A method for preparing an AlN-BN dual-phase ceramic particle synergistically reinforced CuNi30 alloy composite component based on a powder core wire

By pre-encapsulating AlN and BN ceramic particles in CuNi30 alloy powder core wire and utilizing CMT arc additive manufacturing technology, the wear and corrosion problems of CuNi30 alloy in seawater environment were solved, achieving improvements in hardness and wear resistance, and expanding its application in corrosion-resistant and wear-resistant working conditions.

CN123128530APending Publication Date: 2026-11-20CHONGQING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611005205.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-07
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively address the wear and corrosion problems of CuNi30 alloy in seawater environments, and it also suffers from severe thermal softening at high temperatures, limiting its application in integrated corrosion-resistant, wear-resistant, and thermally conductive components.

Method used

Using CMT (Chemical Arc Additive Manufacturing) technology, AlN and BN dual-phase ceramic particles are pre-encapsulated inside CuNi30 alloy powder core wire. AlN/BN dual-phase ceramic particles are deposited layer by layer to synergistically reinforce CuNi30 alloy components, achieving synchronous feeding and melting deposition of ceramic particles and metal materials.

Benefits of technology

It improves the hardness and wear resistance of CuNi30 alloy, enhances the stability of ceramic particle addition, expands its application in corrosion-resistant and wear-resistant conditions, reduces wear and corrosion risks, and improves high-temperature stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128530A_ABST
    Figure CN123128530A_ABST
Patent Text Reader

Abstract

The application discloses a preparation method of an AlN-BN dual-phase ceramic particle synergistically reinforced CuNi30 alloy composite component based on a powder core wire, and the CuNi30 alloy strip is used for coating CuNi30 alloy powder, AlN ceramic particles and BN ceramic particles to prepare a copper-based composite material powder core wire, powder and wire are synchronously fed into a molten pool by taking the powder core wire as feeding material, the uniform dispersion distribution of the ceramic particles is ensured, and the AlN / BN dual-phase ceramic particle synergistically reinforced CuNi30 alloy component is prepared. The AlN / BN ceramic particles are synchronously fed into the CuNi30 metal material and in-situ composite by the powder core wire, the problems of unstable powder feeding, powder scattering and difficult control of actual feeding amount in the external powder feeding process of the fine ceramic powder are avoided. The application is beneficial to improving the hardness, wear resistance, thermal stability and comprehensive service performance of the CuNi30 alloy on the basis of keeping high toughness and high corrosion resistance of the CuNi30 alloy, and is suitable for manufacturing of marine engineering equipment, seawater heat exchangers, ship pipelines, pump valve parts and corrosion-resistant and wear-resistant complex components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of copper-nickel alloy composite materials and arc additive manufacturing technology, specifically a method for preparing CuNi30 alloy composite material components based on AlN-BN dual-phase ceramic particles synergistically reinforced with powder-core wire. Background Technology

[0002] CuNi30 alloy is a typical copper-nickel corrosion-resistant alloy with good seawater corrosion resistance, biofouling resistance, thermal conductivity, and toughness. It is widely used in ships, marine engineering, seawater heat exchangers, seawater pipelines, condensers, pump and valve components, and structural components operating in high-salt-spray corrosion environments. However, as a copper-based alloy, CuNi30 alloy has relatively low matrix hardness, making it susceptible to wear under conditions such as seawater erosion, silt abrasion, powder erosion, and sliding friction. Once wear occurs on the material surface, the protective film is easily damaged, leading to accelerated wear and corrosion coupling and reduced service life of components. Furthermore, CuNi30 alloy also exhibits some thermal softening under high-temperature or thermal cycling environments, limiting its further application in integrated corrosion-resistant, wear-resistant, thermally conductive, and heat-resistant components.

