A double-barrel dynamic powder feeding carbon fiber aluminum-based gradient cladding method

By using a dual-cylinder dynamic powder feeding carbon fiber-aluminum matrix gradient cladding method, and by utilizing SiC internal and external coatings and dynamic powder feeding technology, the problems of interface reaction and interlayer cracking between carbon fiber and aluminum matrix were solved. This method achieved directional reinforcement of carbon fiber and continuous compositional gradient distribution of the coating, thereby improving bonding strength and wear resistance.

CN123128529APending Publication Date: 2026-11-20CHANGCHUN AUTOMOBILE IND INST +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611591880.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-14
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies suffer from severe interfacial reactions between carbon fibers and aluminum substrates, cracking caused by abrupt changes in the physical properties of gradient coating layers, and low fiber reinforcement efficiency. Traditional cladding methods cannot form directional reinforcement in the thickness direction, resulting in insufficient bonding strength and wear resistance.

Method used

By employing a dual-cylinder dynamic powder feeding method, the coating structure of the inner and outer SiC coatings on the carbon fiber surface, combined with dynamic powder feeding and a layered scanning path strategy, achieves a continuous gradient distribution and directional arrangement of carbon fiber content. This collaboratively controls the heat input of the molten pool and the scanning path, avoiding abrupt changes in interlayer properties and interface reactions.

Benefits of technology

It achieves a continuous compositional gradient distribution in the coating, suppresses interlayer cracking, improves the coating's structural continuity and service reliability, and enhances the bonding strength and wear resistance of carbon fiber and aluminum-based alloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128529A_ABST
    Figure CN123128529A_ABST
Patent Text Reader

Abstract

The application discloses a double-barrel dynamic powder feeding carbon fiber aluminum-based gradient cladding method, and relates to the field of laser additive manufacturing, and comprises the following steps: performing double-layer antioxidation coating on a carbon fiber by coating an inner SiC coating and an outer coating; establishing a four-dimensional coupling process model of laser power, scanning speed, total powder feeding rate and single-layer cladding thickness through single-track cladding experiment; planning a dynamic function of the carbon fiber powder feeding rate changing with the cladding height and a layered scanning path; and dynamically adjusting the double-barrel powder feeding rate under the protection of inert gas and performing multi-field collaborative cladding, etc. The application utilizes the outer coating to block the interface reaction between Al and SiC, suppresses the generation of brittle phases, and continuously increases the volume fraction of the carbon fiber from the matrix to the surface layer and orderly arranges the carbon fiber along the main stress direction through continuous gradient composition and layered path, so that the problems of interlayer cracking and low reinforcing efficiency are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of laser additive manufacturing technology, and in particular to a dual-barrel dynamic powder feeding method for gradient cladding of carbon fiber and aluminum matrix. Background Technology

[0002] Carbon fiber reinforced aluminum matrix composites combine the advantages of aluminum alloys (low density, high thermal conductivity) with carbon fibers (high specific strength, low thermal expansion, wear resistance, etc.). The reinforcing coating is prepared by laser cladding on the surface of aluminum alloys, which has the advantages of concentrated energy, low dilution rate, and near-net-shape forming. It has broad application prospects in aerospace, automotive, and mold strengthening fields.

[0003] Traditional cladding processes often use a single barrel to feed premixed powder or a double barrel to feed powder at a fixed ratio. The resulting coating has a uniform composition, and the carbon fibers are randomly distributed and oriented in the molten pool. It is impossible to form directional reinforcement in the main load-bearing direction. In order to balance the bonding strength and surface wear resistance, existing technologies often use layered pre-preparation of powders with different compositions or segmented switching of powder feeding ratios to prepare gradient coatings. However, the composition distribution in the thickness direction is stepped, and there are abrupt interfaces of composition, thermal expansion coefficient and elastic modulus between adjacent layers. Under rapid thermal cycling, stress concentration is easily generated and interlayer cracking is caused. Moreover, the step switching will form composition breakpoints at the overlap.

[0004] Furthermore, carbon fibers readily react with aluminum in high-temperature molten pools, resulting in brittleness. The degree of reaction intensifies with increasing heat input and high-temperature dwell time, leading to fiber etching breakage and coating cracking. Low carbon fiber regions require higher heat input to ensure molten pool spreading and metallurgical bonding with the substrate, while carbon fiber rich regions require lower heat input to suppress interfacial reactions and guide fiber orientation. Existing methods use constant laser parameters and a single scanning path across the entire height range, which cannot simultaneously meet the forming requirements of both types of regions. The fibers are randomly distributed, making it difficult to match with the main force direction of the part, resulting in low reinforcement efficiency and inconvenience in practical use.

[0005] Therefore, it is necessary to provide a new dual-barrel dynamic powder feeding method for carbon fiber aluminum-based gradient cladding to solve the above-mentioned technical problems. Summary of the Invention

[0006] The purpose of this invention is to provide a dual-cylinder dynamic powder feeding method for gradient cladding of carbon fiber and aluminum matrix, which involves SiC inner coating on the surface of carbon fiber and... The dual-layer coating structure of the outer layer synergistically inhibits By combining continuous gradient composition control and layered scanning path strategy with dual-cylinder dynamic powder feeding, the problems of severe interface reaction between carbon fiber and aluminum matrix, cracking caused by abrupt changes in interlayer properties of gradient coating, and low fiber reinforcement efficiency in the existing technology are solved.

