Copper powder and method for manufacturing the same

By coating the surface of copper particles with fatty acid salts and controlling the peak temperature relationship, the problem of hygroscopicity of copper formate on the surface of copper particles was solved, the oxidation resistance and low-temperature sintering properties of copper powder were improved, and the electrical conductivity was ensured to be stable.

CN123128489APending Publication Date: 2026-11-20DOWA ELECTRONICS MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611418814.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2026-07-16
Filing Date
2026-09-14
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In the prior art, the pre-applied copper formate on the surface of copper particles leads to hygroscopic problems, resulting in reduced conductivity and accelerated oxidation. Furthermore, there is room for improvement in the oxidation resistance and low-temperature sintering properties of the coated copper particles.

Method used

By coating the surface of copper particles with fatty acid salts, the peak temperature relationship in thermogravimetric-mass spectrometry analysis can be controlled, making it easier for copper powder to form copper formate during formic acid treatment, thereby improving oxidation resistance and low-temperature sintering properties.

Benefits of technology

This achieves high oxidation resistance and low-temperature sintering properties for copper powder, avoids adverse effects caused by copper formate absorbing water, and ensures stable conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128489A_ABST
    Figure CN123128489A_ABST
Patent Text Reader

Abstract

The present invention provides a copper powder and a method for producing the same. [Problem to be solved by the invention] To provide a copper powder which is high in oxidation resistance and easily produces copper formate by formic acid treatment. [Means for solving the problem] To provide a copper powder which is a collection of a plurality of coated copper particles each containing a copper particle and a fatty acid and a salt thereof provided on the surface of the copper particle, the average particle diameter of the copper powder being 0.1 μm or more and 1.0 μm or less, and in a thermogravimetric-mass spectrometric analysis, the peak temperature T1 of a peak derived from carbon dioxide is lower than the peak temperature T2 of a peak derived from a hydrocarbon portion of the fatty acid and the salt thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to copper powder and its manufacturing method. Background Technology

[0002] Copper paste containing copper particles is used as a conductor, for example, in wiring, by sintering. The surface of the copper particles is sometimes coated with an organic surface treatment agent to achieve properties such as low-temperature sintering and oxidation resistance.

[0003] For example, Patent Document 1 describes copper composite particles comprising copper particles and at least a portion of copper formate adhering to the surface of the copper particles. When a copper paste containing such copper composite particles is calcined, the copper formate thermally decomposes to generate copper nanoparticles. This thermal decomposition increases the specific surface area of ​​the copper composite particles and lowers the sintering temperature, thus indicating that such copper composite particles exhibit excellent low-temperature sintering properties.

[0004] Furthermore, Patent Document 2 describes coated copper particles coated with specific aliphatic carboxylic acids and possessing specific particle size and particle size distribution. It is believed that such coated copper particles can achieve low-temperature sintering and oxidation resistance.

[0005] Existing technical documents

[0006] Patent documents

[0007] Patent Document 1: Japanese Patent Application Publication No. 2015-30869

[0008] Patent Document 2: Japanese Patent Application Publication No. 2016-176146 Summary of the Invention

[0009] The problem that the invention aims to solve

[0010] As described above, Patent Document 1 describes the application of copper formate on the surface of copper particles in order to achieve low-temperature sintering properties.

[0011] However, the inventors have discovered that when copper formate is pre-applied to the surface of copper particles, the copper formate is hygroscopic, thus requiring careful storage and handling. When the copper formate absorbs moisture, water separation / evaporation during sintering can become a major obstacle to the formation of a dense conductive film. Furthermore, the absorbed moisture accelerates the oxidation of the copper particles, resulting in a significant reduction in conductivity. To address this issue, for example, by treating the copper particles with formic acid just before sintering, the aforementioned adverse effects of water absorption can be avoided.

[0012] On the other hand, Patent Document 2 describes coated copper particles that combine oxidation resistance and sinterability by coating with specific aliphatic carboxylic acids. However, although such coated copper particles have excellent oxidation resistance, their sinterability still has room for improvement compared to the sintering-promoting effect of utilizing the thermal decomposition mechanism of copper formate as described in Patent Document 1.

[0013] Therefore, the object of the present invention is to provide a copper powder that maintains oxidation resistance by coating the surface of copper particles with fatty acid salts and readily produces copper formate by formic acid treatment that brings formic acid into contact with the surface of copper particles.

[0014] If the copper powder is easily treated with formic acid to produce copper formate, then the surface of the copper powder obtained after formic acid treatment will have a large amount of copper formate. Therefore, it is expected to have excellent low-temperature sintering properties and is less likely to cause problems caused by the absorption of moisture by copper formate.

[0015] Solution for solving the problem

[0016] To address the aforementioned issues, the inventors conducted in-depth research. As a result, they discovered that by coating the surface of copper particles with fatty acid salts, copper powder with high oxidation resistance and which readily produces copper formate upon formic acid treatment can be obtained.

[0017] The invention based on the above insights is described below.

[0018] The first method is a copper powder, which is an aggregate of multiple coated copper particles, each comprising copper particles and fatty acids and their salts disposed on the surface of the copper particles.

[0019] The average particle size of the aforementioned copper powder is greater than 0.1 μm and less than 1.0 μm.

[0020] In thermogravimetric-mass spectrometry (TGA), the peak temperature T1 of the peak originating from carbon dioxide is lower than the peak temperature T2 of the peak originating from the hydrocarbon fraction of the aforementioned fatty acids and their salts.

[0021] The second method uses the copper powder described in the first method, wherein...

[0022] The carbon content of the copper powder is 0.1% by mass or more and 1.5% by mass or less relative to the mass of the copper powder.

[0023] The third method uses the copper powder described in the first or second method, wherein...

[0024] In thermogravimetric-mass spectrometry analysis, the proportion of the peak area C in the sum of the peak area C of the peak originating from the carbon dioxide and the peak area R of the peak originating from the hydrocarbon fraction is greater than 0.10 and less than 0.70.

[0025] The fourth method uses the copper powder described in any of the methods 1 to 3, wherein...

[0026] The peak temperature T2 mentioned above is below 400℃.

[0027] The fifth method uses the copper powder described in any one of methods 1 to 4, wherein...

[0028] The fatty acids and their salts mentioned above are straight-chain saturated fatty acids and their salts with 11 or more but less than 13 carbon atoms.

[0029] The sixth method uses the copper powder described in the fifth method, wherein...

[0030] The above-mentioned straight-chain saturated fatty acids with 11 or more but less than 13 carbon atoms and their salts are lauric acid and laurate.

