A method for preparing a biomimetic porous titanium alloy micropore structure

By combining parametric biomimetic modeling and multiple processes, a three-level cross-scale biomimetic microporous structure of porous titanium alloy was constructed, which solved the problem of uneven pore structure in the existing technology, improved cell adhesion and osteogenic differentiation ability, and is suitable for the mass production of personalized 3D printed titanium implants.

CN123128533APending Publication Date: 2026-11-20CHENGDU MILITARY GENERAL HOSPITAL OF PLA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611272648.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing porous titanium alloy fabrication processes cannot simultaneously achieve macroscopic gradient pore structures, micron-sized mesopore etching, and nanopore activation, resulting in low osseointegration efficiency and a high risk of loosening after implantation.

Method used

A three-level, multi-scale biomimetic porous titanium alloy microporous structure was constructed using a combination of parametric biomimetic modeling, selective laser melting additive manufacturing, negative pressure etching, and anodizing. This structure includes macroscopic gradient pores, micron-sized mesopores, and nanopores. The interconnected multi-level porous structure was formed through three-dimensional modeling, additive manufacturing, negative pressure etching, and anodizing.

Benefits of technology

A three-layer nested biomimetic microporous structure of porous titanium alloy was realized, which solved the problem of uneven micropores on the inner wall of the channel, improved cell adhesion and osteogenic differentiation ability, reduced stress shielding risk, and is suitable for mass production of personalized 3D printed titanium implants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128533A_ABST
    Figure CN123128533A_ABST
Patent Text Reader

Abstract

The application discloses a method for preparing a biomimetic porous titanium alloy micropore structure and belongs to the technical field of biomedical metal material additive manufacturing and surface modification, and comprises the following steps: (1) three-dimensional modeling, (2) additive manufacturing of a porous base body, (3) negative pressure etching for preparing micrometer biomimetic mesopores, (4) anodic oxidation for preparing nanometer micropores, and (5) vacuum biomimetic mineralization activation. The application provides a parameterized biomimetic modeling + SLM additive manufacturing + physical-chemical composite multistage pore-forming integrated method, which can construct a three-stage cross-scale biomimetic porous titanium alloy micropore structure of a'macro gradient TPMS macropore-micrometer etching mesopore-nanometer oxidized micropore' matching a natural bone in one time, and the three-stage cross-scale biomimetic porous titanium alloy micropore structure has the advantages of matching the gradient elastic modulus of a human bone, a high specific surface area, excellent osteogenesis and drug loading performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of additive manufacturing and surface modification technology of biomedical metallic materials, specifically relating to a method for preparing a biomimetic porous titanium alloy microporous structure. Background Technology

[0002] Natural human bones possess a three-tiered biomimetic porous structure: macroscopic interconnected macropores (200–800 μm, bone ingrowth channels), micron-sized mesopores (10–50 μm, cell adhesion and proliferation sites), and nanopores (0.2–2 μm, protein adsorption, biomimetic mineralization, and drug delivery channels). Furthermore, the porous structure exhibits a gradient distribution along the bone thickness direction, with a gradual change in elastic modulus, significantly reducing stress shielding while simultaneously providing mechanical support and osteoinductive activity.

[0003] Titanium alloys are commonly used in medicine to fabricate bone-like structures, but current porous titanium alloy fabrication processes suffer from the following four major drawbacks:

[0004] 1. Single 3D printing SLM can only prepare macroscopic lattice pores of a single scale. The inner wall of the pore is smooth and there are no micron / nano secondary micropores. The specific surface area is low and the cell adhesion is poor, so it cannot replicate the multi-level structure of natural bone.

[0005] 2. Powder foaming and sintering with pore-forming agents result in disordered pores and uncontrollable connectivity, making it difficult to achieve cortical-cancellous gradient pore matching with human skeletal mechanics.

[0006] 3. Traditional anodizing can only generate nanotubes on the surface of dense titanium. The electric field shielding of the internal channels of the porous scaffold results in uneven micropore coverage and the appearance of dead corners.

[0007] 4. The pore size of pores created by single chemical etching is uncontrollable, which can easily damage the strength of the macroscopic lattice framework of 3D printing, making it prone to breakage after implantation.