[0003] Ceramic particle-reinforced copper-based composites are an important method for improving the wear resistance and high-temperature stability of CuNi30 alloys. AlN ceramic particles possess high hardness, good high-temperature stability, and high thermal conductivity, making them suitable for improving the microhardness and heat resistance of copper-nickel alloys. BN ceramic particles exhibit electrical insulation and self-lubricating properties, forming a solid lubricant during friction and, to some extent, blocking local electrochemical reaction pathways. Introducing AlN and BN dual-phase ceramic particles into the CuNi30 alloy matrix is ​​expected to achieve a synergistic effect of dispersion strengthening, self-lubrication and friction reduction, and interfacial barrier. Existing metal / ceramic composites are mostly prepared using methods such as powder metallurgy, stir casting, laser cladding, or external powder feeding. Powder metallurgy methods suffer from limitations in component size and complex processes; stirring casting methods are prone to ceramic particle agglomeration, macroscopic segregation, and insufficient interfacial bonding; laser cladding methods for manufacturing CuNi30 alloys suffer from high reflectivity and low efficiency in manufacturing large and complex components, and when AlN / BN ceramic particles are fine, problems such as powder clogging and powder scattering easily occur; laser powder bed melting methods also suffer from high reflectivity, and when the ceramic content increases, problems such as reduced powder spreading stability, interfacial thermal stress concentration, and increased cracking tendency easily occur; external powder feeding methods are greatly limited in terms of powder feeding stability and forming adaptability.

[0004] CMT (Continuous Metallurgical Mass Production) arc additive manufacturing technology features low heat input, stable droplet transition, minimal spatter, high forming efficiency, and suitability for manufacturing medium to large-sized components. By pre-encapsulating AlN / BN ceramic particles within CuNi30 alloy core wires and then performing layer-by-layer deposition using CMT, simultaneous feeding, melting, deposition, and in-situ composite of ceramic particles and CuNi30 metal can be achieved. This reduces problems associated with external powder feeding and powder bed laying, such as unstable powder delivery, low powder utilization, limited ceramic content, and component cracking. Therefore, developing a CuNi30 alloy composite component synergistically reinforced with AlN / BN dual-phase ceramic particles based on core wires and CMT additive manufacturing, and its preparation method, is of great significance for improving the hardness of CuNi30 alloy, enhancing particle incorporation stability, and expanding its application in corrosion-resistant and wear-resistant conditions. Summary of the Invention

[0005] The purpose of this invention is to provide a method for preparing AlN-BN dual-phase ceramic particle synergistic reinforcement CuNi30 alloy composite material components based on powder-core wire, comprising the following steps:

[0006] Step 1: Mix CuNi30 alloy powder, AlN ceramic particles and BN ceramic particles to obtain mixed powder, and then dry the mixed powder.

[0007] Step 2: Roll the CuNi30 alloy strip into an open tube, fill the interior of the CuNi30 alloy strip with mixed powder, and prepare CuNi30-based powder core wire.

[0008] Step 3: Establish a three-dimensional digital model based on the shape of the component to be prepared, and plan the CMT arc additive manufacturing deposition path;

[0009] Step 4: Set the CMT arc additive manufacturing process parameters based on the material properties of CuNi30-based powder-core wire;

[0010] Step 5: Using CMT arc additive manufacturing technology, CuNi30-based powder core wire is melted and deposited layer by layer on the substrate, so that the CuNi30-based powder core wire is fed into the molten pool simultaneously with the welding wire to prepare CuNi30 alloy components with AlN / BN dual-phase ceramic particles synergistic reinforcement.

[0011] Furthermore, the mixed powder is dried before being filled into the CuNi30 alloy strip.

[0012] Furthermore, the AlN ceramic particles are hexagonal aluminum nitride, and the BN ceramic particles are hexagonal boron nitride.

[0013] Furthermore, the total mass of the AlN ceramic particles and BN ceramic particles accounts for 2%-10% of the total mass of the core wire.

[0014] Furthermore, the mass ratio of the AlN ceramic particles to the BN ceramic particles is 1:3-3:1.

[0015] Furthermore, the total mass of ceramic particles was controlled within the target range by adding CuNi30 alloy powder.

[0016] Furthermore, the mass fraction of Ni element in the CuNi30 alloy strip and alloy powder is 28%-32%.

[0017] Furthermore, the CMT arc additive manufacturing process parameters include welding characteristic curves, welding current, welding voltage, welding torch travel speed, wire feed speed, shielding gas flow rate, and interpass cooling time.

[0018] A CuNi30 alloy component synergistically reinforced with AlN / BN dual-phase ceramic particles, the component being prepared by the method described above;

[0019] The composite material component includes a CuNi30 alloy matrix and AlN ceramic particles and BN ceramic particles dispersed in the CuNi30 alloy matrix;

[0020] The AlN ceramic particles and BN ceramic particles coexist as two ceramic reinforcing phases in the CuNi30 alloy matrix.