[0031] The seventh method uses copper powder as described in any one of methods 1 to 6, wherein...

[0032] The aforementioned coated copper particles further contain at least one metal selected from nickel and iron on their surface.

[0033] The mass ratio of the aforementioned metal to the mass of the aforementioned copper particles is more than 10 ppm and less than 2000 ppm.

[0034] Method 8 is a method for manufacturing copper powder, which includes:

[0035] In the complex formation process, copper sulfate, ammonia, and water are mixed to obtain an aqueous solution of copper-ammonia complex containing copper-ammonia complex;

[0036] In a single reduction step, a first reducing agent is added to the aqueous solution of the copper-ammonia complex.

[0037] The dispersant addition step involves adding a dispersant to the above-mentioned copper-ammonia complex aqueous solution before or after the above-mentioned primary reduction step.

[0038] A secondary reduction process involves adding a second reducing agent to the aqueous solution obtained after the primary reduction process and the dispersant addition process, to obtain an aqueous solution containing copper particles; and

[0039] In the fatty acid salt addition step, the aqueous solution containing the copper particles is mixed with a salt of fatty acids to obtain an aqueous solution containing coated copper particles, wherein the coated copper particles comprise the copper particles and the fatty acids and their salts disposed on the surface of the copper particles.

[0040] The pH of the aqueous solution containing the copper-coated particles obtained after the above-mentioned fatty acid salt addition process is 8.0 or higher and 11.0 or lower.

[0041] The ninth method is the copper powder manufacturing method described in the eighth method, wherein...

[0042] After the above-mentioned secondary reduction step and before the above-mentioned fatty acid salt addition step, the method further includes: a metal ion addition step, in which at least one metal ion, either nickel or iron, is added to the above-mentioned aqueous solution containing the above-mentioned copper particles.

[0043] The tenth method is the copper powder manufacturing method described in the eighth or ninth method, wherein...

[0044] Following the aforementioned fatty acid salt addition step, the process further includes a copper powder recovery step, in which copper powder, which is an aggregate of the aforementioned coated copper particles, is recovered from the aforementioned aqueous solution containing the aforementioned coated copper particles.

[0045] The 11th method is a method for manufacturing copper powder according to any one of methods 8 to 10, wherein,

[0046] The first reducing agent and the second reducing agent mentioned above are hydrazine.

[0047] The 12th method is a method for manufacturing copper powder according to any one of methods 8 to 11, wherein,

[0048] The dispersant mentioned above is sodium pyrophosphate.

[0049] Method 13 is a method for manufacturing copper powder according to any one of methods 8 to 12, wherein,

[0050] The above-mentioned fatty acid salts are salts of straight-chain saturated fatty acids with 11 or more but less than 13 carbon atoms.

[0051] The 14th method is the copper powder manufacturing method described in the 13th method, wherein...

[0052] The salts of the above-mentioned straight-chain saturated fatty acids with 11 or more but less than 13 carbon atoms are laurates.

[0053] The 15th method is the copper powder manufacturing method described in the 14th method, wherein...

[0054] The aforementioned laurate is sodium laurate.

[0055] Method 16 is a method for manufacturing copper powder according to any one of methods 8 to 15, wherein,

[0056] The average particle size of the copper powder is above 0.1 μm and below 1.0 μm.

[0057] Invention Effects

[0058] According to the present invention, a copper powder is provided that, by using a fatty acid salt to coat the surface of copper particles, exhibits higher oxidation resistance compared to copper powder pre-coated with copper formate, and readily produces copper formate during formic acid treatment. Attached Figure Description

[0059] Figure 1 The image is obtained by taking a picture of copper powder according to an embodiment of the present invention using a scanning electron microscope.

[0060] Figure 2 The image is obtained by taking a picture of copper powder according to an embodiment of the present invention using a scanning electron microscope.

[0061] Figure 3 The image is obtained by taking a picture of copper powder according to an embodiment of the present invention using a scanning electron microscope.

[0062] Figure 4 This is a flowchart illustrating an example of a method for manufacturing copper powder according to an embodiment of the present invention.

[0063] Figure 5 This is a graph showing the TG-MS results of the copper powder in Example 1.

[0064] Figure 6 This is a graph showing the TG-MS results of the copper powder in Example 2.

[0065] Figure 7 This is a graph showing the TG-MS results of the copper powder in Example 3.

[0066] Figure 8 This is a graph showing the TG-MS results of the copper powder in Example 4.

[0067] Figure 9 This is a graph showing the TG-MS results of the copper powder in Example 5.

[0068] Figure 10 This is a graph showing the TG-MS results of the copper powder in Example 6.

[0069] Figure 11 This is a graph showing the TG-MS results of the copper powder in Comparative Example 1.

[0070] Figure 12 This is a graph showing the TG-MS results of the copper powder in Comparative Example 2.

[0071] Figure 13 This is a graph showing the TG-MS results of the copper powder in Comparative Example 3.

[0072] Figure 14This is a graph showing the TG-MS results of the copper powder in Comparative Example 4.

[0073] Figure 15 This is a graph showing the thermogravimetric behavior of copper powders in Example 1 and Comparative Example 5.

[0074] Figure 16 This is a graph showing the thermal shrinkage behavior of copper powder treated with formic acid in Example 4 and Comparative Example 3. Detailed Implementation

[0075] The embodiments of the present invention will be described below. The content described in one embodiment can be incorporated into other embodiments.

[0076] (1) Copper powder

[0077] Hereinafter, a copper powder according to one embodiment of the present invention will be described. Figure 1 , Figure 2 and Figure 3 The image is obtained by taking a picture of copper powder using a scanning electron microscope (SEM). Figure 1 , Figure 2 and Figure 3 The multipliers are 10,000, 20,000 and 50,000 respectively.

[0078] In one embodiment of the present invention, the copper powder is an aggregate of multiple coated copper particles, each comprising copper particles and fatty acids and their salts disposed on the surface of the copper particles.

[0079] Copper particles are particles substantially formed of copper. In addition to copper, copper particles may further contain carbon and oxygen. The mass ratio of carbon to the mass of copper particles is, for example, 0.1% by mass or less. The mass ratio of oxygen to the mass of copper particles is, for example, 1.5% by mass or less. The average particle size of the copper particles is, for example, the same as the average particle size of the copper powder described later. The particle size of the copper particles is obtained by the same method as the method for determining the particle size of the copper powder described later.

