High-performance corrosion-resistant rich-heavy rare earth permanent magnet material and preparation method thereof
By combining nine-component nanocomposite additives with microalloying of the matrix, a continuous three-dimensional network structure is formed, which solves the problems of low utilization rate of heavy rare earth and poor corrosion resistance in heavy rare earth sintered NdFeB permanent magnet materials, and achieves simultaneous improvement of magnetic properties and corrosion resistance, making it suitable for new energy vehicles and offshore wind power.
Patent Information
- Application Number
- CN202611368035.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies for heavy rare earth-rich sintered NdFeB permanent magnet materials suffer from problems such as low utilization of heavy rare earths, poor intrinsic corrosion resistance of grain boundaries, difficulty in simultaneously improving magnetic properties and corrosion resistance, poor dispersibility of nano-additives, and insufficient synergy in the entire process.
By combining nine-component nanocomposite additives with matrix microalloying, a continuous three-dimensional network structure is formed by precisely controlling the distribution of heavy rare earth elements in the grain boundaries and epitaxial shells of the main phase grains. Combined with the synergistic effect of multi-component nanocomposite additives, the electrochemical homogeneity and thermodynamic stability of the grain boundary phase are optimized, thereby achieving simultaneous improvement in magnetic properties and corrosion resistance.
It significantly improves the utilization efficiency of heavy rare earth elements, enhances the coercivity and corrosion resistance of magnets, prolongs the salt spray rust formation time, and reduces the corrosion current density, making it suitable for high-end applications such as new energy vehicles and offshore wind power.
Smart Images

Figure CN123128499A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of rare earth permanent magnet materials technology, specifically to a high-performance corrosion-resistant heavy rare earth-rich permanent magnet material and its preparation method. Background Technology
[0002] With Nd2Fe 14 Boron-based sintered NdFeB magnets, with their high energy product and mature manufacturing processes, have become the most widely used permanent magnet material, earning them the title of "King of Permanent Magnets." However, high-end applications place stringent demands on the overall performance of magnets: motors operating at 120-180°C require high coercivity to prevent high-temperature demagnetization, while offshore wind power and other applications require excellent corrosion resistance to ensure a 20-30 year service life. Therefore, developing NdFeB materials that combine high coercivity, high temperature stability, and intrinsic corrosion resistance has become an urgent need for the industry.
[0003] To improve coercivity, the most common method is to add heavy rare earth elements such as Dy and Tb. (Dy2Fe) 14 B and Tb2Fe 14 The magnetocrystalline anisotropy fields of B reach 150 kOe and 220 kOe, respectively, which are much higher than those of Nd₂Fe. 14 The 73kOe of B, with partial substitution of Nd by heavy rare earth elements, can significantly improve coercivity. However, the current technical route of improving the coercivity of NdFeB by adding heavy rare earth elements still has the following shortcomings: First, heavy rare earth resources are scarce and expensive. In traditional alloying processes, more than 70% of heavy rare earth elements are uniformly distributed inside the main phase grains, while antimagnetic domains mainly nucleate at grain boundaries and defects. The grain interior does not require a high anisotropic field, resulting in serious waste. Second, Dy and Tb are antiferromagnetically coupled with Fe. A large amount of Dy and Tb entering the main phase significantly reduces the saturation magnetization, leading to a decrease in remanence and energy product, forming a performance constraint that "high coercivity is inevitably accompanied by low remanence".
[0004] In addition, poor corrosion resistance is another key issue restricting the application of heavy rare earth-rich magnets in high-end corrosive environments. Sintered NdFeB is a multiphase composite material with a potential of approximately -0.75V for the Nd-rich grain boundary phase and approximately -0.56V for the main phase, resulting in a potential difference of nearly 200mV. The grain boundary phase acts as the anolyte, preferentially corroding and rapidly propagating along the grain boundaries. In heavy rare earth-rich magnets, the uneven distribution of heavy rare earth compounds at the grain boundaries causes nanoscale potential fluctuations, forming more micro-corrosion galvanic cells, thus further worsening corrosion resistance.
[0005] Existing technologies mainly improve along three routes, but all have inherent limitations: surface protection (nickel plating, zinc plating, epoxy, etc.) suffers from pinholes, incomplete edge coverage, and processing damage; once damaged, corrosion spreads rapidly and cannot solve the problem of bulk grain boundary corrosion; bulk alloying (adding Co, Al, Cu, Ga, etc.) has limited effects, often improving corrosion resistance but impairing magnetic properties; grain boundary diffusion improves the utilization rate of heavy rare earth elements, but the diffusion depth is limited (>5mm magnets are difficult to be uniform), the uniformity is poor, the process is complex, and it almost only focuses on coercivity, neglecting the impact on corrosion resistance. Chinese patents CN112017834B, CN115360008A, and CN112562953A improve from the perspectives of bi-alloying, alloying potential modification, and adding oxide nanoparticles, but they either do not conduct nano-multiphase composite design for corrosion resistance, or still use traditional addition of heavy rare earth elements, resulting in waste, or have few additive components and poor mixing uniformity, and none of them have achieved a simultaneous and significant improvement in magnetic properties and corrosion resistance. Against this backdrop, how to achieve efficient utilization of heavy rare earth elements and enhanced intrinsic corrosion resistance through grain boundary nanophase regulation has become a key issue that urgently needs to be addressed in the field of heavy rare earth-rich NdFeB magnets. This requires optimizing the distribution morphology of heavy rare earth elements at grain boundaries and the electrochemical homogeneity of the grain boundary phase, developing multi-component nanocomposite additives and their integrated preparation process for uniform composite with magnetic powder, and solving problems such as low utilization rate of heavy rare earth elements, difficulty in achieving both magnetic properties and corrosion resistance, and poor dispersion of nano-additives, in order to meet the urgent demand for high-performance corrosion-resistant magnets in high-end fields such as new energy vehicles and offshore wind power. Summary of the Invention
[0006] The purpose of this invention is to overcome the technical defects of existing heavy rare earth-rich sintered NdFeB permanent magnet materials, such as low utilization rate of heavy rare earth, poor intrinsic corrosion resistance of grain boundaries, difficulty in simultaneously improving magnetic properties and corrosion resistance, poor dispersion of nano-additives, and insufficient synergy of the entire process. To this end, this invention provides a high-performance corrosion-resistant heavy rare earth-rich permanent magnet material and its preparation method.
[0007] To achieve the above technical objectives, the present invention adopts the following technical solution:
[0008] A high-performance, corrosion-resistant, heavy rare-earth-rich permanent magnet material and its preparation method, comprising the following steps:
[0009] S1. Prepare the permanent magnet material raw materials according to the component ratio. The permanent magnet material raw materials include, by weight percentage: 22-27 wt% praseodymium-neodymium alloy, 5-8 wt% dysprosium-iron alloy, 1.2-3 wt% terbium metal, 0.9-1.2 wt% ferroboron alloy, 1-3 wt% cobalt metal, 0.3-0.8 wt% aluminum metal, 0.1-0.4 wt% copper metal, 0.1-0.3 wt% gallium metal, 0.05-0.2 wt% zirconium metal, 0.05-0.2 wt% niobium metal, with industrial pure iron as the balance; the heavy rare earth elements in the permanent magnet material account for 15-30 wt% of the total rare earth element mass.
[0010] S2. Place the prepared permanent magnet material raw materials into a vacuum induction rapid solidification furnace for melting and casting to obtain rapid solidification casting sheets.
[0011] S3. The rapid-solidifying cast sheets are subjected to hydrogen crushing treatment to prepare coarse powder;
[0012] S4. The coarse powder and the nano-grain boundary regulating composite additive are mixed at a mass ratio of (98.5~99.5):(0.5~1.5) and then subjected to air jet milling to obtain fine powder;
[0013] S5. Under the protection of inert gas, the fine powder is molded in an orientation magnetic field and then subjected to cold isostatic pressing to obtain a green body.
[0014] S6. The green blank is sintered in vacuum in sections, followed by a two-stage tempering heat treatment to finally obtain a high-performance corrosion-resistant heavy rare earth-rich permanent magnet material.
[0015] Furthermore, the raw materials for preparing the nano-grain boundary regulation composite additive in step S4 include, by weight: 15-25 parts of nano-dysprosium oxide, 10-20 parts of nano-terbium fluoride, 8-15 parts of nano-titanium nitride, 5-12 parts of nano-silicon carbide, 5-10 parts of nano-alumina, 3-8 parts of nano-copper powder, 2-6 parts of nano-magnesium powder, 2-5 parts of nano-gallium oxide, and 1-3 parts of nano-zirconium boride.
[0016] Furthermore, the preparation method of the nanograin boundary regulation composite additive in step S4 includes the following steps:
[0017] (1) Nano dysprosium oxide, nano terbium fluoride, nano titanium nitride, nano silicon carbide, nano aluminum oxide, nano copper powder, nano magnesium powder, nano gallium oxide, and nano zirconium boride were respectively placed in anhydrous ethanol and ultrasonically dispersed for 20 to 40 minutes at a power of 300 to 500 W to obtain a uniform suspension of each component.
[0018] (2) Mix the suspensions of each component according to the ratio, add 0.5~1.5% of polyethylene glycol 4000 as a dispersant, and stir at high speed of 800~1200 rpm for 30~60 min to obtain a uniformly mixed slurry;
[0019] (3) The mixed slurry is vacuum dried at 60~100℃ for 10~15h to obtain composite powder;
[0020] (4) Place the composite powder in a high-energy ball mill jar, add grinding balls at a ball-to-material ratio of (15~25):1, the grinding balls are stainless steel balls with diameters of 5mm and 10mm and a mass ratio of 1:1, fill with argon gas for protection, and ball mill at a speed of 300~500rpm for 8~15h.
[0021] (5) The ball-milled powder was vacuum heat-treated at 400~500℃ for 1~3h, then cooled to room temperature under high-purity nitrogen protection, and passed through a 300-mesh sieve to obtain a nano-grain boundary regulating composite additive with an average particle size of 50~150nm.
[0022] Furthermore, in step S1, the mass ratio of Pr to Nd in the praseodymium-neodymium alloy is 25:75, and the purity is not less than 99.5%; the mass content of Dy in the dysprosium-iron alloy is 80%, with the balance being Fe, and the purity is not less than 99.5%; the purity of metallic terbium, metallic cobalt, metallic aluminum, metallic copper, metallic gallium, metallic zirconium, and metallic niobium is not less than 99.9%; the mass content of B in the boron-iron alloy is 20%, with the balance being Fe; the purity of industrial pure iron is not less than 99.9%, and the total content of impurities C, N, and O is not higher than 0.05 wt%.
[0023] Furthermore, in step S2, the melting temperature of the vacuum induction rapid solidification furnace is 1450~1550℃, the refining time is 5~15min, the electromagnetic stirring frequency during the refining process is 2~5Hz; the casting temperature is 1380~1450℃, the copper roller linear speed is 1.5~3.0m / s, the thickness of the obtained rapid solidification casting sheet is 0.2~0.5mm, the main phase grain size of the casting sheet is 2~8μm, and there is no α-Fe soft magnetic phase precipitation.
