A method for preparing an isotropic TC4 titanium alloy part with equiaxed crystal structure by selective laser melting forming technology
By adding Fe powder with particle sizes of 15-53μm and 53-75μm to TC4 titanium alloy powder, the microstructure was changed, which solved the problem of anisotropic mechanical properties caused by columnar crystals in the selective laser melting process of TC4 titanium alloy, and realized the preparation of isotropic TC4 titanium alloy parts with high strength and good plasticity.
Patent Information
- Application Number
- CN202611573800.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-12
- Publication Date
- 2026-11-20
AI Technical Summary
In the current selective laser melting process for preparing TC4 titanium alloy, the anisotropy of mechanical properties caused by columnar crystal growth is severe, affecting the service reliability and design tolerance of the components.
By adding a specific proportion and particle size range of pure Fe powder to TC4 alloy powder, the microstructure is changed by utilizing the non-uniform nucleation of Fe element in the molten pool and the effect of compositional undercooling, so that columnar β grains are transformed into equiaxed grains, thus eliminating the anisotropy of mechanical properties.
The prepared TC4 titanium alloy parts exhibit isotropic high strength and good plasticity at room temperature, significantly improving tensile strength, and require no subsequent heat treatment, simplifying the process and reducing production costs.
Smart Images

Figure CN123128536A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for preparing TC4 titanium alloy parts by selective laser melting forming technology, belonging to the field of metal material preparation technology. Background Technology
[0002] Titanium alloys are widely used in aerospace, biomedical, and automotive industries due to their excellent specific strength, corrosion resistance, and biocompatibility. TC4 (Ti-6Al-4V) is currently the most widely used α+β type titanium alloy, accounting for more than 50% of the total titanium alloy production. Selective laser melting (SLM), as one of the core technologies of additive manufacturing, can directly form complex structural parts, providing great freedom for the design and manufacturing of titanium alloys.
[0003] However, the inherent problems of SLM forming of TC4 alloy limit its industrial application. This is due to the extremely high temperature gradient and cooling rate (up to 10) during the SLM process. 3 -10 8 (K / s), molten pool solidification typically occurs via epitaxial growth, resulting in a final microstructure exhibiting coarse columnar β-grains. This strong... <100> Texture causes the alloy to exhibit significant anisotropy in mechanical properties both parallel to the build direction (Z-direction) and perpendicular to the build direction (X / Y-direction). For example, the elongation and strength in the Z-direction are much lower than in the horizontal direction, which seriously affects the service reliability and design tolerance of the component. In addition, stress concentration at columnar grain boundaries also increases the risk of cracking during use.
[0004] To address these issues, researchers have attempted various post-processing techniques (such as hot isostatic pressing and heat treatment) to control the microstructure. However, these methods increase manufacturing costs and time, and are unlikely to completely eliminate texture. In recent years, controlling the solidification behavior of the molten pool by adding alloying elements or nucleating agents to raw material powders has become a research hotspot. For example, adding boron (B) can form TiB whiskers, which act as grain boundary pinning agents; adding iron (Fe) is a strong β stabilizer that can lower the β phase transformation point and expand the solidification temperature range. Furthermore, Fe exhibits significant solid solution strengthening effects in titanium. However, the method of adding elemental Fe, its particle size distribution, and its content have a significant impact on nucleation efficiency and the equiaxed microstructure.
[0005] In summary, the existing selective laser melting process for preparing TC4 titanium alloy suffers from severe anisotropy in mechanical properties due to columnar crystal growth. Summary of the Invention
[0006] The purpose of this invention is to solve the problem of severe anisotropy in mechanical properties caused by columnar crystal growth in the existing selective laser melting (SLM) process for preparing TC4 titanium alloy. Therefore, it provides a method for preparing isotropic TC4 titanium alloy parts with an equiaxed crystal structure using SLM forming technology. Specifically, it involves a method of thoroughly mixing pure Fe powder of different particle sizes with TC4 alloy powder and preparing titanium alloy parts using SLM forming technology. By adding Fe elements of a specific proportion and size, utilizing their non-uniform nucleation and compositional supercooling effect in the molten pool, the microstructure inside the TC4 titanium alloy is changed, transforming the original columnar β grains into equiaxed grains, thereby significantly eliminating the anisotropy in mechanical properties and enabling the alloy to possess isotropic high strength and good plasticity at room temperature.
