly shaped sand box system after the box assembly process is completed.

[0058] 1. The combined sand box system after integral molding sand curing and demolding operations in Examples 1 to 3, and Comparative Example 3, were used as experimental subjects. The experimental environment was at room temperature in a conventional foundry workshop.

[0059] 2. After completing the box assembly process and placing the pressure irons stably according to the weights set for each group, use a high-precision laser tracker to perform a three-dimensional coordinate scan of the metal detection reference surface pre-established on the outside of the sand box.

[0060] 3. Using the theoretical center reference plane of the machine tool main guide rail pattern arranged inside the bottom box as the origin zero position of the absolute coordinate system, establish the X-axis along the horizontal direction parallel to the long side of the bottom box and establish the Y-axis along the horizontal direction parallel to the short side of the bottom box.

[0061] 4. Measure the coordinate projection of the reference detection point on the top of the cover box onto the horizontal two-dimensional plane, calculate the displacement difference between the actual fastening position of the cover box and the theoretical absolute zero position in the X-axis and Y-axis directions, and record the absolute value of the difference as the misalignment parameter.

[0062] 5. Perform 10 independent lifting and box fastening processes on each group of experimental subjects. After each fastening, independently read and record the misalignment data of the X-axis and Y-axis, and statistically extract the arithmetic mean and the maximum extreme value.

[0063] Table 4. Horizontal two-dimensional dimension offset parameters under multiple snap-fit ​​operations of the combined sand box

[0064] According to the statistical results in Table 4, for large-span irregularly shaped sand box components lacking the original pin sleeve mating conditions, the presence or absence of a box-closing guidance mechanism directly affects the dimensional accuracy of the mating. In Comparative Example 3, relying solely on visual observation and manual stringing for alignment resulted in a wide-ranging, discrete distribution of data points in the horizontal plane, with a maximum offset reaching 14.62 mm. This type of random displacement deviation easily increases the risk of uneven distribution of machining allowances in large machine tool castings. The two-dimensional coordinate offset points in Examples 1 to 3 are all concentrated within the tolerance zone near the zero point, and their maximum offset extreme values ​​are all controlled within 1.6 mm. This coordinate data comparison shows that establishing a secondary positioning pin hole system on the outer wall of the modified sand box can reconstruct the mechanical guiding path under large-span dimensional differences. This positioning method reduces the probability of random error accumulation caused by suspension swing and visual blind spots, providing better structural protection for the geometric forming accuracy of the assembled sand box.

[0065] Test Example 5: This test case is used to determine the sealing and puncture resistance performance of the combined sand box interface structure under the dynamic static load of high-temperature molten metal.

[0066] 1. The solidified structural units containing the interface seam features of the suspended misalignment region prepared in Examples 1 to 3, and Comparative Examples 2 and 4, were used as experimental objects. A specimen with complete interface features was cut and placed at the lower flange of a self-made high-temperature melt static pressure testing device, and rigidly sealed externally using fasteners.

[0067] 2. A graphite crucible with a built-in heating element is connected to the top of the device. Liquid cast iron, melted to 1320℃, is poured into the graphite crucible so that the bottom of the molten metal pool directly contacts the test interface of each group of test blocks.

[0068] 3. High-pressure argon gas is introduced into the molten cast iron surface through a sealed gas passage at the top of the graphite crucible. The gas pressure loading program is set to linearly increase at a rate of 0.01 MPa / min to simulate the static pressure at the bottom of the molten metal that gradually increases as the liquid level rises during the pouring process in a large sand box.

[0069] 4. Arrange a thermocouple temperature measurement array and a photoelectric droplet sensing probe on the bottom surface (non-contact back side) of the sample. Record the temperature response history on the back side in real time.

[0070] 5. When molten iron penetrates the gap, triggering the photoelectric probe or causing a step surge in the back-side temperature, stop the gas pressure loading. Record the critical penetration pressure (MPa) at this point, and record the duration of this process as the penetration resistance holding time (min). If no penetration occurs within the upper limit of the test time set at 80 min, record the corresponding pressure at that time and terminate the test.

[0071] Table 5. High-Temperature Liquid Metal Penetration Resistance Test Data for Interface Unit Structures

[0072] According to Table 5 and Figure 4 The interface units under complex boundary conditions exhibited differences in their resistance to high-temperature hydrostatic penetration. Comparative Example 2, using conventional molding sand without reinforced chilling units, showed a sand structure prone to strength decay at high temperatures, collapsing after 2.6 minutes of loading (0.038 MPa). Comparative Example 4, lacking a sealing and isolation system composed of ceramic fiber ropes and refractory strips, experienced earlier failure at its joints under the stress of molten metal wedging, with the test stopping at 5.3 minutes. The example group integrated reinforced chilling materials and multiple sealing mechanisms, resulting in a generally increased actual critical penetration pressure value above 0.147 MPa and an extended penetration resistance time, as shown in Table 5 and... Figure 4 Based on temperature response data, this combined anti-seepage method limits the microscopic penetration of high-temperature melt, preventing abrupt temperature jumps characteristic of melt penetration on the back side. This combined blocking design helps reduce the incidence of molten iron leakage and fire at the bottom edge during the pouring of large castings in practical applications.

