High wear-resistant powder metallurgy material and preparation process thereof
By introducing a molybdenum disulfide-polytetrafluoroethylene composite lubricating medium and a layered structure of molybdenum disilicide and titanium silicon carbide into powder metallurgy materials, the problems of sintering resistance and long-term lubrication of the lubricating phase are solved, the wear resistance and interlayer bonding strength of the material are improved, and the stability of lubrication performance and anti-galling ability are achieved.
Patent Information
- Application Number
- CN202611266649.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-20
- Publication Date
- 2026-11-20
AI Technical Summary
Existing high wear-resistant powder metallurgy materials cannot simultaneously achieve sintering resistance and long-term lubrication of the lubricating phase. The lubrication mechanism is singular, the synergistic effect of the compound components is insufficient, and the interlayer bonding strength is inadequate, resulting in unstable lubrication performance and delamination.
The material employs a layered composite structure, including a steel substrate, a copper-plated underlayer, and a sintered wear-resistant layer. The sintered wear-resistant layer has molybdenum disulfide-polytetrafluoroethylene composite lubricating medium impregnated and cured in its open pores. A sintering-resistant self-lubricating phase, such as a blend of molybdenum disilicide and titanium silicon carbide, is introduced through a mixing process. The pre-composite self-lubricating phase is formed by utilizing the difference in particle size distribution, combined with copper plating and porosity control.
A tiered lubrication system was achieved, which has a low coefficient of friction, low wear, strong anti-galling ability, and better wear resistance than single-component solutions. The interlayer bonding is tight and the batch performance is stable.
Abstract
Description
Technical Field
[0001] This invention relates to the field of powder metallurgy technology, and in particular to a high wear-resistant powder metallurgy material and its preparation process. Background Technology
[0002] Powder metallurgy materials possess advantages such as near-net-shape forming, high material utilization, and the ability to fabricate porous structures. Layered composite powder metallurgy materials, consisting of a steel-backed copper-based sintered wear-resistant layer impregnated with lubricating media, are widely used in wear-resistant and friction-reducing parts such as guide strips, sliding plates, and bearings. These parts typically operate under dry friction, medium-to-high loads, and high-temperature conditions, requiring materials to possess high wear resistance, low coefficient of friction, good anti-galling ability, and strong interlayer bonding strength. However, the density of the wear-resistant layer and the penetration and storage of the lubricating media are mutually restrictive, and it is difficult to simultaneously achieve sintering resistance and long-term lubrication performance of the lubricating phase. The overall performance of high-wear-resistant powder metallurgy materials still needs improvement.
[0003] Among the published similar technologies, Chinese patent application CN121514501A discloses a high wear-resistant powder metallurgy material and its processing technology based on steam treatment. It uses nickel-plated tungsten carbide composite powder and iron-based alloy powder, which are pressed, sintered, and then steam-treated. However, it relies on surface oxide film reinforcement, and the closed pores prevent lubricating media from penetrating. Furthermore, the composite plating process is complex. Chinese patent application CN113024254A discloses a high wear-resistant powder metallurgy material and its preparation method. The method uses graphene oxide as a precursor and is prepared by high-temperature reaction sintering. However, its sintering temperature is high and energy consumption is large. Moreover, it has a homogeneous and single structure and does not have the tiered lubrication capability of combining oil storage pores and lubricating media. Chinese patent application CN121972667A discloses a copper-graphite alloy and steel bimetallic self-lubricating slide plate material, which adopts layered powdering, pressing sintering and hot isostatic pressing process. However, its lubricating phase is only graphite, the lubrication mechanism is single, and the lubrication performance is difficult to maintain after the graphite is worn out during sintering and service.
[0004] In summary, existing high wear-resistant powder metallurgy technologies still suffer from the following problems: the lubricating phase cannot withstand the sintering temperature and thus remains insufficiently; the single lubrication mechanism leads to a lubrication gap between the running-in and steady-state periods; the random dispersion of composite components results in insufficient synergistic effects; and the wear-resistant layer's bonding strength with the steel substrate is insufficient, making it prone to delamination. Therefore, there is an urgent need for a high wear-resistant powder metallurgy material and its preparation process that features a lubricating phase resistant to sintering, reliable and long-lasting graded lubrication, sufficient synergistic effects of composite components, and strong interlayer bonding. Summary of the Invention
[0005] To address the shortcomings of existing technologies, this invention aims to provide a high wear-resistant powder metallurgy material and its preparation process.
[0006] To achieve the above-mentioned objectives, the present invention adopts the following technical solution:
[0007] A high wear-resistant powder metallurgy material, wherein the high wear-resistant powder metallurgy material has a layered composite structure, comprising, from bottom to top, a steel substrate, a copper-plated underlayer, and a sintered wear-resistant layer. The pores of the sintered wear-resistant layer are impregnated and cured with a molybdenum disulfide-polytetrafluoroethylene composite lubricating medium. The sintered wear-resistant layer is formed by sintering a mixture of sintered wear-resistant powders. The sintered wear-resistant layer mixture consists of the following components in parts by weight: 50-65 parts tin bronze powder, 5-10 parts electrolytic copper powder, 10-18 parts reduced iron powder, 4-8 parts silicon carbide micro powder, 2-4 parts silicon nitride powder, 4-8 parts flake graphite, 2-6 parts sintering-resistant self-lubricating phase, and 0.5-1.5 parts zinc stearate.