[0021] Furthermore, the component serves as a corrosion-resistant and wear-resistant component in marine engineering equipment, seawater heat exchangers, ship pipelines, corrosion-resistant and wear-resistant sliding parts, seawater pump valve components, or in high salt spray environments.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1) This invention uses CuNi30 alloy strip to coat CuNi30 alloy powder, AlN ceramic particles and BN ceramic particles to prepare CuNi30-based composite powder core wire, so that AlN / BN ceramic particles are fed into the CMT molten pool simultaneously with CuNi30 metal material, avoiding problems such as difficulty in fine powder feeding, powder scattering, discontinuous powder feeding and low powder utilization that may occur in external powder feeding, interlayer pre-powdering or laser coaxial powder feeding.

[0024] 2) This invention uses CMT electric arc additive manufacturing technology, which has the characteristics of low heat input, stable droplet transition, less spatter and high forming efficiency. It is beneficial to reduce the burning loss, agglomeration and interfacial thermal cracking tendency of AlN / BN ceramic particles and improve the forming stability of CuNi30-based composite material components.

[0025] 3) This invention controls the total content of AlN and BN ceramic particles to 2%–10% of the total mass of the core wire. When the total ceramic particle content is below 2%, the hardening and strengthening effects of the ceramic particles are not significant; when the total ceramic particle content is above 10%, the ceramic particles are prone to agglomeration, the ceramic / metal interface area increases significantly, and the interfacial thermal stress and local stress concentration increase, leading to an increased risk of interfacial debonding, porosity, lack of fusion, and cracking failure. Therefore, controlling the total content of AlN / BN ceramic particles to 2%–10% can balance the strengthening effect, interfacial bonding quality, and forming crack resistance.

[0026] 4) This invention utilizes the high hardness, high thermal conductivity, and high-temperature stability of AlN ceramic particles to improve the local indentation resistance and hard reinforcement effect of CuNi30 alloy components; utilizes the self-lubricating properties of BN ceramic particles to help reduce the friction coefficient and wear; utilizes the electrical insulation properties of BN ceramic particles to help weaken the tendency of local electrochemical reactions to continue in corrosive media.

[0027] 5) This invention utilizes the good plasticity, toughness and corrosion resistance of the CuNi30 alloy matrix itself to alleviate the local stress concentration caused by the introduction of ceramic particles, so that the AlN / BN ceramic particles mainly exist as dispersed strengthening phases and lubricating functional phases, thereby improving the hardness and wear resistance of the CuNi30 alloy while maintaining its corrosion resistance and toughness.

[0028] 6) Microhardness tests showed that, compared with the CuNi30 alloy without AlN / BN ceramic particles, the hardness of the CuNi30 alloy matrix region increased after the addition of AlN / BN ceramic particles, indicating that the addition of ceramic particles has a significant effect on improving the hardness of the matrix. When the indentation is located in the AlN / BN ceramic particle or ceramic particle-rich area, the local microhardness further increased, indicating that AlN / BN ceramic particles can play a hard reinforcing role in the CuNi30 matrix. The average hardness of the CuNi30 alloy matrix after the addition of AlN / BN ceramic particles was significantly improved. Attached Figure Description

[0029] Figure 1 A schematic diagram of a CuNi30 alloy component synergistically reinforced by AlN / BN dual-phase ceramic particles based on powder-core wire and CMT arc additive manufacturing, provided for an embodiment of the present invention;

[0030] Figure 2 This is a schematic diagram of the dispersion distribution and synergistic mechanism of AlN / BN dual-phase ceramic particles in a CuNi30 alloy matrix.

[0031] Figure 3 Metallographic image of the cross section of the CuNi30 composite material synergistically reinforced by AlN / BN dual-phase ceramic particles.

[0032] Figure 4 Microhardness data of CuNi30 composite material synergistically reinforced by AlN / BN dual-phase ceramic particles.

[0033] Figure 1 In the process, CuNi30 alloy strip 1, CuNi30 alloy powder 2, AlN ceramic particles 3, BN ceramic particles 4, welding torch 5, CuNi30-based powder core wire 6, molten droplet 7, electric arc 8, molten pool 9, substrate 10.

[0034] Figure 2 and Figure 3 In the sample, the round particles are AlN ceramic particles, and the lamellar particles are BN ceramic particles. Both types of ceramic particles are mainly distributed along the grain boundaries. The ceramic reinforcing phase is well bonded to the CuNi30 matrix, with no obvious defects such as cracks, pores, or debonding areas.