[0007] To solve the above-mentioned technical problems, the present invention is achieved through the following technical solution.

[0008] The dual-cylinder dynamic powder feeding method for carbon fiber aluminum-based gradient cladding provided by this invention includes the following steps:

[0009] S1. Substrate and powder pretreatment: The aluminum alloy substrate is degreased, sandblasted and roughened and preheated to relieve stress. The carbon fiber is pretreated with anti-oxidation coating. The carbon fiber and the dried and sieved aluminum alloy powder are separately loaded into the carbon fiber powder cylinder and the aluminum alloy powder cylinder.

[0010] S2. Establishing a process model and path planning: Single-pass cladding experiments were conducted using the controlled variable method to analyze the correspondence between laser power, scanning speed, total powder feeding rate, and single-layer cladding thickness. A four-dimensional coupled process model including laser power, scanning speed, total powder feeding rate, and single-layer cladding thickness was established, and the process window for dense forming was determined. Based on the distribution requirements of carbon fiber volume fraction along the cladding height in the coating design objectives, the dynamic functions of carbon fiber powder feeding rate and aluminum-based alloy powder feeding rate with cladding height were planned. At the same time, based on the main force direction during the service of the part, a layered laser scanning path strategy was planned. The layered laser scanning path strategy includes at least a reciprocating filling path used in the low carbon fiber volume fraction area and a unidirectional parallel scanning path used in the carbon fiber rich area.

[0011] S3. Dynamic Powder Feeding and Multi-Field Collaborative Cladding: Using a high-power laser as the heat source, under inert gas protection, cladding is performed layer by layer from the aluminum alloy substrate side upwards according to the process window, dynamic function, and layered laser scanning path strategy determined in step S2. During the cladding process, the control system of the cladding equipment reads the current cladding height in real time, substitutes it into the dynamic function to calculate and adjust the powder feeding rate of the dual barrels, so that the carbon fiber content increases continuously from the substrate side to the surface layer. At the same time, the total cladding height of the coating is divided into several height intervals. Each height interval corresponds to a set of laser output energy parameters taken from the process window and a scanning path topology. Switching is completed during the idle stage between adjacent layers, so that the output energy parameters of the laser and the scanning path topology are synchronously modulated with the change of cladding height, so as to collaboratively control the heat input of the molten pool and the distribution and orientation of carbon fibers.

[0012] Furthermore, in step S1, the antioxidant coating pretreatment of the carbon fiber involves first preparing a SiC ceramic inner coating layer on the surface of the carbon fiber using chemical vapor deposition, and then preparing a layer on the surface of the SiC ceramic inner coating layer. Ceramic outer coating.

[0013] Furthermore, in step S1, a side-axis converging powder feeding nozzle is used. The convergence angle of the side-axis converging powder feeding nozzle is 30°-60°, the outlet diameter is 2-4mm, and the powder flow focus is located 0.5-1.5mm in front of the laser beam focus. The carbon fiber powder and aluminum-based alloy powder are converged at the nozzle outlet through two independent channels and fed into the molten pool.

[0014] Furthermore, in step S2, the carbon fiber powder feeding rate... With aluminum-based alloy powder feeding rate The dynamic function that varies with height h satisfies: total powder feeding rate Keeping constant, the volume fraction of carbon fiber increases linearly or non-linearly with height h, and .

[0015] Furthermore, in step S2, the layered laser scanning path strategy is as follows: a reciprocating filling path is used in the bottom layer area with low carbon fiber content, and a unidirectional parallel scanning path parallel to the main force direction of the part is used in the surface layer area rich in carbon fiber.

[0016] Furthermore, in step S3, the synchronous modulation of the laser output energy is specifically as follows: a pulsed laser mode is adopted, with a long pulse width and low peak power pulse waveform in the bottom layer region with low carbon fiber content, and a short pulse width and high peak power pulse waveform in the surface layer region rich in carbon fiber.

[0017] Furthermore, in step S3, the laser beam is controlled to oscillate in a circular or figure-eight pattern by means of a galvanometer system, with an oscillation frequency of 50-500Hz.

[0018] Furthermore, in step S3, the length of the chopped carbon fiber... The relationship between the single-layer cladding thickness D in the carbon fiber-rich region and the following is satisfied: .

[0019] Furthermore, in step S3, an integrated molten pool monitoring sensor is also included to collect molten pool radiation signals in real time. When the signal is abnormal, the defect location is automatically marked or the process parameters are adjusted in a closed loop.

[0020] A continuous gradient coating of carbon fiber and aluminum matrix is ​​prepared by a dual-barrel dynamic powder feeding carbon fiber aluminum matrix gradient cladding method. The volume fraction of carbon fiber in the coating increases continuously from the substrate to its surface, and the carbon fibers are arranged in an orderly manner along a predetermined direction in the carbon fiber-rich region of the coating.

