A high-temperature stabilization method for heterogeneous interfaces of immiscible tungsten-copper composite materials
By introducing rare earth oxide particles into the CuCrZr side, combined with the segregation of Cr and Zr elements and the solute dragging effect, the migration and degradation problems of the W/CuCrZr heterogeneous interface at high temperature were solved, and the high temperature stability and long-term service reliability of the heterogeneous interface were achieved.
Patent Information
- Application Number
- CN202611441703.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies have failed to effectively address the microstructure evolution and stability issues of W/CuCrZr heterogeneous interfaces formed by additive manufacturing during high-temperature service, leading to interface migration and microstructure degradation under high-temperature conditions, which affects the long-term service reliability of composite materials.
Rare earth oxide dispersed particles are introduced into the CuCrZr side to increase the migration resistance of the interface and adjacent grain boundaries through particle pinning. The local interface energy is adjusted by utilizing the segregation of Cr and Zr elements in CuCrZr and the solute dragging effect, thereby inhibiting interface migration and microstructure degradation and maintaining the integrity of the interface structure.
Under high-temperature conditions, the introduction of rare earth oxide particles effectively inhibits the migration and microstructure degradation of the W/CuCrZr interface, maintains the continuity and integrity of the interface structure, and ensures the high-temperature stability and reliability of the composite material.
Smart Images

Figure CN123128535A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of heterogeneous metal material preparation technology, and specifically relates to a high-temperature stabilization method for the heterogeneous interface of immiscible tungsten-copper composite materials. Technical Background
[0002] Tungsten, with its high melting point, high high-temperature strength, low vapor pressure, low sputtering rate, and excellent resistance to high-temperature ablation, is a key candidate material for plasma-oriented components in nuclear fusion, high-temperature structures in aerospace, and high-heat-flux-density components. Cu and CuCrZr alloys possess excellent thermal and electrical conductivity, with CuCrZr alloys maintaining high thermal conductivity while also exhibiting good strength and service reliability. Combining W with CuCrZr allows for the integration of W's high-temperature resistance and CuCrZr's high thermal conductivity into a single component, holding significant application value in nuclear fusion heat sinks, high-power electronic devices, and high-heat-flux thermal management structures.
[0003] However, W and Cu are typical immiscible metal systems, exhibiting extremely low solid-state miscibility under equilibrium conditions, and showing significant differences in melting point, coefficient of thermal expansion, elastic modulus, plasticity, and thermophysical properties. These differences make the W / CuCrZr interface prone to generating significant thermal stress and deformation incompatibility during preparation, thus making the interface a critical region determining the overall reliability of the composite material. While traditional methods such as powder metallurgy, melt infiltration, hot pressing, hot isostatic pressing, diffusion bonding, and brazing can achieve the composite of W with Cu or Cu alloys, they often suffer from complex preparation processes, limited component shapes, and the need for intermediate layers or interface structures to separate from the overall forming phase.
[0004] Chinese invention patent CN113351884A (authorization announcement number CN113351884B) discloses a method for joining dissimilar, non-solid-soluble CuCrZr / W alloys based on laser additive manufacturing technology. This method achieves direct bonding of CuCrZr and W through laser additive manufacturing combined with surface laser remelting or low-energy-density laser treatment, improving the interface forming quality and initial mechanical properties of the joined parts. The key focus of this technology is on how to achieve direct bonding of W / CuCrZr dissimilar materials and how to control the initial microstructure and properties of the bonding interface. However, it does not specifically address the microstructural stability of the non-equilibrium heterogeneous interface formed by additive manufacturing under sustained high temperatures.
[0005] Chinese invention patent application CN120619362A discloses a method for preparing multi-element in-situ co-coated core-shell spherical powders for additive manufacturing. This method achieves in-situ co-coating of multiple elements on the surface of spherical metal powders such as Cu and CuCrZr through dissolution with soluble salts of various elements, wetting of spherical metal powders, drying, and multi-stage calcination and reduction. This technology mainly addresses the issues of uniform introduction of multiple elements into additive manufacturing composite powders, maintaining powder sphericity, and ensuring uniform element distribution. However, it does not address the control of the high-temperature stability of the prepared composite powder after it is used at a W / CuCrZr heterogeneous interface.