[0007] The technical solution of this invention is: a method for preparing isotropic TC4 titanium alloy parts with equiaxed grain structure by selective laser melting forming technology, which includes the following steps:
[0008] Step 1: Raw material preparation;
[0009] Step 11: Spherical TC4 alloy powder prepared by gas atomization method is selected as the matrix material;
[0010] Steps 1 and 2: Select two types of pure Fe powder with a particle size range and a purity of ≥99.5% as additives: the first type is fine Fe powder with a particle size of 15-53μm, and the second type is coarse Fe powder with a particle size of 53-75μm.
[0011] Step 13: Place spherical TC4 alloy powder, 2 wt.% fine Fe powder and 1 wt.% coarse Fe powder in a powder mixer and mix them evenly for 4 hours;
[0012] Step 14: After mixing, place the mixed powder in a drying oven and dry it. Set the oven temperature to 60℃ and keep it warm for 2 hours.
[0013] Step 2: Establish a structural model of the target part, then perform two-dimensional slicing on the established three-dimensional model of the target part, and import the two-dimensional slices into a selection area laser melting forming equipment;
[0014] Step 3: Set the processing parameters for the selective laser melting process and perform selective laser melting.
[0015] The processing parameters are as follows:
[0016] The substrate is made of TC4 titanium alloy, the substrate preheating temperature is 200 ℃, the laser power is 350 W, the powder layer thickness is 30 μm, the scanning rate is 1400 mm / s, the scanning spacing is 90 μm, the scanning strategy is cross scanning and each layer scanning path is rotated 67° relative to the previous layer.
[0017] Throughout the manufacturing process, high-purity argon gas is continuously introduced into the equipment's working chamber to control the oxygen content inside the working chamber to be below 300 ppm;
[0018] Step 4: Perform wire cutting and surface treatment on the machined parts in sequence:
[0019] After separating the part from the substrate and removing the support, surface treatment is performed to obtain an isotropic TC4 titanium alloy part with an equiaxed crystal structure.
[0020] Furthermore, the TC4 titanium alloy powder in step one mainly consists of powder with a particle size of less than 15 μm ≤ 5 wt%, powder with a particle size of greater than 53 μm ≤ 5 wt%, and the balance being powder with a particle size of 15 μm ~ 53 μm.
[0021] Furthermore, the loose packing density of the TC4 alloy powder prepared by the gas atomization method in step one is 2.3 g / cm³ to 2.6 g / cm³, and the tap density is 2.8 g / cm³ to 3.1 g / cm³.
[0022] Preferably, the powder mixer in steps one and three is a V-type powder mixer.
[0023] Furthermore, in step two, a structural model of the target part is constructed using 3D software and saved in STL format. Supports are added to the constructed model using additive manufacturing processing software, followed by 2D slicing. The 2D slices are then imported into a selective laser melting device.
[0024] Preferably, the thickness of the two-dimensional slice in step two is 30 μm.
[0025] Furthermore, in step three, before starting selective laser melting, the selective laser melting equipment is first purged with high-purity argon gas to reduce the oxygen content inside the equipment to below 300 ppm before processing begins.
[0026] Furthermore, in step three, the laser used for selective laser melting is a fiber laser with a laser spot diameter of 60 ± 5 μm and a strip scanning strategy with a strip width of 10 mm.
[0027] Preferably, in step three, the flow rate of the high-purity argon gas is 15-20 L / min.
