A low pressure casting method of a high thermal conductivity aluminum alloy material
By combining composition optimization with low-pressure casting technology, the problems of insufficient density and thermal conductivity of aluminum alloy castings have been solved, resulting in aluminum alloy castings with high thermal conductivity and high density, suitable for heat dissipation devices with complex structures.
Patent Information
- Application Number
- CN202610937062.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-26
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies make it difficult to produce complex aluminum alloy heat dissipation devices with high density, high purity, and high thermal conductivity through low-pressure casting processes. There are internal defects in the castings, such as shrinkage cavities and porosity, which make it difficult to meet the heat dissipation requirements of high heat flux density chips.
Using high thermal conductivity aluminum alloy material with optimized composition, combined with low-pressure casting process, including refining, mold preheating, filling and pressure holding control, followed by T5 heat treatment, to ensure high density and excellent thermal conductivity of the casting.
We obtained high-density, low-defect aluminum alloy castings with significantly improved thermal conductivity, meeting the needs of complex heat dissipation devices, and enhanced tensile strength, fully meeting product requirements.
Smart Images

Figure CN123128475A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of metal material processing and casting technology, and in particular relates to a low-pressure casting method for high thermal conductivity aluminum alloy materials. Background Technology
[0002] With the development of 5G communication, high-performance computing (HPC), and power electronic devices, the requirements for heat dissipation systems are becoming increasingly stringent. Aluminum alloys, due to their low density, relatively low cost, and good machinability, are the preferred material for manufacturing heat sinks, cold plates, and other devices. While commonly used die-cast aluminum alloys (such as ADC12) have good casting properties, their high content of impurities such as Fe and Zn results in generally low thermal conductivity (typically below 100 W / (m•K)), making it difficult to meet the heat dissipation requirements of next-generation high heat flux density chips.
[0003] High-purity wrought aluminum alloys (such as 1060 and 6063) have high thermal conductivity (above 200 W / (m•K), but their casting fluidity is poor, making it difficult to form complex structures through traditional casting processes. They usually require subsequent processing such as extrusion, which is costly and restricts design freedom.
[0004] Existing technologies include investment casting and gravity casting to produce high thermal conductivity aluminum alloy parts. However, these methods generally suffer from low casting density and internal shrinkage cavities, which severely scatter phonons and reduce the material's effective thermal conductivity. Low-pressure casting can provide stable filling and higher feeding pressure, but for composition-sensitive high thermal conductivity aluminum alloys, designing matching low-pressure casting process parameters (such as filling pressure, holding pressure, and mold temperature) to simultaneously ensure high purity, high density, and excellent thermal conductivity remains a pressing issue. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a low-pressure casting method for high thermal conductivity aluminum alloy materials specifically used for producing heat dissipation devices with complex structures. This method combines composition optimization with low-pressure casting process to obtain castings with high density, low defects, and thermal conductivity significantly better than traditional cast aluminum alloys.
[0006] This application provides a low-pressure casting method for high thermal conductivity aluminum alloy materials, the method comprising: Raw materials are blended and smelted according to the following mass percentages: Si: 0.8~1.2%, Mg: 0.6~0.9%, Fe: ≤0.20%, Cu: ≤0.05%, Zn: ≤0.05%, Mn: ≤0.03%, Ti: 0.08~0.15%, B: 0.005~0.015%, with the remainder being Al and impurities; The molten aluminum is refined and degassed. The treated molten aluminum is transferred to a low-pressure casting machine. After the mold is preheated to 220~280℃, gas is introduced to complete the filling at a pressure of 0.015~0.025 MPa. Then the pressure is increased to 0.4~0.6 MPa and held for 50~90 seconds. The castings are subjected to T5 treatment: solution treatment at 520±5℃ for 4~6 hours, water quenching, followed by aging treatment at 175±5℃ for 8~10 hours. Preferably, the refining and degassing treatment of the molten aluminum includes: Melt at 730℃, add 0.5% refining agent for refining and degassing, let stand for 15 minutes and then remove the slag.
[0007] Preferably, the refining agent consists of 50% hexachloroethane and 50% Na2SiF6.
[0008] Preferably, the amount of refining agent added is 0.3% to 0.6% of the weight of the molten aluminum.
[0009] Preferably, the method further includes: The gas introduced during the filling stage is high-purity nitrogen or an inert gas.
[0010] Preferably, the holding pressure is 0.5 MPa and the holding time is 70 seconds.
[0011] Preferably, the surface of the mold cavity is coated with a boron nitride-based coating.
[0012] Preferably, the solution treatment lasts for 5 hours and the aging treatment lasts for 9 hours.