[0008] The sintered wear-resistant layer mixture powder is composed of the following components in parts by weight: 55-61 parts tin bronze powder, 6.5-9.5 parts electrolytic copper powder, 12-16 parts reduced iron powder, 5-7 parts silicon carbide micro powder, 2.5-3.5 parts silicon nitride powder, 5-7 parts flake graphite, 3-5 parts sintering-resistant self-lubricating phase, and 0.8-1.2 parts zinc stearate.
[0009] The sintering-resistant self-lubricating phase is selected from one or more of tungsten disulfide, hexagonal boron nitride, barium fluoride, molybdenum disilicide, and titanium silicon carbide.
[0010] The sintering-resistant self-lubricating phase is composed of two components: molybdenum disilicide and titanium silicon carbide, with a mass ratio of molybdenum disilicide to titanium silicon carbide of 1:0.5-1.5.
[0011] The molybdenum disulfide-polytetrafluoroethylene composite lubricating medium is formed by vacuum impregnation, drying and curing of a mixed impregnation emulsion. The mixed impregnation emulsion is composed of the following components in parts by weight: 80-120 parts of concentrated polytetrafluoroethylene dispersion emulsion, 20-30 parts of molybdenum disulfide micro powder, 35-55 parts of water, and 1-2 parts of fatty alcohol polyoxyethylene ether.
[0012] The steel substrate is Q235 cold-rolled steel sheet; the thickness of the copper-plated underlayer is 10-20μm.
[0013] The preparation process of the aforementioned high wear-resistant powder metallurgy material includes the following steps:
[0014] Step 1: The steel substrate blank is subjected to alkaline degreasing, water washing, acid pickling activation and water washing in sequence, and then pure copper is electroplated as the base to obtain copper-plated blank;
[0015] Step 2: Weigh each component according to the weight proportions, put them into a mixer, mix at a speed of 18-22 r / min for 60-90 min, and sieve after discharge to obtain sintered wear-resistant layer mixed powder;
[0016] Step 3: The mixed powder is evenly spread onto the surface of the copper plating layer of the copper plating blank obtained in Step 1, with a powder thickness of 1.8-2.2 mm. After leveling, it is sent into a mesh belt sintering furnace for powder-spreading sintering. A nitrogen-based low-hydrogen protective atmosphere is introduced into the furnace, in which the volume fraction of hydrogen is 5%-8%, and the remainder is nitrogen. The dew point of the protective atmosphere is not higher than -40℃, and the oxygen content in the furnace is not higher than 10ppm. The sintering furnace is divided into six temperature control zones, of which zones 1 and 2 are preheating zones, with the temperature controlled at 640-660℃ respectively. The furnace operates at 60℃ and 770-790℃. Zones 3 and 4 are sintering zones, with temperatures controlled at 845-855℃ and 865-875℃ respectively. Zones 5 and 6 are cooling zones, with zone 5 controlled at 590-610℃ and zone 6 cooled to below 150℃ via a water-cooled jacket before exiting the furnace. The conveyor belt speed is controlled at 60-80 mm / min, and the effective holding time of the billet in the sintering zone is 30-45 minutes. After furnace cooling, a wear-resistant composite billet is obtained, with a porosity of 30%-34% for the resulting wear-resistant layer.
[0017] Step 4: Dilute the polytetrafluoroethylene concentrated dispersion emulsion with water in a mixing tank according to the weight proportions, and add molybdenum disulfide micro powder and fatty alcohol polyoxyethylene ether while stirring to obtain a mixed impregnation emulsion;
[0018] Step 5: Place the wear-resistant composite preform from Step 3 into a vacuum impregnation tank, evacuate the tank to a vacuum level of 0.07-0.08 MPa (i.e., gauge pressure of -0.07 to -0.08 MPa), draw in the mixed impregnation emulsion obtained in Step 4 and completely immerse the preform in vacuum immersion, then depressurize and drain.
[0019] Step 6: Dry the vacuum-impregnated green body in sections at a maximum drying temperature of 155-165℃.
[0020] Step 7: Transfer the dried blank into the curing oven, purge the oven with nitrogen to maintain a slight positive pressure, cure at a maximum temperature of 380-385℃, and keep warm for a total of 8-10 hours. After curing, let it cool to room temperature in the oven.
[0021] Step 8: Place the cured product on a press, measure the pressure area of the wear-resistant layer, apply a load of 1.3-1.7 tons of force per square centimeter according to the pressure area, hold the pressure and then unload to obtain the high wear-resistant powder metallurgy material.