[0024] Furthermore, the hydrogen breakup process in step S3 includes: evacuating to a vacuum of 1×10⁻⁶ at room temperature. -2 Below Pa, high-purity hydrogen gas with a purity of 99.999% is introduced to a pressure of 0.08~0.15MPa, and the mixture is allowed to stand for 1.5~2.5h to absorb hydrogen until saturation. Then, a vacuum is drawn and the temperature is raised to 500~600℃ for dehydrogenation treatment, and the temperature is maintained for 2~4h. After dehydrogenation, the mixture is cooled to room temperature under argon protection. The average particle size of the coarse powder after hydrogen crushing is 150~300μm, and the hydrogen content is not higher than 500ppm.
[0025] Furthermore, in step S4, the grinding pressure of the air jet mill is 0.5~0.7MPa, the sorting wheel speed is 3500~4500rpm, nitrogen protection is maintained throughout the air jet milling process, the oxygen content in the system is controlled below 50ppm, and the dew point is below -60℃; the obtained fine powder laser particle size distribution D 50 The particle size is 2.8~3.2μm, the particle size distribution range is <1.2, and the oxygen content of fine powder is not higher than 1500ppm.
[0026] Further, in step S5, the orientation magnetic field strength for compression molding is 1.8~2.5T, the molding pressure is 150~250MPa, and the holding time is 10~30s; after compression molding, cold isostatic pressing is performed with an isostatic pressing pressure of 150~250MPa and a holding time of 60~120s; the entire molding process is under nitrogen protection, the ambient oxygen content is controlled below 100ppm, and the density of the obtained green body is 3.8~4.2g / cm³. 3 .
[0027] Further, the vacuum segmented sintering in step S6 includes: heating from room temperature to 800°C at a heating rate of 5-10°C / min and holding at that temperature for 1-2 hours for degassing, then heating to 1050-1110°C at a heating rate of 3-5°C / min and holding at that temperature for 3-5 hours for sintering, wherein the vacuum degree during sintering is better than 5×10⁻⁶. -3 Pa; After sintering, 0.08~0.12MPa of high-purity argon gas is introduced and the blower is started to force cooling to room temperature; The two-stage tempering heat treatment includes: the sintered magnet is reheated to 850~950℃ and held for 2~4h for first-stage tempering, then argon gas is introduced to rapidly cool to room temperature, then heated to 450~550℃ and held for 3~5h for second-stage tempering, and finally cooled to room temperature with the furnace.
[0028] This invention also provides a high-performance, corrosion-resistant, heavy rare-earth-rich permanent magnet material. In the microstructure of this material, a heavy rare-earth-rich epitaxial shell with a thickness of 50-200 nm is formed outside the main phase grains, and the grain boundary phase forms a continuous three-dimensional network structure with a grain boundary thickness of 20-100 nm; the room-temperature coercivity H of this material... cj ≥17kOe, remanence Br≥12.5kGs, maximum energy product (BH) max ≥38 MGOe, flexural strength ≥350 MPa; in a 5wt% NaCl neutral salt spray test, the rusting time of the uncoated magnet is ≥192 h, and the corrosion current density measured in a 3.5wt% NaCl solution is ≤8 μA / cm². 2 .
[0029] Compared with the prior art, the present invention has the following technical advantages:
[0030] (1) This invention breaks through the traditional approach of adding heavy rare earth alloys by combining matrix microalloying with grain boundary control of nanocomposite additives. Through precise control of thermodynamic and kinetic parameters, heavy rare earths are mainly enriched in the grain boundaries and the 50-200 nm epitaxial shell layer outside the main phase grains, rather than being uniformly distributed inside the main phase. During sintering and tempering, nano-Dy2O3 and TbF3 diffuse uniformly along the grain boundary channels, forming a thin and continuous Dy and Tb-rich hard magnetic shell layer in situ on the grain surface. This shell layer precisely covers the region where antimagnetic domains are most likely to nucleate, maximizing the anisotropic field on the grain surface with the minimum amount of heavy rare earths. This effectively suppresses the nucleation of antimagnetic domains and avoids the decrease in saturation magnetization caused by a large amount of heavy rare earths entering the main phase. Compared with the traditional alloying process of the same composition, the coercivity of the magnet is improved with the same amount of heavy rare earths added, while the remanence and maximum energy product remain at a high level, significantly improving the utilization efficiency of heavy rare earths. Meanwhile, the irreversible magnetic flux loss at 120℃×100h is reduced from more than 5% to less than 2%, and the magnet can work stably for a long time at 120℃.
[0031] (2) This invention reconstructs grain boundaries from three aspects: composition, electrochemical properties, and three-dimensional morphology, through the synergistic effect of nine-component nanocomposite additives. Highly chemically stable ceramic phases such as nano-TiN, SiC, and Al2O3 are uniformly distributed throughout the grain boundary network during sintering, reducing the potential difference between the grain boundaries and the main phase, thus thermodynamically weakening the driving force of electrochemical corrosion; the chemically inert ceramic phases simultaneously reduce the dissolution rate of grain boundaries in the corrosive medium. After double-stage tempering, a continuous, dense, and uniformly thick three-dimensional network is formed, uniformly encapsulating the main phase grains and kinetically blocking the channels for the diffusion of the corrosive medium along the grain boundaries. Compared with a magnet of the same composition without additives (Comparative Example 1), the rusting time of the uncoated magnet under 5wt% NaCl salt spray increased from 48h to over 192h, more than four times longer than before; the mass loss under 200h salt spray decreased from 12.6mg / cm³. 2 Reduced to 1.2~3.2 mg / cm³ 2 This reduces corrosion current density by more than 74%; the corrosion current density is reduced from 15.8 μA / cm². 2 Reduced to 3.5~6.8 μA / cm 2 This improves the corrosion resistance of heavy rare earth magnets at the intrinsic structural level.
[0032] (3) This invention overcomes the inherent perception in the field that "the addition of heavy rare earth elements improves coercivity but reduces corrosion resistance" by cross-scale synergy between nine additive components and multiple matrix components, and achieves simultaneous improvement of magnetic properties and corrosion resistance. The components in the composite additive work together: Dy2O3 and TbF3, as heavy rare earth sources, diffuse along the grain boundaries to form an epitaxial hard magnetic shell to improve coercivity; TiN, SiC, and Al2O3 ceramic phases improve the chemical stability of grain boundaries, uniform electrode potential, and block corrosion channels; Cu and Mg nano-metal phases form a liquid phase in the early stage of sintering, improve the wettability between the ceramic phase and the grain boundary phase, and promote their uniform spreading; Ga2O3 optimizes the triangular grain boundary phase composition to enhance magnetic decoupling; ZrB2, as a high melting point skeleton, supports the three-dimensional grain boundary network and prevents direct contact between grains. This synergistic effect is not a simple superposition of the effects of individual components: the metallic phase improves the wettability of the ceramic phase, preventing it from agglomerating; the diffusion of heavy rare earth elements alters grain boundary energy, promoting the segregation of the ceramic phase; and the ceramic phase, in turn, regulates the diffusion rate of heavy rare earth elements, causing them to remain on the grain surface and form a uniform shell. Experiments show that the nine-component composite additive enables H... cj While improving efficiency, the salt spray rust formation time was extended by more than four times, achieving unexpected technical results.
[0033] (4) This invention integrates and optimizes the entire process from batching to heat treatment, establishing a full-process oxygen content control system. The oxygen content of the protective gas is controlled to be <50ppm and <100ppm, and the dew point is controlled to be <-60℃, respectively, to reduce rare earth oxidation and avoid the formation of soft magnetic oxide inclusions at grain boundaries. The rapid solidification casting sheet obtains high-quality casting sheets with grain size of 3~8μm, uniform composition, and no α-Fe precipitation by precisely controlling the melting temperature, casting temperature, and copper roller linear speed. The composite additive is added by using the in-situ coating process of air jet milling. The impact and shearing effect of high-speed airflow is used to achieve uniform dispersion and mechanical coating of nano-additives on the surface of magnetic powder while crushing magnetic powder, solving the problems of easy agglomeration of nano-additives and uneven mixing with magnetic powder. Cold isostatic pressing is added after molding to improve the uniformity of green compact density and reduce sintering deformation. The process employs vacuum segmented sintering, argon forced cooling, and two-stage tempering to precisely control the heating rate, holding temperature, and cooling rate. This ensures that densification, grain boundary reactions, element diffusion, and grain boundary structure evolution are synergistically matched, resulting in a magnet density of over 99%. This provides thermodynamic and kinetic conditions for uniform grain boundary distribution and core-shell structure formation. The magnet exhibits uniform structure, good batch stability, and is suitable for large-scale industrial production.
[0034] (5) The preparation method of the present invention can be directly implemented on the existing sintered NdFeB production line without the need for additional special equipment. Only the composite additive preparation process needs to be added and the process parameters optimized. The raw materials for the composite additive are readily available and the preparation is simple. Compared with surface coating treatment, the present invention improves corrosion resistance from the material composition and microstructure. It does not have inherent defects such as pinholes in the coating, insufficient bonding force, incomplete coverage of edges and corners, or processing damage. After the magnet is machined by wire cutting, grinding, drilling, etc., the freshly exposed surface still has the same intrinsic corrosion resistance as the interior, and the processed parts do not become weak points for corrosion. Compared with the existing grain boundary diffusion process, the present invention is not limited by the size and shape of the magnet. It can obtain uniform internal and external performance for large-sized square, cylindrical, tile-shaped, and irregularly shaped magnets. It also eliminates multiple processes such as surface coating, high-temperature diffusion, cleaning, and fine grinding, which can shorten the production cycle. In summary, although it increases the cost of additives by a small amount, the utilization efficiency of heavy rare earth elements is improved, the production process is shortened, and the yield is increased. The overall cost is lower than that of the existing process, making it suitable for large-scale industrial application. Attached Figure Description
[0035] Figure 1 This is a schematic diagram of the overall process flow for the preparation method of high-performance corrosion-resistant heavy rare earth-rich permanent magnet materials of the present invention.
[0036] Figure 2 This is a schematic diagram of the five-step preparation process of the nanocrystalline boundary regulating composite additive of the present invention.
[0037] Figure 3 This is a scanning electron microscope backscattered (BSE) microstructure image of the heavy rare earth-rich permanent magnet material prepared in Example 1 of the present invention;
[0038] Figure 4 The graph shows the trend of sintering temperature affecting the relative density, density, remanence, and maximum energy product of the magnet.
[0039] Figure 5 This is a graph showing the changing trend of the effect of the secondary tempering temperature on the coercivity and corrosion current density of the magnet.
[0040] Figure 6 A graph showing the changing trend of the effect of the amount of nano-grain boundary controlled composite additive on the magnetic properties and salt spray corrosion resistance of the magnet.
[0041] Figure 7 For air-jet milled fine powder particle size D 50 A graph showing the changing trends of the effects on magnet coercivity, magnet oxygen content, and PCT100h mass loss.
[0042] Figure 8 This is a graph showing the changing trend of the effect of high-energy ball milling time on the particle size of composite additives and the coercivity of magnets.
[0043] Figure 9This is a graph showing the trend of the effect of the first-stage tempering temperature on the bending strength and coercivity of the magnet.
