A method of controlling inclusions in steelmaking continuous casting

By real-time monitoring of the liquid level in the ladle and segmented control of the sliding nozzle, combined with the use of covering agents and protective slag, as well as the tundish slag removal device, the problem of inclusion enrichment during continuous casting was solved, thereby improving the quality and production efficiency of the continuously cast billet.

CN123128464APending Publication Date: 2026-11-20HANZHONG STEEL LTDRP OF SHAANXI STEEL GRP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611526458.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-29
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

During continuous casting, the presence of inclusions in the molten steel leads to uneven steel structure, affecting cold and hot working properties and mechanical properties. Furthermore, the extended casting cycle causes inclusions to accumulate in the tundish, affecting billet quality and economic indicators.

Method used

By setting up a weighing detection unit inside the ladle to monitor the liquid level in real time, controlling the opening and closing time of the sliding nozzle in stages, and combining the use of Al₂O₃-CaO-based covering agent and protective slag, as well as the tundish slag discharge device, the simultaneous interception and purification of inclusions can be achieved.

Benefits of technology

It effectively controls the number of inclusions, improves the quality of continuously cast billets, reduces the content of non-metallic inclusions and Al₂O₃ inclusions, increases metal yield, and stabilizes the physicochemical properties of covering agents and protective slags.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128464A_ABST
    Figure CN123128464A_ABST
Patent Text Reader

Abstract

The application discloses a method for controlling inclusions in steelmaking continuous casting, comprising the steps of: S1, obtaining the corresponding relationship between the liquid level height of molten steel in a ladle and the weight of the molten steel; S2, setting a weighing detection unit at a ladle receiving position to detect the weight of the ladle in real time and convert it into a molten steel liquid level height signal; the application has the beneficial effects that: in the late ladle pouring stage, the sliding nozzle is closed in three stages according to the molten steel liquid level falling to different heights, effectively destroying the formation of liquid surface vortex, avoiding the ladle slag entrapment and the erosion products of refractory materials being brought into the tundish from the source; by adding an Al2O3-CaO low basicity covering agent on the liquid surface of the tundish and an Al2O3-CaO high basicity protective slag on the liquid surface of the crystallizer, the principle of CaO reacting with Al2O3 which is difficult to remove in the molten steel to generate Ca(AlO2)2 which floats up at high temperature is utilized, and the inclusions are cooperatively adsorbed and removed in the two links of the tundish and the crystallizer respectively; the tundish slag discharge device is used to actively discharge slag when the slag layer thickness is greater than or equal to 50 mm, and the slag layer thickness is effectively controlled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of iron and steel metallurgical process technology, specifically to a method for controlling inclusions in continuous casting steelmaking. Background Technology

[0002] With the further development of the steel industry, steel products are moving towards higher purity and higher stability. However, inclusions are often mixed into steel during continuous casting. These inclusions mainly exist in the form of non-metallic compounds. Their presence disrupts the continuity of the steel matrix, causes uneven steel structure, deteriorates the cold and hot working properties and some physical and chemical properties of the steel, and also reduces the mechanical properties and fatigue strength of the steel.

[0003] The continuous casting process involves injecting molten steel from a qualified ladle into an intermediate ladle via a sliding mechanism at the bottom of the ladle. The steel is then depressurized and diverted to a crystallizer, where it is cooled and solidified to form the initial continuous casting billet.

[0004] Currently, to achieve continuous steel production and reduce production costs, the casting cycle of continuous casting is controlled at 20-30 heats for special steel and over 50 heats for ordinary carbon structural steel, with some units reaching over 100 heats. As the casting cycle increases, in the later stages of casting, when the molten steel level is low, vortices appear in the center, causing non-metallic inclusions and corroded refractory materials to be drawn into the tundish along with the molten steel. If casting is stopped at this point, it results in a significant waste of molten steel, which is not in line with economic goals. However, as the casting cycle continues, inclusions that have entered the tundish float to the surface of the molten steel and accumulate, leading to a thicker slag layer on the tundish surface. Inclusions such as SiO2 and Al2O3 carried in the molten steel cause changes in the physicochemical properties of the covering agent and protective slag, severely affecting the control of inclusions within the billet.

