Method for judging stability of mold flux film of crystallizer protective flux

By detecting the temperature fluctuation pattern of the thermocouple on the copper plate of the crystallizer, the stability of the protective slag film can be accurately determined, thus solving the problem of longitudinal cracks on the surface of the cast billet caused by the instability of the slag film in the crystallizer, thereby improving the quality of the cast billet and reducing the cost.

CN123128461APending Publication Date: 2026-11-20HBIS LAOTING STEEL CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611514552.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

The lack of effective methods in the current technology to determine the stability of the protective slag film in the crystallizer during the continuous casting process makes it difficult to detect longitudinal cracks on the surface of the billet, increasing quality loss and production costs, which does not meet the requirements of green and low-carbon development.

Method used

The condition and stability of the protective slag film are determined by observing the temperature fluctuation patterns detected by the thermocouples in the second and third rows of the copper plates of the crystallizer. The specific steps include detecting the rate and magnitude of temperature rise and fall, and judging the stability of the slag film by combining synchronous and asynchronous fluctuations.

Benefits of technology

It enables accurate and convenient assessment of the stability of the protective slag film, allowing for timely measures to eliminate surface defects in the billet, reduce costs, improve billet quality, and meet the requirements of green and low-carbon development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128461A_ABST
    Figure CN123128461A_ABST
Patent Text Reader

Abstract

The application discloses a method for judging the stability of a crystallizer protecting slag film, which judges that the slag film is in an unstable state when the temperature fluctuation of the copper plate detected by the second row and the third row of thermocouples in the process of continuous casting is as follows: the temperature fluctuation period of the second row of thermocouples is that the temperature of some column of the second row of thermocouples firstly rises at a rising speed of 1.7-5 ℃ / min by 5-10 ℃, and then falls at a falling speed of 0.4-1.3 ℃ / min to the original temperature; and the temperature fluctuation period of the third row of thermocouples is that the temperature of the same column of the third row of thermocouples firstly rises at a rising speed of 6.7-15 ℃ / min by 20-30 ℃, and then falls at a falling speed of 1.7-3.8 ℃ / min to the original temperature. The method can accurately judge the state of the slag film of the protecting slag in the process of continuous casting, and further can judge the heat transfer state of the crystallizer and the surface quality state of the casting blank, so that measures can be taken in time, the surface defects of the casting blank can be eliminated, and the cost consumption can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of continuous casting technology, and in particular to a method for determining the stability of the protective slag film in a crystallizer. Background Technology

[0002] The use of mold flux in continuous casting is one of the key technological breakthroughs in the development of continuous casting, and it plays a crucial role in improving the quality of cast billets. After being added to the mold, the flux forms a slag film between the mold copper plate and the billet shell, which ensures lubrication and controls heat transfer. The uniformity and stability of this slag film directly affect the uniformity of lubrication and heat transfer in the mold, and thus have a vital impact on the surface quality of the cast billet.