[0013] The beneficial technical effects of this application are as follows: This application provides a low-pressure casting method for producing high thermal conductivity aluminum alloy materials specifically for manufacturing complex structure heat dissipation devices. This method combines composition optimization with low-pressure casting process to obtain castings with high density, low defects, and thermal conductivity significantly better than traditional cast aluminum alloys. Attached Figure Description
[0014] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. The drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0015] Figure 1 This is a flowchart of a low-pressure casting method for a high thermal conductivity aluminum alloy material provided in an embodiment of this application. Detailed Implementation
[0016] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0017] The features and illustrative embodiments of various aspects of the present invention will now be described in detail. Numerous specific details are set forth in the following detailed description to provide a thorough understanding of the invention. However, it will be apparent to those skilled in the art that the invention may be practiced without requiring some of these specific details. The following description of embodiments is merely intended to provide a better understanding of the invention by illustrating examples of the invention. The invention is by no means limited to any specific setups and methods set forth below, but covers any improvements, substitutions, and modifications to structures, methods, and devices without departing from the spirit of the invention. Well-known structures and techniques are not shown in the drawings and the following description to avoid unnecessarily obscuring the invention.
[0018] In the description of this invention, it should be noted that the directions or positional relationships indicated by terms such as "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer" are based on the directions or positional relationships shown in the accompanying drawings and are only for the convenience of describing and simplifying the invention, and should not be construed as limiting the invention. Furthermore, the use of ordinal numbers (e.g., "first and second," etc.) is for distinguishing objects and is not limited to this order, and should not be construed as indicating or implying relative importance.
[0019] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly, encompassing both direct connection and indirect connection via an intermediate medium. Those skilled in the art can understand the specific meaning of these terms in this invention based on the specific circumstances.
[0020] It should be noted that, unless otherwise specified, the embodiments of the present invention and the features thereof can be combined with each other, and the various embodiments can be referenced and cited in each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.
[0021] The following is a description of the embodiments and appendices. Figure 1 The present invention will be described in further detail, but the embodiments of the present invention are not limited thereto.
[0022] This application provides a low-pressure casting method for high thermal conductivity aluminum alloy materials, comprising the following steps: Alloy smelting and composition control: Raw materials are proportioned and smelted according to mass percentage: Si: 0.8~1.2%, Mg: 0.6~0.9%, Fe: ≤0.20%, Cu: ≤0.05%, Zn: ≤0.05%, Mn: ≤0.03%, Ti: 0.08~0.15%, B: 0.005~0.015%, with the remainder being Al and unavoidable impurities; The molten aluminum is refined and degassed; in low-pressure casting, the treated molten aluminum is transferred to a low-pressure casting machine. After the mold is preheated to 220~280℃, gas is introduced to complete the filling at a pressure of 0.015~0.025 MPa. Then the pressure is increased to 0.4~0.6MPa and held for 50~90 seconds. The casting underwent T5 treatment: solution treatment at 525℃ for 5 hours, water quenching, followed by aging at 175℃ for 9 hours. Testing revealed no shrinkage cavities or porosity defects inside the casting, a density of 99.6%, a thermal conductivity of 195 W / (m·K), and a tensile strength of 235 MPa, fully meeting product requirements.
[0023] The refining process employs a composite refining agent of hexachloroethane and fluoride salts, added at a rate of 0.3% to 0.6% of the aluminum liquid weight. High-purity nitrogen or an inert gas is introduced during the filling stage. The mold cavity surface is coated with a boron nitride-based coating.
[0024] The holding pressure is 0.5 MPa, and the holding time is 70 seconds. The T5 heat treatment regime is as follows: solution treatment at 520±5℃ for 4~6 hours, water quenching, followed by aging treatment at 175±5℃ for 8~10 hours.
[0025] Meanwhile, this application also provides a high thermal conductivity aluminum alloy casting manufactured by the aforementioned method, which has a room temperature thermal conductivity of not less than 180 W / (m·K), a tensile strength of not less than 220 MPa, and a density of not less than 99.5%.
[0026] This application provides a low-pressure casting method for producing high thermal conductivity aluminum alloy materials specifically for manufacturing complex structure heat dissipation devices. This method combines composition optimization with low-pressure casting process to obtain castings with high density, low defects, and thermal conductivity significantly better than traditional cast aluminum alloys.
[0027] In other embodiments of this application, the technical solution for preparing an aluminum alloy casting for a heat dissipation housing of a 5G base station power amplifier is as follows: 1) Batching and Smelting: Weigh industrial pure aluminum, Al-20Si master alloy, pure magnesium ingots, and other raw materials according to their mass percentages, and prepare an alloy with Si: 1.0%, Mg: 0.8%, Fe: 0.15%, Cu: 0.03%, Zn: 0.03%, Mn: 0.02%, Ti: 0.10%, and B: 0.01%. Melt the alloy at 730℃, add 0.5% refining agent (composition: 50% hexachloroethane + 50% Na2SiF6) for refining and degassing, and remove slag after standing for 15 minutes.