[0005] Therefore, we propose a method for controlling inclusions in steelmaking continuous casting. Summary of the Invention

[0006] The purpose of this invention is to provide a method for controlling inclusions in molten steel during continuous casting, which can effectively control the amount of inclusions in molten steel and improve the quality of continuously cast billets.

[0007] To achieve the above objectives, a method for controlling inclusions in steelmaking continuous casting includes the following steps:

[0008] S1. Obtain the relationship between the height of the molten steel level in the ladle and the weight of the molten steel;

[0009] S2. A weighing detection unit is set at the ladle receiving position to detect the ladle weight in real time and convert it into a molten steel level height signal.

[0010] S3. During the continuous casting process, when the molten steel level drops to the first preset level range, the sliding gate of the ladle is closed for a first preset time, and then the sliding gate is opened to continue casting.

[0011] S4. When the molten steel level continues to drop to the second preset level range, control the sliding gate of the ladle to close for a second preset time, and then open the sliding gate to continue pouring.

[0012] S5. When the molten steel level continues to drop to the third preset level range, control the ladle sliding gate to close for a third preset time.

[0013] S6. After the molten steel flows from the ladle into the tundish, a covering agent is added to the surface of the molten steel in the tundish.

[0014] S7. When the thickness of the slag layer in the tundish reaches the preset thickness threshold, start the slag discharge operation to control the thickness of the slag layer in the tundish.

[0015] S8. After the molten steel flows from the tundish into the crystallizer, add protective slag to the surface of the molten steel in the crystallizer.

[0016] S9. Continue pouring until the pouring process is complete.

[0017] Preferably, the first preset liquid level range is 280mm~300mm, and the first preset time is 5s~10s; the second preset liquid level range is 185mm~215mm, and the second preset time is 10s~15s; the third preset liquid level range is 90mm~110mm, and the third preset time is 20s~25s.

[0018] Preferably, step S1, which involves obtaining the correspondence between the molten steel level and the weight of the molten steel in the ladle, specifically includes:

[0019] Measure the inner diameter of each part of the newly constructed steel ladle, calculate the weight of molten steel when the molten steel level is 90mm, 110mm, 185mm, 215mm, 280mm and 300mm respectively, and establish a molten steel level-weight comparison table.

[0020] Preferably, the weighing detection unit in step S2 includes: wireless weighing sensors installed at two receiving positions of the butterfly rotary table, with four wireless weighing sensors installed at each receiving position. The weighing instrument signal of each sensor is fed back to the system PLC controller, which determines the current molten steel level by matching the corresponding relationship based on the real-time weight signal.

[0021] Preferably, the slag discharge operation in step S7 includes providing a tundish slag discharge device, which includes a slag inlet trough located below the tundish slag discharge port and a slag pan located below the end of the slag inlet trough.

[0022] During slag discharge, open the sealing material of the tundish slag discharge port to allow the liquid slag on the tundish surface to flow into the slag inlet through the slag discharge port, and then into the slag pan through the slag inlet.

[0023] After the slag discharge is completed, the slag discharge port is resealed, and the slag inlet is cooled and cleaned.

[0024] Preferably, the preset thickness threshold in step S7 is 50 mm.

[0025] Preferably, the covering agent in step S6 is an Al2O3-CaO-based covering agent, and the protective slag is an Al2O3-CaO-based high-alkalinity protective slag.

[0026] Preferably, for the production of low-carbon small square billets, the covering agent comprises, by mass percentage: CaO: 9%~10%, SiO2: 36%~40%, Al2O3: 9%~10%, MgO: 10%~13%, C: 26%~30%, Na2O: 3%~4%, K2O: 2.5%~3.5%; the basicity of the covering agent is 0.23~0.28 for the ratio of CaO / SiO2.