[0003] In existing technologies, the thesis "Study on Simulation of Protective Slag Film Structure and Its Lubricating Performance" (Master's Thesis, Chongqing University, author Cheng Hongyan) studied the protective slag film structure and lubricating performance. Through testing and analysis of the slag film structure and performance, it investigated the interdependence between protective slag composition, molten slag properties, slag film structure, and slag film lubrication. The thesis "Study on Solidification Structure Characteristics of Protective Slag Film in Peritectic Steel Continuous Casting" (Doctoral Dissertation, Chongqing University, author Long Xiao) studied the solidification structure characteristics of protective slag film in peritectic steel continuous casting and clarified the evolution law of the slag film structure. The thesis "Study on the Influence of Molder Protective Slag Film Structure on Heat Transfer" (Master's Thesis, Chongqing University, author Zhao Yanhong) focused on analyzing the factors affecting heat transfer of protective slag from the perspective of slag film structure, based on quantitative testing of heat transfer in continuous casting mold protective slag. The thesis, "Study on the Influence of Mineral Composition of Continuous Casting Protective Slag on its Crystallization Properties" (Master's Thesis, Hebei United University, author Liu Lei), established the relationship between the mineral composition of protective slag and the crystallization behavior of slag film using a hot-wire melting crystallization performance tester. Subsequently, an experimental slag film was obtained using a crystallizer slag film heat flow simulator, and the relationship between the mineral composition of protective slag and the mineral phase structure of slag film was explored. This study laid a theoretical foundation for quantitatively controlling the mineral composition of raw slag and the mineral phase structure of slag film to coordinate the contradiction between heat transfer and lubrication. "Research Progress on Heat Transfer Characteristics of Mold Film in Continuous Casting Molding Machines" (Special Steel, June 2021, author Han Xiuli) reviews the influence of basicity, chemical composition, and crystallization properties of mold film on the heat transfer of traditional fluorine-containing slag system CaO-SiO2-CaF2 and novel fluorine-free slag systems CaO-SiO2-B2O3 and CaO-SiO2-TiO2. It summarizes the research results of metallurgists on the heat transfer of slag film in fluorine-containing and fluorine-free mold film over the past decade, concluding that calcium borosilicate and perovskite in the crystalline mineral phases of fluorine-free mold film exhibit similar crystallization behavior to gunmetal in traditional mold film. "Research Progress on Crystallization Characteristics of Mold Film in Continuous Casting Molding Machines" (Materials Reports, author Yu Xiong) reviews the research progress on the crystallization characteristics of mold film in continuous casting molding machines. It discusses the main influencing factors of the crystallization characteristics of mold film, including crystallization temperature, crystallization rate, crystalline mineral phases, and slag film surface roughness, as well as the research methods for the crystallization process, and proposes research directions for the crystallization characteristics of mold film.

[0004] In summary, current research on protective slag films mainly focuses on the influence of protective slag composition on the slag film's mineral phase structure, and the influence of the slag film structure on the lubrication and heat transfer properties of the protective slag. However, there is very little research on the stability of the slag film after the protective slag melts and fills within the crystallizer during production, and how to assess this stability. Even the best slag film mineral phase structure requires uniform and stable thickness between the copper plate and the billet shell in order to function effectively; that is, the stability of the slag film must be guaranteed. In actual production, if the protective slag film is unstable—that is, its thickness is unstable and uneven—the heat flow and heat transfer in the crystallizer will be unstable, leading to longitudinal cracks on the surface of the billet. These surface cracks in red-hot billets are difficult to detect, and discovering them after rolling into steel plates will increase quality losses and production costs. Removing the billet from the production line, cooling it, and then performing cold inspection and surface cleaning will also increase costs and energy consumption, which is inconsistent with current green and low-carbon development requirements. Therefore, there is an urgent need to find an effective method to promptly assess the stability of the protective slag film in the crystallizer during actual production. Summary of the Invention

[0005] The technical problem to be solved by the present invention is to provide a method for judging the stability of the protective film of crystallizer slag with high accuracy and simplicity.

[0006] To solve the above technical problems, the technical solution adopted by the present invention includes the following steps: (1) During the continuous casting process, observe whether the temperature of the copper plate detected by the thermocouples of the second and third rows of the crystallizer copper plate shows the following temperature fluctuation; The temperature fluctuation cycle of the second row of thermocouples is as follows: the temperature of a certain column of thermocouples in the second row first rises by 5 to 10°C at a rising rate of 1.7°C / min to 5°C / min, and then falls back to the original temperature at a falling rate of 0.4°C / min to 1.3°C / min. The temperature fluctuation cycle of the third row of thermocouples: the temperature of the third row of thermocouples changes synchronously with that of the second row of thermocouples. The temperature of the third row of thermocouples first rises by 20 to 30°C at a rate of 6.7°C / min to 15°C / min, and then falls back to the original temperature at a rate of 1.7°C / min to 3.8°C / min. (2) When two or more rows of thermocouples in the second and third rows exhibit the above fluctuations, and the fluctuations are synchronous in the same row and asynchronous in different rows, it can be determined that the slag film is in an unstable state during the use of the protective slag of the crystallizer.