[0008] Existing technologies cannot simultaneously achieve the following: integrated fabrication of three-level cross-scale biomimetic micropores, namely macroscopic gradient TPMS biomimetic lattice design, micron-sized mesopore etching of pore walls, and global nano-micropore activation. This results in low osseointegration efficiency and a high risk of long-term implantation loosening. Summary of the Invention

[0009] To overcome the shortcomings of traditional processes, such as single pore size, uncontrollable gradient, lack of secondary micropores on the inner wall of the pore, and uneven global modification, this invention provides an integrated method of parametric biomimetic modeling + SLM additive manufacturing + physical and chemical composite multi-level pore-forming. This method constructs a three-level cross-scale biomimetic porous titanium alloy microporous structure that matches natural bone in one go, consisting of "macro-gradient TPMS macropores - micron-etched mesopores - nano-oxidized micropores". It also has gradient elastic modulus matching human bone, high specific surface area, and excellent osteogenic and drug-loading properties.

[0010] A method for preparing a biomimetic porous titanium alloy microporous structure includes the following steps:

[0011] (1) Three-dimensional modeling: Based on human bone CT data, a solid model is constructed, and the gradient porosity and gradient unit cell size are set from the cortical side to the cancellous side along the thickness direction of the implant. The STL printing model is then exported.

[0012] (2) Additive manufacturing of porous matrix: using titanium alloy powder, porous titanium alloy blanks are printed by selective laser melting SLM, and the residual powder inside the pores is removed after printing;

[0013] (3) Preparation of micron-sized biomimetic mesopores by negative pressure etching: The porous titanium alloy blank is placed in a negative pressure immersion tank and etched by negative pressure penetration with a hydrofluoric acid-nitric acid mixed etching solution to generate 10-50 μm interconnected micron-sized biomimetic mesopores on the inner wall of the macroscopic channel;

[0014] (4) Preparation of nanopores by anodizing: The etched blank is subjected to anodizing treatment under negative pressure to generate a 0.2-2 μm nano-TiO2 micropore array in situ on the inner wall of the micron biomimetic mesopore;

[0015] (5) Vacuum biomimetic mineralization activation: The oxidized blank is immersed in simulated body fluid SBF and vacuum impregnated at a constant temperature. After completion, a three-level cross-scale gradient biomimetic microporous porous titanium alloy structure is obtained.

[0016] Furthermore, in step (1), when constructing the solid model, a gradient macroporous structure is designed using a triple-period minimal surface Gyroid unit cell, wherein the gradient porosity is: 15%–35% on the cortical side, 40%–60% on the transition zone, and 65%–85% on the cancellous side; and the unit cell size gradient range is 200–800 μm.

[0017] Furthermore, the titanium alloy powder mentioned in step (2) is Ti6Al4V spherical powder.

[0018] Furthermore, the specific SLM printing process described in step (2) is as follows: laser power 160-220W, scanning speed 800-1400mm / s, layer thickness 30μm, and titanium alloy powder particle size 15-45μm.

[0019] Furthermore, in step (3), the volume ratio of HF:HNO3:H2O in the etching solution is 1:3:10; the corresponding negative pressure during etching is -0.07 to -0.09 MPa, and the etching time is 8 to 18 min.

[0020] Furthermore, the electrolyte in step (4) during the anodizing process is a mixture of ethylene glycol and deionized water at a volume ratio of 98:2, with 0.5% of ammonium fluoride added. During the anodizing process, the oxidation voltage is controlled at 20-40V and the oxidation time is 40-80min. The entire process is under negative pressure to ensure that the electrolyte penetrates all pores.

[0021] Furthermore, in step (5), the vacuum impregnation temperature is controlled at 35-45°C and the impregnation time is 24-48h. After impregnation, a hydroxyapatite biomimetic mineralization layer will be deposited inside the multi-level pores of the blank.

[0022] Furthermore, the pore distribution of the three-level cross-scale gradient biomimetic microporous porous titanium alloy structure described in step (5) is as follows: the first-level gradient Gyroid macropores are 200-800 μm, the second-level coral-like micro-biomimetic mesopores are 10-50 μm, and the third-level nanotube micropores are 0.2-2 μm.

[0023] Furthermore, the elastic modulus of the three-level cross-scale gradient biomimetic microporous porous titanium alloy structure described in step (5) exhibits a continuous gradient distribution of 1 to 18 GPa along the thickness direction.

[0024] The porous titanium alloy prepared by this invention has three nested biomimetic micropores:

[0025] 1) First-order macro-gradient TPMS macropores (200-800μm): mimicking the intertrabecular spaces of cancellous bone, providing channels for new bone to grow inward;

[0026] 2) Secondary micron coral-like mesopores (10-50 μm): etched into the inner wall of macropores, mimicking the structure of bone lacunae, which is conducive to the colonization and spread of bone marrow mesenchymal stem cells;

[0027] 3) Tertiary nano-TiO2 micropores (0.2~2μm): Anodized nanotubes, mimicking the gaps between bone collagen fibers, to enhance protein adsorption, biomimetic mineralization and drug sustained release capabilities;

[0028] The three-layer pore structure is fully interconnected and distributed along the thickness gradient of the implant, ensuring that its mechanical properties match the gradual changes in natural bone and solving the stress shielding problem.