[0027] For the production of low-carbon small square billets, the protective slag comprises, by mass percentage: SiO2: 32.5%~34%, CaO: 24.5%~25.8%, Al2O3: 7.2%~7.9%, K2O: 3.5%~4.5%, Na2O: 3.5%~5.5%, F: 4%~5%, C: 15.5%~18%, MgO≤5%, Fe2O3≤5%; the basicity of the protective slag, α=CaO / SiO2, is 0.72~0.80.

[0028] Preferably, the opening and closing of the sliding gate is achieved by a hydraulic cylinder controlling a lever to drive the sliding slide plate, and the PLC controller automatically issues an execution command based on the real-time liquid level signal.

[0029] Compared with the prior art, the beneficial effects of the present invention are:

[0030] 1. Based on the pattern of slag entrainment vortexes as the molten steel level in the ladle drops to different heights, this invention performs sliding nozzle closing operations for 5s~10s, 10s~15s, and 20s~25s sequentially at three key points: 280mm~300mm, 185mm~215mm, and 90mm~110mm, respectively. This measure effectively disrupts the conditions for vortex formation on the molten steel surface, preventing non-metallic inclusions and corrosive refractory materials from being entrained into the tundish.

[0031] 2. This invention adds an Al2O3-CaO-based low-alkalinity covering agent to the tundish surface and an Al2O3-CaO-based high-alkalinity protective slag to the crystallizer surface. By appropriately increasing the CaO content, the CaO reacts with the difficult-to-remove Al2O3 in the molten steel at high temperature to generate Ca(AlO2)2, which floats to the surface, significantly enhancing the adsorption capacity of the covering agent and protective slag for inclusions. This synergistic approach simultaneously intercepts inclusions in both the tundish and crystallizer stages, achieving purification treatment throughout the entire steel path and effectively preventing inclusions from entering the solidified billet shell.

[0032] 3. When the slag layer thickness in the tundish is ≥50mm, the present invention actively guides the slag discharge through a slag discharge device consisting of a slag discharge port, a slag inlet, and a slag pan, effectively controlling the slag layer thickness on the tundish liquid surface and avoiding the problem of denaturation of the physicochemical properties of the covering agent and protective slag due to the extension of the casting cycle. Attached Figure Description

[0033] Figure 1 This is a schematic diagram of the continuous casting steel pouring process of the method of the present invention;

[0034] Figure 2 This is a schematic diagram of the intermediate ladle slag discharge device used in the method of the present invention;

[0035] Figure 3 This is a schematic diagram of the continuous casting steel pouring process of the present invention.

[0036] In the diagram: 1. Ladle; 2. Ladle nozzle; 3. Tundish; 4. Crystallizer; 5. Slag chute; 6. Slag pan; 31. Slag discharge port. Detailed Implementation

[0037] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0038] Please see Figure 1 and Figure 3 The present invention provides a technical solution: a method for controlling inclusions in steelmaking continuous casting, comprising the following steps:

[0039] S1. Obtain the correspondence between the molten steel level and the weight of the molten steel in the ladle; specifically including:

[0040] Measure the inner diameter of each part of the newly constructed steel ladle, calculate the weight of molten steel when the molten steel level is 90mm, 110mm, 185mm, 215mm, 280mm and 300mm respectively, and establish a molten steel level-weight comparison table.

[0041] It should be noted that the main equipment involved in the continuous casting molten steel pouring process in this embodiment includes: ladle 1, ladle nozzle 2, tundish 3, crystallizer 4, and corresponding control systems and auxiliary devices; before the newly constructed ladle 1 is put into use, the inner diameter dimensions of various parts of the ladle 1 (including the bottom diameter, mouth diameter, wall inclination angle, and body height) are measured first, and the weight of molten steel corresponding to different molten steel levels in the ladle 1 is calculated accordingly. Specifically, the weight of molten steel corresponding to molten steel levels of 90mm, 110mm, 185mm, 215mm, 280mm, and 300mm needs to be calculated.