[0028] 2) Low-pressure casting: Transfer the molten aluminum into a low-pressure casting machine. Preheat the mold to 250°C and spray it with boron nitride coating. Set the filling pressure to 0.02 MPa and the filling time to approximately 20 seconds. Then rapidly increase the pressure to 0.5 MPa and hold the pressure for 70 seconds.
[0029] 3) Heat treatment: The casting was subjected to T5 treatment: solution treatment at 525℃ for 5 hours, water quenching, followed by aging at 175℃ for 9 hours. Testing revealed that the casting had no shrinkage cavities or porosity defects, a density of 99.6%, a thermal conductivity of 195 W / (m·K), and a tensile strength of 235 MPa, fully meeting the product requirements.
[0030] 4) Final inspection: 100% inspection of casting dimensions and surface quality. For defects on machined surfaces, grinding or machining is permitted, but the casting must have a allowance of no less than one-third. The removal of defects should be smooth and rounded. 100% inspection of the markings on the casting.
[0031] In other embodiments of this application, a low-pressure casting method is provided for producing high thermal conductivity aluminum alloy materials specifically for manufacturing complex structure heat dissipation devices. This method combines optimized alloy composition design with precisely controlled low-pressure casting processes to obtain castings with high density, low defects, and significantly superior thermal conductivity compared to traditional cast aluminum alloys. The method includes the following steps: S1. Alloy Smelting and Composition Control: Raw materials are proportioned by mass percentage as follows: Si: 0.8~1.2%, Mg: 0.6~0.9%, Fe: ≤0.20%, Cu: ≤0.05%, Zn: ≤0.05%, Mn: ≤0.03%, Ti: 0.08~0.15%, B: 0.005~0.015%, with the remainder being Al and unavoidable impurities; The raw materials are melted into aluminum alloy liquid in a smelting furnace at 720~750℃, and then 0.3%~0.6% of refining agent by weight of aluminum liquid is added for rotary degassing refining. After refining, the mixture is allowed to stand and slag is removed. S2, Low-Pressure Casting: Transfer the molten aluminum treated in S1 into the insulated crucible of the low-pressure casting machine, seal it, and connect the gas filling pipe; a) Mold Preheating: Preheat the mold to 220~280℃ and spray boron nitride-based coating on the cavity surface; b) Filling Stage: Introduce dry compressed air or inert gas into the insulated crucible to allow the molten aluminum to rise steadily and fill the mold cavity under a low pressure of 0.015~0.025 MPa, with the filling time controlled at 15~25 seconds; c) Pressure Increasing and Holding Stage: After filling, quickly increase the pressure to 0.4~0.6 MPa and maintain this pressure for 50~90 seconds until the casting is completely solidified; d) Pressure Relief and Mold Opening: After holding the pressure, release the pressure, open the mold, and remove the casting.
[0032] S3. Heat treatment: The obtained castings are subjected to T5 heat treatment: solution treatment at 520±5℃ for 4~6 hours, water quenching, followed by aging treatment at 175±5℃ for 8~10 hours.
[0033] S4. Final Inspection: 100% inspection of casting dimensions and surface quality. For defects on machined surfaces, grinding or machining is permitted, but at least one-third of the casting must remain as allowance. The removal of defects should be smoothly transitioned. 100% inspection of casting markings. Optional markings include casting number, batch number, and sequence number. Machining is used to remove the gating and riser from the casting. Sandblasting is used to remove oxide scale from the casting surface, and flexible tools or tumbling are used to remove excess material from the inside of the casting piping. Fluorescent penetrant and X-ray inspection are used to detect the internal quality of the casting. The casting undergoes heat treatment. Chemical composition analysis of the casting is performed. Final inspection of the cast parts; The final inspection includes: 100% inspection of the chemical composition of castings; 100% inspection of the mechanical properties of castings; 100% inspection of the fluorescent penetrant and internal X-ray quality of the castings; 100% inspection of markings.
[0034] This invention relates to the field of metal material processing and casting technology, specifically to an aluminum alloy casting method, particularly a method that combines composition optimization with low-pressure casting process to mainly solve problems such as low density of castings and easy formation of shrinkage cavities and porosity defects inside.
[0035] The purpose of this invention is to provide an aluminum alloy casting method to obtain castings with high density, low defects, and significantly better thermal conductivity than traditionally cast aluminum alloys. The technical solution of this invention for preparing an aluminum alloy casting for a heat sink housing of a 5G base station power amplifier is as follows: 1) Batching and Smelting: Weigh industrial pure aluminum, Al-20Si master alloy, pure magnesium ingots, and other raw materials according to their mass percentages, and prepare an alloy with Si: 1.0%, Mg: 0.8%, Fe: 0.15%, Cu: 0.03%, Zn: 0.03%, Mn: 0.02%, Ti: 0.10%, and B: 0.01%. Melt the alloy at 730℃, add 0.5% refining agent (composition: 50% hexachloroethane + 50% Na2SiF6) for refining and degassing, and remove slag after standing for 15 minutes.