[0080] In this invention, fatty acids and their salts include aliphatic carboxylic acids having a carboxyl group and compounds whose carboxyl groups form salts. Preferably, these are straight-chain saturated fatty acids (hereinafter also referred to as straight-chain saturated fatty acids) and their salts having 11 or more and 13 carbon atoms. Specifically, these are undecanoic acid (C11), lauric acid (C12), or tridecanoic acid (C13) and their salts. More preferably, they are lauric acid and laurates. In this case, copper formate is particularly readily produced by treatment with formic acid.

[0081] As described below, this invention obtains coated copper particles containing fatty acids and fatty acid salts disposed on the surface of copper particles by mixing fatty acid salts in a fatty acid salt addition process. In obtaining coated copper particles using fatty acid salts in this way, fatty acids, fatty acid salts, or forms in which they interact with the metal surface can be formed on the surface of the copper particles. This is due to protonation / deprotonation of carboxyl groups, coordination with metal ions, etc. In this invention, all these arbitrary forms are included and referred to as "coated copper particles containing fatty acids and fatty acid salts".

[0082] Furthermore, the coated copper particles may further contain at least one metal selected from nickel and iron on the surface of the copper particles. In this case, it is easy to increase the mass ratio of fatty acids and fatty acid salts to the mass of copper particles, thus obtaining copper powder with excellent oxidation resistance. The mass ratio of at least one metal selected from nickel and iron to the mass of copper particles is preferably 10 ppm or more and 2000 ppm or less. For example, the coated copper particles may further contain only one metal selected from nickel and iron on the surface of the copper particles.

[0083] The average particle size of the copper powder is greater than 0.1 μm and less than 1.0 μm.

[0084] The average particle size of the copper powder was obtained using the following method. First, the copper powder was imaged using a scanning electron microscope (SEM). The magnification was set to 20,000x and the accelerating voltage to 10kV. Next, the maximum diameter of each of the 200 fully identifiable coated copper particles in the image was determined. This maximum diameter was taken as the particle size of the copper powder. Then, the average of the obtained particle sizes was taken as the average particle size of the copper powder.

[0085] The carbon content in the copper powder is preferably 0.1% by mass or more and 1.5% by mass or less. Under these conditions, copper powder with excellent oxidation resistance can be obtained.

[0086] In this invention, the ratio of carbon content (mass%) in the copper powder to the average particle size (μm) of the copper powder is preferably 0.5 or more and 6.0 or less, more preferably 0.6 or more and 5.0 or less.

[0087] Thermogravimetric-mass spectrometry (TG-MS) is an analytical method that combines thermogravimetric analysis and mass spectrometry. In thermogravimetric analysis, the weight change (TG) produced by heating the sample is measured. In mass spectrometry, the gaseous components generated by heating the sample are ionized, and the ionized gaseous components are separated and detected according to their mass-to-charge ratio (m / z). TG-MS allows for mass spectrometric analysis of the gaseous components generated by heating, thus enabling continuous capture of changes in the types and amounts of gases produced during heating.

[0088] When copper powder is heated in TG-MS, the carboxyl groups (COO portion) of fatty acids and fatty acid salts present on the powder surface decompose to produce carbon dioxide gas. Additionally, heating also produces gases originating from the portions of fatty acids and fatty acid salts other than the COO portion (i.e., the hydrocarbon portions of fatty acids and fatty acid salts). These gases have different m / z values; in TG-MS analysis, the change in ionic intensity relative to temperature is obtained for each m / z as the intensity distribution.

[0089] Therefore, when copper powder is analyzed by TG-MS, multiple m / z intensity distributions originating from the COO and hydrocarbon fractions are obtained. In this invention, the thermal decomposition of the COO fraction is mainly detected as m / z 44, and therefore m / z 44 is used as the index peak originating from the COO fraction. On the other hand, multiple organic fragment ions are generated by the thermal decomposition of the hydrocarbon fraction, but in this invention, the m / z of the peaks originating from the hydrocarbon fraction that exhibit the highest intensity is used as the index of the hydrocarbon fraction. In this specification, "fragment ion" refers to an ion of a molecular fragment generated when a portion of the original molecule dissociates during the ionization of the generated gas. In mass spectrometry analysis, the mass-to-charge ratio (m / z) of these fragment ions is detected, and a spectrum is obtained in the form of ion intensity at each m / z. For example, in the case where the fatty acid and fatty acid salt are lauric acid and laurate, the peak exhibiting the highest intensity among the fragments originating from the hydrocarbon fraction is m / z 73.

[0090] The peak temperature T1 of the peaks in the spectrum originating from the COO portion (hereinafter also referred to as peaks originating from carbon dioxide) is lower than the peak temperature T2 of the peaks in the spectrum originating from the hydrocarbon portion (hereinafter also referred to as peaks originating from the hydrocarbon portion of fatty acids and fatty acid salts). When the peak temperature T1 is lower than the peak temperature T2, copper powder that readily forms copper formate can be obtained.

[0091] Here, when the spectrum originating from the COO portion has two or more peaks, the peak temperature of the peak with the greatest intensity among the two or more peaks is taken as peak temperature T1. Similarly, when the spectrum originating from the hydrocarbon portion has two or more peaks, the peak temperature of the peak with the greatest intensity among the two or more peaks is taken as peak temperature T2.

[0092] The peak temperature T1 is, for example, 200°C or higher and 260°C or lower. The peak temperature T2 is preferably 400°C or lower. In this case, copper powder that readily produces copper formate can be obtained. The peak temperature T2 can be 220°C or higher and 310°C or lower. The difference between the peak temperature T1 and the peak temperature T2 is, for example, 20°C or higher and 50°C or lower.

[0093] The ratio of peak area C (C) to peak area R (R) of the peak originating from carbon dioxide is preferably 0.10 or more and 0.70 or less. In this case, copper powder that readily produces copper formate can be obtained.

[0094] (Effect)

[0095] As described above, the copper powder of the present invention is coated with fatty acids and fatty acid salts, the average particle size of the copper powder is within the aforementioned range, and the peak temperature T1 is lower than the peak temperature T2. It is believed that in such copper powder, the balance between the physical and chemical adsorption of copper particles by fatty acids and fatty acid salts is good. Therefore, the copper powder of the present invention has high oxidation resistance and readily forms copper formate through formic acid treatment. Consequently, the copper powder obtained by this formic acid treatment (hereinafter referred to as formic acid-treated copper powder) exhibits excellent low-temperature sintering properties. Here, low-temperature sintering properties refer to sintering at temperatures, for example, below 300°C, below 250°C, or below 200°C.