[0042] Taking a 150t ladle as an example, actual measurements show that the corresponding weights of molten steel at the above liquid level heights are approximately: 300mm for approximately 13.93t, 280mm for approximately 13.04t, 215mm for approximately 9.90t, 185mm for approximately 8.55t, 110mm for approximately 5.15t, and 90mm for approximately 4.23t. Specific values ​​may vary depending on the actual lining dimensions of the ladle and the degree of wear and tear during use, and should be recalibrated before each ladle is used.

[0043] The correspondence between the liquid level and the weight of molten steel is entered into the system PLC controller as a reference parameter for subsequent automatic control.

[0044] S2. A weighing detection unit is set at the ladle receiving position to detect the ladle weight in real time and convert it into a molten steel level height signal.

[0045] It should be noted that in this embodiment, four wireless load cells are installed at each of the two receiving positions on the butterfly rotary table, and the weighing instrument signals from each sensor are fed back to the system PLC controller. Wireless transmission type load cells with an accuracy of not less than 0.02%FS are selected to ensure the stability and real-time performance of signal transmission in harsh environments such as high temperature and vibration in continuous casting sites.

[0046] The PLC controller collects the weight signals from each sensor in real time. After filtering, noise reduction, and averaging, the signals are matched with the liquid level-weight comparison table established in step S1 to calculate the current molten steel level in the ladle in real time.

[0047] S3. During the continuous casting process, when the molten steel level drops to the first preset level range, the ladle sliding gate is closed for a first preset time, and then the sliding gate is opened to continue casting.

[0048] S4. When the molten steel level continues to drop to the second preset level range, control the ladle sliding gate to close for a second preset time, and then open the sliding gate to continue pouring.

[0049] S5. When the molten steel level continues to drop to the third preset level range, control the ladle sliding gate to close for a third preset time.

[0050] It should be noted that, in this embodiment, after the ladle 1 is placed on the continuous casting platform, as molten steel is continuously injected into the tundish 3 through the long nozzle 2, the gross weight of the ladle gradually decreases, and the PLC controller tracks the changes in the molten steel level in real time. When the level drops to a preset trigger condition, the PLC controller automatically sends a command to the sliding nozzle actuator, which drives the pull rod through the hydraulic cylinder to move the sliding slide plate, thereby closing or opening the sliding nozzle.

[0051] The specific steps are as follows:

[0052] The first stage of the shutdown operation: When the PLC system detects that the molten steel level has dropped to the 280mm~300mm range (i.e., the pouring has entered the later stage), the ladle sliding gate is automatically closed for 5s~10s. The purpose of this operation is to disrupt the weak vortices that initially form on the molten steel surface, preventing scum and refractory corrosion products from being sucked into the gate. A shutdown time that is too short will not effectively disrupt the vortices, while a shutdown time that is too long may cause excessive fluctuations in the tundish surface or even a risk of low liquid level. The preferred shutdown time for the first stage is 6s~8s. Immediately after the shutdown, the sliding gate is opened to resume molten steel pouring.

[0053] The second stage of closure: When the molten steel level continues to drop to the 185mm~215mm range, the sliding gate nozzle is closed again for 10s~15s. At this time, the vortex on the molten steel surface tends to intensify, and the closure time needs to be extended to fully break up the vortex and promote steel-slag separation. The preferred closure time for this stage is 12s~14s. After closure, the sliding gate nozzle is reopened.

[0054] The third stage of closure: When the molten steel level drops to the 90mm-110mm range, the final closure operation is performed, lasting 20-25 seconds. At this point, the molten steel is nearing the end of the pouring process, with the most intense surface vortices and the highest concentration of inclusions. Sufficient time is needed for the vortices to completely dissipate and for inclusions to rise fully to the surface. The preferred closure time for this stage is 21-23 seconds. After this closure, the ladle will not be reopened, or it may be briefly reopened to replenish molten steel depending on the volume of steel in the tundish before ending the pouring process.