[0006] Chinese invention patent application CN113102747A discloses a method for preparing rare earth oxides by doping metal powders for additive manufacturing. This method uses a chemical method to uniformly coat the surface of spherical powders made of copper, tungsten, stainless steel, and nickel-based alloys with rare earth oxides such as Y₂O₃ and La₂O₃, achieving uniform introduction of rare earth oxides while maintaining the spherical structure of the metal powder. This technology mainly addresses the preparation and particle dispersion of rare earth oxide composite powders, but does not address the high-temperature stabilization effect of rare earth oxides on the non-equilibrium heterogeneous interface of W / CuCrZr in additive manufacturing.
[0007] Therefore, existing technologies have solved problems such as how to achieve direct additive bonding of W / CuCrZr, how to uniformly introduce rare earth oxides into metal powder, and how to co-coat multiple elements in situ on the surface of additively manufactured powders. However, existing technologies do not pay enough attention to the microstructure evolution and stability of the W / CuCrZr interface formed by additive manufacturing during high-temperature service.
[0008] Laser powder bed melting exhibits strong non-equilibrium characteristics, including localized rapid melting, high cooling rates, and high temperature gradients. When CuCrZr is formed on the surface of a fine-grained W matrix, the W surface layer can undergo localized remelting and form a transient liquid phase contact with the CuCrZr melt, creating a direct metallurgical interface during rapid solidification. This interface can be composed of larger Cu grains on the CuCrZr side, nanoscale W grains near the interface, and micron-sized equiaxed W grains on the W side, forming a grain-size heterogeneous structure. This type of multi-scale heterogeneous interface possesses high interfacial area, grain boundary density, and non-equilibrium structure, which is beneficial for interfacial bonding and load transfer. However, under high-temperature conditions, there are simultaneously driving forces for microstructure evolution that reduce both interfacial energy and grain boundary energy.
[0009] Under sustained high temperatures, interface migration, grain boundary migration, nanograin coarsening, and local element redistribution can all occur, gradually weakening or reconstructing the original grain size gradient and interface morphology. For W / CuCrZr composite components subjected to long-term high-temperature and high-heat-flux environments, simply achieving high initial bonding strength is insufficient to guarantee long-term service reliability. How to suppress the migration and microstructure degradation of non-equilibrium heterogeneous interfaces at high temperatures without introducing a macroscopically thick intermediate layer or altering the direct metallurgical bonding method of W / CuCrZr remains a problem that needs to be solved by existing technologies.
[0010] Rare earth oxides possess high thermal stability, and their dispersed particles can pin grain boundaries and interfaces, increasing the resistance to migration. Conversely, Cr and Zr elements in CuCrZr can segregate at and near the W / CuCrZr interface, altering the local interfacial chemical state and interfacial energy, and reducing the interfacial migration rate through solute dragging. Combining rare earth oxide particle pinning with Cr and Zr interfacial segregation and solute dragging can suppress interfacial migration and microstructure degradation from both thermodynamic and kinetic perspectives, improving the structural integrity and high-temperature stability of the W / CuCrZr heterogeneous interface while maintaining the original direct metallurgical bonding and grain size heterogeneity. Therefore, it is necessary to propose a high-temperature stabilization method specifically for additive manufacturing of W / CuCrZr heterogeneous interfaces. Summary of the Invention
[0011] The purpose of this invention is to address the risk of interface migration and microstructure degradation at high temperatures in additively manufactured W / CuCrZr composite materials with heterogeneous grain sizes, and to provide a high-temperature stabilization method for the heterogeneous interface of immiscible tungsten-copper composite materials.
[0012] Based on existing W / CuCrZr direct bonding technology and rare earth oxide composite powder preparation technology, this invention further focuses on high-temperature stability as a specific control target. Rare earth oxides are introduced into the CuCrZr side, and the W / CuCrZr grain size heterogeneous interface formed by laser powder bed melting is used as the stabilizing object. By the hindrance effect of dispersed particles on the migration of the interface and adjacent grain boundaries, the structural stability of the heterogeneous interface under high-temperature conditions is improved.
[0013] To achieve the above objectives, the present invention adopts the following technical solution:
[0014] Step S1: Fine-grained tungsten is used as the tungsten side material to grind, polish and clean the surface to be formed to obtain a clean surface to be bonded.