[0096] Furthermore, the copper powder of the present invention does not contain copper formate before formic acid treatment, thus reducing the likelihood of water absorption associated with copper formate and improving oxidation resistance. Additionally, for example, by performing formic acid treatment just before sintering, the copper powder treated with formic acid is less likely to absorb water as described above.

[0097] Formic acid treatment, for example, involves treating copper powder with formic acid or a solution containing formic acid. It is believed that when copper powder is treated with formic acid, the fatty acids of the coated copper particles are removed by the treatment over several minutes. Furthermore, whether copper formate is formed by formic acid treatment can be confirmed, for example, using a C / S ratio meter, X-ray diffraction (XRD), or TG-MS, as described later.

[0098] (2) Method for manufacturing copper powder

[0099] The following is for reference Figure 4 An example of a method for manufacturing copper powder according to one embodiment of the present invention will be described. Figure 4 This is a flowchart illustrating an example of a method for manufacturing copper powder according to an embodiment of the present invention.

[0100] like Figure 4 As shown, the copper powder manufacturing method of this embodiment includes a complex formation step S1, a primary reduction step S2, a dispersant addition step S3, a secondary reduction step S4, a metal ion addition step S5, a fatty acid salt addition step S6, a pH adjustment step S7, and a copper powder recovery step S8. These steps will be described below.

[0101] (Complex formation process S1)

[0102] First, copper sulfate, ammonia, and water are mixed to obtain an aqueous solution of a copper-ammonia complex. In this step, the copper-ammonia complex is a divalent copper-ammonia complex. The copper sulfate can be mixed in the form of anhydrous copper sulfate or in the form of copper sulfate pentahydrate. Preferably, copper sulfate free of impurities such as nickel and iron is used.

[0103] The molar ratio of ammonia to copper is, for example, more than 3 and less than 5.

[0104] Mixing is preferably carried out under heating, with the aqueous solution temperature preferably between 70°C and 90°C. If the solution temperature is below 70°C, copper sulfate will precipitate, making it difficult to form a copper-ammonia complex, which is therefore not preferred. Furthermore, temperatures above 90°C are not preferred in terms of operability. It should be noted that mixing can also be carried out while blowing in gases such as nitrogen.

[0105] (S2, a single reduction process)

[0106] Next, a first reducing agent is added to the aqueous solution of the copper-ammonia complex. If the first reducing agent is added, the copper-ammonia complex becomes a monovalent copper-ammonia complex.

[0107] The preferred reducing agent is hydrazine. Hydrazine has excellent reducing properties for copper. The method of addition is not particularly limited; for example, the first reducing agent can be added continuously over a period of time. The first reducing agent is added, for example, in an amount of 0.2 moles or more and 0.3 moles or less relative to 1 mole of copper.

[0108] The temperature of the aqueous solution in the first reduction step S2 is, for example, the same as the temperature in the complex formation step S1.

[0109] (Dispersant addition step S3)

[0110] Next, a dispersant is added to the aqueous solution of the copper-ammonia complex obtained after the first reduction step S2. Adding a dispersant allows for adjustment of the copper particle size. The dispersant is preferably phosphoric acid or a salt of phosphoric acid. Phosphoric acid is, for example, pyrophosphate. Sodium pyrophosphate is more preferred. In this case, it is easier to make the average particle size of the copper powder within the aforementioned range.

[0111] Dispersants, for example, are added in an amount of more than 0.05 mol and less than 0.2 mol relative to 1 mol of copper.

[0112] The aqueous solution obtained after adding the dispersant can be cooled. The temperature of the aqueous solution after adding the dispersant is preferably above 40°C and below 60°C. If the temperature of the aqueous solution is below 40°C, the dispersant is prone to precipitation, which is therefore not preferred.

[0113] (Secondary reduction process S4)

[0114] Next, a second reducing agent is added to the aqueous solution obtained after the dispersant addition step S3 to obtain an aqueous solution containing copper particles.

[0115] The second reducing agent is preferably the same as the first reducing agent. The amount of the second reducing agent added is, for example, more than the amount of the first reducing agent added. The second reducing agent is added, for example, in an amount of 0.3 moles or more and 3.0 moles or less relative to 1 mole of copper.

[0116] The temperature of the aqueous solution in the secondary reduction step S4 is preferably 40°C or higher and 60°C or lower. As mentioned above, if the temperature of the aqueous solution containing copper particles is below 40°C, the dispersant is prone to precipitation, which is therefore undesirable. Furthermore, at temperatures exceeding 60°C, foaming problems arise due to the reduction reaction, which is also undesirable.

[0117] (Metal ion addition process S5)

[0118] Next, at least one metal ion, either nickel or iron, can be added to the aqueous solution containing copper particles obtained after the secondary reduction step S4. In the metal ion addition step S5, the metal ions can be added while stirring. There are no particular limitations on the source of the metal ions; any source that forms metal ions in the aqueous solution, such as nickel chloride hexahydrate or ferric chloride (III) hexahydrate, is acceptable. When performing the metal ion addition step S5, the copper particles are easily coated with fatty acids and fatty acid salts in the fatty acid salt addition step S6.

[0119] The mass ratio of the aforementioned metal ions to the mass of copper is, for example, 0.01% by mass or more and 1.0% by mass or less. In this case, the copper particles are particularly easily coated with fatty acids and fatty acid salts. It should be noted that the temperature of the aqueous solution containing copper particles in the metal ion addition step S5 and thereafter is not particularly limited; for example, it can be 40°C or 30°C.

[0120] (Fat fatty acid salt addition process S6)

[0121] Next, the aqueous solution containing copper particles obtained after the metal ion addition step S5 is mixed with a fatty acid salt. Through this mixing, an aqueous solution containing coated copper particles is obtained, which includes copper particles and fatty acids and fatty acid salts disposed on the surface of the copper particles.

[0122] The fatty acid salt is preferably a salt of a straight-chain saturated fatty acid with 11 or more and 13 or less carbon atoms. Specifically, it is undecanoate (C11), laurate (C12), or tridecanoate (C13). Furthermore, the salt of a straight-chain saturated fatty acid with 11 or more and 13 or less carbon atoms is more preferably laurate. Laurate is preferably sodium laurate or potassium laurate, and more preferably sodium laurate. In this case, a fatty acid salt that readily produces copper formate through formic acid treatment is added, for example, in the form of an aqueous solution of the fatty acid salt to an aqueous solution containing copper particles obtained after the secondary reduction step S4 or the metal ion addition step S5.

[0123] Fatty acid salts are added, for example, in an amount of 0.001 mol or more and 0.015 mol or less relative to 1 mol of copper. The average particle size of the coated copper particles obtained by the fatty acid salt addition step S6 is, for example, 0.1 μm or more and 1.0 μm or less.