Claims

1. A method for using a sand box in machine tool casting production, characterized in that, Includes the following steps: External positioning ear plates are fixed at corresponding positions on the outer side wall of the cover box (which is larger than the bottom box) and the outer side wall of the bottom box, respectively. The cover box is placed upside down on top of the base box, which is a pre-set machine tool casting pattern. Due to the size difference between the cover box and the base box, a suspended misalignment area is formed. Locally reinforced chilled sand is filled into the suspended misalignment area and solidified to form a suspended reinforced retaining wall. The remaining area of ​​the internal box space formed by the combination of the cover box, the bottom box and the suspended reinforced retaining wall is filled with conventional main body furan self-hardening sand, and a temperature measuring hole is reserved on the cover box. After solidification, the machine tool casting pattern is pulled out to form a casting cavity. After the mold is removed, ceramic fiber ropes are laid on the parting surface of the bottom box and the joint of the suspended misalignment area and refractory mud strips are applied. The box is then closed by the external positioning ear plate. Liquid cast iron is injected into the casting cavity, and after the casting cools, the mold is opened and the sand is removed.

2. The method of using a sand box in machine tool casting production according to claim 1, characterized in that, A 10-20mm thick low-carbon steel plate is fully welded around the outside of the top surface of the cover box to increase the height of the box. Using a three-dimensional scribing instrument to refer to the center line of the machine tool casting pattern, the coaxiality of the corresponding external positioning ear plates is calibrated and positioning pin holes are drilled. The box closing operation is achieved by inserting a long rod positioning pin into the positioning pin hole.

3. The method of using a sand box in machine tool casting production according to claim 2, characterized in that, Before placing the cover box upside down on the bottom box of the pre-set machine tool casting pattern, place the bottom box on the molding base plate, put in the machine tool casting pattern and the elliptical pouring cup with built-in temperature sensor, and place a metal top column on the outside of the bottom box directly below the suspended misalignment area corresponding to the size of the cover box. A suspension tie rod is welded obliquely downwards to the inner wall of the low-carbon steel plate, so that the suspension tie rod extends into the suspended misalignment area.

4. The method of using a sand box in machine tool casting production according to claim 3, characterized in that, The locally reinforced chilled sand is composed of chromite sand, a curing catalyst, and furan resin. The amount of the curing catalyst added is 30-40 wt% of the mass of the furan resin, and the amount of the furan resin added is 1.0-1.5 wt% of the mass of the chromite sand; the curing catalyst is first added to the chromite sand and mixed evenly, and then the furan resin is added and mixed evenly again. The thickness of the locally reinforced chilled sand in the suspended misalignment area is controlled to be 50-80mm, so that the suspension tie rod is completely embedded in the locally reinforced chilled sand and compacted.

5. The method of using a sand box in machine tool casting production according to claim 1, characterized in that, During the process of filling the suspended misalignment area with locally reinforced chilled sand and solidifying it, the solidification method is as follows: hot air at a temperature of 60-80℃ is continuously blown into the sand layer in the suspended misalignment area for 10-20 minutes to accelerate dehydration, cross-linking and solidification.

6. The method of using a sand box in machine tool casting production according to claim 1, characterized in that, The raw materials for mixing the conventional main body furan self-hardening sand include natural quartz sand, curing catalyst and furan resin; The amount of the curing catalyst added is 25-35 wt% of the mass of the furan resin, and the amount of the furan resin added is 0.8-1.2 wt% of the mass of the natural quartz sand; first, the curing catalyst is added to the natural quartz sand and mixed evenly, and then the furan resin is added and mixed evenly again.

7. The method of using a sand box in machine tool casting production according to claim 1, characterized in that, The remaining area of ​​the internal box space formed by the combination of the cover box, the bottom box, and the suspended reinforced retaining wall is filled with conventional bulk furan self-hardening sand. After curing, the machine tool casting pattern is pulled out to form the casting cavity. During this process, the curing time of the conventional bulk furan self-hardening sand at room temperature is controlled to be 30-60 minutes.

8. The method of using a sand box in machine tool casting production according to claim 1, characterized in that, After the mold is removed, a ring of ceramic fiber rope with a diameter of 15-20mm is laid at the joint of the parting surface of the bottom box and the suspended misalignment area, and a refractory clay strip with a thickness of 3-8mm is applied to the ceramic fiber rope.

9. A method for using a sand box in machine tool casting production according to claim 1, characterized in that, After the box is assembled using the external positioning ear plate, refractory putty is used to seal the external joints after assembly.

10. A method for using a sand box in machine tool casting production according to claim 1, characterized in that, The process of injecting liquid cast iron into the casting cavity, and then opening the mold and removing sand after the casting has cooled includes: placing a pressure iron weighing 40-60T on top of the mold cover; The liquid cast iron at a temperature of 1300-1350℃ is injected into the casting cavity; after pouring, it is kept warm for 5-7 days, and the internal temperature is measured to be 250-300℃ through the temperature measuring hole reserved in the cover box. When the temperature drops, the box is opened and the sand is removed.