[0035] Figure 4 The figures show the microhardness of samples prepared from CuNi30 alloy solid welding wire, the microhardness of the CuNi30 matrix of samples prepared from AlN / BN / CuNi30 powder core wire, the microhardness of BN particles in the matrix, and the microhardness of AlN particles in the matrix, respectively. Detailed Implementation

[0036] The present invention will be further described below with reference to embodiments, but it should not be construed that the scope of the present invention is limited to the following embodiments. Various substitutions and modifications made based on ordinary technical knowledge and common practices in the art without departing from the above-described technical concept of the present invention should be included within the scope of protection of the present invention.

[0037] Example 1:

[0038] A method for preparing AlN-BN dual-phase ceramic particle synergistic reinforcement CuNi30 alloy composite material components based on powder-core wire, comprising the following steps:

[0039] 1) Design of powder core composition: wherein the powder core includes CuNi30 alloy powder 2, spherical hexagonal AlN ceramic particles and layered hexagonal BN ceramic particles; the CuNi30 alloy powder, AlN ceramic particles 3 and BN ceramic particles 4 are fully mixed in a ball mill according to a preset ratio, and the mixed powder is dried.

[0040] 2) Preparation of CuNi30-based powder core wire: The CuNi30 alloy strip 1 is rolled into an open tube, and the mixed powder obtained in step 1) is filled into the interior of the CuNi30 alloy strip. After closing, drawing, annealing and sizing treatment, CuNi30-based powder core wire 6 is obtained.

[0041] 3) Establish a three-dimensional digital model based on the shape of the prepared component, and plan the corresponding CMT arc additive manufacturing deposition path;

[0042] 4) Set the CMT arc additive manufacturing process parameters based on the material properties of CuNi30-based powder-core wire;

[0043] 5) Using CMT arc additive manufacturing technology, CuNi30-based powder core wire is melted and deposited layer by layer on substrate 10. Multiple powders are fed into the molten pool simultaneously with the welding wire to prepare CuNi30 alloy components with AlN / BN dual-phase ceramic particles synergistic reinforcement.

[0044] Example 2:

[0045] A method for preparing a CuNi30 alloy composite material component based on AlN-BN dual-phase ceramic particles synergistically reinforced with powder core wire is described, with the technical content being the same as in Example 1. Further, the AlN ceramic particles and BN ceramic particles are two different ceramic reinforcing phases.

[0046] Example 3:

[0047] A method for preparing a CuNi30 alloy composite material component based on AlN-BN dual-phase ceramic particles synergistically reinforced with powder-core wire is provided, with the technical content being the same as any one of Examples 1-2. Further, the AlN ceramic particles are hexagonal aluminum nitride, and the BN ceramic particles are hexagonal boron nitride.

[0048] Example 4:

[0049] A method for preparing a CuNi30 alloy composite material component based on AlN-BN dual-phase ceramic particles synergistically reinforced with powder core wire is provided, with the technical content being the same as any one of Examples 1-3. Further, the total mass of the AlN ceramic particles and BN ceramic particles accounts for 2%-10% of the total mass of the powder core wire.

[0050] Example 5:

[0051] A method for preparing a CuNi30 alloy composite material component based on AlN-BN dual-phase ceramic particles synergistically reinforced with powder core wire is provided. The technical content is the same as any one of Examples 1-4. Further, the mass ratio of the AlN ceramic particles to the BN ceramic particles is 1:3-3:1, preferably 1:1-2:1.

[0052] Example 6:

[0053] A method for preparing a CuNi30 alloy composite material component based on AlN-BN dual-phase ceramic particles synergistically reinforced with powder-core wire is provided, with the technical content being the same as any one of Examples 1-5. Further, the CuNi30 alloy powder has a particle size of 53μm-105μm, the AlN ceramic particles have a particle size of 5μm-60μm, preferably 10μm, and the BN ceramic particles have a particle size of 1μm-25μm, preferably 5μm.

[0054] Example 7:

[0055] A method for preparing AlN-BN biphase ceramic particles synergistically reinforced CuNi30 alloy composite material components based on powder core wire is provided. The technical content is the same as any one of Examples 1-6. Further, the total mass of ceramic particles is controlled by adding CuNi30 alloy powder to maintain it within the target range, that is, the total mass of AlN ceramic particles and BN ceramic particles accounts for 2%-10% of the total mass of powder core wire.