[0015] Step S2: Using CuCrZr pre-alloyed powder as the copper-side main powder, rare earth oxide particles are introduced onto its surface to obtain rare earth oxide / CuCrZr composite powder; the rare earth oxide is selected from at least one of Y2O3, La2O3, and CeO2, wherein the amount of Y2O3 added is 0.2-1.0 wt.%, and the representative amount of La2O3 or CeO2 added is 0.5 wt.%. The composite powder can be prepared using a disclosed in-situ coating method.
[0016] Step S3 involves using laser powder bed melting to form CuCrZr regions layer by layer on the surface of fine-grained tungsten, causing transient liquid phase contact and rapid solidification between the tungsten matrix surface layer and the CuCrZr melt, forming a W / CuCrZr interface with direct metallurgical bonding and a grain size heterogeneous structure composed of CuCrZr side grains, interface-adjacent nanoscale tungsten grains, and tungsten side micron-scale tungsten grains.
[0017] In step S4, during the high-temperature process, the dispersed rare-earth oxide particles increase the migration resistance at the interface and adjacent grain boundaries through particle pinning. Simultaneously, Cr and Zr elements in CuCrZr segregate at the interface and in adjacent regions, and regulate the local interface energy and reduce the interface migration rate through solute dragging. These effects synergistically suppress high-temperature migration and microstructural degradation at the W / CuCrZr interface from both thermodynamic and kinetic perspectives, thereby maintaining the integrity of the interface structure.
[0018] Furthermore, the rare earth oxide is preferably Y2O3; the representative addition amount of Y2O3 is 0.2 wt.%, 0.5 wt.%, and 1.0 wt.%.
[0019] Furthermore, when the rare earth oxide is La2O3 or CeO2, the representative addition amount is 0.5 wt.%.
[0020] Furthermore, the laser powder bed melting parameters are preferably: laser power 400W, scanning speed 200mm / s, scanning spacing 90μm, and layer thickness 30μm.
[0021] Furthermore, the high-temperature stability was verified by holding the sample at 800℃ for 3 hours. The sample was exposed to high temperature under a high-purity Ar protective atmosphere and then cooled to room temperature in the furnace under a high-purity Ar protective atmosphere.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The technical object of this invention has been further changed from "whether the W / CuCrZr interface can be formed and its initial bonding performance" to "whether the grain size heterogeneous interface formed by additive manufacturing can remain stable under high temperature conditions", which solves the high temperature interface stability problem that is different from existing bonding technologies.
[0024] 2. In this invention, rare earth oxide dispersed particles are introduced on the CuCrZr side, wherein Y2O3 is added in a representative range of 0.2 to 1.0 wt.%, and La2O3 and CeO2 are added in a representative amount of 0.5 wt.%. The high thermal stability of the dispersed particles is used to improve the migration resistance of the interface and adjacent grain boundaries, and to suppress interface migration and microstructure degradation under high temperature conditions.
[0025] 3. This invention fully utilizes the segregation and solute dragging effect of Cr and Zr elements contained in CuCrZr material itself at the interface and in the adjacent region to adjust the local interface energy and reduce the interface migration rate. It does not require the additional macroscopic thick intermediate layer, which is beneficial to maintaining the direct metallurgical bonding structure of W / CuCrZr and the original thermophysical properties of the material.
[0026] 4. This invention uses 800℃×3h as a representative high-temperature exposure condition to verify different amounts of Y2O3 and representative amounts of La2O3 and CeO2. Within the SEM observation range, the W / CuCrZr interface in each embodiment remained continuous and intact, and no defects such as pores, cracks and interface delamination were observed.