[0124] (pH adjustment process S7)

[0125] Next, the pH of the aqueous solution containing the copper-coated particles obtained after the fatty acid salt addition step S6 is adjusted so that the pH is 8.0 or higher and 11.0 or lower. There are no particular limitations on the pH adjustment method; for example, sulfuric acid or hydrochloric acid can be used for pH adjustment.

[0126] (Copper powder recovery process S8)

[0127] Next, copper powder, which is an aggregate of multiple coated copper particles, is recovered from the aqueous solution containing the coated copper particles. In the copper powder recovery step S8, for example, the solid component obtained after pressurizing and filtering the above aqueous solution is washed with pure water, and then the washed solid component is vacuum dried.

[0128] The above describes the manufacturing method of copper powder.

[0129] (Effect)

[0130] According to the above-described method for manufacturing copper powder, copper powder that exhibits the aforementioned effects can be obtained.

[0131] As described above, in the method for manufacturing copper powder of the present invention, the aforementioned fatty acid salt is mixed with an aqueous solution containing copper powder, and the pH of the aqueous solution obtained after the fatty acid salt addition step S6 is 8.0 or higher and 11.0 or lower. Therefore, copper powder in which copper formate is easily formed on the surface of copper particles by formic acid treatment can be obtained. When fatty acids are used instead of fatty acid salts, copper formate is less likely to form on the surface of copper particles by formic acid treatment compared to the case where fatty acid salts are used. The inventors believe this is because fatty acids are difficult to dissolve in water, while fatty acid salts are water-soluble. Furthermore, when the pH of the aqueous solution obtained after the fatty acid salt addition step S6 is not 8.0 or higher and 11.0 or lower, as shown in the comparative examples described later, a high copper formate ratio cannot be achieved.

[0132] Furthermore, as described above, according to the metal ion addition step S5, copper particles are easily coated with fatty acids and fatty acid salts. The inventors believe this is because ions of at least one of the metals, nickel and iron, react with fatty acids and their salts to form fatty acid metal salts, which are readily adsorbed onto the surface of the copper particles.

[0133] (Modified Example)

[0134] It should be noted that the dispersant addition step S3 can also be performed before the reduction step S2.

[0135] Alternatively, the metal ion addition step S5, pH adjustment step S7, and copper powder recovery step S8 can be omitted. Furthermore, if the pH of the aqueous solution containing coated copper particles obtained after the fatty acid salt addition step S6 is 8.0 or higher and 11.0 or lower, the pH adjustment step S7 can be omitted, or it can be performed.

[0136] [Example]

[0137] Hereinafter, examples related to the present invention will be described.

[0138] (Example 1)

[0139] (Complex formation process S1)

[0140] First, 1173g of copper sulfate pentahydrate (Upinorg, a registered trademark, manufactured by JX Metals Co., Ltd.), 1342g of 25% ammonia solution, and 71g of pure water were mixed by heating to 80°C and stirring. Then, an aqueous solution of a copper-ammonia complex was obtained. In this process, the rotation speed was set to 400 rpm, and nitrogen gas was bubbled. The nitrogen supply rate was set to 0.5 L / min.

[0141] (S2, a single reduction process)

[0142] Next, 74 g of 80% by mass hydrazine monohydrate was added continuously over 10 minutes to the aqueous solution of the copper-ammonia complex as the first reducing agent.

[0143] (Dispersant addition step S3)

[0144] Next, 314 g of sodium pyrophosphate decahydrate was added as a dispersant to the aqueous solution of the copper-ammonia complex after the addition of the first reducing agent, and the mixture was stirred for 20 minutes. Then, the resulting aqueous solution was cooled to 50°C.

[0145] (Secondary reduction process S4)

[0146] Next, 309 g of 80% (w / w) hydrazine monohydrate was added continuously over 7 minutes as a second reducing agent to the copper-ammonia complex aqueous solution after the dispersant was added. The resulting aqueous solution was then aged for 60 minutes. The pH of the aged aqueous solution was 9.2.

[0147] Next, a portion of the obtained aqueous solution was collected. The collected aqueous solution was filtered, washed with water, and dried to obtain copper particles. Drying was carried out using a vacuum dryer at 60°C for 10 hours.

[0148] (Metal ion addition process S5)

[0149] Next, a 10% by mass solution of nickel chloride hexahydrate was added to the remaining aqueous solution after a portion of the aqueous solution was collected, and the mixture was stirred for 10 minutes. The nickel chloride hexahydrate aqueous solution was added to the remaining aqueous solution at a ratio of nickel to copper of 0.1% by mass.

[0150] (Fat fatty acid salt addition process S6)

[0151] Next, a 5% (w / w) sodium laurate aqueous solution as a fatty acid salt was added to the aqueous solution containing nickel chloride, and the mixture was stirred for 60 minutes. The heating temperature was maintained at 50°C. The 5% (w / w) sodium laurate aqueous solution was added to the aqueous solution containing nickel chloride at a ratio of sodium laurate to copper of 2.0% (w / w). It should be noted that the pH of the aqueous solution did not change before and after the addition of the fatty acid salt.

[0152] (Copper powder recovery process S8)

[0153] Next, the aqueous solution containing the added fatty acid salt was filtered using a pressure filtration device, followed by washing and drying to obtain copper powder. Drying was performed using the same method as for copper powder.

[0154] (Example 2)

[0155] In the secondary reduction step S4, 80% by mass of hydrazine monohydrate was continuously added for 30 minutes. After the fatty acid salt addition step S6 and before the copper powder recovery step S8, a pH adjustment step was performed. Otherwise, copper powder was obtained by the same method as in Example 1.

[0156] pH adjustment was performed using a 20% (w / w) sulfuric acid aqueous solution. The pH of the adjusted aqueous solution was 8.9.

[0157] (Example 3)

[0158] In the secondary reduction step S4, 80% by mass of hydrazine monohydrate was continuously added for 30 minutes. In the metal ion addition step S5, 10% by mass of ferric(III) nitrate nonahydrate aqueous solution was added instead of 10% by mass of nickel chloride hexahydrate aqueous solution. After the fatty acid salt addition step S6 and before the copper powder recovery step S8, a pH adjustment step S7 was performed. Otherwise, copper powder was obtained by the same method as in Example 1.

[0159] In the metal ion addition step S5, 10% by mass of an aqueous solution of ferric(III) nitrate nonahydrate is added to achieve a ratio of iron to copper of 1.0% by mass. Furthermore, pH adjustment is performed using a 20% by mass sulfuric acid aqueous solution. The pH of the adjusted aqueous solution is 8.9.