[0056] Example 8:

[0057] A method for preparing AlN-BN dual-phase ceramic particles synergistically reinforced CuNi30 alloy composite material components based on powder core wire is provided. The technical content is the same as any one of Examples 1-7. Further, the mass fraction of Ni element in the CuNi30 alloy strip and alloy powder is 28%-32%, and the balance is Cu and trace elements.

[0058] Example 9:

[0059] A method for preparing a CuNi30 alloy composite material component based on AlN-BN dual-phase ceramic particles synergistically reinforced with powder core wire is provided. The technical content is the same as any one of Examples 1-8. Further, the diameter of the CuNi30-based powder core wire is 1.2 mm and 1.6 mm, preferably 1.2 mm, and the powder core filling rate is 15%-30%, preferably 25%.

[0060] Example 10:

[0061] A method for preparing AlN-BN dual-phase ceramic particles synergistically reinforced CuNi30 alloy composite material components based on powder-core wire, the technical content of which is the same as any one of Examples 1-9. Further, the CMT arc additive manufacturing process parameters include welding characteristic curves, welding current, welding voltage, welding torch travel speed, wire feed speed, shielding gas flow rate, and interpass cooling time.

[0062] Example 11:

[0063] A method for preparing AlN-BN dual-phase ceramic particle synergistic reinforcement CuNi30 alloy composite material components based on powder-core wire is provided. The technical content is the same as any one of Examples 1-10. Further, in the CMT arc additive manufacturing process, the welding current is 60-184 A, preferably 136 A, the welding voltage is 9.5-17 V, preferably 12.6 V, the wire feed speed is 3.0 m / min-8.0 m / min, preferably 6.0 m / min, the welding torch travel speed is 0.2 m / min-0.8 m / min, preferably 0.3 m / min, the shielding gas is argon or argon-helium mixture, and the shielding gas flow rate is 15 L / min-25 L / min.

[0064] Example 12:

[0065] A CuNi30 alloy component synergistically reinforced by AlN / BN dual-phase ceramic particles is disclosed. The component is prepared by any one of the methods described in Examples 1-11. The composite material component includes a CuNi30 alloy matrix and AlN ceramic particles and BN ceramic particles dispersed in the CuNi30 alloy matrix. The AlN ceramic particles and BN ceramic particles coexist as two ceramic reinforcing phases in the CuNi30 alloy matrix.

[0066] Example 13:

[0067] A CuNi30 alloy component synergistically reinforced by AlN / BN dual-phase ceramic particles, with the same technical content as in Example 12, further wherein the AlN ceramic particles and BN ceramic particles form a good interfacial bond with the CuNi30 alloy matrix, and no obvious ceramic agglomeration bands, continuous interfacial cracks, or interfacial debonding regions are formed in the microstructure.

[0068] Example 14:

[0069] According to the AlN / BN dual-phase ceramic particle synergistic reinforcement CuNi30 alloy component described in Example 12, the component is further used in marine engineering equipment, seawater heat exchangers, ship pipelines, corrosion-resistant and wear-resistant sliding parts, seawater pump valve components, or corrosion-resistant and wear-resistant components serving in high salt spray environments.

[0070] Example 15:

[0071] This embodiment provides a method for preparing AlN / BN dual-phase ceramic particle synergistic reinforcement CuNi30 alloy composite components based on powder-core wire. CuNi30-based powder-core wire is prepared by coating CuNi30 alloy powder, AlN ceramic particles, and BN ceramic particles onto CuNi30 alloy strip. The CuNi30 alloy strip contains 28%–32% Ni by mass, with the balance being Cu and trace amounts of other elements. The CuNi30 alloy powder has a particle size of 53 μm–105 μm, and the AlN and BN ceramic particles have particle sizes of 10 μm and 5 μm, respectively.

[0072] CuNi30 alloy powder, AlN ceramic particles, and BN ceramic particles are placed in a powder mixing device according to a preset ratio for mechanical mixing or low-energy ball milling at a speed of 150 rpm for 2 to 8 hours. After mixing, the mixed powder is placed in a vacuum drying oven for drying at a temperature of 80°C to 150°C for 1 hour.

[0073] CuNi30 alloy strip was rolled into an open tube, and dried mixed powder was filled into the interior of the CuNi30 alloy strip. After closing, drawing and reducing diameter, annealing and sizing treatment, CuNi30-based composite powder core wire with a diameter of 1.2 mm was prepared.