[0022] In step 2, the material is discharged through a 100-mesh sieve; in step 4, molybdenum disulfide micro powder and fatty alcohol polyoxyethylene ether are first added under stirring at 300-400 r / min, then the speed is increased to 800-1000 r / min and stirred for 30-40 min, and then allowed to stand for defoaming for 15-25 min; in step 5, the vacuum soaking is done in two stages, each soaking for 25-30 min, and after soaking, the emulsion in the tank is pumped back to the stirring tank.
[0023] In step 6, the segmented drying is carried out in three stages: the first stage is heated to 95-105℃ and held for 25-35 minutes; the second stage is heated to 125-135℃ and held for 25-35 minutes; and the third stage is heated to 155-165℃ and held for 55-65 minutes. In step 7, the curing is carried out in six stages: the first stage is heated to 95-105℃ and held for 25-35 minutes; the second stage is heated to 155-165℃ and held for 55-65 minutes; the third stage is heated to 375-382℃ and held for 110-125 minutes; the fourth stage is heated to 380-385℃ and held for 110-125 minutes; and the fifth and sixth stages are both held at 380-385℃ for 110-125 minutes. In step 8, the pressure holding time is 8-12 minutes.
[0024] Preferably, when the sintering-resistant self-lubricating phase is composed of two components, molybdenum disilicide and titanium silicon carbide, step 2 can also be performed as follows: weigh each component according to the above-mentioned weight proportions; first, put the molybdenum disilicide powder and titanium silicon carbide powder into a mixer and premix them separately for 10-20 minutes to form a pre-composite self-lubricating phase; then, put them into a mixer together with tin bronze powder, electrolytic copper powder, reduced iron powder, silicon carbide micro powder, silicon nitride powder, flake graphite and zinc stearate, mix them at a speed of 18-22 r / min for 60-90 minutes, and after discharge, sieve to obtain the sintering wear-resistant layer mixed powder.
[0025] Existing copper-based powder metallurgy wear-resistant layers mostly rely on graphite for lubrication. However, graphite suffers significant losses during sintering and exhibits weak interfacial bonding with the copper matrix, resulting in insufficient supply of low-shear transfer film at the friction interface. Furthermore, it has been found that conventional lubricants such as molybdenum disulfide and polytetrafluoroethylene (PTFE) cannot withstand the sintering temperature and cannot remain within the sintered layer, leaving a persistent lack of lubrication reserves within the matrix. To address this, this invention introduces a thermally stable, sintering-resistant self-lubricating phase into the sintering wear-resistant layer mixture powder and vacuum impregnates and cures the PTFE composite lubricating medium within the pores of the wear-resistant layer. This solves the problems of difficulty in retaining the lubricating phase in the sintered layer and insufficient interfacial lubrication supply, thereby reducing the material's coefficient of friction and improving its anti-galling ability.
[0026] The lubrication mechanism of a single self-lubricating phase is relatively simple. While layered slip-type lubricating phases can take effect immediately, they are continuously consumed. In-situ glaze-type lubricating phases have a slow start-up and insufficient protection during the running-in period. Furthermore, it was found that if the lubrication mechanisms of the compound components overlap and their effective temperature zones are mismatched, simple mixing not only does not provide any benefit but also dilutes the effective content. To address this, this invention combines molybdenum disilicide with titanium silicon carbide. Utilizing the layered basal slip of titanium silicon carbide, a low-shear film can be rapidly established at the friction interface during the running-in period without the need for induction conditions. Under dry friction conditions, the instantaneous flash temperature of the local contact micro-area is significantly higher than the service environment temperature. Under the action of flash temperature, the surface of molybdenum disilicide gradually undergoes controlled oxidation, generating an in-situ lubricating glaze layer containing silicon and molybdenum oxides, which takes over the lubrication function during the steady-state period. This solves the problem of the interruption in the lubrication effect period and achieves a synergistic effect superior to any single component.
[0027] In conventional mixing, the two self-lubricating phases are randomly dispersed and isolated from each other, making it difficult for both components to appear simultaneously in the same friction micro-region. This hinders the continuous formation of the lubricating glaze and reduces the synergistic effect. Furthermore, it was found that while the fine-particle-size component has high activity, it is also more prone to agglomeration and segregation. To address this, the present invention premixes the two self-lubricating phases separately before mixing. By utilizing the difference in particle size distribution, the fine-particle-size molybdenum disilicide is embedded on the surface of the coarse-sheet titanium silicon carbide to form a pre-composite self-lubricating phase before being mixed with the remaining components. This solves the problem of spatial separation of the compounded components, resulting in a continuous anchored glaze layer that is less prone to peeling, and further enhancing the synergistic effect.
[0028] Compared with the prior art, the present invention has the following beneficial technical effects:
[0029] 1) This invention introduces a sintering-resistant self-lubricating phase and forms a tiered lubrication system with an impregnated and cured polytetrafluoroethylene composite lubricating medium. The material has a low coefficient of friction, low wear, and strong anti-galling ability.
[0030] 2) In this invention, molybdenum disilicide and titanium silicon carbide are combined to achieve immediate film formation during the running-in period and in-situ lubrication relay of the glaze layer during the steady-state period, resulting in synergistic effect and wear resistance performance superior to any single-component solution.