[0007] Furthermore, in step (1), the temperature of the rising peak of the thermocouples in the third row is not higher than the temperature of the rising peak of the thermocouples in the first row, but is higher than the temperature of the rising peak of the thermocouples in the second row.

[0008] Furthermore, in step (1), the period of temperature fluctuation of the second and third rows of thermocouples is 10 to 15 minutes.

[0009] The beneficial effects of adopting the above technical solution are as follows: This invention uses the temperature change pattern of the copper plates detected by the thermocouples in the second and third rows of the crystallizer as a basis to determine the state and stability of the protective slag film. This invention can accurately determine the state of the protective slag film during continuous casting, and thus determine the heat transfer state of the crystallizer and the surface quality state of the cast billet, allowing for timely measures to eliminate surface defects and reduce costs. This invention is highly accurate and simple, playing a crucial role in improving the quality of cast billets, creating conditions for direct rolling and hot charging of cast billets, and conforming to the requirements of green and low-carbon development. Attached Figure Description

[0010] The present invention will now be described in further detail with reference to the accompanying drawings and specific embodiments.

[0011] Figure 1 This is a schematic diagram of the structure of the copper plate thermocouple of the crystallizer described in this invention.

[0012] In the diagram: 1 - Column 1 thermocouples, 2 - Column 11 thermocouples, 3 - Row 1 thermocouples, 4 - Row 2 thermocouples, 5 - Row 3 thermocouples, 6 - Thermocouples. Detailed Implementation

[0013] The present invention will now be described in further detail with reference to specific embodiments.

[0014] This method for determining the stability of the protective slag film in a crystallizer uses the temperature of the copper plates measured by thermocouples in the second and third rows of the crystallizer as the basis for judging the state and stability of the protective slag film; it includes the following steps: (1) Temperature fluctuation cycle: Figure 1 As shown, the thermocouples 6 are arranged in several rows and columns on the copper plate of the crystallizer, with the rows extending along the length of the copper plate of the crystallizer being the columns, such as... Figure 1 The first row of thermocouples 3, the second row of thermocouples 4, and the third row of thermocouples 5; the columns extending along the width direction of the copper plate of the crystallizer are as follows, such as... Figure 1 Thermocouple 1 in column 1 and thermocouple 2 in column 11; observe whether the temperature fluctuations of the copper plates detected by the thermocouples in the second and third rows of the crystallizer copper plates are as follows; The temperature fluctuation cycle of the second row of thermocouples is as follows: the temperature of a certain column of thermocouples in the second row first rises at a rate of 1.7℃ / min to 5℃ / min, with an increase of 5 to 10℃; then it falls at a rate of 0.4℃ / min to 1.3℃ / min, returning to the original temperature; the above temperature fluctuation is a continuous periodic fluctuation with a fluctuation period of 10 to 15 minutes. The temperature fluctuation cycle of the third row of thermocouples is as follows: the temperature of the thermocouples in the same row of the third row first rises at a rate of 6.7℃ / min to 15℃ / min, with an increase of 20℃ to 30℃; then it falls at a rate of 1.7℃ / min to 3.8℃ / min, until it returns to the original temperature. Furthermore, the temperature at the peak of the temperature rise of the thermocouples in the third row is less than or equal to the temperature at the peak of the temperature rise of the thermocouples in the first row, and exceeds the temperature at the peak of the temperature rise of the thermocouples in the second row.

[0015] The temperature fluctuations described above are in a continuous periodic pattern, with the period preferably being 10 to 15 minutes.

[0016] (2) Judgment method: When two or more columns of thermocouples in the second and third rows show the above fluctuations, and the same column fluctuates synchronously and different columns fluctuate asynchronously, it can be judged that the slag film is in an unstable state during the use of the crystallizer protective slag.