[0074] During the forming process, the outer CuNi30 strip is first melted by the electric arc 8 and forms droplets 7. The core CuNi30 powder is preheated and partially melted during the droplet formation and transition process, and continues to absorb heat, melt and diffuse after entering the molten pool 9 with the droplets.

[0075] During the preparation of the drawn wire, vibration and annealing processes are simultaneously employed. The vibration process promotes the compaction of the mixed powder within the tubular outer sheath of the CuNi30 alloy, while the annealing process reduces work hardening of the CuNi30 alloy strip during the drawing deformation process.

[0076] In this embodiment, by adjusting the size of the CuNi30 alloy strip, the core filling rate, and the total content of AlN and BN ceramic particles, CuNi30-based composite core wires with different ceramic particle contents and different AlN / BN ratios can be obtained.

[0077] Example 16:

[0078] A method for preparing AlN / BN dual-phase ceramic particle synergistic reinforcement CuNi30 alloy composite material components based on powder-core wire is described in Example 13. Further, the total mass of AlN ceramic particles and BN ceramic particles accounts for 2% of the total mass of the powder-core wire, the mass ratio of AlN ceramic particles to BN ceramic particles is 1:1, and the remainder is CuNi30 alloy powder.

[0079] In this embodiment, the content of AlN / BN ceramic particles is low, and the ceramic particles are well dispersed in the CuNi30 alloy matrix without forming a distinct continuous ceramic network. Compared with CuNi30 alloy components without added ceramic particles, the microhardness of the CuNi30 matrix region in this embodiment is improved, indicating that a small amount of AlN / BN ceramic particles can already play a hardening and reinforcing role.

[0080] Example 17:

[0081] A method for preparing AlN / BN dual-phase ceramic particle synergistic reinforcement CuNi30 alloy composite material components based on powder-core wire is described in Example 14. Further, the total mass of AlN ceramic particles and BN ceramic particles accounts for 6% of the total mass of the powder-core wire, the mass ratio of AlN ceramic particles to BN ceramic particles is 1:1, and the remainder is CuNi30 alloy powder.

[0082] In this embodiment, the AlN / BN ceramic particle content is within the preferred range of this invention. During CMT arc additive manufacturing, the CuNi30 alloy strip and CuNi30 alloy powder in the lead wire melt to form a continuous metal matrix. The AlN / BN ceramic particles enter the molten pool simultaneously with the molten metal and are dispersed during the stirring and layer-by-layer solidification process. AlN ceramic particles, as a hard reinforcing phase, can improve the local indentation resistance of the CuNi30 alloy matrix; BN ceramic particles, as a layered ceramic phase, are beneficial for solid lubrication during friction. The co-dispersion of AlN and BN ceramic particles within the CuNi30 alloy matrix creates a synergistic effect of hard reinforcement and lubrication / friction reduction. Microscopic observation shows that AlN / BN ceramic particles are relatively uniformly distributed in the CuNi30 alloy matrix, and the particle-matrix interface is well bonded. No obvious continuous cracks, continuous pores or continuous debonding areas were observed around the particles. The good plasticity and toughness of the CuNi30 alloy matrix can alleviate the local stress concentration caused by the introduction of ceramic particles to a certain extent, thereby reducing the tendency of brittle cracking caused by ceramic reinforcing phase.

[0083] Microhardness testing showed that the hardness of the CuNi30 matrix region in this embodiment was higher than that of the CuNi30 alloy component without AlN / BN ceramic particles; the local hardness of the ceramic particles or the ceramic particle-rich regions was significantly higher than that of the CuNi30 matrix region. This result indicates that AlN / BN ceramic particles can play a hardening and reinforcing role in the CuNi30 matrix, and provide a basis for improving the wear resistance and load-bearing capacity of the material.

[0084] Example 18:

[0085] A method for preparing a CuNi30 alloy composite material component based on AlN / BN dual-phase ceramic particles synergistically reinforced with powder-core wire is described in Example 14. Further, the total mass of AlN ceramic particles and BN ceramic particles accounts for 10% of the total mass of the powder-core wire, the mass ratio of AlN ceramic particles to BN ceramic particles is 1:1, and the remainder is CuNi30 alloy powder.

[0086] In this embodiment, the ceramic particle content is close to the upper limit of the range defined in this invention. By controlling the powder particle size, mixing time, core filling rate, CMT heat input, interlayer cooling time, and interlayer temperature, the tendency of ceramic particle agglomeration and interface cracking can be reduced, allowing AlN / BN ceramic particles to still be well distributed in the CuNi30 alloy matrix.