[0031] 3) This invention achieves a tight bond between the wear-resistant layer and the steel substrate through copper plating, porosity control, and pressure molding, resulting in stable batch performance. Detailed Implementation
[0032] Some material sources or parameters:
[0033] Tin bronze powder: Sn content 9%-11%, balance Cu, loose packing density 2.4-2.8 g / cm³ 3 Particle size ≤75μm, oxygen content ≤0.3%;
[0034] Electrolytic copper powder: CAS number 7440-50-8, purity ≥99.7%, particle size 20-45μm;
[0035] Reduced iron powder: CAS number 7439-89-6, total iron content (TFe) ≥98.5%, particle size 45-150μm;
[0036] Silicon carbide micro powder: CAS number 409-21-2, purity ≥98.5%, particle size 5-7μm;
[0037] Silicon nitride powder: CAS number 12033-89-5, α phase content ≥92%, particle size 1-3μm;
[0038] Flake graphite: CAS number 7782-42-5, fixed carbon content ≥99%, particle size ≤75μm;
[0039] Tungsten disulfide: CAS number 12138-09-9, purity ≥99%, particle size 1.5-4.0μm;
[0040] Hexagonal boron nitride: CAS number 10043-11-5, purity ≥99%, particle size 1.5-4.0μm;
[0041] Barium fluoride: CAS number 7787-32-8, purity ≥99%, particle size 1.5-4.0μm;
[0042] Molybdenum disilicide: CAS number 12136-78-6, purity ≥99%, particle size 1-3μm;
[0043] Titanium silicon carbide: MAX phase ternary ceramic, commercially available with main content (Ti3SiC2) ≥98% and particle size 5-10μm;
[0044] Zinc stearate: CAS 557-05-1, main content ≥99% (zinc content 10.3%-11.3%), industrial grade 1 product.
[0045] Polytetrafluoroethylene concentrated dispersion emulsion, purchased from Chemours, brand name: DISP 30, solid content 60%±2%, primary particle size 0.05-0.5μm, pH value 8-10.
[0046] Molybdenum disulfide micro powder: CAS 1317-33-5, purity ≥98.5%, particle size 1.5-3.0μm;
[0047] Fatty alcohol polyoxyethylene ether (AEO-9): ethylene oxide addition number 9, HLB value 12.5-13.5, cloud point (1% aqueous solution) ≥75℃.
[0048] Q235 cold-rolled steel sheet: conforms to GB / T 700, carbon content ≤0.22%, thickness 2.5mm;
[0049] All raw materials used in the embodiments of this invention are commercially available products.
[0050] Example 1
[0051] This embodiment provides a high wear-resistant powder metallurgy material, which has a layered composite structure, comprising a steel substrate, a copper-plated underlayer, and a sintered wear-resistant layer from bottom to top. The sintered wear-resistant layer has a molybdenum disulfide-polytetrafluoroethylene composite lubricating medium impregnated and cured in its pores.
[0052] All raw material formulas are in parts by weight:
[0053] The sintered wear-resistant layer mixture powder is composed of the following components in parts by weight: 58 parts tin bronze powder, 8 parts electrolytic copper powder, 14 parts reduced iron powder, 6 parts silicon carbide micro powder, 3 parts silicon nitride powder, 6 parts flake graphite, 4 parts sintering-resistant self-lubricating phase, and 1 part zinc stearate.
[0054] The molybdenum disulfide-polytetrafluoroethylene mixed impregnation emulsion is composed of the following components in parts by weight: 100 parts of concentrated polytetrafluoroethylene dispersion emulsion, 25 parts of molybdenum disulfide micro powder, 45 parts of water, and 1.5 parts of fatty alcohol polyoxyethylene ether.
[0055] The steel substrate is made of Q235 cold-rolled steel sheet.
[0056] The preparation process of the high wear-resistant powder metallurgy material includes the following steps:
[0057] Step 1: The steel substrate blank is subjected to alkaline degreasing, water washing, acid pickling activation and water washing in sequence. Then, pure copper is electroplated as the base layer. The thickness of the copper plating layer is controlled to be 15μm. It is required that the surface after plating is uniform and complete, without oil stains, bubbles and black spots, to obtain the copper-plated blank.
[0058] Step 2: Weigh out the tin bronze powder, electrolytic copper powder, reduced iron powder, silicon carbide micro powder, silicon nitride powder, flake graphite, sintering-resistant self-lubricating phase and zinc stearate according to the above weight proportions, put them into a V-type mixer, mix them at a speed of 20 r / min for 80 min, and after discharge, pass them through a 100 mesh sieve to obtain the sintered wear-resistant layer mixed powder.