[0160] (Example 4)

[0161] The metal ion addition step S5 is omitted. The pH adjustment step S7 is performed after the fatty acid salt addition step S6 and before the copper powder recovery step S8. Otherwise, copper powder is obtained by the same method as in Example 1.

[0162] pH adjustment was performed using a 20% (w / w) sulfuric acid aqueous solution. The pH of the adjusted aqueous solution was 8.0.

[0163] (Example 5)

[0164] In the complex formation step S1, the amount of copper sulfate pentahydrate was changed to 1564g, the amount of pure water was changed to 94g, and the amount of 25% by mass ammonia was changed to 1790g. In the primary reduction step S2, the amount of 80% by mass hydrazine monohydrate was changed to 98g. In the dispersant addition step S3, the amount of sodium pyrophosphate decahydrate was changed to 419.2g. In the secondary reduction step S4, the amount of 80% by mass hydrazine monohydrate was changed to 157.8g. 80% by mass hydrazine monohydrate was added continuously for 60 minutes. After the fatty acid salt addition step S6 and before the copper powder recovery step S8, a pH adjustment step was performed. Otherwise, copper powder was obtained by the same method as in Example 1.

[0165] pH adjustment was performed using a 20% (w / w) sulfuric acid aqueous solution. The pH of the adjusted aqueous solution was 8.2.

[0166] (Example 6)

[0167] In the secondary reduction process S4, the amount of 80% by mass hydrazine monohydrate was changed to 465g, and 80% by mass hydrazine monohydrate was added over 1 second. Otherwise, copper powder was obtained by the same method as in Example 1.

[0168] The pH of the aqueous solution after the secondary reduction process S4 is 9.4.

[0169] (Comparative Example 1)

[0170] The metal ion addition step S5 is omitted. Lauric acid is added in place of 5% sodium lauryl salt aqueous solution in fatty acid salt addition step S6. The pH adjustment step S7 is performed after fatty acid salt addition step S6 and before copper powder recovery step S8. Otherwise, copper powder is obtained by the same method as in Example 1.

[0171] Lauric acid was added at a ratio of 2.0% by mass to copper. pH was adjusted using a 20% by mass sulfuric acid aqueous solution. The pH of the adjusted aqueous solution was 8.5.

[0172] (Comparative Example 2)

[0173] The metal ion addition step S5 is omitted, and lauric acid is added in the fatty acid salt addition step S6 instead of 5% sodium lauryl salt aqueous solution. Otherwise, copper powder is obtained by the same method as in Example 1.

[0174] Lauric acid was added in such a way that the mass ratio of lauric acid to copper was 2.0% by mass.

[0175] (Comparative Example 3)

[0176] The metal ion addition step S5 is omitted. The pH adjustment step S7 is performed after the fatty acid salt addition step S6 and before the copper powder recovery step S8. Otherwise, copper powder is obtained by the same method as in Example 1.

[0177] pH adjustment was performed using a 20% (w / w) sulfuric acid aqueous solution. The pH of the adjusted aqueous solution was 7.5.

[0178] (Comparative Example 4)

[0179] Without performing the metal ion addition step S5 and the fatty acid salt addition step S6, copper powder was obtained using the same method as in Example 1. Then, 100g of the obtained copper powder and 12.5g of isopropanol (dissolving 1.0g of lauric acid) were mixed for 2 minutes (2000rpm rotation, 800rpm revolution) using a mixing and degassing apparatus (THINKY ARE-310), and dried at 60°C for 10 hours using a vacuum dryer to obtain the copper powder of Comparative Example 4.

[0180] (Comparative Example 5)

[0181] The metal ion addition step S5 and the fatty acid salt addition step S6 are omitted. Otherwise, copper powder is obtained by the same method as in Example 1.

[0182] (Determination of carbon content)

[0183] The carbon content of the copper powders from Examples 1-6 and Comparative Examples 1-4, and the copper particles from Examples 1-6 and Comparative Examples 1-5, was determined using the C / S meter described above. Carbon content is the ratio (mass %) of the mass of carbon to the mass of the copper powder or copper particles.

[0184] (Determination of oxygen content)

[0185] For the copper powders of Examples 1-6 and Comparative Examples 1-4, and the copper particles of Examples 1-6 and Comparative Examples 1-5, the oxygen content was determined using an oxygen-nitrogen-hydrogen simultaneous determination apparatus (ONH836, manufactured by LECO Japan). The oxygen content is the ratio (mass%) of the mass of oxygen to the mass of the copper powder or copper particles.

[0186] (Determination of BET specific surface area)

[0187] The BET specific surface area of ​​the copper powders of Examples 1-6 and Comparative Examples 1-4, and the copper particles of Examples 1-6 and Comparative Examples 1-5, was determined by the following methods.

[0188] Specifically, using a fully automated specific surface area measuring device (Macsorb (registered trademark), manufactured by Mounttech Co., Ltd.), after degassing by passing nitrogen gas through the measuring device at 105°C for 20 minutes, the BET specific surface area of ​​copper powder or copper particles is measured by passing a mixed gas of 30% by volume nitrogen and 70% by volume helium through the device.

[0189] (Method for determining TAP density)

[0190] The TAP density of the copper powders of Examples 1-6 and Comparative Examples 1-4, and the copper particles of Examples 1-6 and Comparative Examples 1-5, was determined by the following methods.

[0191] In this invention, the TAP density was determined according to the method described in Japanese Patent Application Publication No. 2007-263860. Specifically, a copper powder sample was filled into a bottomed cylindrical container with an inner diameter of 6 mm to form a copper powder sample layer, and a pressure of 0.16 N / m was applied to the layer from above. 2 After pressure is applied, the height of the copper powder sample layer is measured. The density of the copper powder sample is determined from the measured height of the copper powder sample layer and the weight of the filled copper powder sample. This density is defined as the TAP density of the copper powder in this invention.

[0192] (Determination of nickel and iron content)

[0193] For each copper powder from Examples 1-6 and Comparative Examples 1-4, the nickel or iron content was determined using an inductively coupled plasma (ICP) emission spectrometer (SPS3520V, manufactured by Hitachi High-Tech Analysis Co., Ltd.). The nickel or iron content was expressed as the ratio of the mass of nickel or iron to the mass of copper powder or copper particles (ppm).