[0021] Compared with related technologies, the dual-cylinder dynamic powder feeding carbon fiber aluminum-based gradient cladding method provided by the present invention has the following beneficial effects:

[0022] 1. This invention reads the current cladding height in real time during the cladding process and substitutes it into a dynamic function to adjust the powder feeding rate of the carbon fiber powder cylinder and the aluminum-based alloy powder cylinder online. This allows the carbon fiber content to continuously increase from the matrix side to the surface layer, resulting in a coating with a continuous compositional gradient in the thickness direction. The coefficient of thermal expansion and the elastic modulus transition smoothly, avoiding stress concentration caused by abrupt changes in properties between adjacent layers. This suppresses the tendency for interlayer cracking under rapid thermal cycling conditions. At the same time, since the process of layered pre-powdering is eliminated, the powder feeding rate of carbon fiber and aluminum-based alloy powder is dynamically adjusted according to a continuous function during the cladding process, resulting in a continuous gradient distribution of coating composition in the thickness direction, rather than a step-like abrupt change. There are no compositional discontinuities at the overlap, significantly improving the continuity of the coating structure and its service reliability. Furthermore, the carbon fiber and aluminum-based alloy powder are independently packed and metered, avoiding segregation, agglomeration, and stratification caused by differences in density and flowability of premixed powder. Without changing the powder, any target gradient curve can be flexibly set by adjusting the dynamic function. The same set of equipment can adapt to the gradient design requirements of different working conditions.

[0023] 2. This invention divides the total cladding height into several height intervals, each interval being matched with a set of laser output energy parameters taken from the process window. Higher heat input is used in the low-carbon fiber region near the substrate to ensure the molten pool fully spreads, wets the substrate, and forms a dense metallurgical bonding layer with low dilution. In the carbon fiber-rich region, heat input is actively reduced and the high-temperature dwell time is shortened, effectively suppressing the reaction between carbon fibers and the aluminum matrix to generate brittleness. This reduces fiber etching and breakage, and minimizes coating cracking caused by interface compounds and thermal stress, solving the problem that existing technologies cannot simultaneously meet the forming requirements of two types of regions by using constant laser parameters across the entire height range.

[0024] 3. The present invention plans a layered scanning path strategy based on the main force direction of the part during service: the low carbon fiber area adopts a reciprocating filling path to ensure uniform overlap of the melt channel, dense structure and good transition with the substrate; the carbon fiber rich area adopts a unidirectional parallel scanning path, and uses the stable temperature gradient and melt pool flow direction formed by unidirectional scanning to guide the carbon fibers to preferential orientation and arrangement along the main force direction, overcoming the defect of low reinforcement efficiency caused by random distribution.

[0025] 4. This invention obtains the correspondence between laser power, scanning speed, total powder feeding rate and single-layer cladding thickness through single-pass cladding experiments, constructs a four-dimensional coupled process model and determines the process window for dense forming accordingly. The dynamic powder feeding rate and layered laser energy parameters are both taken from this window for matching, so that the cladding layer thickness in each height range is stable and the cladding overlap is continuous, thereby reducing defects such as incomplete fusion, porosity, undercut and excessive dilution. Attached Figure Description

[0026] Figure 1The overall process flow diagram of the dual-cylinder dynamic powder feeding carbon fiber aluminum-based gradient cladding method provided by the present invention;

[0027] Figure 2 This is a logic diagram of dynamic powder feeding and process parameter control in this invention. Detailed Implementation

[0028] The present invention will be further described below with reference to the accompanying drawings and embodiments.

[0029] In this invention, a stirring shaft is provided inside the carbon fiber powder cylinder, and a flexible stirring blade is mounted on the stirring shaft with a rotation speed of 5-20 r / min; a pneumatic vibrator is installed in the cone part of the cylinder with a vibration frequency of 50-100 Hz to prevent the short-cut carbon fibers from bridging and agglomerating inside the cylinder; argon is used as the carrier gas with a flow rate of 5-15 L / min.

[0030] The carbon fiber volume fraction was determined by metallographic image analysis. A 10mm×10mm sample was cut from the coating section, and after grinding and polishing, five fields of view were randomly selected and images were taken using a metallographic microscope at 500x magnification. ImageJ software was used for binarization to calculate the percentage of area occupied by carbon fiber. The average value of the five fields of view was taken as the carbon fiber volume fraction at that location.

[0031] Example 1

[0032] Please see Figure 1 and Figure 2 This invention is a method for gradient cladding of carbon fiber and aluminum matrix using a dual-cylinder dynamic powder feeding system.

[0033] S1. Substrate and Powder Pretreatment: 6061 aluminum alloy was selected as the substrate material, with dimensions of... The substrate surface was subjected to ultrasonic degreasing with acetone for 15 min, sandblasting roughening treatment, and then preheating stress relief treatment in a vacuum heat treatment furnace at 200℃ for 2 h.

[0034] It is worth noting that the sandblasting roughening treatment used brown corundum abrasive with a particle size of 80 mesh and a sandblasting pressure of 0.5 MPa;

[0035] It is worth noting that the carbon fiber used is T700 short-cut carbon fiber, with an average length of 0.15 mm and a diameter of... A SiC inner coating was first prepared on the carbon fiber surface using chemical vapor deposition (CVD). The deposition temperature was 1050℃, the deposition time was 30 min, and the SiC coating thickness was approximately 0.3 mm. Subsequently, a coating was prepared on the surface of the SiC inner coating. The outer coating was applied using metal-organic chemical vapor deposition at a temperature of 900 ℃ for 45 min. The coating thickness is approximately The aluminum-based alloy powder used is AlSi10Mg powder with a particle size range of 45-105. After drying at 80 °C for 4 h in a vacuum drying oven, the carbon fibers were sieved for later use. The coated carbon fibers were loaded into a carbon fiber powder cylinder, and the aluminum-based alloy powder was loaded into an aluminum-based alloy powder cylinder.