[0055] The total time for the above three shut-off operations should be controlled within the range of 35s to 50s, with the specific value determined comprehensively based on the steel grade, ladle capacity, and tundish liquid level. Taking the production of HRB400 steel with a 150t ladle as an example, the preferred scheme is: shut off for 5s when the liquid level is 297mm, shut off for 13s when the liquid level is 202mm, and shut off for 21s when the liquid level is 100mm.

[0056] S6. After the molten steel flows from the ladle into the tundish, a covering agent is added to the surface of the molten steel in the tundish.

[0057] It should be noted that in this embodiment, after the molten steel flows from the ladle 1 into the tundish 3 through the long nozzle 2, some inclusions enter the tundish along with the molten steel. An Al2O3-CaO-based covering agent is added to the surface of the molten steel in the tundish. The amount of covering agent added is 0.3 kg to 0.5 kg per ton of molten steel. The specific amount is dynamically adjusted according to the coverage of the tundish surface and the thickness of the slag layer, ideally ensuring that the surface is completely covered by the covering agent without any obvious exposed molten steel.

[0058] For the production of low-carbon small square billets (steel grade HRB400), the mass percentage of each component of the covering agent is as follows: CaO: 9%~10%, SiO2: 36%~40%, Al2O3: 9%~10%, MgO: 10%~13%, C: 26%~30%, Na2O: 3%~4%, K2O: 2.5%~3.5%, with the balance being unavoidable impurities. The basicity of the covering agent is R = CaO / SiO2 = 0.23~0.28. Preferably, the composition of the covering agent is: CaO: 10%, SiO2: 36%, Al2O3: 9.6%, MgO: 11%, C: 27.3%, Na2O: 3.2%, K2O: 2.9%, and basicity R = 0.28.

[0059] The covering agent is designed with low alkalinity. Its functions are as follows: on the one hand, it forms a good liquid surface covering layer to isolate the air and prevent secondary oxidation of the molten steel; on the other hand, it utilizes an appropriate amount of CaO to react with the Al2O3 inclusions suspended in the molten steel at high temperature to generate calcium aluminate Ca(AlO2)2. This product has a low melting point and is easy to float to the slag layer and be adsorbed.

[0060] S7. When the thickness of the slag layer in the intermediate bag reaches the preset thickness threshold, start the slag discharge operation to control the thickness of the slag layer in the intermediate bag.

[0061] It should be noted that, in this embodiment, as the casting process continues (especially during multi-heat casting, the casting cycle can reach 20-100 heats), the slag layer on the surface of the molten steel in the tundish continuously thickens. The slag layer is enriched with a large amount of inclusions such as Al2O3 and SiO2 that float from the molten steel, as well as reaction products of the covering agent. When the thickness of the slag layer in the tundish reaches 50 mm or more, the excessive thickness of the slag layer will cause the following problems: hindering the effective contact between the covering agent and the molten steel, deteriorating the heat preservation effect of the molten steel, causing the physical and chemical properties of the covering agent to change, and even some of the slag layer may be drawn into the nozzle and flow into the crystallizer.

[0062] Therefore, an tundish slag removal device is used for active slag removal. For example... Figure 2As shown, the slag discharge device includes a slag inlet 5 located below the slag discharge port 31 of the tundish. The slag inlet 5 is made of high-temperature resistant steel plate, lined with refractory material, and is arranged at an inclination. A slag pan 6 is placed below its end.

[0063] The specific slag removal procedure is as follows:

[0064] During non-slag discharge periods, the tundish slag discharge port 31 is tightly sealed with refractory mortar (composed of high-alumina refractory powder and binder). When the slag layer thickness in the tundish is measured to be ≥50mm (slag layer thickness is measured by an insertion slag measuring rod or laser rangefinder), slag discharge is performed.

[0065] First, use tools such as steel chisels to pry open the refractory mud sealing material at the slag discharge port 31. Then, appropriately raise the molten steel level in the tundish (by increasing the ladle pouring speed or slightly reducing the casting speed), so that the molten slag on the tundish surface automatically overflows from the slag discharge port 31 under hydrostatic pressure. The overflowing molten slag flows downward along the slag guide trough 5 and finally falls into the slag pan 6 to cool and solidify.