[0044] Figure 10 This is a graph showing the changing trend of the influence of the orientation magnetic field strength on the orientation degree and magnetic properties of the magnet.
[0045] Figure 11 Comparison diagram of remanence between the embodiment and the comparative example;
[0046] Figure 12 A comparison diagram of coercivity between the embodiments and comparative examples;
[0047] Figure 13 This is a comparison chart of the maximum magnetic energy product between the embodiment and the comparative example;
[0048] Figure 14 This is a comparison graph of corrosion current density between the examples and the comparative examples;
[0049] Figure 15 This is a comparison chart of salt spray rust formation time for the examples and comparative examples;
[0050] Figure 16 This is a comparison diagram of the bending strength of the embodiment and the comparative example. Detailed Implementation
[0051] To further illustrate the technical means and effects of the present invention, the following description, in conjunction with embodiments of the present invention, further explains the technical solution of the present invention. However, the present invention is not limited to the scope of the embodiments. The following description, in conjunction with the process flow diagram of the present invention (see...), further illustrates the technical solution of the present invention. Figure 1 and Figure 2 The specific embodiments will be described in detail below.
[0052] A method for preparing a high-performance, corrosion-resistant, heavy rare-earth-rich permanent magnet material includes the following steps:
[0053] (1) Raw material preparation: Weigh the following by weight percentage: praseodymium-neodymium alloy (Pr:Nd=25:75, purity ≥99.5%) 22~27wt%, dysprosium-iron alloy (Dy80wt, purity ≥99.5%) 5~8wt%, metallic terbium (purity ≥99.9%) 1.2~3wt%, boron-iron alloy (B20wt%) 0.9~1.2wt%, metallic cobalt (purity ≥99.9%) 1~3wt%, metallic aluminum (purity ≥99.9%) 0 0.3~0.8wt%, metallic copper (purity ≥99.9%) 0.1~0.4wt%, metallic gallium (purity ≥99.9%) 0.1~0.3wt%, metallic zirconium (purity ≥99.9%) 0.05~0.2wt%, metallic niobium (purity ≥99.9%) 0.05~0.2wt%, with industrial pure iron (purity ≥99.9%, C / N / O ≤0.05wt%) as the balance; heavy rare earth elements account for 15~30% of the total rare earth element mass.
[0054] (2) Preparation of nano-grain boundary regulation composite additives: Weigh the following nano-powders with an initial particle size of 20~50nm and a purity of ≥99.9% by weight: 15~25 parts of nano-dysprosium oxide, 10~20 parts of nano-terbium fluoride, 8~15 parts of nano-titanium nitride, 5~12 parts of nano-silicon carbide, 5~10 parts of nano-alumina, 3~8 parts of nano-copper powder, 2~6 parts of nano-magnesium powder, 2~5 parts of nano-gallium oxide, and 1~3 parts of nano-zirconium boride. Each nanoparticle was separately placed in anhydrous ethanol and ultrasonically dispersed at 300-500W for 20-40 min; after mixing, 0.5-1.5% of polyethylene glycol 4000 was added according to the total mass of the powder, and the mixture was stirred at 800-1200rpm for 30-60 min; vacuum dried at 60-100℃ for 10-15 h; stainless steel balls with a diameter of 5 mm and 10 mm (mass ratio 1:1) were added at a ball-to-particle ratio of (15-25):1, and the mixture was vacuumed to 1×10⁻⁶. -3 After Pa, the mixture is protected by argon gas and ball-milled at 300-500 rpm for 8-15 hours; then vacuum heat-treated at 400-500℃ for 1-3 hours, cooled under high-purity nitrogen protection, and passed through a 300-mesh sieve to obtain a composite additive with an average particle size of 50-150 nm.
[0055] (3) Rapid solidification casting: Place the raw material in a magnesium oxide crucible and evacuate it to 5×10 in a vacuum induction rapid solidification furnace. -3 The material is melted at 1450~1550℃ below Pa, refined for 5~15 min, and the electromagnetic stirring frequency is 2~5Hz. It is then cast into a copper roller at 1380~1450℃ with a copper roller linear speed of 1.5~3.0m / s to obtain a rapidly solidified sheet with a thickness of 0.2~0.5mm. The main phase grain size of the sheet is 2~8μm, and no α-Fe soft magnetic phase precipitation occurs.
[0056] (4) Hydrogen crushing: The cast sheet is loaded into the hydrogen crushing furnace and vacuumed to 1×10 -2 Below Pa, 99.999% high-purity hydrogen is introduced at room temperature to 0.08~0.15 MPa, and hydrogen is absorbed for 1.5~2.5 h; vacuum is applied and the temperature is raised to 500~600℃ to remove hydrogen for 2~4 h, and then cooled under argon protection to obtain coarse powder with an average particle size of 150~300 μm and a hydrogen content ≤500 ppm.
[0057] (5) In-situ coating by air jet mill: The coarse powder and composite additive are added to the air jet mill at a mass ratio of (98.5~99.5):(0.5~1.5), under nitrogen protection, with the system oxygen content <50ppm, dew point <-60℃, grinding pressure 0.5~0.7MPa, and sorting wheel speed 3500~4500rpm to obtain D 50 It is a fine powder with a particle size of 2.8~3.2μm and an oxygen content of ≤1500ppm.
[0058] (6) Low-oxygen molding: The fine powder is fed into a magnetic field press under nitrogen protection. The ambient oxygen content is <100ppm. It is molded at 150~250MPa under an orientation magnetic field of 1.8~2.5T for 10~30s. After demolding, it is vacuum sealed and cold isostatically pressed at 150~250MPa for 60~120s to obtain a density of 3.8~4.2g / cm³. 3 The raw clay.
[0059] (7) Vacuum segmented sintering and two-stage tempering: The green billets are fed into a vacuum sintering furnace with a vacuum degree better than 5×10 -3 The process involves heating the material to 800℃ at a rate of 5-10℃ / min and holding it for 1-2 hours for degassing; heating it to 1050-1100℃ at a rate of 3-5℃ / min and holding it for 3-5 hours for sintering; then charging it with 0.08-0.12MPa of high-purity argon gas for forced cooling to room temperature; reheating it to 850-950℃ and holding it for 2-4 hours for primary tempering, followed by rapid cooling with argon; and then holding it at 450-550℃ for secondary tempering, followed by furnace cooling to obtain a high-performance, corrosion-resistant, heavy rare-earth-rich permanent magnet material.
[0060] Technical principle of this invention:
[0061] 1. The role of each raw material in the permanent magnet matrix and the synergistic mechanism of multiple elements
[0062] The matrix composition of this invention follows the principle of "main phase optimization – grain boundary regulation – impurity suppression – multi-performance synergy". Praseodymium-neodymium alloy (Pr:Nd=25:75) forms (Pr,Nd)2Fe with Fe and B. 14 B is the main phase and the primary source of magnetic energy product; Dy (using a dysprosium-iron alloy containing 80% Dy) and Tb (metallic state) work together to improve coercivity, controlling the proportion of heavy rare earth elements to 15-30% of the total rare earth elements. Fe is the balance (purity ≥99.9%, C / N / O ≤0.05%); B (using a boron-iron alloy containing 20% B) stabilizes Nd2Fe. 14 The boron tetragonal structure is controlled at around 0.9-1.2% to avoid a boron-rich soft magnetic phase. Co partially replaces Fe to increase the Curie temperature and grain boundary potential, with a dosage of 1-3%. Al segregates at grain boundaries to increase potential and improve wettability. Cu forms a low-melting-point eutectic with RE to promote liquid phase spreading. Ga forms a RE-Fe-Ga nonmagnetic grain boundary phase to enhance magnetic decoupling. Zr and Nb form high-melting-point borides with B to refine grains and pin grain boundaries to inhibit abnormal growth. Co, Al, Cu, and Ga synergistically optimize grain boundary electrochemistry and wettability, Zr and Nb synergistically refine the microstructure, and Dy and Tb form an epitaxial shell with the assistance of additives. This multi-element synergy lays the foundation for high-performance magnets.
[0063] 2. The role of each raw material in the compound additive and the synergistic mechanism of multiple components
[0064] In the nine-component nanocomposite additive, Dy₂O₃ and TbF₃ serve as heavy rare earth donors, slowly diffusing along grain boundaries to form (Pr,Nd,Dy,Tb)₂Fe. 14 The B-phase epitaxial hard magnetic shell and TbF3 release trace amounts of F to improve grain boundary wettability; TiN and SiC are highly chemically stable ceramic phases that increase grain boundary potential, reduce corrosion current, and pin grain boundaries to improve flexural strength; Al2O3 reacts with rare earth oxides to form a dense aluminate passivation layer that blocks corrosion channels; Cu melts in the early stages of sintering to form a liquid phase, improving the wettability between the ceramic phase and grain boundaries and smoothing the grain boundaries; Mg is reduced to purify the grain boundaries; Ga2O3 optimizes the triangular grain boundary phase composition, promoting the formation of non-magnetic grain boundaries to enhance magnetic decoupling; ZrB2 is a high-melting-point grain boundary framework that supports a three-dimensional network to prevent direct grain contact. The nine components are uniformly mixed at the nanoscale through a five-step wet process. The Cu and Mg liquid phases promote ceramic phase dispersion, heavy rare earth diffusion promotes ceramic phase segregation, and the ceramic phase slows down heavy rare earth diffusion, causing it to remain on the grain surface to form a uniform shell, producing a nonlinear synergistic effect that simultaneously improves coercivity and corrosion resistance.
[0065] 3. Selection criteria and synergistic control mechanism of key process parameters
[0066] All key process parameters in this invention have clear physical and metallurgical basis. In the preparation of the composite additive, ultrasonic dispersion breaks up the initial soft agglomerates of nanoparticles; PEG4000 at 0.5-1.5% provides steric hindrance to prevent re-agglomeration; high-energy ball milling breaks up hard agglomerates with appropriate energy while avoiding wear and cold welding; vacuum heat treatment at 400-500℃ removes the dispersant and eliminates stress. The rapid solidification casting process controls the copper roller linear speed at 1.5-3.0 m / s to prevent α-Fe precipitation or excessively thick amorphous layers; the melting temperature at 1450-1550℃ balances sufficient melting with suppression of rare earth volatilization. Hydrogen breakage controls the hydrogen absorption pressure at 0.08-0.15 MPa and the dehydrogenation temperature at 500-600℃ to ensure intergranular fracture and avoid ultrafine powder and residual hydrogen. The air jet mill then... 50 The grain size is controlled within the range of 2.8~3.2μm to balance the grain size and oxygen content. Forming employs an orientation magnetic field of over 1.8T to ensure high orientation, and cold isostatic pressing eliminates density gradients. Sintering involves degassing at 800℃, densification at 1050~1100℃, and forced argon cooling, combined with a primary tempering at 850~950℃ to repair grain boundaries and a secondary tempering at 450~550℃ to regulate the nanostructure, achieving a synergistic match between densification, grain boundary reactions, and element diffusion.