[0028] Compared with the prior art, the present invention has the following advantages:
[0029] 1. This invention successfully eliminated the columnar grain structure of SLM-formed TC4 alloy by composite addition of Fe powder with different particle size ranges (2 wt.% fine powder of 15-53 μm and 1 wt.% coarse powder of 53-75 μm), obtaining a nearly equiaxed β-grain structure. The coarse Fe powder (53-75 μm) was partially incompletely dissolved during laser melting, acting as a heterogeneous nucleation substrate and promoting the formation of equiaxed crystals; the fine Fe powder (15-53 μm) was fully dissolved in the matrix, utilizing its strong β-stabilizing effect to expand the solidification range and further hinder the epitaxial growth of columnar crystals. Simultaneously, the solid solution strengthening effect of Fe significantly improved the strength of the alloy.
[0030] 2. The SLM-TC4 titanium alloy prepared by this invention exhibits excellent isotropic mechanical properties even in its formed state. Through room temperature tensile testing, the difference in ultimate tensile strength between the horizontal (X / Y) and vertical (Z) directions is minimal, and the elongation is almost identical, essentially eliminating anisotropy. Specifically, after adding Fe, the average ultimate tensile strength in the horizontal direction (transverse) is 1306 MPa, the yield strength is 1285 MPa, and the elongation is 8.40%; the average ultimate tensile strength in the vertical direction (longitudinal) is 1349 MPa, the yield strength is 1284 MPa, and the elongation is 8.50%. The difference in elongation between the horizontal and vertical directions is only 0.1%, fully demonstrating the significant effect of the method of this invention in eliminating anisotropy and achieving true isotropic mechanical properties.
[0031] 3. Compared with the SLM-TC4 alloy without Fe, the tensile strength of this invention is significantly increased from approximately 1070-1096 MPa to approximately 1306-1349 MPa, demonstrating a significant strengthening effect (an increase of over 220 MPa). This is attributed to the combined effect of solid solution strengthening and grain refinement by Fe. Simultaneously, the elongation remains essentially at the original level (approximately 8.4%-8.5%), achieving an excellent balance of strength and plasticity without a decrease in ductility.
[0032] 4. This invention eliminates the need for complex subsequent heat treatment processes, enabling the production of TC4 titanium alloy parts with uniform microstructure, few defects (density higher than 99.5%), high strength, and isotropy. This simplifies the process, reduces production costs, and is suitable for the direct forming of aerospace structural components and high-performance industrial parts. Attached Figure Description
[0033] Figure 1 These are scanning electron microscope (SEM) images of the original TC4 powder, 15-53 μm Fe powder, and 53-75 μm Fe powder used in this invention.
[0034] Figure 2This is a macroscopic metallographic image of a sample manufactured using the SLM process in this invention. It compares the columnar crystal structure (a) of the TC4 sample without added Fe powder with the equiaxed crystal structure (b) obtained after adding Fe powder in this invention.
[0035] Figure 3 This is a comparison of room temperature tensile stress-strain curves for different printing directions (horizontal and vertical) in this invention, demonstrating the isotropic mechanical properties. Detailed Implementation
[0036] Specific Implementation Method 1: This embodiment describes a method for preparing isotropic TC4 titanium alloy parts with equiaxed grain structures using selective laser melting forming technology, which includes the following steps:
[0037] Step 1: Raw material preparation;
[0038] Step 11: Spherical TC4 alloy powder prepared by gas atomization method is selected as the matrix material;
[0039] Steps 1 and 2: Select two types of pure Fe powder with a particle size range and a purity of ≥99.5% as additives: the first type is fine Fe powder with a particle size of 15-53μm, and the second type is coarse Fe powder with a particle size of 53-75μm.
[0040] Step 13: Place spherical TC4 alloy powder, 2 wt.% fine Fe powder and 1 wt.% coarse Fe powder in a powder mixer and mix them evenly for 4 hours;
[0041] Step 14: After mixing, place the mixed powder in a drying oven and dry it. Set the oven temperature to 60℃ and keep it warm for 2 hours.
[0042] Step 2: Establish a structural model of the target part, then perform two-dimensional slicing on the established three-dimensional model of the target part, and import the two-dimensional slices into a selection area laser melting forming equipment;
[0043] Step 3: Set the processing parameters for the selective laser melting process and perform selective laser melting.