[0027] 5. This invention uses rare earth oxide dispersed particles to stabilize the W / CuCrZr grain size heterogeneous interface formed by LPBF at high temperature, so that material modification, heterogeneous interface construction and high temperature service stability are synergistically linked, providing a new interface control approach for the reliable service of W / CuCrZr composite materials under high temperature and high heat flux environments. Attached Figure Description
[0028] Figure 1 SEM image of the W / CuCrZr interface of a 0.2 wt.% Y₂O₃ / CuCrZr sample after being kept at 800℃ for 3 h;
[0029] Figure 2 SEM image of the W / CuCrZr interface of a 0.5 wt.% Y2O3 / CuCrZr sample after being kept at 800℃ for 3 h;
[0030] Figure 3 SEM image of the W / CuCrZr interface of a 1.0 wt.% Y2O3 / CuCrZr sample after being kept at 800℃ for 3 h;
[0031] Figure 4 SEM image of the W / CuCrZr interface of a 0.5 wt.% La2O3 / CuCrZr sample after being kept at 800℃ for 3 h;
[0032] Figure 5 SEM image of the W / CuCrZr interface after a 0.5 wt.% CeO2 / CuCrZr sample was kept at 800℃ for 3 h. Detailed Implementation
[0033] The present invention will be further described below with reference to the embodiments. The embodiments are used to illustrate the applicability of different rare earth oxide types and typical addition amounts to the high-temperature stability of the W / CuCrZr heterogeneous interface. The in-situ coating process of rare earth oxide composite CuCrZr powder in the present invention can adopt the disclosed powder preparation method, and this embodiment does not take the powder preparation method itself as the inventive point.
[0034] Fine-grained tungsten was used as the tungsten-side material, and the surface to be formed was mechanically ground, polished, and cleaned. CuCrZr pre-alloyed powder was used as the main copper-side powder, with Cu as the main component and containing Cr and Zr alloying elements. Rare earth oxide / CuCrZr composite powder was prepared according to the types and mass fractions of rare earth oxides specified in the examples.
[0035] A CuCrZr region was formed layer by layer on the surface of fine-grained tungsten using a laser powder bed melting system. The preferred process parameters were: laser power 400W, scanning speed 200mm / s, scanning spacing 90μm, and layer thickness 30μm. During the forming process, local remelting of the tungsten matrix surface layer occurred, resulting in transient liquid-phase contact with the CuCrZr melt. This led to the formation of a direct metallurgical interface and a grain size heterogeneous structure consisting of CuCrZr side grains, adjacent nanoscale tungsten grains, and tungsten side micron-sized tungsten grains during rapid solidification.
[0036] To evaluate the high-temperature stability of the heterogeneous interface, the obtained samples were placed under a high-purity Ar protective atmosphere and held at 800°C for 3 hours. After the holding period, the samples were cooled to room temperature in the furnace under the same high-purity Ar protective atmosphere. The continuity and structural integrity of the W / CuCrZr interface after high-temperature exposure were observed using a scanning electron microscope. No defects such as pores, cracks, or interface delamination were observed in any of the embodiments within the SEM observation range.
[0037] Example 1
[0038] W / CuCrZr composite materials were prepared using CuCrZr composite powder containing 0.2 wt.% Y₂O₃. The resulting samples were heated at 800℃ for 3 h under a high-purity Ar protective atmosphere, and then cooled to room temperature in the furnace under the same atmosphere before interfacial SEM observation. Figure 1 As shown, within the SEM observation range, the W / CuCrZr interface remained continuous and intact, with no defects such as pores, cracks, or interface delamination observed, indicating that the sample has good high-temperature interface structure stability.
[0039] Example 2
[0040] W / CuCrZr composite materials were prepared using CuCrZr composite powder containing 0.5 wt.% Y₂O₃. The resulting samples were subjected to the same high-temperature exposure conditions of 800℃ for 3 hours as in Example 1. Figure 2 As shown, within the SEM observation range, the W / CuCrZr interface remained continuous and intact, with no defects such as pores, cracks, or interface delamination observed, indicating that the sample has good high-temperature interface structure stability.
[0041] Example 3
[0042] W / CuCrZr composite materials were prepared using CuCrZr composite powder containing 1.0 wt.% Y₂O₃. The resulting samples were subjected to the same high-temperature exposure conditions of 800℃ for 3 hours as in Example 1. Figure 3 As shown, within the SEM observation range, the W / CuCrZr interface remained continuous and intact, with no defects such as pores, cracks, or interface delamination observed, indicating that the sample has good high-temperature interface structure stability.
[0043] Example 4
[0044] W / CuCrZr composite materials were prepared using CuCrZr composite powder containing 0.5 wt.% La₂O₃. The resulting samples were subjected to the same high-temperature exposure conditions of 800℃ for 3 hours as in Example 1. Figure 4 As shown, within the SEM observation range, the W / CuCrZr interface remained continuous and intact, with no defects such as pores, cracks, or interface delamination observed, indicating that the sample has good high-temperature interface structure stability.