[0059] Step 3: The mixed powder is evenly spread on the surface of the copper plating layer of the copper-plated blank obtained in Step 1, with a powder thickness of 2mm. After leveling, it is sent into a mesh belt sintering furnace for powder-spreading sintering. A nitrogen-based low-hydrogen protective atmosphere is introduced into the furnace. The volume fraction of hydrogen in the protective atmosphere is 6%, and the balance is nitrogen. The dew point of the protective atmosphere is ≤-40℃, and the oxygen content in the furnace is ≤10ppm. The sintering furnace is divided into six temperature control zones. Zones 1 and 2 are preheating zones, with temperatures controlled at 650℃ and 780℃, respectively. Zones 3 and 4 are sintering zones, with temperatures controlled at 850℃ and 870℃, respectively. Zones 5 and 6 are cooling zones. The temperature in zone 5 is controlled at 600℃, and zone 6 is cooled to below 150℃ by a water-cooled jacket before being removed from the furnace. The mesh belt speed is controlled at 70mm / min, and the effective holding time of the blank in the sintering zone is 40min. After cooling in the furnace, a wear-resistant composite blank is obtained. The porosity of the obtained wear-resistant layer is 32%±1%.
[0060] Step 4: Add the polytetrafluoroethylene concentrated dispersion emulsion and water to the mixing tank according to the above weight proportions to dilute. Add molybdenum disulfide micro powder and fatty alcohol polyoxyethylene ether while stirring at 350 r / min. Then increase the speed to 800 r / min and stir for 40 min. Let it stand to defoam for 20 min to obtain the mixed impregnation emulsion.
[0061] Step 5: Place the wear-resistant composite preform from Step 3 with the wear-resistant layer facing up in the vacuum impregnation tank, evacuate to a vacuum pressure of 0.075 MPa, draw in the mixed impregnation emulsion obtained in Step 4 and completely immerse the preform, vacuum soak for 30 minutes, release the pressure, remove and drain, and then perform a second vacuum impregnation according to the same process. After the impregnation is completed, pump the emulsion in the tank back to the mixing tank.
[0062] Step 6: Place the vacuum-impregnated green body in a hot air circulating oven for segmented drying. The first stage is to raise the temperature to 100℃ and hold for 30 minutes, the second stage is to raise the temperature to 130℃ and hold for 30 minutes, and the third stage is to raise the temperature to 160℃ and hold for 60 minutes.
[0063] Step 7: Transfer the dried blank to a curing oven. Nitrogen gas is introduced into the oven to maintain a slight positive pressure. The curing temperature is controlled in six stages, with a maximum temperature of 382℃ and a total holding time of 9.5 hours. Specifically: the first stage is to raise the temperature to 100℃ and hold for 30 minutes; the second stage is to raise the temperature to 160℃ and hold for 60 minutes; the third stage is to raise the temperature to 380℃ and hold for 120 minutes; the fourth stage is to raise the temperature to 382℃ and hold for 120 minutes; the fifth stage is to hold for 120 minutes at 382℃; and the sixth stage is to hold for 120 minutes at 382℃. After curing, the blank is cooled to room temperature in the oven. The slight positive pressure of nitrogen gas in the curing oven can isolate oxygen and prevent the PTFE from undergoing thermo-oxidative degradation at the curing temperature. The six-stage segmented heat preservation can make the internal temperature of the wear-resistant layer pores uniform, fully melt and plasticize the PTFE, and firmly anchor the molybdenum disulfide to the inner wall of the pores.
[0064] Step 8: Place the cured product on a press, measure the pressure area of the wear-resistant layer, apply a load of 1.5 tons of force per square centimeter, hold the pressure for 10 minutes and then unload. After the powder layer undergoes sintering shrinkage and pressure compaction, the thickness of the wear-resistant layer is 1.5 mm. The total thickness of the obtained high wear-resistant powder metallurgy material is 4.0 mm, which is the high wear-resistant powder metallurgy material.
[0065] The sintering-resistant self-lubricating phase is tungsten disulfide.
[0066] Example 2
[0067] The preparation process of a high wear-resistant powder metallurgy material is basically the same as that in Example 1, except that the sintering-resistant self-lubricating phase is hexagonal boron nitride powder.
[0068] Example 3
[0069] The preparation process of a high wear-resistant powder metallurgy material is basically the same as that in Example 1, except that the sintering-resistant self-lubricating phase is barium fluoride.
[0070] Example 4
[0071] The preparation process of a high wear-resistant powder metallurgy material is basically the same as that in Example 1, except that the sintering-resistant self-lubricating phase is molybdenum disilicide.
[0072] Example 5
[0073] The preparation process of a high wear-resistant powder metallurgy material is basically the same as that in Example 1, except that the sintering-resistant self-lubricating phase is titanium silicon carbide.
[0074] Example 6
[0075] The preparation process of a high wear-resistant powder metallurgy material is basically the same as that in Example 1, except that the sintering-resistant self-lubricating phase is composed of molybdenum disilicide and silicon carbide in a mass ratio of 1:1.
[0076] Example 7
[0077] The preparation process of a high wear-resistant powder metallurgy material is basically the same as that in Example 1, except that the sintering-resistant self-lubricating phase is composed of tungsten disulfide and barium fluoride in a mass ratio of 1:1.
[0078] Example 8
[0079] The preparation process of a high wear-resistant powder metallurgy material is basically the same as that in Example 6, except that step 2 is different.