[0044] The processing parameters are as follows:
[0045] The substrate is made of TC4 titanium alloy, the substrate preheating temperature is 200 ℃, the laser power is 350 W, the powder layer thickness is 30 μm, the scanning rate is 1400 mm / s, the scanning spacing is 90 μm, the scanning strategy is cross scanning and each layer scanning path is rotated 67° relative to the previous layer.
[0046] Throughout the manufacturing process, high-purity argon gas is continuously introduced into the equipment's working chamber to control the oxygen content inside the working chamber to be below 300 ppm;
[0047] Step 4: Perform wire cutting and surface treatment on the machined parts in sequence:
[0048] After separating the part from the substrate and removing the support, surface treatment is performed to obtain an isotropic TC4 titanium alloy part with an equiaxed crystal structure.
[0049] This invention uses spherical TC4 alloy powder prepared by gas atomization as the matrix material, and adds 2 wt.% fine Fe powder with a particle size of 15-53 μm and 1 wt.% coarse Fe powder with a particle size of 53-75 μm, which are uniformly mixed and used as raw materials for selective laser melting forming. By optimizing the selective laser melting process parameters (laser power 350 W, scanning speed 1400 mm / s, scanning spacing 90 μm, layer thickness 30 μm, scanning rotation angle 67°), the powder is melted and deposited layer by layer, and finally an isotropic TC4 titanium alloy part with an equiaxed crystal structure is obtained. The TC4-Fe titanium alloy prepared by this invention exhibits almost identical transverse and longitudinal elongation under formed conditions (8.40% transverse and 8.50% longitudinal), with a difference of only 0.1%, achieving excellent isotropy. Simultaneously, its tensile strength reaches 1306-1349 MPa, an increase of over 220 MPa compared to the TC4 alloy without Fe addition, achieving a superior strength-ductility balance with a significant increase in strength without a decrease in ductility. This invention requires no subsequent heat treatment and is suitable for the direct forming of titanium alloy structural components for aerospace and high-performance industrial applications.
[0050] Specific Implementation Method Two: In step one of this implementation method, the TC4 titanium alloy powder mainly consists of powder with a particle size of less than 15 μm ≤ 5 wt%, powder with a particle size of greater than 53 μm ≤ 5 wt%, and the balance being powder with a particle size of 15 μm ~ 53 μm.
[0051] As a preferred embodiment, the particle size distribution of TC4 titanium alloy powder is as follows: 5 wt% of powder with a particle size less than 15 μm, 3 wt% of powder with a particle size greater than 53 μm, and the remainder being powder with a particle size of 15 μm to 53 μm.
[0052] This embodiment limits the particle size distribution of the TC4 matrix powder to ensure good powder flowability, uniform powder spreading, and stable laser melting, thereby providing a qualified raw material basis for subsequent addition of Fe powder to achieve equiaxed crystallization and isotropy, while ensuring process repeatability.
[0053] Specific Implementation Method 3: The loose packing density of the TC4 alloy powder prepared by the gas atomization method in step one of this implementation method is 2.3 g / cm³ ~ 2.6 g / cm³, and the tapped density is 2.8 g / cm³ ~ 3.1 g / cm³.
[0054] This implementation limits the packing density of the original TC4 powder, ensuring powder spreading quality, melt pool stability and final forming density, while providing raw material standards for process repeatability.
[0055] Specific implementation method four: The powder mixer in steps one and three of this implementation method is a V-type powder mixer.
[0056] This ensures that TC4 powder and two types of Fe powder with different particle sizes can be mixed uniformly under low stress and without grinding, avoiding powder breakage, particle size changes and contamination, while ensuring mixing efficiency and batch consistency.
[0057] Specific implementation method five: In step two of this implementation method, a structural model of the target part is constructed using three-dimensional software and saved as an STL format. Supports are added to the constructed model using additive manufacturing processing software, and then two-dimensional slicing is performed. After two-dimensional slicing, the model is imported into a selective laser melting device.