[0067] 4. Principle Analysis of Achieving Unexpected Technical Effects
[0068] Existing technologies generally believe that adding non-metallic ceramic phases to grain boundaries worsens wettability and hinders densification, and that heavy rare earth compounds increase grain boundary chemical inhomogeneity. However, this invention has found that these problems can be overcome through nano-sizing and multi-component synergy: nano-Cu and Mg form low-melting-point liquid phases in the early stages of sintering, significantly improving the wettability between the ceramic phase and the grain boundary phase, allowing the ceramic phase to spread uniformly rather than agglomerate; the nano-ceramic phase inhibits abnormal grain growth by pinning grain boundaries, promoting uniform densification, and achieving a magnet relative density of over 99.5%. Simultaneously, after heavy rare earth compounds are combined with the ceramic and metallic phases at the nanoscale, Dy and Tb diffuse along the grain boundaries to form a continuous compositional gradient shell rather than isolated oxide particles, resulting in a uniform gradient distribution of grain boundary potential and reducing localized nano-corrosion microcells; the continuous ceramic network blocks corrosion channels, significantly improving corrosion resistance. This "uniform gradient core-shell + continuous ceramic network" structure relies on the precise proportioning of nine components and the synergistic control of the entire process. Each component works in conjunction with the others to produce nonlinear synergistic enhancement, achieving technical effects that are difficult for those skilled in the art to anticipate.
[0069] To make the present invention more fully disclosed, more specific embodiments are described below:
[0070] Example 1
[0071] A method for preparing a high-performance, corrosion-resistant, heavy rare-earth-rich permanent magnet material includes the following steps:
[0072] (1) Precise formulation of raw materials: 25wt% praseodymium-neodymium alloy (Pr:Nd=25:75, purity 99.5%), 6wt% dysprosium-iron alloy (Dy80wt%, balance Fe, purity 99.5%), 2wt% terbium (purity 99.9%), 62.85wt% industrial pure iron (purity 99.9%), 1.05wt% ferroboron alloy (B20wt%, balance Fe), 2wt% cobalt (purity 99.9%), 0.5wt% aluminum (purity 99.9%), 0.2wt% copper (purity 99.9%), 0.2wt% gallium (purity 99.9%), 0.1wt% zirconium (purity 99.9%), and 0.1wt% niobium (purity 99.9%).
[0073] (2) Preparation of nano-grain boundary regulation composite additives: Weigh each nano-material (initial particle size 30nm, purity 99.9%) by weight: 20 parts of nano-dysprosium oxide, 15 parts of nano-terbium fluoride, 12 parts of nano-titanium nitride, 8 parts of nano-silicon carbide, 7 parts of nano-alumina, 5 parts of nano-copper powder, 4 parts of nano-magnesium powder, 3 parts of nano-gallium oxide, and 2 parts of nano-zirconium boride. The nine nanopowders were placed separately into beakers containing anhydrous ethanol and ultrasonically dispersed for 30 min at 400 W to obtain uniform single-component suspensions. The suspensions were then mixed according to the specified ratio, and 1% (by weight) of polyethylene glycol 4000 was added as a dispersant. The mixture was stirred at 1000 rpm for 45 min in a high-speed stirrer to obtain a uniformly mixed composite slurry. The slurry was placed in a vacuum drying oven and vacuum dried at 80°C for 12 h to completely remove the anhydrous ethanol, resulting in a loose mixed powder. The dried mixed powder was then loaded into a stainless steel ball mill jar, and stainless steel grinding balls with diameters of 5 mm and 10 mm (mass ratio 1:1) were added, resulting in a ball-to-powder ratio of 20:1. The jar was then evacuated to a vacuum level of 1 × 10⁻⁶. -3 After Pa, the powder was purged with 0.08 MPa high-purity argon gas for protection and ball-milled at 400 rpm for 12 hours. After ball milling, the powder was removed under argon protection and placed in a vacuum heat treatment furnace, where it was held at 450℃ for 2 hours with a vacuum degree better than 1×10⁻⁶. -2 After heat treatment, the material was rapidly cooled to room temperature under high-purity nitrogen protection and passed through a 300-mesh nylon sieve to obtain a nanocrystalline boundary regulating composite additive with an average particle size of about 100 nm.
[0074] (3) Preparation of rapid solidification casting sheets: The prepared permanent magnet material raw materials are placed in a magnesium oxide crucible, loaded into a vacuum induction rapid solidification casting sheet furnace, and evacuated to 5×10⁻⁶. -3 Below Pa, the raw material is heated to 1500℃ to completely melt it. It is then refined for 10 minutes. During the refining process, a 3Hz electromagnetic stirring is applied to ensure uniform composition. The temperature of the alloy liquid is adjusted to 1420℃ for casting. The molten metal is poured through an intermediate ladle onto the surface of a water-cooled copper roller with a rotation speed of 2.0m / s. Rapid cooling is then performed to obtain a fast-solidifying casting sheet with a thickness of 0.25~0.35mm.
[0075] (4) Hydrogen decomposition: The rapidly solidified casting sheet is loaded into a stainless steel hydrogen decomposition furnace and vacuumed to 1×10⁻⁶. -2 Below Pa, high-purity hydrogen gas with a purity of 99.999% was introduced to a pressure of 0.1 MPa at room temperature. The gas valve was closed and the casting was allowed to stand for 2 hours to allow the casting to fully absorb hydrogen and become embrittled. Then, a vacuum was drawn and the temperature was increased to 550℃ at 5℃ / min and held for 3 hours to fully remove hydrogen. After the hydrogen removal was completed, high-purity argon gas was introduced for protective cooling to room temperature. The hydrogen fragments were taken out and passed through a 50-mesh sieve to obtain coarse powder with an average particle size of about 200 μm. The hydrogen content of the coarse powder was tested to be 320 ppm.
[0076] (5) In-situ coating by air jet milling: The coarse powder and the prepared nano-grain boundary regulating composite additive were added to the feed hopper of the air jet mill at a mass ratio of 99:1. The nitrogen protection system was turned on to control the oxygen content in the system to be below 30ppm, the dew point to be below -60℃, the pulverizing pressure to be 0.6MPa, and the sorting wheel speed to be 4000rpm. Closed-loop air jet milling was carried out. The fine powder obtained was detected by a laser particle size analyzer. 50 The particle size is 3.0 μm, and the oxygen content of the fine powder is 1200 ppm.
[0077] (6) Low-oxygen molding: Fine powder is fed into the mold cavity of a closed magnetic field molding press under nitrogen protection. The oxygen content in the nitrogen-protected environment is below 80ppm throughout the process. First, a 2.0T DC orientation magnetic field is applied to make the easily magnetized powder particles neatly aligned along the direction of the magnetic field. Then, while maintaining the magnetic field, a pressure of 200MPa is applied and held for 20s for vertical molding. After demolding, the compact is quickly vacuum-sealed with plastic film and placed in a cold isostatic press. It is held at 200MPa for 90s for isostatic pressing to obtain a cylindrical green compact with dimensions of Φ20×30mm and a green compact density of 4.0g / cm³. 3 .
[0078] (7) Segmented sintering: The green billets are stacked in a molybdenum sintering box and sent into a high-vacuum sintering furnace, where a vacuum of 3×10⁻⁶ is applied. -3 Below Pa, the powder is heated to 800℃ at a heating rate of 8℃ / min and held for 1.5h for degassing to remove adsorbed gases and residual lubricant. Then, it is sintered by heating to 1080℃ at a rate of 4℃ / min and holding for 4h, maintaining a vacuum level better than 5×10⁻⁶ during the sintering process. -3 Pa; immediately after sintering, purge with 0.1 MPa of high-purity argon gas and start the fan to rapidly quench and cool the magnet to room temperature;
[0079] (8) Two-stage tempering heat treatment: The sintered magnet is reheated to 900℃ and held for 3 hours for the first stage of tempering. After being rapidly cooled to room temperature by argon gas, it is then heated to 500℃ and held for 4 hours for the second stage of tempering. Finally, it is naturally cooled to room temperature with the furnace and the magnet is taken out for surface cleaning and performance testing.
[0080] The magnet prepared in Example 1 was tested, and the results are as follows: Figure 3 As shown. By Figure 3It can be seen that: (1) In the magnet obtained by the present invention, the rare earth-rich phase is mainly distributed at the grain boundaries of the main phase, forming a grain boundary isolation layer. This grain boundary phase can effectively isolate the magnetic exchange coupling between adjacent main phase grains, which is beneficial to improving the coercivity of the permanent magnet material. (2) The rare earth-rich phase does not undergo large-scale agglomeration, but is uniformly distributed in a fine network / island shape at the grain boundaries, indicating that the process of this embodiment can effectively enrich heavy rare earth elements at the grain boundaries, avoid local agglomeration of heavy rare earth, and is beneficial to taking into account both high coercivity and remanence. (3) The material has few internal pores, indicating that the magnet has high sintering density, which is beneficial to obtaining excellent magnetic and mechanical properties.
[0081] Example 2
[0082] A method for preparing a high-performance, corrosion-resistant, heavy rare-earth-rich permanent magnet material includes the following steps:
[0083] This embodiment prepares a high-coercivity, high-performance, corrosion-resistant, heavy rare-earth-rich permanent magnet material with the following raw material ratio: praseodymium-neodymium alloy 22wt%, dysprosium-iron alloy 8wt%, terbium metal 3wt%, industrial pure iron 60.95wt%, ferroboron alloy 1.2wt%, cobalt metal 3wt%, aluminum metal 0.8wt%, copper metal 0.4wt%, gallium metal 0.3wt%, zirconium metal 0.15wt%, and niobium metal 0.2wt%.
[0084] The raw material ratio for preparing the nano-grain boundary regulation composite additive was as follows: 25 parts nano-dysprosium oxide, 20 parts nano-terbium fluoride, 15 parts nano-titanium nitride, 12 parts nano-silicon carbide, 10 parts nano-alumina, 8 parts nano-copper powder, 6 parts nano-magnesium powder, 5 parts nano-gallium oxide, and 3 parts nano-zirconium boride. During the preparation of the composite additive, polyethylene glycol 4000 was added at 1.5% of the total powder mass, and the mixture was stirred at 1200 rpm for 60 min; high-energy ball milling was performed at a ball-to-particle ratio of 25:1 at 500 rpm for 15 h; and vacuum heat treatment was performed at 500℃ for 3 h. The average particle size of the obtained composite additive was approximately 80 nm.
[0085] Preparation of rapidly solidified cast sheets: melting temperature 1550℃, refining for 15min, electromagnetic stirring frequency 5Hz, casting temperature 1450℃, copper roller linear speed 3.0m / s, casting sheet thickness 0.2~0.3mm, grain size 2~5μm.
[0086] Hydrogen crushing process: hydrogen pressure 0.15MPa, hydrogen absorption time 2.5h, dehydrogenation temperature 600℃, heat preservation for 4h, coarse powder average particle size about 150μm, hydrogen content 280ppm.
[0087] Airflow milling process: coarse powder to composite additive mass ratio 98.5:1.5, grinding pressure 0.7MPa, sorting wheel speed 4500rpm, system oxygen content controlled below 40ppm, fine powder D50 It has a diameter of 2.8 μm and an oxygen content of 1350 ppm.