[0029] The present invention has the following advantages over the prior art:

[0030] 1. The three-level cross-scale biomimetic pore integrated molding process of this invention can perfectly replicate the multi-level microstructure of natural cortex-cancellous bone. The negative pressure-assisted global modification during the process completely solves the problem of fluid shielding inside the porous deep pores, and all micropores on the inner wall of the channels are uniformly and leak-free.

[0031] 2. The gradient TPMS lattice precisely controls the elastic modulus from 1 to 18 GPa, significantly reducing the stress shielding between the implant and the host bone, and effectively reducing long-term bone resorption and implant loosening.

[0032] 3. The three-level pore structure of this structure synergistically increases the specific surface area by 3 to 6 times, significantly improving cell adhesion, proliferation, and osteogenic differentiation capabilities. The nanopores can also provide long-lasting drug delivery for antibacterial and bone regeneration promotion.

[0033] 4. The design of first forming the macroscopic framework by SLM and then creating secondary micropores by chemical / electrochemical methods can maintain the overall mechanical strength and take into account both load-bearing capacity and bioactivity.

[0034] 5. The overall process of this invention is controllable and highly repeatable, and it is suitable for the mass production of various personalized 3D printed titanium implants such as spinal fusion devices, artificial joints, and bone defect filling blocks, making it highly valuable for promotion and application. Attached Figure Description

[0035] Figure 1 This is a cross-sectional view of the corresponding material in Embodiment 4 of the present invention. Detailed Implementation

[0036] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions in the embodiments of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of the embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0037] In the embodiments, it should be noted that any processes not specifically described below are those that can be implemented or understood by those skilled in the art by referring to existing technology. Reagents or instruments whose manufacturers are not specified are considered to be conventional products that can be purchased commercially.

[0038] Example 1

[0039] A method for preparing a biomimetic porous titanium alloy microporous structure includes the following steps:

[0040] (1) Three-dimensional modeling: Based on human bone CT data, a solid model was constructed. The gradient macroporous structure was designed using triple-period minimal surface Gyroid unit cell. The gradient porosity and gradient unit cell size were set from the cortical side to the cancellous side along the thickness direction of the implant. The gradient porosity was 15% on the cortical side and 85% on the cancellous side. The gradient range of the unit cell size was 200-800 μm. The STL printing model was then exported.

[0041] (2) Additive manufacturing of porous matrix: Ti6Al4V spherical titanium alloy powder is used to print porous titanium alloy blanks by selective laser melting SLM. The laser power is controlled at 160W, the scanning speed is 800mm / s, the layer thickness is 30μm, and the titanium alloy powder particle size is 15~45μm. After printing, the residual powder inside the pores is removed by cleaning.

[0042] (3) Preparation of micron-sized biomimetic mesopores by negative pressure etching: The porous titanium alloy blank is placed in a negative pressure immersion tank and etched by negative pressure penetration with a mixed hydrofluoric acid-nitric acid etching solution. The volume ratio of HF:HNO3:H2O in the etching solution is 1:3:10. The corresponding negative pressure during etching is -0.07MPa and the etching time is 8min. Interconnected micron-sized biomimetic mesopores of 10-50μm are generated on the inner wall of the macroscopic channel.

[0043] (4) Preparation of nanopores by anodizing: The etched blank was anodized under negative pressure. The electrolyte was a mixture of ethylene glycol and deionized water in a volume ratio of 98:2, and then 0.5% ammonium fluoride was added. During the anodizing process, the oxidation voltage was controlled at 20V and the oxidation time was 40min. A 0.2-2μm nano-TiO2 micropore array was generated in situ on the inner wall of the micron-inspired biomimetic mesopore.

[0044] (5) Vacuum biomimetic mineralization activation: The oxidized billet is immersed in simulated body fluid SBF and vacuum impregnated at a constant temperature. The impregnation temperature is controlled at 35℃ and the impregnation time is 24h. After impregnation, a hydroxyapatite biomimetic mineralization layer will be deposited inside the multi-level pores of the billet. After completion, a three-level cross-scale gradient biomimetic microporous porous titanium alloy structure is obtained.

[0045] The pore distribution of this three-level, multi-scale gradient biomimetic microporous titanium alloy structure is as follows: the first-level gradient Gyroid macropores are 200–800 μm, the second-level coral-like micro-biomimetic mesopores are 10–50 μm, and the third-level nanotube-like micropores are 0.2–2 μm. Its elastic modulus exhibits a continuous gradient distribution of 1–18 GPa along the thickness direction.