[0087] Due to the high content of ceramic particles, the ductility, toughness, and crack resistance of the components in this embodiment are more sensitive to process parameters. Therefore, controlling the total content of AlN / BN ceramic particles to no more than 10% is beneficial for balancing hardening effect, interfacial bonding quality, and forming stability.

[0088] Example 19:

[0089] A method for preparing a CuNi30 alloy composite component based on AlN / BN dual-phase ceramic particles synergistically reinforced with powder-core wire is described in Example 14. Further, the mass ratio of AlN ceramic particles to BN ceramic particles is set to 1:3, 1:1, and 3:1, respectively, with the total mass of AlN and BN ceramic particles accounting for 6% of the total mass of the powder-core mixture. When the BN content is high, the proportion of layered ceramic phase in the component increases, which is beneficial for improving the material's self-lubricating properties, but the hardening reinforcement effect is relatively weakened. When the AlN content is high, the proportion of hard ceramic phase in the component increases, which is beneficial for improving local microhardness and indentation resistance, but the friction reduction effect is relatively weakened. When AlN and BN are in an appropriate ratio, the component can achieve a good balance between hardness improvement, particle dispersion, and potential friction reduction effect. This example illustrates that by adjusting the ratio of AlN ceramic particles to BN ceramic particles, the hardness, wear resistance, load-bearing capacity, and functional ceramic phase ratio of the CuNi30 composite component can be controlled according to different service conditions.

[0090] Example 20:

[0091] This embodiment presents microhardness tests on CuNi30 alloy components without added ceramic particles and CuNi30 composite material components with added AlN / BN ceramic particles.

[0092] Indentation tests were conducted on the CuNi30 matrix region, the region near the ceramic particles, and the region containing or enriched with ceramic particles. The microhardness test load was 0.2 kgf, and the holding time was 10 s. It was preferred to use the same load and the same holding time for comparative testing of all samples.

[0093] Test results show that the microhardness of the CuNi30 matrix region is improved after adding AlN / BN ceramic particles compared with CuNi30 alloy components without ceramic particles; when the indentation is located in the AlN / BN ceramic particle or ceramic particle enrichment area, the local microhardness is further increased.

[0094] The results indicate that the addition of AlN / BN ceramic particles can improve the hardness of the CuNi30 alloy matrix. When indentation is applied to the ceramic particles or the particle-rich area, the tested hardness further increases, indicating that AlN / BN ceramic particles can play a hard reinforcing role in the CuNi30 matrix.

[0095] Comparative Example 1:

[0096] This comparative example uses CuNi30 alloy strip to coat CuNi30 alloy powder to prepare powder core wire, without adding AlN ceramic particles and BN ceramic particles. The main technical contents are described in Example 1.

[0097] The CuNi30 component prepared in this comparative example has good plasticity, toughness and corrosion resistance. However, due to the absence of hard ceramic reinforcing phase, its microhardness in the matrix region is lower than that of the CuNi30 composite component with added AlN / BN ceramic particles.

[0098] This comparative example illustrates that the addition of AlN / BN ceramic particles can improve the microhardness of CuNi30 alloy components, providing a basis for improving their indentation resistance and wear resistance.

[0099] Comparative Example 2:

[0100] In this comparative example, the total mass of AlN ceramic particles and BN ceramic particles accounts for 1% of the total mass of the powder core wire, and the mass ratio of AlN ceramic particles to BN ceramic particles is 1:1. The main technical contents are described in Example 2.

[0101] In this comparative example, the content of AlN / BN ceramic particles is relatively low, and the ceramic particles do not provide sufficient hard reinforcement to the CuNi30 matrix, resulting in a limited increase in the microhardness of the matrix region of the component.

[0102] This comparative example illustrates that controlling the total content of AlN / BN ceramic particles to no less than 2% is beneficial to ensuring the hardening and reinforcing effect of the ceramic particles.

[0103] Comparative Example 3:

[0104] In this comparative example, the total mass of AlN ceramic particles and BN ceramic particles accounts for 10% to 12% of the total mass of the powder core mixture, and the mass ratio of AlN ceramic particles to BN ceramic particles is 1:1. The main technical contents are described in Example 2.

[0105] In this comparative example, due to the excessively high ceramic particle content, the interparticle spacing is reduced, making local particle agglomeration more likely. The increased interfacial area between the ceramic particles and the CuNi30 matrix raises the risk of interfacial defects, porosity, and thermal stress concentration. During deposition, agglomerated ceramic particles can hinder molten pool flow and interlayer bonding, leading to localized incomplete fusion, interfacial debonding, or microcracks.