[0036] S2. Establishing the process model and path planning: A single-pass cladding experiment was conducted using the controlled variable method. The laser spot diameter was fixed at 3 mm, and the laser power P, scanning speed v, and total powder feeding rate were used as variables. Using variables, the single-layer cladding thickness D and coating density were measured under various parameter combinations;

[0037] Among them, the laser power P ranges from 600 to 1200 W, the scanning speed v ranges from 1 to 5 mm / s, and the total powder feeding rate... The range was 5-30 g / min. The experimental design and results are shown in Table 1 below:

[0038] Table 1. Experimental parameters and results of single-pass cladding.

[0039] serial number Laser power / W Scanning speed (mm / s) Total powder feeding rate (g / min) Single layer thickness / mm density 1 600 2 10 0.28 Pores 2 700 2 10 0.32 dense 3 750 2 10 0.35 dense 4 800 2 10 0.38 dense 5 900 2 10 0.42 Mild overheating 6 750 1 10 0.35 dense 7 750 3 10 0.25 Unfused 8 750 5 10 0.15 Unfused 9 750 2 5 0.18 dense 10 750 2 15 0.48 dense 11 750 2 20 0.60 dense 12 750 2 25 0.75 Slight non-fusion

[0040] It is worth noting that, as shown in Table 1, for No. 3 and No. 6, under the same conditions of laser power P=750W and total powder feeding rate F=10g / min, the scanning speed is reduced by half, that is, the heat input per unit length P / v increases from 375 to 750W·s / mm, but the single layer thickness is 0.35mm. The physical mechanism is as follows: under the condition of low total powder feeding rate, reducing the scanning speed increases the heat input. The width of the molten pool increases due to lateral heat diffusion, but the powder supply is constant. The powder spreads on a wider molten pool cross section. Under the condition of limited powder supply, the single layer thickness tends to saturate, so the thicknesses of the two are similar.

[0041] On the other hand, the powder feed rate F / v per unit length is the same for No. 6 and No. 11, but No. 11 has a higher total powder feed rate, more powder in the molten pool that can participate in melting, and the molten pool flow is more intense and the powder capture efficiency is higher at a higher scanning speed. Therefore, the single layer thickness of No. 11 (0.60 mm) is significantly greater than that of No. 6 (0.35 mm). This shows that when F / v is the same, the single layer thickness is not only determined by the F / v ratio, but mainly by the total powder feed rate F.

[0042] It is worth noting that the laser power in Table 1 is the power in continuous wave mode. In pulse mode, this invention adjusts the peak power, pulse width and frequency to make the peak temperature of the molten pool equivalent to 700-800W continuous wave, and the peak power is 900-1200W. Pulse mode can reduce the high temperature dwell time, which is beneficial to suppressing the interface reaction.

[0043] Furthermore, as shown in Table 1, the comparison between No. 6 and No. 10 indicates that under the condition of low total powder feeding rate, even if the scanning speed is reduced to increase heat input, the single layer thickness is still limited by the powder supply, making it difficult to achieve the thickness level under high powder feeding rate. Moreover, a dense and defect-free cladding layer can be obtained within the range of laser power 700-800 W, scanning speed 1-2 mm / s, and total powder feeding rate 10-20 g / min, with a single layer thickness between 0.28-0.60 mm.

[0044] Based on this, a four-dimensional coupled process model was established, and the compact forming process window was determined as follows:

[0045] Laser power 700-800 W, scanning speed 1-2 mm / s, total powder feeding rate 10-20 g / min, single layer thickness 0.28-0.60 mm;

[0046] The target coating design has a total height of 3.0 mm, with the carbon fiber volume fraction continuously increasing from 5 vol% on the substrate side to 25 vol% on the surface. The planned carbon fiber powder feeding rate is... The dynamic function is of linearly increasing form:

[0047]

[0048] in, The feed rate of the bottom carbon fiber is given by k, which is the gradient coefficient. The calculated value of k is 0.74 g / min. mm;

[0049] During the dynamic powder feeding process with dual cylinders, the control system maintains the total powder feeding rate. Constant carbon fiber powder feeding rate With aluminum-based alloy powder feeding rate The sum always equals the total powder delivery rate, that is, it satisfies:

[0050]

[0051]

[0052] in, The carbon fiber powder feeding rate at the cladding height h is... The powder feeding rate of the aluminum-based alloy at the cladding height h is [value missing]. For the total powder feeding rate, take 15. , The carbon fiber powder feeding rate is 0.51 g / min when h=0 at the bottom layer, and h is the current cladding height;

[0053] From formulas (1) and (2), it can be seen that, It increases linearly with height h. The sum of the two values ​​remains constant as the height h decreases linearly. =15 The specific values ​​are as follows:

[0054] When h=0: At this point, the volume fraction of carbon fiber is 5%. The volume fraction of the aluminum-based alloy is 95%. That is, the matrix side uses aluminum-based alloy as the continuous phase and carbon fiber as the dispersed reinforcing phase;

[0055] When h = 3.0 mm: At this point, the carbon fiber volume fraction is 25 vol%, and the aluminum-based alloy volume fraction is 75 vol%.