[0080] Step 2 is as follows: Weigh each component according to the above weight proportions; first, add the two sintering-resistant self-lubricating phases, molybdenum disilicide powder and titanium silicon carbide powder, into a mixer at a mass ratio of 1:1 and premix them separately for 15 minutes. Utilize the difference in particle size distribution between the two to allow the fine-particle molybdenum disilicide to be embedded on the surface of the coarse-flake titanium silicon carbide, forming a pre-composite self-lubricating phase; then add them together with tin bronze powder, electrolytic copper powder, reduced iron powder, silicon carbide micro powder, silicon nitride powder, flake graphite, and zinc stearate into a V-type mixer and mix at a speed of 20 r / min for 80 minutes. After discharge, pass the mixture through a 100-mesh sieve to obtain the sintered wear-resistant layer mixed powder.
[0081] Comparative Example 1
[0082] The preparation process of a high wear-resistant powder metallurgy material is basically the same as that in Example 1, except that the sintering-resistant self-lubricating phase is not added.
[0083] Test Example 1
[0084] Steady-state friction coefficient determination:
[0085] Samples were taken from Examples 1-8 and Comparative Example 1, with each sample measuring 70mm × 20mm × 4.0mm. Five samples were prepared in parallel for each group. The samples were mounted on the upper mold fixture of a reciprocating friction testing machine, and fitted with a hardened steel mating part (hardness ≥ 50HRC, surface roughness Ra ≤ 0.4μm). The machine was subjected to dry friction at a test temperature of 180℃, a running speed of 1200mm / min, and a contact stress of 1kN / cm. 2 Under the condition of 12,000 reciprocating friction cycles, the testing machine collected the friction force in real time, and calculated according to the friction coefficient μ = friction force / normal force. The arithmetic mean of the friction coefficient from the 6001st to the 12,000th cycle (steady-state section) was taken as the steady-state friction coefficient of the test block. The arithmetic mean of the results of 5 test blocks in each group was taken as the final result of the group. The results are shown in Table 1.
[0086] Table 1
[0087] sample steady-state friction coefficient Example 1 0.17 Example 2 0.19 Example 3 0.23 Example 4 0.21 Example 5 0.16 Example 6 0.12 Example 7 0.20 Example 8 0.10 Comparative Example 1 0.26
[0088] Test Example 2
[0089] Determination of ultimate occlusal stress:
[0090] Samples were taken from Examples 1-8 and Comparative Example 1, with each sample measuring 70mm × 20mm × 4.0mm, and 5 parallel samples per group. A stepped loading method was used on a reciprocating friction testing machine at a test temperature of 180℃, a speed of 1200mm / min, and dry friction, with a contact stress starting from 0.5kN / cm. 2 The starting point increases by 0.2 kN / cm for each level. 2 The test block was subjected to 1000 reciprocating cycles under each load level. When the friction coefficient increased by more than 50% compared to the previous level, or when the test block and its mating part became stuck, a seizing failure was determined. The contact stress of the previous level before failure was recorded as the seizing limit stress of the test block. The arithmetic mean of the five test blocks in each group was taken. Elemental analysis of the wear surface of the test block in Example 6 revealed characteristic signals of silicon and molybdenum oxides, confirming the formation of a lubricating glaze layer during the friction process. The results are shown in Table 2.
[0091] Table 2
[0092] sample <![CDATA[Seizure resistance limit stress (kN / cm 2 )]]> Example 1 1.7 Example 2 1.4 Example 3 1.3 Example 4 1.6 Example 5 1.8 Example 6 2.2 Example 7 1.5 Example 8 2.6 Comparative Example 1 1.1
[0093] As can be seen from the test results in Tables 1 and 2, the tribological properties of Examples 1-5 are all superior to those of Comparative Example 1. The reason for this may be that: in Comparative Example 1, the sintered wear-resistant layer relies solely on flake graphite for lubrication. Graphite is significantly lost during sintering and has weak interfacial bonding with the copper substrate, resulting in insufficient supply of low-shear transfer film at the friction interface. This intensifies the adhesion and ploughing between the micro-protrusions on the mating surface and the wear-resistant layer, leading to a higher coefficient of friction and lower anti-galling ability. In contrast, the sintering-resistant self-lubricating phase introduced in Examples 1-5 retains its lubricating activity after sintering and continuously replenishes the low-shear medium to the friction interface as the wear progresses. The supply of transfer film is stable, and the contact state of the friction pair is improved. The titanium silicon carbide used in Example 5 combines the high hardness of ceramics with the basal slip characteristics of a layered structure. Its interlayer shear strength is low, and it is easy to slip along the basal surface to form a film under load. At the same time, its layered structure can absorb frictional work through microcrack deflection and interlayer slip, suppressing the brittle spalling of the hard phase in the wear-resistant layer. Less wear debris is generated and the lubricating film is continuous and complete. Therefore, it has better performance in the single-component scheme.