[0066] During slag removal, the slag removal speed and amount must be controlled. Each slag removal session should last approximately 2 to 5 minutes, with the slag layer thickness reduced to 20 to 30 mm to avoid excessive slag removal and loss of molten steel. After slag removal, immediately reseal the slag removal port 31 with freshly prepared refractory mortar, and spray cooling water onto the slag inlet trough 5 to accelerate its cooling. Clean the solidified steel slag remaining on the inner wall of the slag inlet trough 5, and replace the slag pan 6 with a new one for the next slag removal.

[0067] S8. After the molten steel flows from the tundish into the crystallizer, a protective slag is added to the surface of the molten steel in the crystallizer.

[0068] It should be noted that, in this embodiment, after the molten steel flows from the tundish 3 into the crystallizer 4, some small inclusions that failed to float and be removed in the tundish may enter the crystallizer with the molten steel flow. A high-basicity protective slag based on Al2O3-CaO is added to the surface of the molten steel in the crystallizer 4. The amount of protective slag added is controlled at 0.4 kg to 0.6 kg per ton of molten steel, ideally forming a uniform covering layer on the surface of the crystallizer with a thickness maintained at 25 mm to 40 mm.

[0069] For the production of low-carbon small square billets (HRB400 steel grade), the mass percentages of the components in the protective slag are as follows: SiO2: 32.5%~34%, CaO: 24.5%~25.8%, Al2O3: 7.2%~7.9%, K2O: 3.5%~4.5%, Na2O: 3.5%~5.5%, F: 4%~5%, C: 15.5%~18%, MgO≤5%, Fe2O3≤5%; the basicity R of the protective slag, CaO / SiO2, is controlled between 0.72 and 0.80. Preferably, the composition of the protective slag is: SiO2: 32.5%, CaO: 25.8%, Al2O3: 7.5%, K2O: 3.8%, Na2O: 3.9%, F: 4.5%, C: 17.1%, MgO: 2.3%, Fe2O3: 2.6%, and the basicity is R=0.79.

[0070] The functions of this high-alkali protective slag include: (1) forming a three-layer structure of molten layer, sintered layer and powder layer on the surface of molten steel in the crystallizer, effectively isolating air and lubricating the surface of the billet; (2) using high CaO content (basicity 0.72~0.80) to enhance the adsorption capacity of Al2O3 inclusions, and fixing the Al2O3 inclusions floating to the liquid surface in the slag layer through the reaction formula: Al2O3+CaO→Ca(AlO2)2, preventing them from being rolled back into the molten steel; (3) the appropriate content of Na2O and K2O can reduce the melting point and viscosity of the protective slag, and promote the dissolution and diffusion of inclusions in the slag.

[0071] The covering agent and protective slag are used together to form a two-stage purification system of "pre-adsorption in the intermediate package + secondary adsorption in the crystallizer", which significantly improves the removal efficiency of inclusions throughout the process.

[0072] S9. Continue pouring until the pouring process is complete.

[0073] Example 1

[0074] Taking the production of HRB400 steel using a 150t ladle as an example (section 165×165mm, casting speed 2.7~3.3m / min), when the ladle weight is reduced to 13.93t, 9.34t, and 4.55t (corresponding to molten steel level heights of 297mm, 202mm, and 100mm), the sliding gate is closed for 6s, 13s, and 21s, respectively. The covering agent composition is: CaO: 10%, SiO2: 36%, Al2O3: 9.6%, MgO: 11%, C: 27.3%, Na2O: 3.2%, K2O: 2.9% (basicity R=0.28). The protective slag composition is: SiO2: 32.5%, CaO: 25.8%, Al2O3: 7.5%, K2O: 3.8%, Na2O: 3.9%, F: 4.5%, C: 17.1%, MgO: 2.3%, Fe2O3: 2.6% (basicity R=0.79). Slag removal is performed when the intermediate slag layer is ≥50mm.