[0194] (Determination of average particle size)

[0195] The average particle size of the copper powders from Examples 1-6 and Comparative Examples 1-4, and the copper particles from Examples 1-6 and Comparative Examples 1-5, was determined according to the method described above. An S-4700 (manufactured by Hitachi High Technology Co., Ltd.) was used as the scanning electron microscope, and Mac-View (Ver.4) (manufactured by Mountech Co., Ltd.) was used as the image processing software.

[0196] (TG-MS determination)

[0197] For each copper powder from Examples 1-6 and Comparative Examples 1-4, TG-MS determination was performed according to the following determination conditions.

[0198] The TG-MS apparatus used was a combination of a high-sensitivity differential thermal balance (STA 2500Regulus, NETZSCH) used as a TG-DTA apparatus and a gas chromatograph-quadrupole mass spectrometer (JMS-Q1500GC, NEC Corporation). The sample volume was set to 10 mg, the heating rate to 10 °C / min, the carrier gas to helium at a supply rate of 20 mL / min, and the measurement temperature to be between 50 °C and 600 °C. The carrier gas was supplied after purging the apparatus under vacuum.

[0199] Then, TG-MS measurements were performed to obtain spectra (m / z 44, m / z 73) originating from the COO and hydrocarbon fractions, respectively. Based on these spectra, peak temperatures T1 and T2 were obtained. Furthermore, the peak areas in the range of 50 to 400 degrees Celsius were calculated using a qualitative analysis processing program (MS-66080QLA), and the aforementioned ratio C / (C+R) was determined.

[0200] (Determination of copper formate content)

[0201] For each copper powder of Examples 1-6 and Comparative Examples 1-4, the ease of copper formate production, i.e., the copper formate rate, was determined by the following method.

[0202] First, the copper powder was treated with formic acid. Specifically, the following mixture was prepared: 42.22g of 2-propanol (manufactured by Fujifilm and Kohden Chemical Co., Ltd.) and 3.33g of 90% formic acid (manufactured by Fujifilm and Kohden Chemical Co., Ltd.) were mixed and heated to 30°C. Next, 5g of copper powder was added to the mixture and stirred. Stirring was performed using a magnetic stirrer at 500 rpm for 1 hour. Then, solid-liquid separation was performed by vacuum filtration, and the obtained solid component was washed twice with 50cc of 2-propanol. Next, the solid component was dried at 60°C for 10 hours using a vacuum dryer. Thus, the copper powder was treated with formic acid.

[0203] Next, for the dried copper powder (hereinafter referred to as formic acid-treated copper powder), a carbon / sulfur analyzer (EMIA-22V, manufactured by Horiba Manufacturing Co., Ltd., also known as a C / S meter) was used to obtain the mass percentage (mass %) of carbon in the mass of the formic acid-treated copper powder. The obtained percentage was taken as the copper formic acid ratio.

[0204] (Determination of thermogravimetric behavior)

[0205] The thermogravimetric behavior of each copper powder from Example 1 and Comparative Example 5 was determined by the following method.

[0206] Specifically, using a high-sensitivity differential thermal balance (STA 2500 Regulus, NETZSCH), 25 mg of copper powder (i.e., copper powder before formic acid treatment) from Example 1 and Comparative Example 5 was weighed in a specified alumina pan, and the sample was heated from room temperature (25°C ± 5) to 300°C in air at a heating rate of 5°C / min to perform thermogravimetric analysis (i.e., TG).

[0207] (Determination of thermal shrinkage behavior)

[0208] For the copper powders of Example 4 and Comparative Example 3, the thermal shrinkage behavior was determined by the following method.

[0209] Specifically, firstly, the copper powders of Example 4 and Comparative Example 3 were treated with formic acid using the same method as in the determination of the copper formic acid ratio described above. Next, 0.3 g of the formic acid-treated copper powders from Example 4 and Comparative Example 3 were weighed and placed into a pre-defined mold with a diameter of 5 mm φ. The mold was then compacted for 1 minute using a press under a load of 50 kg to prepare a cylindrical test sample. This test sample was placed on the sample holder of a thermomechanical analysis (TMA) apparatus (Thermo EVO 2 series TMA8311). A test load of 98 mN was applied using a test probe, and the temperature was increased from room temperature (25 °C ± 5) to 300 °C at a rate of 10 °C / min in nitrogen atmosphere to perform thermomechanical analysis (TMA) on the test sample.

[0210] The results regarding the embodiments and comparative examples are shown in the tables below. Figures 5-16 .

[0211] [Table 1]

[0212]

[0213] [Table 2]

[0214]

[0215] [Table 3]

[0216]

[0217] As shown in the table, the copper powders of Examples 1-6 exhibit a high rate of transformation to copper formate because the proportion of carbon in the mass of the copper powder after formic acid treatment (copper formate ratio) is all above 1%. Therefore, the copper powders of Examples 1-6 readily form copper formate. Furthermore, in the copper powders of Examples 1-6, the copper particles are coated with lauric acid and laurate, resulting in excellent oxidation resistance. Additionally, the copper powders of Examples 1-6 also exhibit excellent low-temperature sintering properties.

[0218] On the other hand, in the copper powders of Comparative Examples 1, 2, and 4, lauric acid was used instead of laurate to coat the copper particles, so the copper formate content of the copper powder after formic acid treatment was less than 1%. Furthermore, although sodium laurate was used in the copper powder of Comparative Example 3, the pH of the aqueous solution after the fatty acid salt addition step S6 was low, so the copper formate content of the copper powder after formic acid treatment was less than 1%. Therefore, the copper powders of Comparative Examples 1-4 were less likely to produce copper formate compared to the copper powders of Examples 1-6. Additionally, although the copper powder of Comparative Example 5 had a copper formate content of more than 1% after formic acid treatment, its surface was not coated with fatty acids and their salts, therefore its oxidation resistance was not excellent.

[0219] Figures 5-14The graphs represent the TG-MS results of copper powders from Examples 1-6 and Comparative Examples 1-4. The horizontal axis of the graphs represents temperature (°C), the left vertical axis represents the weight reduction ratio, and the right vertical axis represents the mass spectrometry intensity. Additionally, the graphs show spectra for ions with m / z 44 (i.e., carbon dioxide gas), spectra for ions with m / z 73 (i.e., hydrocarbon fraction), and spectra showing the relationship between temperature and the weight reduction ratio of the sample.

[0220] like Figures 5-10 As shown, in the copper powders of Examples 1-6, the peak temperature T1 is lower than the peak temperature T2. On the other hand, as... Figure 11-14 As shown, in the copper powders of Comparative Examples 1-4, the peak temperature T1 is higher than the peak temperature T2. Furthermore, in the copper powders of Comparative Examples 1, 3, and 4, the aforementioned ratio C / (C+R) is outside the range of 0.10 or higher and 0.70 or lower.