[0056] Therefore, from the matrix side to the surface layer, the carbon fiber feed rate increases from 0.51 g / min to 2.73 g / min, while the aluminum-based alloy feed rate decreases from 14.49 g / min to 12.27 g / min. The sum of the two always equals the total feed rate of 15 g / min, thereby achieving a gradient distribution of carbon fiber volume fraction that continuously increases from 5 vol% on the matrix side to 25 vol% on the surface layer.

[0057] At this point, take At constant density, during dynamic powder feeding with dual feeders, the carbon fiber mass fraction is: ;

[0058] Total powder delivery rate: ;

[0059] The conversion formula between carbon fiber volume fraction and mass fraction is as follows:

[0060] The conversion formula for carbon fiber powder feeding rate is:

[0061]

[0062] in, This refers to the carbon fiber powder feeding rate, i.e., the carbon fiber mass flow rate, expressed in g / min.

[0063] This refers to the aluminum-based alloy powder feeding rate, i.e., the aluminum-based alloy mass flow rate, expressed in g / min.

[0064] This represents the volume fraction of carbon fiber.

[0065] This refers to the mass fraction of carbon fiber.

[0066] For the density of carbon fiber, take 1.8 g / L. ;

[0067] The density of the aluminum-based alloy is taken as 2.7 g / L. ;

[0068] At h=0, the target carbon fiber volume fraction ,correspond =0.51 ;

[0069] At h=3.0mm, the target carbon fiber volume fraction ,correspond =2.73 ;

[0070] The dynamic function planned accordingly is:

[0071]

[0072]

[0073] Then, based on the main force direction of the part during service, set it to be along the X-axis, and plan the layered scanning path:

[0074] In the low carbon fiber region (h=0-1.5mm), a reciprocating filling path is used with an overlap rate of 40%. In the high carbon fiber region (h=1.5-3.0mm), a unidirectional parallel scanning path parallel to the X-axis is used. After setting, proceed to the next step.

[0075] It is worth noting that the CF volume fraction in the low-carbon fiber region is 5-15 vol%, while the CF volume fraction in the high-carbon fiber region is 15-25 vol%.

[0076] S3. Dynamic powder feeding and multi-field coordinated cladding: A fiber laser with a wavelength of 1070nm, a maximum power of 2000W, and a spot diameter of 3mm is used for cladding under the protection of argon gas with a protective gas flow rate of 15 L / min. The bottom layer region adopts a long pulse width and low peak power pulse mode, while the surface region switches to a short pulse width and high peak power pulse mode.

[0077] It is worth noting that the powder delivery delay time should be pre-calibrated based on the pipeline length and carrier gas flow rate. Introduce height prediction into the control algorithm: ;

[0078] in, It's the scanning speed. The powder delivery delay time allows the powder delivery rate adjustment command to be issued τ time in advance, so that the powder speed when it reaches the nozzle corresponds exactly to the actual cladding height.

[0079] It is worth noting that the height range is defined based on the height corresponding to a target carbon fiber volume fraction of 15 vol%, according to a dynamic function. ,when When, we can solve for h. 1.45mm, rounded down to 1.5mm as the dividing line;

[0080] It is worth noting that the bottom layer region, denoted as h = 0-1.5 mm, adopts a long pulse width and low peak power pulse mode with a pulse width of 8 ms, a peak power of 900 W, a frequency of 50 Hz, and a duty cycle of 40%.

[0081] The surface region, denoted as h = 1.5-3.0 mm, uses a short pulse width and high peak power pulse mode with a pulse width of 3 ms, a peak power of 1200 W, a frequency of 80 Hz, and a duty cycle of 24%. The galvanometer system controls the laser beam to oscillate in a circular motion with a oscillation frequency of 200 Hz and an amplitude of 1.5 mm.

[0082] It is worth noting that in pulsed laser mode, although the average power of 288-360W is lower than that of continuous wave power of 700-800W, the peak power of 900-1200W is higher. The instantaneous temperature of the molten pool is higher during pulse conduction, and the effective heat input is comparable to that of 700-800W continuous wave. The advantage of pulsed mode is that the cooling effect during the off period shortens the high temperature dwell time, which is beneficial to suppressing the interfacial reaction between carbon fiber and aluminum matrix.

[0083] During the cladding process, the control system reads the current cladding height h in real time and substitutes it into the dynamic function for calculation. and The powder feeding rate is precisely controlled by adjusting the carrier gas flow rate of the two powder cylinders and the rotation speed of the turntable. The powder feeding nozzle adopts a bypass converging structure. Carbon fiber powder and aluminum-based alloy powder are converged at the nozzle outlet through two independent channels and fed into the molten pool. At the same time, the molten pool monitoring sensor collects the molten pool radiation signal in real time, with a sampling frequency of 1000 Hz. The interface analysis results of the prepared gradient coating are shown in Table 2 below:

[0084] Table 2. Composition and Performance Analysis of Gradient Coating Sections