[0088] Molding process: Orientation magnetic field strength 2.5T, molding pressure 250MPa, holding pressure 30s; cold isostatic pressing pressure 250MPa, holding pressure 120s; ambient oxygen content controlled below 100ppm, green body density 4.2g / cm³ 3 .
[0089] Sintering and heat treatment process: Degassing at 800℃ for 2 hours, sintering at 1100℃ for 5 hours; first-stage tempering at 950℃ for 4 hours, second-stage tempering at 550℃ for 5 hours. The remaining process steps are the same as in Example 1.
[0090] Example 3
[0091] A method for preparing a high-performance, corrosion-resistant, heavy rare-earth-rich permanent magnet material includes the following steps:
[0092] This embodiment prepares a high-energy-product type high-performance corrosion-resistant heavy rare-earth-rich permanent magnet material with the following raw material ratio: praseodymium-neodymium alloy 27wt%, dysprosium-iron alloy 5wt%, terbium metal 1.2wt%, industrial pure iron 64.3wt%, ferroboron alloy 0.9wt%, cobalt metal 1wt%, aluminum metal 0.3wt%, copper metal 0.1wt%, gallium metal 0.1wt%, zirconium metal 0.05wt%, and niobium metal 0.05wt%.
[0093] The raw material ratio for preparing the nano-grain boundary regulation composite additive is as follows: 15 parts nano-dysprosium oxide, 10 parts nano-terbium fluoride, 8 parts nano-titanium nitride, 5 parts nano-silicon carbide, 5 parts nano-alumina, 3 parts nano-copper powder, 2 parts nano-magnesium powder, 2 parts nano-gallium oxide, and 1 part nano-zirconium boride. During the preparation of the composite additive, polyethylene glycol 4000 was added at 0.5% of the total powder mass, and the mixture was stirred at 800 rpm for 30 min; high-energy ball milling was performed at a ball-to-particle ratio of 15:1 at 300 rpm for 8 h; and vacuum heat treatment was performed at 400℃ for 1 h. The average particle size of the obtained composite additive was approximately 150 nm.
[0094] Preparation of rapid solidification castings: melting temperature 1450℃, refining for 5 min, electromagnetic stirring frequency 2 Hz, casting temperature 1380℃, copper roller linear speed 1.5 m / s, casting thickness 0.4~0.5 mm, grain size 5~8 μm.
[0095] Hydrogen crushing process: hydrogen pressure 0.08MPa, hydrogen absorption time 1.5h, dehydrogenation temperature 500℃, heat preservation for 2h, coarse powder average particle size about 300μm, hydrogen content 420ppm.
[0096] Airflow milling process: coarse powder to composite additive mass ratio 99.5:0.5, grinding pressure 0.5MPa, sorting wheel speed 3500rpm, system oxygen content controlled below 20ppm, fine powder D 50 It has a diameter of 3.2 μm and an oxygen content of 1050 ppm.
[0097] Molding process: Orientation magnetic field strength 1.8T, molding pressure 150MPa, holding pressure 10s; cold isostatic pressing pressure 150MPa, holding pressure 60s; ambient oxygen content controlled below 50ppm, green density 3.8g / cm³ 3 .
[0098] Sintering and heat treatment process: Degassing at 800℃ for 1 hour, sintering at 1050℃ for 3 hours; first-stage tempering at 850℃ for 2 hours, second-stage tempering at 450℃ for 3 hours. The remaining process steps are the same as in Example 1.
[0099] Example 4
[0100] A method for preparing a high-performance, corrosion-resistant, heavy rare-earth-rich permanent magnet material includes the following steps:
[0101] This embodiment prepares a high-performance, corrosion-resistant, heavy rare-earth-rich permanent magnet material with balanced comprehensive performance. The raw material ratio is as follows: praseodymium-neodymium alloy 24wt%, dysprosium-iron alloy 7wt%, terbium metal 2.5wt%, industrial pure iron 62.7wt%, ferroboron alloy 1.0wt%, cobalt metal 1.5wt%, aluminum metal 0.6wt%, copper metal 0.25wt%, gallium metal 0.25wt%, zirconium metal 0.12wt%, and niobium metal 0.08wt%.
[0102] The raw material ratio for preparing the nano-grain boundary regulation composite additive was as follows: 22 parts nano-dysprosium oxide, 18 parts nano-terbium fluoride, 10 parts nano-titanium nitride, 10 parts nano-silicon carbide, 8 parts nano-alumina, 6 parts nano-copper powder, 3 parts nano-magnesium powder, 4 parts nano-gallium oxide, and 1.5 parts nano-zirconium boride. During the preparation of the composite additive, polyethylene glycol 4000 was added at 0.8% of the total powder mass. The mixture was stirred at 900 rpm for 40 min; then ball-milled at 350 rpm for 10 h with a ball-to-particle ratio of 18:1; and finally vacuum heat-treated at 420℃ for 1.5 h. The resulting composite additive had an average particle size of approximately 120 nm.
[0103] Preparation of rapidly solidified cast sheets: melting temperature 1480℃, refining for 8 min, electromagnetic stirring frequency 3 Hz, casting temperature 1400℃, copper roller linear speed 2.5 m / s, casting sheet thickness 0.25~0.35 mm, grain size 3~6 μm.
[0104] Hydrogen crushing process: hydrogen pressure 0.12MPa, hydrogen absorption time 2h, dehydrogenation temperature 580℃, heat preservation for 2.5h, coarse powder average particle size about 250μm, hydrogen content 350ppm.
[0105] Airflow milling process: coarse powder to composite additive mass ratio 99.2:0.8, grinding pressure 0.55MPa, sorting wheel speed 3800rpm, system oxygen content controlled below 30ppm, fine powder D 50 It has a diameter of 3.1 μm and an oxygen content of 1150 ppm.
[0106] Molding process: Orientation magnetic field strength 2.2T, molding pressure 180MPa, holding pressure 15s; cold isostatic pressing pressure 180MPa, holding pressure 80s; ambient oxygen content controlled below 70ppm, green density 3.9g / cm³ 3 .
[0107] Sintering and heat treatment process: degassing at 800℃ for 1.5h, sintering at 1060℃ for 3.5h; first-stage tempering at 880℃ for 2.5h, second-stage tempering at 480℃ for 3.5h. The remaining process steps are the same as in Example 1.
[0108] Example 5
[0109] A method for preparing a high-performance, corrosion-resistant, heavy rare-earth-rich permanent magnet material includes the following steps:
[0110] This embodiment prepares another high-performance, corrosion-resistant, heavy rare-earth-rich permanent magnet material with balanced comprehensive performance. The raw material ratio is as follows: praseodymium-neodymium alloy 26wt%, dysprosium-iron alloy 5wt%, terbium metal 1.8wt%, industrial pure iron 62.7wt%, ferroboron alloy 1.1wt%, cobalt metal 2.5wt%, aluminum metal 0.4wt%, copper metal 0.15wt%, gallium metal 0.15wt%, zirconium metal 0.08wt%, and niobium metal 0.12wt%.
[0111] The raw material ratio for preparing the nano-grain boundary regulation composite additive was as follows: 18 parts nano-dysprosium oxide, 12 parts nano-terbium fluoride, 14 parts nano-titanium nitride, 6 parts nano-silicon carbide, 6 parts nano-alumina, 4 parts nano-copper powder, 5 parts nano-magnesium powder, 2.5 parts nano-gallium oxide, and 2.5 parts nano-zirconium boride. During the preparation of the composite additive, polyethylene glycol 4000 was added at 1.2% of the total powder mass. The mixture was stirred at 1100 rpm for 50 min; high-energy ball milling was performed at a ball-to-particle ratio of 22:1 at 450 rpm for 13 h; and vacuum heat treatment was performed at 480℃ for 2.5 h. The resulting composite additive had an average particle size of approximately 90 nm.
[0112] Preparation of rapidly solidified casting sheets: melting temperature 1520℃, refining for 12min, electromagnetic stirring frequency 4Hz, casting temperature 1430℃, copper roller linear speed 1.8m / s, casting sheet thickness 0.3~0.4mm, grain size 4~7μm.
[0113] Hydrogen crushing process: hydrogen pressure 0.09MPa, hydrogen absorption time 1.8h, dehydrogenation temperature 520℃, heat preservation for 3.5h, coarse powder average particle size about 180μm, hydrogen content 300ppm.
[0114] Airflow milling process: coarse powder to composite additive mass ratio 98.8:1.2, grinding pressure 0.65MPa, sorting wheel speed 4200rpm, system oxygen content controlled below 35ppm, fine powder D 50 It has a diameter of 2.9 μm and an oxygen content of 1280 ppm.
[0115] Molding process: Orientation magnetic field strength 1.9T, molding pressure 220MPa, holding pressure 25s; cold isostatic pressing pressure 220MPa, holding pressure 100s; ambient oxygen content controlled below 90ppm, green density 4.1g / cm³ 3 .
[0116] Sintering and heat treatment process: Degassing at 800℃ for 2 hours, sintering at 1090℃ for 4.5 hours; first-stage tempering at 920℃ for 3.5 hours, second-stage tempering at 520℃ for 4.5 hours. The remaining process steps are the same as in Example 1.
[0117] Comparative Example 1
[0118] This comparative example uses a conventional process to prepare heavy rare earth-rich permanent magnet materials without adding the nano-grain boundary control composite additive of this invention. The raw material ratio is exactly the same as in Example 1. No composite additives are prepared or added during the preparation process. The rapid solidification casting, hydrogen crushing, air jet milling, molding, and sintering heat treatment processes are all the same as in Example 1, except that no additives are added during air jet milling, and cold isostatic pressing is performed after molding.
[0119] Comparative Example 2
[0120] In this comparative example, heavy rare earth-rich permanent magnet materials were prepared. The composite additive only contained nano-dysprosium oxide, without the other eight components. The amount of nano-dysprosium oxide added was 1% of the magnetic powder mass. The particle size and purity of nano-dysprosium oxide were the same as in Example 1. The remaining raw material ratios and preparation processes were exactly the same as in Example 1.
[0121] Comparative Example 3
[0122] In this comparative example, a heavy rare earth-rich permanent magnet material was prepared. The composite additive did not contain the three ceramic phase components of nano-titanium nitride, nano-silicon carbide, and nano-alumina. Instead, it only contained six components: nano-dysprosium oxide, nano-terbium fluoride, nano-copper powder, nano-magnesium powder, nano-gallium oxide, and nano-zirconium boride. The proportions of each component remained unchanged. The total amount of composite additive added was 1% of the mass of the magnetic powder. The preparation process of the composite additive was the same as in Example 1, and the proportions and preparation processes of the other raw materials were exactly the same as in Example 1.
[0123] Comparative Example 4
[0124] In this comparative example, a heavy rare earth-rich permanent magnet material was prepared. The composite additive did not contain the two metal phase components of nano copper powder and nano magnesium powder, but only seven components: nano dysprosium oxide, nano terbium fluoride, nano titanium nitride, nano silicon carbide, nano aluminum oxide, nano gallium oxide, and nano zirconium boride. The proportions of each component remained unchanged, and the total amount of composite additive added was 1% of the mass of the magnetic powder. The preparation process of the composite additive was the same as in Example 1, and the proportions and preparation processes of the other raw materials were exactly the same as in Example 1.