[0036] 2) Low-pressure casting: Transfer the molten aluminum into a low-pressure casting machine. Preheat the mold to 250°C and spray it with boron nitride coating. Set the filling pressure to 0.02 MPa and the filling time to approximately 20 seconds. Then rapidly increase the pressure to 0.5 MPa and hold the pressure for 70 seconds.
[0037] 3) Heat treatment: The casting was subjected to T5 treatment: solution treatment at 525℃ for 5 hours, water quenching, followed by aging at 175℃ for 9 hours. Testing revealed that the casting had no shrinkage cavities or porosity defects, a density of 99.6%, a thermal conductivity of 195 W / (m·K), and a tensile strength of 235 MPa, fully meeting the product requirements.
[0038] 4) Final inspection: 100% inspection of casting dimensions and surface quality. For defects on machined surfaces, grinding or machining is permitted, but the casting must have a allowance of no less than one-third. The removal of defects should be smooth and rounded. 100% inspection of the markings on the casting.
[0039] This application solves the quality problems of low density in castings and the tendency for shrinkage cavities and porosity to occur inside.
[0040] In other embodiments of this application, the technical solution for preparing an aluminum alloy casting for a heat dissipation housing of a 5G base station power amplifier is as follows: Batching and Smelting: Weigh industrial pure aluminum, Al-20Si master alloy, pure magnesium ingots, and other raw materials according to their mass percentages to prepare an alloy with the following composition: Si: 1.0%, Mg: 0.8%, Fe: 0.15%, Cu: 0.03%, Zn: 0.03%, Mn: 0.02%, Ti: 0.10%, and B: 0.01%. Melt the alloy at 730℃ until clean. Add 0.5% refining agent (composition: 50% hexachloroethane + 50% Na2SiF6) for refining and degassing. After standing for 15 minutes, remove the slag.
[0041] Low-pressure casting: The molten aluminum is transferred to a low-pressure casting machine. The mold is preheated to 250°C and coated with boron nitride. The filling pressure is set to 0.02 MPa, and the filling time is approximately 20 seconds. The pressure is then rapidly increased to 0.5 MPa and held for 70 seconds.
[0042] The casting underwent T5 treatment: solution treatment at 525℃ for 5 hours, water quenching, followed by aging at 175℃ for 9 hours. Testing revealed no shrinkage cavities or porosity defects inside the casting, a density of 99.6%, a thermal conductivity of 195 W / (m·K), and a tensile strength of 235 MPa, fully meeting product requirements.
[0043] The above detailed embodiments are a description of the present invention. It should not be considered that the specific embodiments of the present invention are limited to these descriptions. For those skilled in the art, several simple deductions and substitutions can be made without departing from the concept of the present invention, and all of these should be considered to fall within the protection scope of the present invention.
Claims
1. A low-pressure casting method for a high thermal conductivity aluminum alloy material, characterized in that, The method includes: Raw materials are blended and smelted according to the following mass percentages: Si: 0.8~1.2%, Mg: 0.6~0.9%, Fe: ≤0.20%, Cu: ≤0.05%, Zn: ≤0.05%, Mn: ≤0.03%, Ti: 0.08~0.15%, B: 0.005~0.015%, with the remainder being Al and impurities; The molten aluminum is refined and degassed. The treated molten aluminum is transferred to a low-pressure casting machine. After the mold is preheated to 220~280℃, gas is introduced to complete the filling at a pressure of 0.015~0.025MPa. Then the pressure is increased to 0.4~0.6 MPa and held for 50~90 seconds. The castings are subjected to T5 treatment: solution treatment at 520±5℃ for 4~6 hours, water quenching, followed by aging treatment at 175±5℃ for 8~10 hours.
2. The method according to claim 1, characterized in that, The refining and degassing treatment of the molten aluminum includes: Melt at 730℃, add 0.5% refining agent for refining and degassing, let stand for 15 minutes and then remove the slag.
3. The method according to claim 2, characterized in that, The refining agent consists of 50% hexachloroethane and 50% Na2SiF6.
4. The method according to claim 3, characterized in that, The amount of refining agent added is 0.3% to 0.6% of the weight of the molten aluminum.
5. The method according to claim 1, characterized in that, The method further includes: The gas introduced during the filling stage is high-purity nitrogen or an inert gas.
6. The method according to claim 1, characterized in that, The holding pressure is 0.5 MPa, and the holding time is 70 seconds.
7. The method according to claim 1, characterized in that, The surface of the mold cavity is coated with boron nitride-based paint.
8. The method according to claim 1, characterized in that, Solution treatment for 5 hours, aging treatment for 9 hours.