[0085] Height h / mm CF volume fraction / vol% Microhardness / HV content Fiber orientation coefficient 0.3 6.2 128 Not detected 0.15 0.8 9.5 142 Not detected 0.18 1.5 15.3 168 0.05 0.32 2.2 20.1 195 0.08 0.58 3.0 24.8 218 0.12 0.76

[0086] It is worth noting that in Table 2 The content is equivalent to the relative intensity of XRD;

[0087] Table 2 shows that the volume fraction of carbon fiber in the coating increases continuously from the aluminum alloy substrate side to the surface layer, and the microhardness gradually increases from 128 HV to 218 HV. XRD analysis indicates that... The content is extremely low, and the relative strength is ≤0.12, indicating that SiC / The double coating effectively suppressed the interfacial reaction, and the fiber orientation coefficient reached 0.58-0.76 in the carbon fiber rich region with h = 2.2-3.0 mm, indicating that the carbon fibers achieved good preferred orientation along the X-axis.

[0088] Example 2

[0089] Based on Example 1, this example optimizes and compares the carbon fiber surface coating structure to demonstrate the effectiveness of the SiC internal coating. The outer coating provides synergistic protection. All comparative samples were prepared using the same laser parameters, scanning path, and cladding process as in Example 1. The coating was prepared under single-pass cladding conditions, and the sampling location was 5 mm from the starting end of the cladding layer in the middle.

[0090] S1. In the carbon fiber pretreatment step, five groups of carbon fiber samples with different coating structures were prepared:

[0091] Comparative Example 1: Bare carbon fiber, without any surface coating treatment;

[0092] Comparative Example 2, None The outer coating consists of only a 0.3 mm SiC inner coating. :

[0093] Sample A: SiC inner coating 0.3 + Outer coating 0.2 ;

[0094] Sample B: SiC inner coating 0.3 + Outer coating 0.5 ;

[0095] Sample C: SiC inner coating 0.3 + Outer coating 1.0 ;

[0096] The SiC inner coating preparation parameters are the same as in Example 1;

[0097] S2. The cladding process parameters are exactly the same as in Example 1. Single-pass cladding is used. The sampling position is 5 mm away from the starting end of the cladding layer in the middle. Three parallel samples are prepared for each group of samples.

[0098] S3, the coatings prepared for the five groups of samples The content was quantitatively analyzed by XRD using a CuKa target, tube voltage of 40 kV, tube current of 30 mA, scanning range of 10°-80°, step size of 0.02°, and scanning rate of 2° / min. The Al(111) peak was used as a reference for calculation. The relative intensity of the (012) peaks was used to observe the interface morphology of the carbon fiber using SEM, and the average etching depth of the fiber was measured. The tensile strength of the coating was tested using a tensile testing machine, and the average value of three samples in each group was taken. The results are shown in Table 3:

[0099] Table 3 reflects the different Effect of outer coating thickness on interfacial reaction

[0100] sample Coating structure relative strength Average fiber etching depth / nm Coating tensile strength / MPa Comparative Example 1 bare carbon fiber 0.65 120 320 Comparative Example 2 Only the SiC internal coating is 0.3. 0.42 85 385 A SiC 0.3 + 0.2 0.18 32 512 B SiC 0.3 + 0.5 0.06 12 598 C SiC 0.3 + 1.0 0.05 10 605

[0101] Table 3 shows that the bare carbon fiber... With a relative strength as high as 0.65, a fiber etching depth of 120 nm, and a coating tensile strength of only 320 MPa, it is evident that the unprotected carbon fibers underwent a severe interfacial reaction with the Al matrix at the high temperature of laser cladding, resulting in severe fiber damage and only a SiC inner coating without any protective coating. In control sample 2 with outer coating, The relative strength dropped to 0.42, and the average etching depth of the fiber was 85 nm, indicating that although the SiC coating itself was eroded by Al to a certain extent, the direct exposure of the carbon fiber was delayed, but the reaction between SiC and Al still existed and caused obvious interface damage.

[0102] When adding 0.2μm After the outer coating is applied, as shown in sample A, The relative strength decreased to 0.18, and the fiber etching depth decreased to 32 nm;

[0103] when When the outer coating thickness is 0.5 μm, as shown in sample B, The relative strength further decreased to 0.06, and the fiber etching depth was only 12 nm, indicating that The outer coating acts as a diffusion barrier layer, effectively blocking the diffusion channels of Al atoms into the SiC inner coating and the carbon fiber surface.

[0104] when When the thickness continues to increase to 1.0 μm, as shown in sample C, The content and etching depth did not decrease significantly further, indicating that the content is around 0.5μm. The outer coating is sufficient to provide an effective diffusion barrier.

[0105] Example 3

[0106] Based on Example 1, this example optimizes different process parameters for carbon fiber-rich regions to verify the forming quality under high carbon fiber content conditions.

[0107] S1. Carbon fiber pretreatment is the same as in Example 1, and aluminum-based alloy powder is the same as in Example 1;

[0108] S2, the target coating carbon fiber volume fraction increases continuously from 5 vol% on the matrix side to 30 vol% on the surface, with a total height of 4.0 mm. , k = 3.0 g / ,but = 13.2 g / min, the carbon fiber rich region was set at h = 2.0-4.0 mm, and the CF volume fraction was approximately 17.5-30 vol%.