[0125] Comparative Example 5
[0126] In this comparative example, heavy rare earth-rich permanent magnet materials were prepared. The composite additive did not contain the nano-zirconium boride component, but only the other eight components were added. The proportions of each component remained unchanged. The total amount of composite additive added was 1% of the mass of the magnetic powder. The preparation process of the composite additive was the same as in Example 1, and the proportions and preparation processes of the other raw materials were exactly the same as in Example 1.
[0127] Comparative Example 6
[0128] In this comparative example, the composite additives for preparing heavy rare earth permanent magnet materials were prepared by dry mixing without wet ultrasonic dispersion, high-speed stirring and vacuum drying steps, or high-energy ball milling and vacuum heat treatment. The nine nanoparticles were directly mixed in a three-dimensional mixer at 200 rpm for 2 hours and then added. The amount added was 1% of the mass of the magnetic powder. The proportions of the remaining raw materials and the preparation process were exactly the same as in Example 1.
[0129] Comparative Example 7
[0130] In this comparative example, the preparation of heavy rare earth-rich permanent magnet materials adopted the traditional single-stage tempering heat treatment process. After sintering and argon cooling, the materials were directly tempered at 500°C for 4 hours without undergoing a first-stage high-temperature tempering treatment at 900°C. The remaining raw material ratios and preparation processes were exactly the same as in Example 1.
[0131] Single-factor experimental study of key process parameters:
[0132] To verify the scientific validity and rationality of the selection of key process parameters in this invention and to fully demonstrate the inventiveness of the invention, seven sets of single-factor comparative experiments on key process parameters were conducted based on Example 1. In each set of experiments, only one process parameter was changed, while all other parameters remained completely consistent with Example 1. The magnetic properties and corrosion resistance of the prepared magnets were systematically tested, and the physical mechanism of performance degradation when parameters deviate from the optimal value was analyzed in depth to determine the better range and optimal range of each parameter.
[0133] Single-factor experiment 1: Effect of sintering temperature on magnet performance
[0134] Comparative experiments were conducted at sintering temperatures of 1010℃, 1030℃, 1050℃, 1070℃, 1080℃, 1090℃, 1110℃, and 1130℃. The magnet density was tested using Archimedes' displacement method, and the room-temperature magnetic properties, including remanence (Br) and coercivity (H), were measured using an NIM-10000H automatic permanent magnet material measuring instrument. cj Maximum energy product (BH) max The experimental results are shown in Table 1 and Figure 4 As shown.
[0135] Table 1 Effect of sintering temperature on magnet properties
[0136]
[0137] As shown in Table 1, when the sintering temperature is below 1050℃, the sintering temperature is insufficient, resulting in a low amount of rare-earth-rich liquid phase with high viscosity. The densification process is incomplete, leading to numerous interconnected pores within the magnet, significantly reducing density and relative density. These pores not only reduce the volume fraction of the ferromagnetic main phase, causing a linear decrease in remanence, but also generate large local demagnetizing fields at the pore edges, becoming preferential nucleation sites for antimagnetizing domains, thus drastically reducing coercivity. Simultaneously, the interconnected pores become three-dimensional channels for the rapid diffusion of corrosive media, significantly worsening corrosion resistance. When the sintering temperature exceeds 1110℃, the excessive temperature leads to abnormal grain growth, with some main phase grains growing to over 10μm. Excessive volatilization of the grain boundary phase results in discontinuous grain boundary structures. The coarse grains are prone to dislocations and subgrain boundary defects, where antimagnetizing domains easily nucleate and rapidly expand, causing a sharp decrease in coercivity. Simultaneously, severe volatilization of rare-earth elements at high temperatures creates new pores within the magnet, further reducing magnetic properties. Figure 4 It can be seen that the density and Br content are within the range of 1070~1090℃. j All reached their peak values. Therefore, considering both magnet density and magnetic properties, the optimal range for sintering temperature was determined to be 1050~1110℃, with the optimal value being 1080℃.
[0138] Single-factor experiment 2: The effect of second-stage tempering temperature on magnet performance
[0139] Comparative experiments were conducted at secondary tempering temperatures of 410℃, 430℃, 450℃, 480℃, 500℃, 520℃, 550℃, and 570℃ to test the coercivity H of the magnet. cj The potentiodynamic polarization curves were tested using a PARSTAT 4000 electrochemical workstation in a 3.5 wt% NaCl solution to obtain the corrosion current density. The experimental results are shown in Table 2 and... Figure 5 As shown.
[0140] Table 2. Effect of Secondary Tempering Temperature on Magnet Performance
[0141]
[0142] As shown in Table 2, when the secondary tempering temperature is below 450℃, the atomic diffusion kinetic energy is insufficient, and the amplitude modulation decomposition and homogenization process of the grain boundary phase is incomplete. This prevents the formation of continuous, straight, non-magnetic thin-layer grain boundaries, and ferromagnetic exchange coupling exists between adjacent main phase grains, resulting in low coercivity. Simultaneously, the grain boundary phase distribution is uneven, with numerous micro-regions exhibiting drastic fluctuations in electrode potential, forming numerous nano-corrosion micro-cells with high corrosion current density and poor corrosion resistance. When the secondary tempering temperature exceeds 550℃, the excessive temperature leads to grain boundary phase aggregation and spheroidization, disrupting the continuous three-dimensional grain boundary network. Some main phase grains directly contact each other, resulting in exchange coupling and a decrease in coercivity. Furthermore, at high temperatures, the grain boundary phase undergoes compositional segregation, increasing electrochemical inhomogeneity, raising the corrosion current density, and deteriorating corrosion resistance. Figure 5 It can be seen that H cj The peak temperature is reached at 500℃, while Icorr reaches its trough at 500℃. Therefore, the preferred range for the secondary tempering temperature is determined to be 450~550℃, with the optimal value being 500℃.
[0143] Single-factor experiment 3: Effect of composite additive dosage on magnet performance
[0144] Comparative experiments were conducted with nanograin boundary control composite additives added at concentrations of 0%, 0.3%, 0.5%, 0.8%, 1.0%, 1.2%, 1.5%, and 1.8%, respectively, to test the remanence (Br) and coercivity (H) of the magnets. cj A neutral salt spray test (5wt% NaCl, 35℃) was conducted according to GB / T 46762-2025 standard. The time when the first red rust spot appeared on the surface of the bare magnet was recorded. The experimental results are shown in Table 3 and... Figure 6 As shown.
[0145] Table 3 Effect of Composite Additive Dosage on Magnet Performance
[0146]
[0147] As shown in Table 3, when the amount of composite additive is less than 0.5%, the addition is insufficient, and a continuous modified layer cannot be formed at all grain boundaries. Some grain boundaries remain unmodified original rare-earth-rich phases, and heavy rare-earth elements cannot form a complete core-shell structure on all grain surfaces, resulting in a limited improvement in coercivity. Simultaneously, the grain boundary network is discontinuous, failing to effectively block corrosion channels, and the improvement in corrosion resistance is not significant. When the amount of composite additive is greater than 1.5%, excessive non-magnetic additives enter the magnet, reducing the volume fraction of the ferromagnetic main phase, leading to a significant decrease in remanence. At the same time, excessive additives agglomerate at triangular grain boundaries, forming large impurity phase particles, disrupting the uniformity and continuity of the grain boundaries, becoming new demagnetizing domain nucleation centers and preferential corrosion areas, resulting in a simultaneous decrease in coercivity and corrosion resistance. Figure 6 It can be seen that when the addition amount is 1.0%, H cj Both the salt spray rust formation time and the optimal values were achieved. Therefore, the optimal range for the amount of composite additive was determined to be 0.5~1.5wt%, with an optimal value of 1.0wt%.
[0148] Single-factor experiment 4: Particle size D of air-jet milled powder 50 Impact on magnet performance
[0149] Select airflow milled fine powder D 50 Comparative experiments were conducted for magnets with diameters of 2.0 μm, 2.4 μm, 2.8 μm, 3.0 μm, 3.2 μm, 3.6 μm, 4.0 μm, and 4.5 μm to test the coercivity H of the magnets. cj The oxygen content of the magnet was tested using the inert gas pulsed infrared method. A high-pressure accelerated aging (PCT) test was conducted at 120℃, 2 atm, and 100% RH for 100 hours. The mass loss before and after the test was measured. The experimental results are shown in Table 4. Figure 7 As shown.
[0150] Table 4 Fine Particle Size D 50 Impact on magnet performance
[0151]
[0152] As can be seen from the analysis in Table 4, when fine powder D 50 When the particle size is less than 2.8 μm, the powder particle size is too fine, the specific surface area is too large, and the powder surface activity is extremely high. It is easily oxidized during powder preparation, molding, and sintering, leading to a significant increase in the oxygen content of the magnet. A large number of soft magnetic rare earth oxide impurities form at the grain boundaries, destroying the magnetic decoupling effect of the grain boundaries and resulting in a decrease in coercivity. Simultaneously, a large number of oxide inclusions are distributed at the grain boundaries, destroying the compactness of the grain boundaries. Corrosion is accelerated in the high-temperature, high-humidity, and high-pressure PCT test environment, leading to a significant increase in mass loss. When the fine powder D... 50When the particle size is greater than 3.2 μm, the powder particle size is too coarse, resulting in large grain size after sintering, with an average grain size exceeding 6 μm. This increases internal defects within the large grains, making it easier for antimagnetic domains to nucleate and rapidly expand, leading to a significant decrease in coercivity. Simultaneously, the coarse grains cause uneven distribution of the grain boundary phase, with some areas having excessively thick or thin grain boundaries, resulting in decreased corrosion resistance. Figure 7 It can be seen that D 50 H = 3.0 μm cj It has the highest PCT loss and the lowest overall performance, although its oxygen content is not the lowest. Therefore, the fine powder D is determined to be the best. 50 The optimal range is 2.8~3.2μm, and the optimal value is 3.0μm.
[0153] Single-factor experiment 5: Effect of high-energy ball milling time on the effect of composite additives
[0154] Comparative experiments were conducted using high-energy ball milling times of 2h, 4h, 6h, 8h, 12h, 15h, 18h, and 24h during the preparation of the composite additive. With a fixed ball-to-material ratio of 20:1 and a rotation speed of 400rpm, the average particle size of the prepared composite additive was measured using a laser particle size analyzer. Then, magnets were prepared according to the process in Example 1, and the coercivity H of the magnets was tested. cj The experimental results are shown in Table 5 and Figure 8 As shown.