[0046] Example 2

[0047] A method for preparing a biomimetic porous titanium alloy microporous structure includes the following steps:

[0048] (1) Three-dimensional modeling: Based on human bone CT data, a solid model was constructed. The gradient macroporous structure was designed using triple-period minimal surface Gyroid single cell. The gradient porosity and gradient single cell size were set from the cortical side to the cancellous side along the thickness direction of the implant. The gradient porosity was 35% for the cortical side and 65% for the cancellous side. The single cell size gradient range was 200-800 μm. The STL printing model was exported.

[0049] (2) Additive manufacturing of porous matrix: Ti6Al4V spherical titanium alloy powder is used to print porous titanium alloy blanks by selective laser melting SLM. The laser power is controlled at 220W, the scanning speed is 1400mm / s, the layer thickness is 30μm, and the titanium alloy powder particle size is 15~45μm. After printing, the residual powder inside the pores is removed by cleaning.

[0050] (3) Preparation of micron-sized biomimetic mesopores by negative pressure etching: The porous titanium alloy blank is placed in a negative pressure immersion tank and etched by negative pressure penetration with a mixed etching solution of hydrofluoric acid and nitric acid. The volume ratio of HF:HNO3:H2O in the etching solution is 1:3:10. The corresponding negative pressure during etching is -0.09MPa and the etching time is 18min. Interconnected micron-sized biomimetic mesopores of 10-50μm are generated on the inner wall of the macroscopic channel.

[0051] (4) Preparation of nanopores by anodizing: The etched blank was anodized under negative pressure. The electrolyte was a mixture of ethylene glycol and deionized water in a volume ratio of 98:2, and then 0.5% ammonium fluoride was added. During the anodizing process, the oxidation voltage was controlled at 40V and the oxidation time was 80min. A 0.2-2μm nano-TiO2 micropore array was generated in situ on the inner wall of the micron biomimetic mesopore.

[0052] (5) Vacuum biomimetic mineralization activation: The oxidized billet is immersed in simulated body fluid SBF and vacuum impregnated at a constant temperature. The impregnation temperature is controlled at 45℃ and the impregnation time is 48h. After impregnation, a hydroxyapatite biomimetic mineralization layer will be deposited inside the multi-level pores of the billet. After completion, a three-level cross-scale gradient biomimetic microporous porous titanium alloy structure is obtained.

[0053] The pore distribution of this three-level, multi-scale gradient biomimetic microporous titanium alloy structure is as follows: the first-level gradient Gyroid macropores are 200–800 μm, the second-level coral-like micro-biomimetic mesopores are 10–50 μm, and the third-level nanotube-like micropores are 0.2–2 μm. Its elastic modulus exhibits a continuous gradient distribution of 1–18 GPa along the thickness direction.

[0054] Example 3

[0055] A method for preparing a biomimetic porous titanium alloy microporous structure, specifically for use as a lumbar interbody fusion device, includes the following steps:

[0056] (1) CT scans were used to collect lumbar vertebral body data. Gyroid gradient TPMS modeling was used: the porosity of the outer cortical region of the fusion cage was 30%, the porosity of the inner cancellous region was 70%, and the single cell size gradient was 280μm→650μm.

[0057] (2) Ti6Al4V powder SLM printing, laser 190W, layer thickness 30μm, ultrasonic cleaning and drying after printing;

[0058] (3) -0.08MPa negative pressure acid and alkali etching for 12min, forming 20-40μm interconnected micron-sized mesopores on the hole wall;

[0059] (4) 30V low-voltage anodizing for 60 min, generating nano-TiO2 microporous tubes of about 800nm ​​throughout the entire area;

[0060] (5) SBF vacuum impregnation for 36 h to deposit HA mineralization layer in the pores. The remaining process details are the same as in Example 1.

[0061] The structural characterization results of the structure prepared in Example 3 are as follows: the tertiary pores are fully interconnected, the elastic modulus is distributed in a gradient of 3.5 to 12 GPa; the specific surface area is increased by 4.8 times compared with single SLM porous titanium; the amount of osteoblast adhesion in vitro is increased by 160%, and the drug sustained release period can reach 28 days.

[0062] Example 4

[0063] A method for preparing a biomimetic porous titanium alloy microporous structure, specifically for use as a repair scaffold for weight-bearing tibial bone defects, is disclosed. The method involves a modeling gradient porosity of 20%–82% and a unit cell pore size of 220–750 μm. The etching time is 15 min, and the anodic oxidation conditions are 35V / 70 min. Other undisclosed process details are the same as in Example 1. A cross-sectional view of the material is attached. Figure 1 As shown.