[0094] Example 6 uses a combination of molybdenum disilicide and titanium silicon carbide, which exhibits a significant synergistic effect. The mechanism may be as follows: the layered basal slip of titanium silicon carbide does not require inducing conditions and can quickly establish a low-shear film at the friction interface during the running-in period, inhibiting early adhesion and plowing; as friction proceeds, the instantaneous flash temperature of the local contact micro-area is significantly higher than the test environment temperature. Under the action of flash temperature, the surface layer of molybdenum disilicide gradually undergoes controlled oxidation, generating a lubricating glaze layer containing silicon and molybdenum oxides in situ, which takes over the lubrication function during the steady state period, and the coverage of the glaze layer, in turn, slows down the consumption rate of titanium silicon carbide; the two have different lubrication mechanisms and their action periods are connected to form a complete lubrication relay, thus the performance is better than any single-component scheme. In Example 7, the lubrication mechanisms of tungsten disulfide and barium fluoride are both the formation of a low-shear film at the interface, and their functions are completely overlapping. Moreover, the effective temperature of the barium fluoride lubricating film is higher than the service temperature of the present invention. It is in a dormant state throughout the test, only playing an inert filling role and diluting the effective content of tungsten disulfide. The compounding effect is only between that of the two components used alone, and does not constitute a synergy.
[0095] Example 8 improves upon Example 6 by refining the mixing process, resulting in further enhanced performance. This improvement may be attributed to the following: The premixing process utilizes the particle size difference between molybdenum disilicide and titanium silicon carbide, allowing fine-grained molybdenum disilicide to be embedded on the surface of coarse-grained titanium silicon carbide. The two components are transformed from random, isolated dispersion in the matrix to co-existing distribution within the same particle size. During service, layered slippage and in-situ glaze formation occur simultaneously within the same friction micro-region. The generated glaze is directly anchored to the surface of the titanium silicon carbide particles, resulting in continuous and firmly bonded film formation, making it less prone to peeling off in whole pieces. Simultaneously, the fine-grained molybdenum disilicide has a larger specific surface area and higher surface oxidation activity, accelerating the formation rate and achieving more complete coverage of the lubricating glaze. The lubrication relay of the two components is completed in a closed loop within the same micro-region, fully leveraging their synergistic effect. Therefore, it exhibits the lowest coefficient of friction and the strongest anti-galling capability.
Claims
1. A high wear-resistant powder metallurgy material, characterized in that: The high wear-resistant powder metallurgy material has a layered composite structure, comprising, from bottom to top, a steel substrate, a copper-plated underlayer, and a sintered wear-resistant layer. The pores of the sintered wear-resistant layer are impregnated and cured with a molybdenum disulfide-polytetrafluoroethylene composite lubricating medium. The sintered wear-resistant layer is formed by sintering a mixture of sintered wear-resistant powders. The sintered wear-resistant layer mixture consists of the following components in parts by weight: 50-65 parts tin bronze powder, 5-10 parts electrolytic copper powder, 10-18 parts reduced iron powder, 4-8 parts silicon carbide micro powder, 2-4 parts silicon nitride powder, 4-8 parts flake graphite, 2-6 parts sintering-resistant self-lubricating phase, and 0.5-1.5 parts zinc stearate.
2. The high wear-resistant powder metallurgy material according to claim 1, characterized in that: The sintered wear-resistant layer mixture powder is composed of the following components in parts by weight: 55-61 parts tin bronze powder, 6.5-9.5 parts electrolytic copper powder, 12-16 parts reduced iron powder, 5-7 parts silicon carbide micro powder, 2.5-3.5 parts silicon nitride powder, 5-7 parts flake graphite, 3-5 parts sintering-resistant self-lubricating phase, and 0.8-1.2 parts zinc stearate.
3. The high wear-resistant powder metallurgy material according to claim 1 or 2, characterized in that: The sintering-resistant self-lubricating phase is selected from one or more of tungsten disulfide, hexagonal boron nitride, barium fluoride, molybdenum disilicide, and titanium silicon carbide.
4. The high wear-resistant powder metallurgy material according to claim 3, characterized in that: The sintering-resistant self-lubricating phase is composed of two components: molybdenum disilicide and titanium silicon carbide, with a mass ratio of molybdenum disilicide to titanium silicon carbide of 1:0.5-1.
5.
5. The high wear-resistant powder metallurgy material according to claim 1, characterized in that: The molybdenum disulfide-polytetrafluoroethylene composite lubricating medium is formed by vacuum impregnation, drying and curing of a mixed impregnation emulsion. The mixed impregnation emulsion is composed of the following components in parts by weight: 80-120 parts of concentrated polytetrafluoroethylene dispersion emulsion, 20-30 parts of molybdenum disulfide micro powder, 35-55 parts of water, and 1-2 parts of fatty alcohol polyoxyethylene ether.
6. The high wear-resistant powder metallurgy material according to claim 1, characterized in that: The steel substrate is Q235 cold-rolled steel sheet; the thickness of the copper-plated underlayer is 10-20μm.