[0075] Compared with the conventional casting process (without adopting the three-stage closure of the sliding gate, without using the covering agent and protective slag of this invention, and without slag removal from the tundish), the non-metallic inclusion level of the continuous casting billet produced in this embodiment was reduced by 6.3% and the Al2O3 inclusion level was reduced by 17.8% in the low-magnification inspection.

[0076] Example 2

[0077] When the ladle weight decreased to 13.04t, 9.90t, and 5.15t (corresponding to liquid level heights of 278mm, 214mm, and 113mm), the sliding gate nozzle was closed for 10s, 10s, and 25s, respectively. The basicity of the covering agent was R=0.27, the basicity of the protective slag was R=0.75, and the other conditions were the same as in Example 1. Compared with the conventional casting process, the non-metallic inclusion level of the continuously cast billet produced in this example decreased by 0.35 grades in low-magnification inspection, and the metal yield increased by 0.79 kg / t steel.

[0078] Example 3

[0079] When the ladle weight decreased to 13.51t, 8.55t, and 4.23t (corresponding to liquid level heights of 288mm, 185mm, and 93mm), the sliding gate nozzle was closed for 8s, 15s, and 20s, respectively. The basicity of the covering agent was R=0.27, and the basicity of the protective slag was R=0.79; all other conditions were the same as in Example 1. Compared with the conventional casting process, the non-metallic inclusion level in the low-magnification inspection of the continuously cast billets produced in this example decreased by 0.43 levels, and the metal yield increased by 0.89 kg / t steel.

[0080] Comparative Example 1

[0081] The casting process was the same as in Example 1, except that the slag was not guided by a tundish slag removal device. The slag overflowed directly from the slag discharge port and fell freely to the ground. After cooling, it was manually cleaned, with a slag removal frequency of 6-8 hours per cycle. All other conditions were exactly the same as in Example 1. The results showed that without the slag removal device, the average thickness of the slag layer on the molten steel surface in the tundish increased by 20 mm, and the level of non-metallic inclusions in the low-magnification inspection of the continuously cast billet increased by 0.16 levels compared to Example 1. This indicates that the tundish slag removal device of the present invention has a significant effect on controlling the slag layer thickness and reducing the inclusion content.

[0082] The data from the examples show that, after adopting the method of the present invention, the level of metal inclusions in continuously cast billets is reduced by more than 6.3% year-on-year, Al2O3 inclusions are reduced by 17.8%, and the metal yield is increased by 0.89 kg / t steel. The comparative examples further verify that the slag removal device can reduce the slag layer thickness by 20 mm and reduce the inclusion level by 0.16 grades.

[0083] In summary, this invention firstly, by closing the sliding nozzle in three stages according to the different heights the molten steel level drops during the later stages of ladle casting, effectively disrupts the formation of surface vortices, thus preventing slag entrapment and refractory material corrosion products from being carried into the tundish from the source. Secondly, by adding an Al2O3-CaO-based low-alkalinity covering agent to the tundish surface and an Al2O3-CaO-based high-alkalinity protective slag to the crystallizer surface, the invention utilizes the principle that CaO reacts with the difficult-to-remove Al2O3 in the molten steel at high temperatures to generate Ca(AlO2)2, which then floats upwards, thereby synergistically adsorbing and removing inclusions in both the tundish and crystallizer stages. Thirdly, by cooperating with the tundish slag discharge device to actively discharge slag when the slag layer thickness is ≥50mm, the invention effectively controls the slag layer thickness and ensures the stability of the physicochemical properties of the covering agent and protective slag under multi-furnace continuous casting conditions.