[0064] The finished product of Embodiment 4 of the present invention was tested and found to have a compressive strength of 85 MPa, which is suitable for lower limb weight-bearing. In an in vivo experiment of 12 weeks, new bone grew completely into the scaffold along the multi-level pores.

[0065] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, substitutions, combinations, simplifications, etc. made based on the principles or spirit of the present invention should be equivalent and are included within the protection scope of the present invention.

Claims

1. A method for preparing biomimetic porous titanium alloy microporous structures, characterized in that, Includes the following steps: (1) Three-dimensional modeling: Based on human bone CT data, a solid model is constructed, and the gradient porosity and gradient unit cell size are set from the cortical side to the cancellous side along the thickness direction of the implant. The STL printing model is then exported. (2) Additive manufacturing of porous matrix: using titanium alloy powder, porous titanium alloy blanks are printed by selective laser melting SLM, and the residual powder inside the pores is removed after printing; (3) Preparation of micron-sized biomimetic mesopores by negative pressure etching: The porous titanium alloy blank is placed in a negative pressure immersion tank and a hydrofluoric acid-nitric acid mixed etching solution is used for negative pressure penetration etching to generate 10-50 μm interconnected micron-sized biomimetic mesopores on the inner wall of the macroscopic channel; (4) Preparation of nanopores by anodizing: The etched blank is subjected to anodizing treatment under negative pressure to generate a 0.2-2 μm nano-TiO2 micropore array in situ on the inner wall of the micron biomimetic mesopore; (5) Vacuum biomimetic mineralization activation: The oxidized blank is immersed in simulated body fluid SBF and vacuum impregnated at a constant temperature. After completion, a three-level cross-scale gradient biomimetic microporous porous titanium alloy structure is obtained.

2. The method for preparing a biomimetic porous titanium alloy microporous structure according to claim 1, characterized in that, When constructing the solid model in step (1), a gradient macroporous structure is designed using a triple-period minimal surface Gyroid unit cell. The gradient porosity is: 15%–35% on the cortical side, 40%–60% on the transition zone, and 65%–85% on the cancellous side. The unit cell size gradient range is 200–800 μm.

3. The method for preparing a biomimetic porous titanium alloy microporous structure according to claim 1, characterized in that, The titanium alloy powder mentioned in step (2) is Ti6Al4V spherical powder.

4. The method for preparing a biomimetic porous titanium alloy microporous structure according to claim 1, characterized in that, The specific SLM printing process described in step (2) is as follows: laser power 160-220W, scanning speed 800-1400mm / s, layer thickness 30μm, and titanium alloy powder particle size 15-45μm.

5. The method for preparing a biomimetic porous titanium alloy microporous structure according to claim 1, characterized in that, In step (3), the volume ratio of HF:HNO3:H2O in the etching solution is 1:3:10; the corresponding negative pressure during etching is -0.07 to -0.09 MPa, and the etching time is 8 to 18 min.

6. The method for preparing a biomimetic porous titanium alloy microporous structure according to claim 1, characterized in that, The electrolyte used in step (4) for anodizing is a mixture of ethylene glycol and deionized water in a volume ratio of 98:2, with 0.5% ammonium fluoride added. During the anodizing process, the oxidation voltage is controlled at 20-40V and the oxidation time is 40-80min. The entire process is under negative pressure to ensure that the electrolyte penetrates all pores.

7. The method for preparing a biomimetic porous titanium alloy microporous structure according to claim 1, characterized in that, In step (5), the vacuum impregnation temperature is controlled at 35-45°C and the impregnation time is 24-48h. After impregnation, a hydroxyapatite biomimetic mineralization layer will be deposited inside the multi-level pores of the blank.

8. The method for preparing a biomimetic porous titanium alloy microporous structure according to claim 1, characterized in that, The pore distribution of the three-level cross-scale gradient biomimetic microporous porous titanium alloy structure mentioned in step (5) is as follows: the first-level gradient Gyroid macropores are 200-800 μm, the second-level coral-like micro-biomimetic mesopores are 10-50 μm, and the third-level nanotube micropores are 0.2-2 μm.

9. The method for preparing a biomimetic porous titanium alloy microporous structure according to claim 1, characterized in that, The elastic modulus of the three-level cross-scale gradient biomimetic microporous porous titanium alloy structure described in step (5) is distributed in a continuous gradient of 1 to 18 GPa along the thickness direction.