[0109] In carbon fiber-rich regions, the effects of three laser parameter strategies on fiber orientation and... The effects of the generation are shown in Table 4:

[0110] Table 4. Comparison of laser parameters in carbon fiber-rich regions;

[0111] Strategy Laser mode Pulse width / ms Peak power / W Scan path Fiber orientation coefficient relative strength I Continuous wave - 800 One-way parallel 0.35 0.28 II pulse 5 1000 One-way parallel 0.52 0.15 III pulse 3 1200 One-way parallel 0.76 0.10

[0112] Table 4 shows that using the pulsed laser mode of Strategy III, combined with a unidirectional parallel scanning path, achieved the highest fiber orientation coefficient of 0.76 and the lowest [missing information] in the carbon fiber-rich region. With a relative intensity of 0.10, the short pulse width reduces the high-temperature residence time of the molten pool, and... The diffusion barrier layer works synergistically to effectively suppress interfacial reactions. Meanwhile, the stable temperature gradient formed by unidirectional parallel scanning guides the carbon fibers to align preferentially along the scanning direction.

[0113] S3: During the cladding process, the length of the short-cut carbon fiber... = 0.15 mm, the single-layer cladding thickness D in the carbon fiber rich region is 0.40 mm. = 0.375, which satisfies the condition. These conditions are conducive to the directional alignment of carbon fibers in the molten pool.

[0114] Example 4

[0115] Based on Example 1, this example verifies the effectiveness of the closed-loop control system for the molten pool monitoring sensor.

[0116] S1, the steps and process parameters are the same as in Example 1;

[0117] S2, the steps and process parameters are the same as in Example 1;

[0118] S3. Based on the process of Example 1, an infrared temperature sensor and a high-speed CCD camera are integrated as molten pool monitoring sensors. The infrared temperature sensor collects the surface temperature signal of the molten pool in real time with a sampling frequency of 1000 Hz. The high-speed CCD camera collects the morphology image of the molten pool in real time with a frame rate of 500 fps. The normal range of molten pool temperature is set to 1000-1100 ℃. The CVD deposition atmosphere is an inert atmosphere, such as argon / hydrogen. Under this atmosphere, carbon fiber will not undergo significant oxidation and degradation at 1050°C. When the temperature exceeds the range, closed-loop adjustment is automatically triggered.

[0119] The closed-loop adjustment is as follows: reduce laser power by 5% when the temperature is too high, and increase laser power by 5% when the temperature is too low; adjust the scanning speed by ±10% when the molten pool area deviates from the set value by ±15%.

[0120] Comparative experiment: Comparative group 1 used the process of Example 1 but without the use of closed-loop control for molten pool monitoring; comparative group 2 used the process of Example 1 and used closed-loop control. Five samples were prepared for each group, and the porosity and crack density in the coating were detected. The specific results are shown in Table 5.

[0121] Table 5. Impact of Closed-Loop Control on Coating Defects

[0122] Group Average porosity / % Crack density / Incomplete fusion defect rate / % Control group 1, no closed loop 2.8±0.4 0.45±0.08 12% Comparison Group 2, Closed-Loop Control 0.9±0.2 0.12±0.03 2%

[0123] It is worth noting that the data in the table are the average value ± standard deviation of 5 samples;

[0124] Furthermore, as shown in Table 5, after introducing a closed-loop control system based on molten pool monitoring sensors, the coating porosity decreased from 2.8% to 0.9%, and the crack density decreased from 0.45%. Reduced to 0.12 The rate of non-fusion defects decreased from 12% to 2%, resulting in a significant improvement in coating quality.

[0125] Example 5

[0126] Based on Example 1, this example verifies the influence of different carbon fiber volume fraction gradient distributions on the residual stress of the coating.

[0127] S1. Carbon fiber pretreatment is the same as in Example 1, with a SiC inner coating of 0.3%. , Outer coating 0.5 ;

[0128] S2. Prepare 3 parallel samples for each sample. Data are taken as mean ± standard deviation. Design three gradient distribution forms: linear gradient (i.e., the scheme in Example 1), concave nonlinear gradient (where the carbon fiber content in the bottom layer increases slowly and the surface layer increases rapidly), and convex nonlinear gradient (where the carbon fiber content in the bottom layer increases rapidly and the surface layer increases slowly). Total height 3.0 mm, total powder feeding rate. Similar to Example 1, the sum of the carbon fiber powder feeding rate and the aluminum-based alloy powder feeding rate is always equal to... =15 g / min;

[0129] S3. The laser process parameters are the same as in Example 1. The residual stress on the coating surface is measured by X-ray diffraction, and the results are shown in Table 6.

[0130] Table 6 Residual stress of coatings with different gradient distributions

[0131] gradient form CF content in the bottom layer / vol% Surface CF content / vol% Surface residual stress / MPa Bond strength / MPa linear 5.0 24.8 -85±6 185±8 concave upward type 5.0 25.1 -62±5 210±7 Convex type 5.2 24.5 -98±7 172±6

[0132] Among them, the concave nonlinear gradient: (g / min), the growth rate is slow in the lower layer and fast in the upper layer;

[0133] Convex nonlinear gradient: The underlying layer grows rapidly, while the surface layer grows slowly.