[0058] Step two of this embodiment uses 3D software (such as UG, SolidWorks) to construct the structural model of the target part and save it in STL format. The constructed model is then supported by additive manufacturing processing software, and then 2D slicing is performed. The slice thickness is set to 30μm, and the slice data is imported into the selected area laser melting forming equipment.
[0059] Specific Implementation Method Six: In step two of this implementation method, the thickness of the two-dimensional slice is 30 μm.
[0060] The two-dimensional slice layer thickness is limited in this embodiment to be consistent with the actual powder layer thickness of SLM, ensuring the dimensional accuracy of the part and the stability of the interlayer overlap. Together with the laser power, scanning speed and scanning spacing, it forms an optimized energy density window to ensure that the solidification behavior of the molten pool is conducive to the formation of equiaxed crystals, and finally obtains a TC4 titanium alloy part with uniform structure and isotropic properties.
[0061] Specific Implementation Method Seven: In step three of this implementation method, before starting selective laser melting, the selective laser melting equipment is first purged with high-purity argon gas to reduce the oxygen content inside the equipment to below 300 ppm before processing begins.
[0062] This embodiment specifies that the gas must be washed before processing and the oxygen content must be reduced to below 300 ppm before processing begins. This is to remove residual oxygen in the working chamber, prevent oxidation and nitriding of the titanium alloy molten pool, ensure the cleanliness of the molten pool and the stability of powder spreading, thereby providing the necessary atmospheric conditions for obtaining high density, equiaxed grain structure and good plasticity.
[0063] Specific Implementation Method 8: In step 3 of this implementation method, the laser used for selective laser melting is a fiber laser with a laser spot diameter of 60 ± 5 μm and a strip scanning strategy with a strip width of 10 mm.
[0064] This embodiment limits the fiber laser, spot diameter, strip scanning strategy, and strip width to ensure moderate laser energy density, good continuous overlap of the melt channel, and uniform internal thermal history of the single layer. It also works in conjunction with the 67° interlayer rotation in Specific Embodiment 1 to jointly suppress columnar crystal epitaxial growth and promote equiaxed crystal formation, ultimately obtaining a high-density, isotropic TC4 titanium alloy part.
[0065] Specific Implementation Method Nine: In step three of this implementation method, the flow rate of the high-purity argon gas is 15-20 L / min to ensure that the smoke and dust are effectively blown away during the printing process, while maintaining stable pressure inside the chamber.
[0066] Specific Implementation Method 10: The surface treatment in step four of this implementation method consists of surface cleaning and surface polishing. The surface cleaning process is as follows: ultrasonic cleaning is performed using anhydrous ethanol as the cleaning medium for 10 min to 30 min. The surface polishing process is as follows: polishing is performed sequentially on #400, #800, #1000, #2000 and #3000 sandpaper until the surface is flat and smooth.
[0067] This implementation method aims to remove wire cutting residue and surface defects, ensure that the surface condition of the transverse and longitudinal specimens is consistent, eliminate the interference of surface factors on tensile testing, thereby truly and reliably reflecting the isotropy of the material, while ensuring process integrity and repeatability.
[0068] Example 1
[0069] Step 1, Raw Material Pretreatment: Spherical TC4 alloy powder (particle size 15-53 μm) prepared by gas atomization was selected as the matrix. Two types of pure Fe powder (purity 99.7%) with particle sizes of 15-53 μm and 53-75 μm were selected, such as... Figure 1 As shown. Weigh the powder according to the weight percentage of TC4:15-53 μm Fe:53-75 μm Fe = 97:2:1. Pour the weighed powder into a V-type powder mixer and mix for 4 hours. After it is evenly mixed, place it in a vacuum oven and dry it at 60℃ for 2 hours.
[0070] Step 2: Place the mixed titanium alloy powder into the powder feeding cylinder of the selective laser melting equipment (BLT-S210 type).
[0071] Step 3: Install the TC4 substrate and calibrate the substrate working platform, ensuring that the platform's levelness error is less than 0.02 mm. After the substrate debugging is completed, close the working chamber door of the selective laser melting equipment.