7. A process for preparing the high wear-resistant powder metallurgy material as described in any one of claims 1-6, characterized in that, Includes the following steps: Step 1: The steel substrate blank is subjected to alkaline degreasing, water washing, acid pickling activation and water washing in sequence, and then pure copper is electroplated as the base to obtain copper-plated blank; Step 2: Weigh each component according to the weight proportions, put them into a mixer, mix at a speed of 18-22 r / min for 60-90 min, and sieve after discharge to obtain sintered wear-resistant layer mixed powder; Step 3: The mixed powder is evenly spread onto the surface of the copper plating layer of the copper plating blank obtained in Step 1, with a powder thickness of 1.8-2.2 mm. After leveling, it is sent into a mesh belt sintering furnace for powder-spreading sintering. A nitrogen-based low-hydrogen protective atmosphere is introduced into the furnace, in which the volume fraction of hydrogen is 5%-8%, and the remainder is nitrogen. The dew point of the protective atmosphere is not higher than -40℃, and the oxygen content in the furnace is not higher than 10ppm. The sintering furnace is divided into six temperature control zones, of which zones 1 and 2 are preheating zones, with the temperature controlled at 640-660℃ respectively. The furnace operates at 60℃ and 770-790℃. Zones 3 and 4 are sintering zones, with temperatures controlled at 845-855℃ and 865-875℃ respectively. Zones 5 and 6 are cooling zones, with zone 5 controlled at 590-610℃ and zone 6 cooled to below 150℃ via a water-cooled jacket before exiting the furnace. The conveyor belt speed is controlled at 60-80 mm / min, and the effective holding time of the billet in the sintering zone is 30-45 minutes. After furnace cooling, a wear-resistant composite billet is obtained, with a porosity of 30%-34% for the resulting wear-resistant layer. Step 4: Dilute the polytetrafluoroethylene concentrated dispersion emulsion with water in a mixing tank according to the weight proportions, and add molybdenum disulfide micro powder and fatty alcohol polyoxyethylene ether while stirring to obtain a mixed impregnation emulsion; Step 5: Place the wear-resistant composite preform from Step 3 into a vacuum impregnation tank, evacuate the tank to a vacuum level of 0.07-0.08 MPa, draw in the mixed impregnation emulsion obtained in Step 4 and completely immerse the preform in vacuum immersion, then depressurize and drain. Step 6: Dry the vacuum-impregnated green body in sections at a maximum drying temperature of 155-165℃. Step 7: Transfer the dried blank into the curing oven, purge the oven with nitrogen to maintain a slight positive pressure, cure at a maximum temperature of 380-385℃, and keep warm for a total of 8-10 hours. After curing, let it cool to room temperature in the oven. Step 8: Place the cured product on a press, measure the pressure area of the wear-resistant layer, apply a load of 1.3-1.7 tons of force per square centimeter according to the pressure area, hold the pressure and then unload to obtain the high wear-resistant powder metallurgy material.
8. The preparation process according to claim 7, characterized in that: In step 2, the material is discharged through a 100-mesh sieve; in step 4, molybdenum disulfide micro powder and fatty alcohol polyoxyethylene ether are added first under stirring at 300-400 r / min, then the speed is increased to 800-1000 r / min and stirred for 30-40 min, and then allowed to stand for defoaming for 15-25 min; in step 5, the vacuum soaking is done in two stages, each soaking for 25-30 min, and after soaking, the emulsion in the tank is pumped back to the stirring tank.
9. The preparation process according to claim 7, characterized in that: In step 6, the segmented drying is carried out in three stages: the first stage is heated to 95-105℃ and held for 25-35 minutes; the second stage is heated to 125-135℃ and held for 25-35 minutes; and the third stage is heated to 155-165℃ and held for 55-65 minutes. In step 7, the curing is carried out in six stages: the first stage is heated to 95-105℃ and held for 25-35 minutes; the second stage is heated to 155-165℃ and held for 55-65 minutes; the third stage is heated to 375-382℃ and held for 110-125 minutes; the fourth stage is heated to 380-385℃ and held for 110-125 minutes; and the fifth and sixth stages are both held at 380-385℃ for 110-125 minutes. In step 8, the pressure holding time is 8-12 minutes.
10. The preparation process according to claim 7, characterized in that: When the sintering-resistant self-lubricating phase is composed of two components, molybdenum disilicide and titanium silicon carbide, step 2 can also be performed as follows: weigh each component according to the above-mentioned weight proportions; first, put the molybdenum disilicide powder and titanium silicon carbide powder into a mixer and premix them separately for 10-20 minutes to form a pre-composite self-lubricating phase; then, put them into a mixer together with tin bronze powder, electrolytic copper powder, reduced iron powder, silicon carbide micro powder, silicon nitride powder, flake graphite and zinc stearate, mix them at a speed of 18-22 r / min for 60-90 minutes, and after discharge, sieve them to obtain the sintering wear-resistant layer mixed powder.
Citation Information
Patent Citations
High-wear-resistance powder metallurgy material and preparation method thereof
CN113024254A
High-wear-resistance powder metallurgy material based on steam treatment and processing technology of high-wear-resistance powder metallurgy material
CN121514501A
Copper graphite alloy-steel bimetallic self-lubricating sliding plate material and application thereof
CN121972667A