[0221] It should be noted that for Comparative Examples 1 and 5, the oxidation in formic acid treatment resulted in the detection of a copper oxide (I) peak by XRD. This is believed to be because, in Comparative Example 1, fatty acids were used instead of fatty acid salts, resulting in uneven coating, while in Comparative Example 5, the mixture was not coated with fatty acids or their salts.

[0222] Figure 15 This is a graph showing the thermogravimetric behavior (i.e., TG measurement results) of the copper powders in Example 1 and Comparative Example 5. Figure 15 As shown, the copper powder of Example 1 coated with lauric acid and its salts exhibits a slower increase in thermogravimetric intensity compared to the copper powder of Comparative Example 5, which is not coated with fatty acids and their salts. This indicates that the copper powder of Example 1 can suppress the increase in mass, including the increase in mass caused by oxidation, compared to the copper powder of Comparative Example 5. Thus, the copper powder coated with lauric acid and its salts exhibits excellent oxidation resistance. Therefore, the copper powders of Examples 2-6 also exhibit excellent oxidation resistance.

[0223] Figure 16 This is a graph showing the thermal shrinkage behavior (i.e., TMA measurement results) of the formic acid-treated copper powders in Example 4 and Comparative Example 3. Figure 16As shown, the copper powder of Example 4, obtained by formic acid treatment, exhibited significant shrinkage around 180°C. On the other hand, no significant shrinkage was observed in the copper powder of Comparative Example 3, obtained by formic acid treatment. In the copper powder of Example 4, obtained by formic acid treatment, large thermal shrinkage was observed up to 300°C, indicating that sintering of the copper powder had occurred. It is believed that the sintering of this copper powder was promoted by the decomposition of copper formate. This indicates that the copper powder of Example 4, compared to the copper powder of Comparative Example 3, has better low-temperature sintering properties after formic acid treatment. Thus, copper powder with a high copper formate ratio exhibits excellent low-temperature sintering properties. Therefore, the copper powders of Examples 1-3, as well as 5 and 6, also exhibit excellent low-temperature sintering properties.

[0224] Explanation of reference numerals in the attached figures

[0225] S1… Complex formation process, S2… Primary reduction process, S3… Dispersant addition process, S4… Secondary reduction process, S5… Metal ion addition process, S6… Fatty acid salt addition process, S7… pH adjustment process, S8… Copper powder recovery process.

Claims

1. A copper powder comprising an aggregate of multiple coated copper particles, each comprising copper particles and fatty acids and their salts disposed on the surface of the copper particles. The copper powder has an average particle size of 0.1 μm or more and 1.0 μm or less. In thermogravimetric-mass spectrometry (TGA), the peak temperature T1 of the peak originating from carbon dioxide is lower than the peak temperature T2 of the peak originating from the hydrocarbon fraction of the fatty acid and its salt.

2. The copper powder according to claim 1, wherein, The carbon content in the copper powder is above 0.1% by mass and below 1.5% by mass.

3. The copper powder according to claim 1, wherein, In thermogravimetric-mass spectrometry analysis, the proportion of the peak area C in the sum of the peak area C of the peak originating from the carbon dioxide and the peak area R of the peak originating from the hydrocarbon fraction is greater than 0.10 and less than 0.

70.

4. The copper powder according to claim 1, wherein, The peak temperature T2 is below 400℃.

5. The copper powder according to claim 1, wherein, The fatty acids and their salts are straight-chain saturated fatty acids and their salts with 11 or more but less than 13 carbon atoms.

6. The copper powder according to claim 5, wherein, The straight-chain saturated fatty acids with 11 or more but less than 13 carbon atoms and their salts are lauric acid and laurate.

7. The copper powder according to claim 1, wherein, The coated copper particles further contain at least one metal selected from nickel and iron on their surface. The mass ratio of the metal to the mass of the copper particles is more than 10 ppm and less than 2000 ppm.

8. A method for manufacturing copper powder, comprising: In the complex formation process, copper sulfate, ammonia, and water are mixed to obtain an aqueous solution of copper-ammonia complex containing copper-ammonia complex; In a first reduction step, a first reducing agent is added to the aqueous solution of the copper-ammonia complex; The dispersant addition step involves adding a dispersant to the aqueous solution of the copper-ammonia complex before or after the primary reduction step. A secondary reduction process involves adding a second reducing agent to the aqueous solution obtained after the primary reduction process and after the dispersant addition process, to obtain an aqueous solution containing copper particles; and In the fatty acid salt addition step, the aqueous solution containing the copper particles is mixed with a salt of fatty acids to obtain an aqueous solution containing coated copper particles, wherein the coated copper particles comprise the copper particles and the fatty acids and their salts disposed on the surface of the copper particles. The aqueous solution containing the coated copper particles obtained after the fatty acid salt addition step has a pH of 8.0 or higher and 11.0 or lower.

9. The method for manufacturing copper powder according to claim 8, wherein, After the secondary reduction step and before the fatty acid salt addition step, the method further includes a metal ion addition step, in which at least one metal ion, either nickel or iron, is added to the aqueous solution containing the copper particles.

10. The method for manufacturing copper powder according to claim 8, wherein, After the fatty acid salt addition step, a copper powder recovery step is further included, in which copper powder, which is an aggregate of the coated copper particles, is recovered from the aqueous solution containing the coated copper particles.

11. The method for manufacturing copper powder according to claim 8, wherein, The first reducing agent and the second reducing agent are hydrazine.

12. The method for manufacturing copper powder according to claim 8, wherein, The dispersant is sodium pyrophosphate.

13. The method for manufacturing copper powder according to claim 8, wherein, The fatty acid salt is a salt of a straight-chain saturated fatty acid with 11 or more but less than 13 carbon atoms.

14. The method for manufacturing copper powder according to claim 13, wherein, The salt of the straight-chain saturated fatty acid with 11 or more but less than 13 carbon atoms is laurate.

15. The method for manufacturing copper powder according to claim 14, wherein, The lauryl salt is sodium lauryl salt.

16. The method for manufacturing copper powder according to claim 8, wherein, The average particle size of the copper powder is greater than 0.1 μm and less than 1.0 μm.

Citation Information

Patent Citations

  • Tap density measuring method and device of powder

    JP2007263860A

  • Copper composite particle, copper paste comprising the same and method of producing circuit board using the same

    JP2015030869A

  • Coated copper particle

    JP2016176146A