[0045] Example 5
[0046] W / CuCrZr composite materials were prepared using CuCrZr composite powder containing 0.5 wt.% CeO2. The resulting samples were subjected to the same high-temperature exposure conditions of 800℃ for 3 hours as in Example 1. Figure 5 As shown, within the SEM observation range, the W / CuCrZr interface remained continuous and intact, with no defects such as pores, cracks, or interface delamination observed, indicating that the sample has good high-temperature interface structure stability.
[0047] The present invention has been described in detail above through embodiments, but the content described is only an exemplary embodiment of the present invention and should not be considered as limiting the scope of the present invention. The scope of protection of the present invention is defined by the claims. Any technical solutions designed by those skilled in the art using the technical solutions described in the present invention, or designed by those skilled in the art under the inspiration of the technical solutions of the present invention, within the substance and protection scope of the present invention, to achieve the above-mentioned technical effects, or any equivalent changes and improvements made to the scope of the application, should still fall within the patent protection scope of the present invention.
Claims
1. A method for high-temperature stabilization of the heterogeneous interface of immiscible tungsten-copper composite materials, characterized in that: Rare earth oxide-modified CuCrZr composite powder was used as the copper-side raw material, and fine-grained tungsten was used as the tungsten-side material. CuCrZr regions were formed layer by layer on the surface of the fine-grained tungsten by laser powder bed melting, so that the surface layer of the tungsten matrix and the CuCrZr melt had transient liquid phase contact and rapid solidification, forming a W / CuCrZr interface with direct metallurgical bonding and a grain size heterogeneous structure composed of CuCrZr-side grains, nano-sized tungsten grains adjacent to the interface, and micron-sized tungsten grains on the tungsten side. After the composite material was kept at 800℃ for 3 hours, the W / CuCrZr interface remained continuous and intact within the SEM observation range, and no defects such as pores, cracks and interface delamination were observed.
2. The method according to claim 1, characterized in that, The rare earth oxide is selected from at least one of Y2O3, La2O3 and CeO2.
3. The method according to claim 1 or 2, characterized in that, When the rare earth oxide is Y2O3, its addition amount accounts for 0.2 to 1.0 wt.% of the total mass of the CuCrZr composite powder.
4. The method according to claim 1 or 2, characterized in that, When the rare earth oxide is La2O3 or CeO2, its representative addition amount accounts for 0.5 wt.% of the total mass of CuCrZr composite powder.
5. The method according to claim 1, characterized in that, The CuCrZr pre-alloyed powder contains Cr and Zr. The Cr and Zr segregate at the W / CuCrZr interface and in the adjacent region, and adjust the local interfacial chemical state and reduce the interfacial migration rate through solute dragging.
6. The method according to claim 1, characterized in that, The rare earth oxide modified CuCrZr composite powder was prepared by in-situ coating.
7. The method according to claim 1, characterized in that, The laser power used for the laser powder bed melting is 400W, the scanning speed is 200mm / s, the scanning spacing is 90μm, and the layer thickness is 30μm.
8. The method according to claim 1, characterized in that, The size of the nanoscale tungsten grains adjacent to the interface is smaller than that of the micrometer-scale tungsten grains on the tungsten side, and a grain size gradient is formed at the W / CuCrZr interface from the CuCrZr side to the tungsten side.
9. The method according to claim 1, characterized in that, The high-temperature stability verification conditions were: holding at 800℃ for 3 hours, exposing the sample to high temperature under a high-purity Ar protective atmosphere, and then cooling it to room temperature in the furnace under a high-purity Ar protective atmosphere.
10. The method according to claim 1, characterized in that, The rare earth oxide dispersed particles increase the migration resistance of the interface and adjacent grain boundaries through particle pinning, and the Cr and Zr elements in CuCrZr regulate the local interface energy and reduce the interface migration rate through interface segregation and solute dragging.
Citation Information
Patent Citations
Preparation method of doping rare earth oxide in metal powder for additive manufacturing
CN113102747A
Method for connecting CuCrZr / W dissimilar immiscible alloys based on laser additive manufacturing technology
CN113351884A
A method for joining dissimilar, non-solid-solution CuCrZr / W alloys based on laser additive manufacturing technology
CN113351884B
Preparation method of multi-element in-situ co-coated core-shell powder for additive manufacturing