[0017] Specifically, the following three conditions must be met for judgment: ① When two or more thermocouples in the second and third rows exhibit the aforementioned fluctuation period in temperature changes; ② Synchronous fluctuation within the same row, meaning that when two or more thermocouples in the second row exhibit the aforementioned fluctuation period, the thermocouples in the same row of the third row exhibit the same fluctuation period simultaneously; ③ Asynchronous fluctuation across different rows, meaning that the temperature fluctuations in different rows change sequentially or at different intervals. Once all three conditions are met, it can be determined that the slag film in the protective slag of this crystallizer is in an unstable state during use.

[0018] (3) Handling measures: When it is determined that the slag film of a certain protective slag is in an unstable state during use, measures such as replacing the protective slag can be taken in time to eliminate the occurrence of longitudinal cracks on the surface of the billet.

[0019] (4) This method is applicable to all steel grades, especially low carbon alloy steel, medium carbon steel and medium carbon alloy steel, and is applicable to crystallizers equipped with 3 or more rows of thermocouples. Example 1

[0020] In a continuous casting operation, a 700L steel grade, a low-carbon alloy steel, was used with a specific protective slag. During the casting process, the temperature of a certain column of thermocouples in the second row began to rise abnormally, with an increase of 10°C at a rate of 5°C / min. The temperature then dropped back to its original temperature at a rate of 1.3°C / min. This temperature fluctuation exhibited a continuous cyclical pattern with a period of 10 minutes. Simultaneously, the temperature of the thermocouples in the third row changed synchronously with the second row and exhibited the same characteristics. The temperature of the third row of thermocouples rose abnormally by 30°C at a rate of 15°C / min, then dropped back to its original temperature at a rate of 3.8°C / min, also exhibiting a continuous cyclical pattern with a period of 10 minutes. The peak temperature of the third row of thermocouples equaled that of the first row and exceeded that of the second row. Since three columns of thermocouples in the second and third rows exhibited the above-mentioned temperature changes, and the temperatures of different columns changed at varying intervals, it was determined that the slag film was in an unstable state during the use of the protective slag. After the protective slag was used to produce billets that were rolled into steel plates, longitudinal cracks were found on the surface, and all of them were downgraded.

[0021] After timely replacement of the protective slag, the longitudinal crack defect disappeared, and all steel plates rolled from the cast billets produced using the replaced protective slag were qualified. Example 2

[0022] In a continuous casting process, the steel grade DP590, a low-carbon alloy steel, was used. A certain protective slag was employed. During casting, the temperature of a certain column of thermocouples in the second row began to rise abnormally, with an increase of 5°C at a rate of 1.7°C / min. The temperature then dropped back to its original temperature at a rate of 0.4°C / min. This temperature fluctuation exhibited a continuous cyclical pattern with a period of 15 minutes. Simultaneously, the temperature of the thermocouples in the third row changed synchronously with the second row, exhibiting the same characteristics. The temperature of the third row of thermocouples rose abnormally by 20°C at a rate of 6.7°C / min, then dropped back to its original temperature at a rate of 1.7°C / min, also exhibiting a continuous cyclical pattern with a period of 15 minutes. The peak temperature of the third row of thermocouples approached that of the first row and exceeded that of the second row. When two columns of thermocouples in the second and third rows exhibited the above characteristics, and the temperatures of different columns changed sequentially, it was determined that the slag film was in an unstable state during the use of the protective slag. After steel plates were rolled from billets produced using this protective slag, longitudinal cracks were found on the surface, resulting in a complete downgrade. After timely replacement of the protective slag, the longitudinal crack defect disappeared, and all steel plates rolled from the cast billets produced using the replaced protective slag were qualified. Example 3