[0155] Table 5. Effect of high-energy ball milling time on the effect of composite additives
[0156]
[0157] As shown in Table 5, when the high-energy ball milling time is less than 8 hours, the mechanical energy input is insufficient, the hard agglomerates of nanoparticles are not fully broken down, the average particle size of the composite additives is too large, and uniform nanoscale composites are not achieved among the nine components. Large additive particles are unevenly dispersed in the magnetic powder, and cannot spread uniformly at the grain boundaries during sintering, easily forming large inclusion defects, resulting in poor grain boundary control and insignificant improvement in coercivity. When the ball milling time exceeds 15 hours, excessively long milling leads to severe wear of the stainless steel grinding media, introducing a large amount of impurities such as iron and chromium. Simultaneously, excessively high milling energy causes cold welding agglomeration of nanoparticles, actually increasing the particle size. The entry of impurities into the grain boundaries disrupts the composition and magnetic structure of the grain boundary phase, leading to a decrease in magnetic properties. Combined with… Figure 8 It can be seen that the particle size of the additive first decreases rapidly with the extension of ball milling time and then tends to level off. cj It shows a trend of first rising and then falling, reaching a peak at 12 hours. Continuing to extend the ball milling time H cj Instead, it decreased. Therefore, the optimal range for high-energy ball milling time was determined to be 8–15 h, with the optimal value being 12 h.
[0158] Single-factor experiment 6: The effect of first-stage tempering temperature on magnet performance
[0159] Comparative experiments were conducted at first-stage tempering temperatures of 750℃, 800℃, 850℃, 880℃, 900℃, 930℃, 950℃, and 1000℃. The three-point bending strength and coercivity H of the magnets were tested according to GB / T 31967.1-2015 standard. cj The experimental results are shown in Table 6 and Figure 9 As shown.
[0160] Table 6. Effect of First-Stage Tempering Temperature on Magnet Performance
[0161]
[0162] As shown in Table 6, when the first-stage tempering temperature is below 850℃, the temperature is insufficient, and the grain boundary phase does not fully melt and flow, failing to effectively repair the grain boundary microcracks and defects generated during the quenching process after sintering. The weak bonding force between the grain boundaries and the main phase results in low bending strength of the magnet. Simultaneously, discontinuous grain boundary defects lead to ferromagnetic exchange coupling between adjacent main phase grains, resulting in low coercivity. When the first-stage tempering temperature is above 950℃, approaching the sintering temperature, the main phase grains begin to grow. Excessive volatilization of the grain boundary phase causes new pores at the grain boundaries, and abnormal grain growth leads to a decrease in coercivity. Simultaneously, at high temperatures, the grain boundary phase composition segregates, reducing the grain boundary bonding force and consequently decreasing the bending strength. Figure 9 It can be seen that the bending strength and H cj As the first-stage tempering temperature increases, both curves exhibit an inverted U-shaped trend, first rising and then falling, with both reaching their peaks simultaneously around 900℃. Therefore, the optimal range for the first-stage tempering temperature is determined to be 850~950℃, with the optimal value being 900℃.
[0163] Single-factor experiment 7: The effect of the forming orientation magnetic field strength on magnet performance
[0164] Comparative experiments were conducted using orientation magnetic field strengths of 1.0T, 1.4T, 1.8T, 2.0T, 2.2T, 2.5T, 2.8T, and 3.2T during the forming process. X-ray diffraction was used to test the orientation degree of the magnets, as well as the remanence (Br) and maximum energy product (BH). max The experimental results are shown in Table 7 and Figure 10 As shown.
[0165] Table 7. Effect of Orientation Magnetic Field Strength on Magnet Performance
[0166]
[0167] As shown in Table 7, when the orientation magnetic field strength is below 1.8T, the magnetic force is insufficient to overcome the frictional force and magnetic agglomeration force between powders, and the easily magnetized shafts cannot be fully oriented, resulting in an orientation degree of less than 94%, leading to (BH). max Significantly reduced. When the orientation magnetic field strength increases to above 2.5T, the orientation degree reaches 96.2% and then stops increasing, Br and (BH) max It also remains essentially unchanged. This is because, under compression molding conditions, some powder particles are mechanically interlocked by adjacent particles or locked by inter-powder friction during the pressing process. Even if the external magnetic field is further increased, these particles cannot be rotated; the orientation has reached the physical limit under these process conditions. Further increasing the magnetic field strength will only increase equipment investment and energy consumption, without making a substantial contribution to the magnetic properties. Figure 10 It is evident that the orientation and magnetic property curves tend to flatten out after 2.0T. Therefore, the optimal range for the orientation magnetic field strength is determined to be 1.8~2.5T, with the optimal value being 2.0T.
[0168] Magnet performance testing and comparative analysis:
[0169] The magnets prepared in Examples 1-5 and Comparative Examples 1-7 of this invention were subjected to comprehensive and systematic performance testing according to the latest national standards. All test samples underwent the same pretreatment: wire-cut into 10mm×10mm×10mm cubic specimens, the surface wire-cut alteration layer was removed by polishing with 2000# sandpaper, and the samples were ultrasonically cleaned in acetone and anhydrous ethanol for 10 minutes in sequence, dried with cold air, and placed in a desiccator for testing. The testing standards and methods used are as follows:
[0170] Room temperature magnetic property testing: Following GB / T 3217-2013 "Magnetic Test Methods for Permanent Magnet (Hard Magnetic) Materials", the room temperature demagnetization curve was tested using the NIM-10000H type automatic measuring device for permanent magnet materials from the National Institute of Metrology, China, to obtain the remanence (Br) and coercivity (H). cj Maximum energy product (BH) max .
[0171] High-temperature magnetic properties and temperature stability testing: The demagnetization curve at 120℃ was tested according to GB / T 40794-2021 "Test Method for Irreversible Flux Loss at High Temperature in Rare Earth Permanent Magnet Materials", and the coercivity temperature coefficient α(H) was calculated. cj ); Keep it in an oven at 120℃ for 100h, test the open-circuit magnetic flux before and after the heat preservation, and calculate the irreversible magnetic flux loss hirr.
[0172] Corrosion resistance testing: A neutral salt spray test was conducted according to GB / T 10125-2021 "Artificial Atmosphere Corrosion Test - Salt Spray Test," using a 5% sodium chloride solution at a test temperature of 35℃, with continuous spraying. The time when the first red rust spot appeared on the surface of the bare magnet sample was recorded. After a cumulative 200 hours of salt spray testing, the sample was removed, and salt deposits and corrosion products on the sample surface were cleaned. After drying, the sample mass was determined using an analytical balance, and the mass loss was calculated. A constant damp heat test at 85℃ and 85%RH for 300 hours was conducted according to GB / T 43489-2023 "Sintered NdFeB Permanent Magnets - Constant Damp Heat Test," testing the open-circuit magnetic flux loss before and after the test. Potentiodynamic polarization curves were tested using a PARSTAT 4000 electrochemical workstation. The test solution was a 3.5wt% NaCl solution, the reference electrode was a saturated calomel electrode, the auxiliary electrode was a platinum sheet, and the scan rate was 1mV / s to obtain the corrosion current density Icorr.
[0173] Mechanical property testing: Following GB / T 31967.1-2015 "Test Methods for Physical Properties of Rare Earth Permanent Magnet Materials", the bending strength of the magnet was tested using the three-point bending method, with a span of 14.5 mm and a pressure head movement speed of 0.1 mm / min. All performance test results are shown in Table 8 and... Figures 11-16 As shown.
[0174] Table 8. Comparison of overall performance of magnets in the examples and comparative examples
[0175]
[0176] From the system test results in Table 8 and Figures 11-16 It can be seen that the magnets prepared in Examples 1-5 of this invention have significantly better overall performance than all comparative examples. Comparative Example 1, prepared without composite additives using a traditional same-component process, although having remanence comparable to Example 1, exhibits a coercivity of only 15.3 kOe, 4.3 kOe lower than Example 1, and a corrosion current density as high as 15.8 μA / cm². 2 The rust formation time of 5wt% NaCl salt spray is only 48 hours, which is only 1 / 6 of that of Example 1. The bending strength is also 55 MPa lower. This fully demonstrates that the nano-grain boundary regulating composite additive of the present invention plays a decisive role in simultaneously improving coercivity, corrosion resistance and mechanical properties.
[0177] Comparative Example 2, which only added single nano-dysprosium oxide, showed a 2.3 kOe increase in coercivity compared to Comparative Example 1, but was still 2.0 kOe lower than Example 1, resulting in a very limited improvement in corrosion resistance. The corrosion current density remained as high as 12.3 μA / cm². 2 This indicates that a single heavy rare earth compound cannot achieve the synergistic enhancement effect of multiple components; a composite of nine components is necessary to simultaneously optimize magnetic properties and corrosion resistance.
[0178] Comparative Example 3, without the addition of the three nano-ceramic phases, showed a significant decrease in corrosion resistance compared to Example 1, with the corrosion current density increasing to 10.5 μA / cm². 2 The salt spray rust formation time was shortened to 96 hours, proving that nano-titanium nitride, silicon carbide, aluminum oxide and other ceramics play an irreplaceable role in improving the chemical stability of grain boundaries and blocking corrosion channels.
[0179] Comparative Example 4, without the addition of nano-copper powder and nano-magnesium powder, showed a decrease in corrosion resistance, coercivity, and remanence compared to Example 1. This indicates that nano-metals play an important role in improving wettability, promoting liquid phase sintering, and achieving uniform distribution of the ceramic phase. Without the assistance of the metal phase, the ceramic phase and heavy rare earth compounds cannot spread uniformly at the grain boundaries, resulting in a deterioration in densification and grain boundary control effects.
[0180] Comparative Example 5, without the addition of nano-zirconium boride, showed a decrease in both coercivity and corrosion resistance compared to Example 1, demonstrating that nano-zirconium boride, as a high-melting-point grain boundary framework, plays an important role in supporting the three-dimensional grain boundary network and preventing abnormal grain growth.
[0181] Comparative Example 6 uses a simple dry mixing method to prepare composite additives without wet dispersion and high-energy ball milling. The composite additives have poor dispersibility and a large number of agglomerated particles, resulting in poor grain boundary control. The magnetic properties, corrosion resistance and mechanical properties are far lower than those of Example 1. This proves that the five-step composite additive preparation process of the present invention is crucial for achieving uniform composites at the nanoscale.
[0182] Comparative Example 7 did not undergo a first-stage high-temperature tempering, but only a single-stage low-temperature tempering. As a result, the grain boundary defects could not be fully repaired, and the grain boundary structure was discontinuous. Consequently, the coercivity, corrosion resistance, and flexural strength were significantly lower than those of Example 1, demonstrating the necessity of a two-stage tempering heat treatment process for optimizing the grain boundary structure.
[0183] From a theoretical perspective, the fundamental reason why the technical solution of this invention can achieve such a significant improvement in comprehensive performance lies in the synergistic innovation of composition and process, which realizes the "three-fold" deep regulation of grain boundary structure: First, the homogenization of grain boundary composition, through the uniform dispersion of nanocomposite additives and in-situ solid-phase reaction, eliminates the compositional segregation and nanoscale potential fluctuations at the grain boundaries of traditional heavy rare earth magnets, reducing the number of grain boundary corrosion microcells by an order of magnitude; Second, the continuity of grain boundary structure, through optimized sintering and double-stage tempering processes, forms a continuous, dense, and uniformly thick three-dimensional grain boundary network, which effectively blocks the diffusion channels of corrosive media and enhances the magnetic decoupling effect between adjacent grains; Third, the integration of grain boundary functions, the grain boundary phase is no longer the traditional weak corrosion phase, but a reinforcing phase that integrates multiple functions such as hard magnetic shell reinforcement, corrosion resistance isolation, and interface bonding strengthening, fundamentally changing the role of grain boundaries.