[0106] This comparative example illustrates that while excessive AlN / BN ceramic particles may further increase local hardness, they can impair particle dispersion and interfacial bonding quality, increasing the risk of component cracking and failure. Therefore, this invention limits the total AlN / BN ceramic particle content to 2%–10%.

Claims

1. A method for preparing AlN-BN dual-phase ceramic particle synergistic reinforcement CuNi30 alloy composite material components based on powder-core wire, characterized in that, Includes the following steps: Step 1: Mix CuNi30 alloy powder, AlN ceramic particles and BN ceramic particles to obtain a mixed powder, and then dry the mixed powder. Step 2: The CuNi30 alloy strip is rolled into an open tube, and the mixed powder is filled into the interior of the CuNi30 alloy strip to prepare CuNi30-based powder core wire. Step 3: Establish a three-dimensional digital model based on the shape of the component to be prepared, and plan the CMT arc additive manufacturing deposition path; Step 4: Set the CMT arc additive manufacturing process parameters based on the material properties of CuNi30-based powder-core wire; Step 5: Using CMT arc additive manufacturing technology, CuNi30-based powder core wire is melted and deposited layer by layer on the substrate, so that the CuNi30-based powder core wire is fed into the molten pool simultaneously with the welding wire to prepare CuNi30 alloy components with AlN / BN dual-phase ceramic particles synergistic reinforcement.

2. The method for preparing a CuNi30 alloy composite material component based on powder-core wire and AlN / BN dual-phase ceramic particles synergistically reinforced, as described in claim 1, is characterized in that: Before filling the CuNi30 alloy strip with the mixed powder, the mixed powder is also dried.

3. The method for preparing a CuNi30 alloy composite material component based on powder-core wire and AlN / BN dual-phase ceramic particles synergistically reinforced, as described in claim 1, is characterized in that: The AlN ceramic particles are hexagonal aluminum nitride, and the BN ceramic particles are hexagonal boron nitride.

4. The method for preparing a CuNi30 alloy composite material component based on powder-core wire and AlN / BN dual-phase ceramic particles synergistically reinforced, as described in claim 1, is characterized in that: The total mass of the AlN ceramic particles and BN ceramic particles accounts for 2%-10% of the total mass of the core wire.

5. The method for preparing a CuNi30 alloy composite material component based on powder-core wire and AlN / BN dual-phase ceramic particles synergistically reinforced, as described in claim 3, is characterized in that: The mass ratio of AlN ceramic particles to BN ceramic particles is 1:3-3:

1.

6. A method for preparing a CuNi30 alloy composite material component based on AlN / BN dual-phase ceramic particles synergistically reinforced with powder-core wire, as described in claim 1 or 4, characterized in that: The total mass of ceramic particles was controlled within the target range by adding CuNi30 alloy powder.

7. The method for preparing a CuNi30 alloy composite material component based on AlN / BN dual-phase ceramic particles synergistically reinforced with powder-core wire according to claim 1, characterized in that: The mass fraction of Ni in the CuNi30 alloy strip and alloy powder is 28%-32%.

8. The method for preparing a CuNi30 alloy composite material component based on powder-core wire and AlN / BN dual-phase ceramic particles synergistically reinforced, as described in claim 1, is characterized in that: The CMT arc additive manufacturing process parameters include welding characteristic curves, welding current, welding voltage, welding torch travel speed, wire feed speed, shielding gas flow rate, and interpass cooling time.

9. A CuNi30 alloy component synergistically reinforced with AlN / BN dual-phase ceramic particles, characterized in that: The component is manufactured using the method described in any one of claims 1-8; The composite material component includes a CuNi30 alloy matrix and AlN ceramic particles and BN ceramic particles dispersed in the CuNi30 alloy matrix; The AlN ceramic particles and BN ceramic particles coexist as two ceramic reinforcing phases in the CuNi30 alloy matrix.

10. A CuNi30 alloy component synergistically reinforced with AlN / BN dual-phase ceramic particles according to claim 9, characterized in that: The components are used as corrosion-resistant and wear-resistant components in marine engineering equipment, seawater heat exchangers, ship pipelines, corrosion-resistant and wear-resistant sliding parts, seawater pump valve components, or in high salt spray environments.