[0023] In a continuous casting process, the steel grade was SS400, a medium carbon steel. A certain protective slag was used. During the casting process, the temperature of a certain column of thermocouples in the second row began to rise abnormally, with an increase of 7°C at a rate of 3°C / min. The temperature then dropped back to its original temperature at a rate of 0.8°C / min. This temperature fluctuation exhibited a continuous cyclical pattern with a period of 13 minutes. Simultaneously, the temperature of the thermocouples in the third row changed synchronously with the second row and exhibited the same characteristics. The temperature of the third row of thermocouples rose abnormally by 24°C at a rate of 10°C / min, then dropped back to its original temperature at a rate of 2.7°C / min, also exhibiting a continuous cyclical pattern with a period of 13 minutes. The peak temperature of the third row of thermocouples approached that of the first row and exceeded that of the second row. When four columns of thermocouples in the second and third rows exhibited the above characteristics, and the temperatures of different columns changed sequentially, it was determined that the slag film was in an unstable state during the use of the protective slag. After steel plates were rolled from billets produced using this protective slag, longitudinal cracks were found on the surface, resulting in a complete downgrade. After timely replacement of the protective slag, the longitudinal crack defect disappeared, and all steel plates rolled from the cast billets produced using the replaced protective slag were qualified. Example 4

[0024] In a continuous casting process, the steel grade 22MnB5, a medium-carbon alloy steel, was used. A certain protective slag was employed. During casting, the temperature of a certain column of thermocouples in the second row began to rise abnormally, with an increase of 6°C at a rate of 4°C / min. The temperature then dropped back to its original temperature at a rate of 0.9°C / min. This temperature fluctuation exhibited a continuous cyclical pattern with a period of 12 minutes. Simultaneously, the temperature of the thermocouples in the third row changed synchronously with the second row, exhibiting the same characteristics. The temperature of the third row of thermocouples rose abnormally by 26°C at a rate of 11°C / min, then dropped back to its original temperature at a rate of 2.9°C / min, also exhibiting a continuous cyclical pattern with a period of 12 minutes. The peak temperature of the third row of thermocouples equaled that of the first row and exceeded that of the second row. Five columns of thermocouples in the second and third rows exhibited the above characteristics, and the temperature changes in different columns occurred at varying intervals. This indicated that the slag film was unstable during the application of the protective slag. After the protective slag was used to produce billets that were rolled into steel plates, longitudinal cracks were found on the surface, and all of them were downgraded.

[0025] After timely replacement of the protective slag, the longitudinal crack defect disappeared, and all steel plates rolled from the cast billets produced using the replaced protective slag were qualified.

[0026] Statistical case studies: Low-carbon alloy steel, medium-carbon steel, and medium-carbon alloy steel were statistically analyzed to determine the proportion of longitudinal crack defects before and after the implementation of this method. The statistical results are shown in Table 1. Table 1: Comparison of Statistical Results

[0027] As shown in Table 1, this method effectively reduced the proportion of longitudinal cracks in various steel grades.

Claims

1. A method for determining the stability of the protective film in a crystallizer, characterized in that, Includes the following steps: (1) During the continuous casting process, observe whether the temperature of the copper plates detected by the thermocouples in the second and third rows of the crystallizer exhibits the following temperature fluctuations; The temperature fluctuation cycle of the second row of thermocouples is as follows: the temperature of a certain column of thermocouples in the second row first rises by 5 to 10°C at a rising rate of 1.7°C / min to 5°C / min, and then falls back to the original temperature at a falling rate of 0.4°C / min to 1.3°C / min. The temperature fluctuation cycle of the third row of thermocouples: the temperature of the third row of thermocouples changes synchronously with that of the second row of thermocouples. The temperature of the third row of thermocouples first rises by 20 to 30°C at a rate of 6.7°C / min to 15°C / min, and then falls back to the original temperature at a rate of 1.7°C / min to 3.8°C / min. (2) When two or more rows of thermocouples in the second and third rows exhibit the above fluctuations, and the fluctuations are synchronous in the same row and asynchronous in different rows, it can be determined that the slag film is in an unstable state during the use of the protective slag of the crystallizer.

2. The method for determining the stability of the protective film in a crystallizer according to claim 1, characterized in that: In step (1), the temperature of the rising peak of the thermocouples in the third row is not higher than the temperature of the rising peak of the thermocouples in the first row, but is higher than the temperature of the rising peak of the thermocouples in the second row.