[0184] The performance comparison between the examples shows that Example 2 has the highest amount of heavy rare earth elements, resulting in the highest coercivity (22.8 kOe) and the best corrosion resistance, but its remanence (12.7 kGs) is relatively low, making it suitable for applications with higher operating temperatures. Example 3 has the lowest amount of heavy rare earth elements, resulting in the highest remanence (13.4 kGs) and the highest magnetic energy product (43.8 MGOe), but its coercivity and corrosion resistance are relatively low, making it suitable for applications with lower operating temperatures. Examples 1, 4, and 5 are magnets with balanced overall performance, with coercivity between 18.5 and 20.7 kOe, exhibiting excellent overall performance and suitable for most new energy vehicle and wind power applications.
[0185] In summary, this invention, through a nine-component nano-grain boundary controlled composite additive and a fully integrated preparation process, solves the technical problems of low heavy rare earth utilization, poor intrinsic corrosion resistance, and difficulty in simultaneously improving magnetic properties and corrosion resistance in traditional heavy rare earth-rich permanent magnet materials. It overcomes the inherent perception that "high coercivity inevitably comes with low corrosion resistance," and the prepared magnet simultaneously possesses high magnetic properties, good temperature stability, intrinsic corrosion resistance, and mechanical properties. The process of this invention is controllable, requires no additional large-scale specialized equipment, and can be directly implemented on existing sintered NdFeB production lines. It is applicable to fields such as new energy vehicle drive motors, offshore wind turbines, high-speed traction motors, and high-end servo motors.
[0186] Those skilled in the art will recognize that numerous variations are possible with respect to the above description, and therefore the embodiments are merely illustrative of one or more specific implementations. Although exemplary embodiments considered to be part of the invention have been described and illustrated, those skilled in the art will understand that various changes and substitutions can be made thereto without departing from the spirit of the invention. Furthermore, many modifications can be made to adapt specific situations to the doctrine of the invention without departing from the central concepts of the invention described herein. Therefore, the invention is not limited to the specific embodiments disclosed herein, but may include all embodiments and equivalents that fall within the scope of the invention.
Claims
1. A method for preparing a high-performance, corrosion-resistant, heavy rare-earth-rich permanent magnet material, characterized in that, Includes the following steps: S1. Prepare the permanent magnet material raw materials according to the component ratio. The permanent magnet material raw materials include, by weight percentage: 22-27 wt% praseodymium-neodymium alloy, 5-8 wt% dysprosium-iron alloy, 1.2-3 wt% terbium metal, 0.9-1.2 wt% ferroboron alloy, 1-3 wt% cobalt metal, 0.3-0.8 wt% aluminum metal, 0.1-0.4 wt% copper metal, 0.1-0.3 wt% gallium metal, 0.05-0.2 wt% zirconium metal, 0.05-0.2 wt% niobium metal, with industrial pure iron as the balance; the heavy rare earth elements in the permanent magnet material account for 15-30 wt% of the total rare earth element mass. S2. Place the prepared permanent magnet material raw materials into a vacuum induction rapid solidification furnace for melting and casting to obtain rapid solidification casting sheets. S3. The rapid-solidifying cast sheets are subjected to hydrogen crushing treatment to prepare coarse powder; S4. The coarse powder and the nano-grain boundary regulating composite additive are mixed at a mass ratio of (98.5~99.5):(0.5~1.5) and then subjected to air jet milling to obtain fine powder; S5. Under the protection of inert gas, the fine powder is molded in an orientation magnetic field and then subjected to cold isostatic pressing to obtain a green body. S6. The green blank is sintered in vacuum in sections, followed by a two-stage tempering heat treatment to finally obtain a high-performance corrosion-resistant heavy rare earth-rich permanent magnet material.
2. The method for preparing high-performance corrosion-resistant heavy rare earth-rich permanent magnet material according to claim 1, characterized in that, The nano-grain boundary regulation composite additive comprises, by weight, the following raw materials: 15-25 parts of nano-dysprosium oxide, 10-20 parts of nano-terbium fluoride, 8-15 parts of nano-titanium nitride, 5-12 parts of nano-silicon carbide, 5-10 parts of nano-alumina, 3-8 parts of nano-copper powder, 2-6 parts of nano-magnesium powder, 2-5 parts of nano-gallium oxide, and 1-3 parts of nano-zirconium boride.
3. The method for preparing high-performance corrosion-resistant heavy rare earth-rich permanent magnet materials according to claim 2, characterized in that, The preparation method of the nanocrystalline boundary regulating composite additive is characterized by comprising the following steps: (1) Nano dysprosium oxide, nano terbium fluoride, nano titanium nitride, nano silicon carbide, nano aluminum oxide, nano copper powder, nano magnesium powder, nano gallium oxide, and nano zirconium boride were respectively placed in anhydrous ethanol and ultrasonically dispersed for 20 to 40 minutes at a power of 300 to 500 W to obtain a uniform suspension of each component. (2) Mix the suspensions of each component according to the ratio, add 0.5~1.5% of polyethylene glycol 4000 as a dispersant, and stir at high speed of 800~1200 rpm for 30~60 min to obtain a uniformly mixed slurry; (3) The mixed slurry is vacuum dried at 60~100℃ for 10~15h to obtain composite powder; (4) Place the composite powder in a high-energy ball mill jar, add grinding balls at a ball-to-material ratio of (15~25):1, the grinding balls are stainless steel balls with diameters of 5mm and 10mm and a mass ratio of 1:1, fill with argon gas for protection, and ball mill at a speed of 300~500rpm for 8~15h. (5) The ball-milled powder was vacuum heat-treated at 400~500℃ for 1~3h, then cooled to room temperature under high-purity nitrogen protection, and passed through a 300-mesh sieve to obtain a nano-grain boundary regulating composite additive with an average particle size of 50~150nm.
4. The method for preparing high-performance corrosion-resistant heavy rare earth-rich permanent magnet material according to claim 1, characterized in that, In step S1: the mass ratio of Pr to Nd in the praseodymium-neodymium alloy is 25:75, and the purity is not less than 99.5%; the mass content of Dy in the dysprosium-iron alloy is 80%, with the balance being Fe, and the purity is not less than 99.5%; the purity of metallic terbium, metallic cobalt, metallic aluminum, metallic copper, metallic gallium, metallic zirconium, and metallic niobium is not less than 99.9%; the mass content of B in the boron-iron alloy is 20%, with the balance being Fe; the purity of industrial pure iron is not less than 99.9%, and the total content of impurities C, N, and O is not higher than 0.05 wt%.
5. The method for preparing high-performance corrosion-resistant heavy rare earth-rich permanent magnet material according to claim 1, characterized in that, In step S2, the melting temperature of the vacuum induction rapid solidification furnace is 1450~1550℃, the refining time is 5~15min, and the electromagnetic stirring frequency during the refining process is 2~5Hz; the casting temperature is 1380~1450℃, the copper roller linear speed is 1.5~3.0m / s, the thickness of the obtained rapid solidification casting sheet is 0.2~0.5mm, the main phase grain size of the casting sheet is 2~8μm, and no α-Fe soft magnetic phase precipitation occurs.
6. The method for preparing high-performance corrosion-resistant heavy rare earth-rich permanent magnet material according to claim 1, characterized in that, The hydrogen crushing process in step S3 includes: evacuating to a vacuum of 1×10⁻⁶ at room temperature. -2 Below Pa, high-purity hydrogen gas with a purity of 99.999% is introduced to a pressure of 0.08~0.15MPa, and the mixture is allowed to stand for 1.5~2.5h to absorb hydrogen until saturation. Then, a vacuum is drawn and the temperature is raised to 500~600℃ for dehydrogenation treatment, and the temperature is maintained for 2~4h. After dehydrogenation, the mixture is cooled to room temperature under argon protection. The average particle size of the coarse powder after hydrogen crushing is 150~300μm, and the hydrogen content is not higher than 500ppm.
7. The method for preparing high-performance corrosion-resistant heavy rare earth-rich permanent magnet material according to claim 1, characterized in that, In step S4, the grinding pressure of the air jet mill is 0.5~0.7MPa, the sorting wheel speed is 3500~4500rpm, nitrogen protection is maintained throughout the air jet milling process, the oxygen content in the system is controlled below 50ppm, and the dew point is below -60℃; the obtained fine powder laser particle size distribution D 50 The particle size is 2.8~3.2μm, the particle size distribution range is <1.2, and the oxygen content of fine powder is not higher than 1500ppm.
8. The method for preparing high-performance corrosion-resistant heavy rare earth-rich permanent magnet material according to claim 1, characterized in that, In step S5, the orientation magnetic field strength for compression molding is 1.8~2.5T, the molding pressure is 150~250MPa, and the holding time is 10~30s. After compression molding, cold isostatic pressing is performed at a pressure of 150~250MPa for a holding time of 60~120s. The entire molding process is under nitrogen protection, with the ambient oxygen content controlled below 100ppm. The resulting green compact density is 3.8~4.2g / cm³. 3 .
9. The method for preparing high-performance corrosion-resistant heavy rare earth-rich permanent magnet material according to claim 1, characterized in that, The vacuum segmented sintering in step S6 includes: heating from room temperature to 800℃ at a heating rate of 5~10℃ / min and holding at that temperature for 1~2 hours for degassing; then heating to 1050~1110℃ at a heating rate of 3~5℃ / min and holding at that temperature for 3~5 hours for sintering; the vacuum degree during sintering is better than 5×10⁻⁶. -3 Pa; After sintering, 0.08~0.12MPa of high-purity argon gas is introduced and the blower is started to force cooling to room temperature; The two-stage tempering heat treatment includes: the sintered magnet is reheated to 850~950℃ and held for 2~4h for first-stage tempering, then argon gas is introduced to rapidly cool to room temperature, then heated to 450~550℃ and held for 3~5h for second-stage tempering, and finally cooled to room temperature with the furnace.
10. A high-performance corrosion-resistant heavy rare earth-rich permanent magnet material prepared by the method according to any one of claims 1 to 9, characterized in that: In the microstructure of the material, a heavy rare earth-rich epitaxial shell with a thickness of 50-200 nm is formed outside the main phase grains, and the grain boundary phase forms a continuous three-dimensional network structure with a grain boundary thickness of 20-100 nm; the room temperature coercivity H of the material is... cj ≥17kOe, remanence Br≥12.5kGs, maximum energy product (BH) max ≥38 MGOe, flexural strength ≥350 MPa; in a 5wt% NaCl neutral salt spray test, the rusting time of the uncoated magnet is ≥192 h, and the corrosion current density measured in a 3.5wt% NaCl solution is ≤8 μA / cm². 2 .
Citation Information
Patent Citations
A high-performance sintered NdFeB magnet and its preparation method
CN112017834B
High-corrosion-resistance rare earth permanent magnet and preparation method thereof
CN112562953A
Sintered neodymium-iron-boron magnet with high corrosion resistance and high magnetic performance and preparation method of sintered neodymium-iron-boron magnet
CN115360008A