[0084] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for controlling inclusions in continuous casting steelmaking, characterized in that, Includes the following steps: S1. Obtain the relationship between the height of the molten steel level in the ladle and the weight of the molten steel; S2. A weighing detection unit is set at the ladle receiving position to detect the ladle weight in real time and convert it into a molten steel level height signal. S3. During the continuous casting process, when the molten steel level drops to the first preset level range, the sliding gate of the ladle is closed for a first preset time, and then the sliding gate is opened to continue casting. S4. When the molten steel level continues to drop to the second preset level range, control the sliding gate of the ladle to close for a second preset time, and then open the sliding gate to continue pouring. S5. When the molten steel level continues to drop to the third preset level range, control the ladle sliding gate to close for a third preset time. S6. After the molten steel flows from the ladle into the tundish, a covering agent is added to the surface of the molten steel in the tundish. S7. When the thickness of the slag layer in the tundish reaches the preset thickness threshold, start the slag discharge operation to control the thickness of the slag layer in the tundish. S8. After the molten steel flows from the tundish into the crystallizer, add protective slag to the surface of the molten steel in the crystallizer. S9. Continue pouring until the pouring process is complete.

2. The method for controlling inclusions in continuous casting steelmaking according to claim 1, characterized in that, The first preset liquid level range is 280mm~300mm, and the first preset time is 5s~10s; the second preset liquid level range is 185mm~215mm, and the second preset time is 10s~15s; the third preset liquid level range is 90mm~110mm, and the third preset time is 20s~25s.

3. The method for controlling inclusions in continuous casting steelmaking according to claim 1, characterized in that, Step S1, which involves obtaining the correspondence between the molten steel level and the weight of the molten steel in the ladle, specifically includes: Measure the inner diameter of each part of the newly constructed steel ladle, calculate the weight of molten steel when the molten steel level is 90mm, 110mm, 185mm, 215mm, 280mm and 300mm respectively, and establish a molten steel level-weight comparison table.

4. The method for controlling inclusions in continuous casting steelmaking according to claim 1, characterized in that, The weighing detection unit in step S2 includes: wireless weighing sensors installed at two receiving positions of the butterfly rotary table, with four wireless weighing sensors installed at each receiving position. The weighing instrument signal of each sensor is fed back to the system PLC controller, which determines the current molten steel level by matching the corresponding relationship based on the real-time weight signal.

5. The method for controlling inclusions in continuous casting steelmaking according to claim 1, characterized in that, The slag discharge operation in step S7 includes providing a tundish slag discharge device, which includes a slag inlet trough located below the tundish slag discharge port and a slag pan located below the end of the slag inlet trough. During slag discharge, open the sealing material of the tundish slag discharge port to allow the liquid slag on the tundish surface to flow into the slag inlet through the slag discharge port, and then into the slag pan through the slag inlet. After the slag discharge is completed, the slag discharge port is resealed, and the slag inlet is cooled and cleaned.

6. The method for controlling inclusions in continuous casting steelmaking according to claim 1, characterized in that, The preset thickness threshold in step S7 is 50 mm.

7. The method for controlling inclusions in continuous casting steelmaking according to claim 1, characterized in that, The covering agent in step S6 is an Al2O3-CaO-based covering agent, and the protective slag is an Al2O3-CaO-based high-alkalinity protective slag.

8. The method for controlling inclusions in continuous casting steelmaking according to claim 7, characterized in that, For the production of low-carbon small square billets, the covering agent comprises, by mass percentage: CaO: 9%~10%, SiO2: 36%~40%, Al2O3: 9%~10%, MgO: 10%~13%, C: 26%~30%, Na2O: 3%~4%, K2O: 2.5%~3.5%; the basicity of the covering agent is 0.23~0.28 (i = CaO / SiO2). For the production of low-carbon small square billets, the protective slag comprises, by mass percentage: SiO2: 32.5%~34%, CaO: 24.5%~25.8%, Al2O3: 7.2%~7.9%, K2O: 3.5%~4.5%, Na2O: 3.5%~5.5%, F: 4%~5%, C: 15.5%~18%, MgO≤5%, Fe2O3≤5%; the basicity of the protective slag, α=CaO / SiO2, is 0.72~0.

80.

9. The method for controlling inclusions in continuous casting steelmaking according to claim 1, characterized in that, The opening and closing of the sliding gate is achieved by a hydraulic cylinder controlling a lever to drive the sliding slide plate, and the PLC controller automatically issues execution commands based on the real-time liquid level signal.