[0134] The linear gradient is: ;

[0135] As shown in Table 6, the coating with the concave nonlinear gradient distribution, where the carbon fiber content increases slowly in the bottom layer and rapidly in the surface layer, exhibits the lowest residual compressive stress (-62±5MPa) and the highest bonding strength (210±7MPa). This indicates that maintaining high aluminum matrix continuity in the low-carbon fiber area of ​​the bottom layer is beneficial for forming a good metallurgical bond with the substrate, while the rapid increase in the carbon fiber-rich area of ​​the surface layer can effectively improve surface hardness and wear resistance.

[0136] The above are merely embodiments of the present invention and do not limit the patent scope of the present invention. Any equivalent structural or procedural transformations made based on the content of the present invention specification and drawings, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.

Claims

1. A method for gradient cladding of carbon fiber and aluminum matrix using a dual-cylinder dynamic powder feeding system, characterized in that, Includes the following steps: S1. Substrate and powder pretreatment: The aluminum alloy substrate is degreased, sandblasted and roughened and preheated to relieve stress. The carbon fiber is pretreated with anti-oxidation coating. The carbon fiber and the dried and sieved aluminum alloy powder are separately loaded into the carbon fiber powder cylinder and the aluminum alloy powder cylinder. S2. Establishing a process model and path planning: Single-pass cladding experiments were conducted using the controlled variable method to analyze the correspondence between laser power, scanning speed, total powder feeding rate, and single-layer cladding thickness. A four-dimensional coupled process model including laser power, scanning speed, total powder feeding rate, and single-layer cladding thickness was established, and the process window for dense forming was determined. Based on the distribution requirements of carbon fiber volume fraction along the cladding height in the coating design target, the dynamic functions of carbon fiber powder feeding rate and aluminum-based alloy powder feeding rate with cladding height were planned. At the same time, based on the main force direction during the service of the part, a layered laser scanning path strategy was planned. The layered laser scanning path strategy includes at least a reciprocating filling path used in the low carbon fiber volume fraction area and a unidirectional parallel scanning path used in the carbon fiber rich area. S3. Dynamic powder feeding and multi-field coordinated cladding: Using a high-power laser as the heat source, under inert gas protection, cladding is performed layer by layer from the aluminum alloy substrate side upwards according to the process window, dynamic function, and layered laser scanning path strategy determined in step S2. During the cladding process, the control system of the cladding equipment reads the current cladding height in real time, substitutes it into the dynamic function to calculate and adjust the powder feeding rate of the dual barrels, so that the carbon fiber content increases continuously from the substrate side to the surface layer. At the same time, the output energy parameters of the laser and the scanning path topology are synchronously modulated with the change of coating height to coordinately control the heat input of the molten pool and the distribution and orientation of the carbon fibers.

2. The dual-cylinder dynamic powder feeding carbon fiber aluminum-based gradient cladding method according to claim 1, characterized in that, In step S1, the antioxidant coating pretreatment of carbon fiber involves first preparing a SiC ceramic inner coating layer on the surface of the carbon fiber using chemical vapor deposition, and then preparing a layer on the surface of the SiC ceramic inner coating layer. Ceramic outer coating.

3. The dual-cylinder dynamic powder feeding carbon fiber aluminum-based gradient cladding method according to claim 1, characterized in that, In step S1, a side-axis converging powder feeding nozzle is used, and carbon fiber powder and aluminum-based alloy powder are converged at the nozzle outlet through two independent channels and fed into the molten pool.

4. The dual-cylinder dynamic powder feeding carbon fiber aluminum-based gradient cladding method according to claim 1, characterized in that, In step S2, the carbon fiber powder feeding rate With aluminum-based alloy powder feeding rate The dynamic function that varies with height h satisfies: total powder feeding rate Keeping constant, the volume fraction of carbon fiber increases linearly or non-linearly with height h, and .

5. The dual-cylinder dynamic powder feeding method for carbon fiber aluminum-based gradient cladding according to claim 1, characterized in that, In step S2, the layered laser scanning path strategy is as follows: a reciprocating filling path is used in the bottom layer area with low carbon fiber content, and a unidirectional parallel scanning path parallel to the main force direction of the part is used in the surface layer area rich in carbon fiber.

6. The dual-cylinder dynamic powder feeding method for carbon fiber aluminum-based gradient cladding according to claim 1, characterized in that, In step S3, the synchronous modulation of the laser output energy is specifically as follows: a pulsed laser mode is adopted, with a long pulse width and low peak power pulse waveform in the bottom layer region with low carbon fiber content, and a short pulse width and high peak power pulse waveform in the surface layer region rich in carbon fiber.

7. The dual-cylinder dynamic powder feeding method for carbon fiber aluminum-based gradient cladding according to claim 1, characterized in that, In step S3, the laser beam is controlled to swing in a circular or figure-eight pattern via a galvanometer system, with a swing frequency of 50-500Hz.

8. The dual-cylinder dynamic powder feeding method for carbon fiber aluminum-based gradient cladding according to claim 1, characterized in that, In step S3, the length of the chopped carbon fiber The thickness D of the single-layer cladding in the carbon fiber-rich region times.

9. The dual-cylinder dynamic powder feeding method for carbon fiber aluminum-based gradient cladding according to claim 1, characterized in that, Step S3 also includes an integrated molten pool monitoring sensor to collect molten pool radiation signals in real time, and automatically mark the defect location or adjust the process parameters in a closed loop when the signal is abnormal.