[0072] Step 4: Turn on the selective laser melting equipment and preheat the substrate using the substrate heating system, with a preset temperature of 200℃. At the same time, introduce high-purity argon gas (99.999% purity) into the equipment's working chamber to purge the selective laser melting equipment, reducing the oxygen content inside the equipment to below 300 ppm.
[0073] Step 5: When the oxygen content meets the equipment requirements (<300 ppm), import the part structure file into the equipment control system. Perform a pre-powdering operation, repeating the pre-powdering process three times to ensure that the first layer of powder is uniform and in good contact with the substrate.
[0074] Step 6: Begin selective laser melting printing of parts. During the printing process, ensure a continuous supply of argon gas at a flow rate of 18 L / min to maintain the oxygen content in the printing chamber below 300 ppm. Set the processing parameters for selective laser melting: laser power 350 W; cross-scanning method with a 67° rotation after each layer, scanning speed 1400 mm / s, scanning interval 90 μm, and titanium alloy powder layer thickness 30 μm.
[0075] Step 7, the specific selective laser melting process is as follows: After the laser heat source completes scanning of the previous layer of metal powder, the substrate descends by one layer thickness (30 μm), the powder feeding cylinder rises by one layer thickness (30 μm), and the scraper pushes the powder in the powder cylinder onto the substrate for powder spreading. After powder spreading is completed, the laser adjusts the scanning path angle of the next layer according to the slice data (rotating 67° relative to the previous layer) and begins scanning the next layer. The powder spreading-scanning operation is repeated until all preset slices are completed, finally obtaining a part of the target size. After printing, the part is cooled to room temperature in the furnace.
[0076] Step 8: Remove the printed part along with the substrate. Use wire cutting to separate the part from the substrate, and then remove the support structure using a tool. Place the part without support in anhydrous ethanol for ultrasonic cleaning for 20 minutes to remove powder and oil adhering to the surface. Finally, sand the surface of the part sequentially on sandpaper ranging from #400 to #3000 until the surface roughness Ra is less than 3.2 μm.
[0077] Samples were taken from the TC4-3Fe (mixed) titanium alloy block obtained in this embodiment, and tensile specimens were cut along the horizontal direction (X / Y direction, i.e., transverse) and the vertical direction (Z direction, i.e., longitudinal). Room temperature tensile tests were performed according to GB / T 228.1 standard.
[0078] Test results show that the ultimate tensile strength in the transverse (horizontal direction) is 1306 MPa, the yield strength is 1285 MPa, and the elongation is 8.40%; the ultimate tensile strength in the longitudinal (vertical direction) is 1349 MPa, the yield strength is 1284 MPa, and the elongation is 8.50%. The difference in elongation between the transverse and longitudinal directions is only 0.1%, and the difference in strength is also minimal, exhibiting excellent isotropy. Microstructural observation shows that the internal grain morphology of the sample is mainly equiaxed crystals, and the columnar crystal characteristics have been basically eliminated.
[0079] The anisotropy (IPA) of mechanical properties under different load directions is quantified by the following equation:
[0080]
[0081] Among them, T H ,T v The mechanical properties in the construction direction (BD direction) and scanning direction (SD direction) are represented respectively. Substituting the data (yield strength, ultimate tensile strength, and elongation) obtained from the above test results into the above formula, the IPA values of the elongation at break are 3.23, 0.07, and 1.18, respectively. Since the anisotropy values obtained are all less than 5, they can be considered as isotropic. This further indicates that the anisotropy is minimal.
[0082] Comparative Example 1 (Original TC4 without Fe addition)
[0083] Using the exact same TC4 powder and process parameters as in Example 1, but without adding any Fe powder, selective laser melting printing was performed directly.
[0084] Tensile test results showed that the TC4-1 sample without Fe had a tensile strength of 1070 MPa, a yield strength of 966 MPa, and an elongation of 9.2%; the TC4-2 sample had a tensile strength of 1096 MPa, a yield strength of 974 MPa, and an elongation of 6.9%. The average tensile strength was approximately 1083 MPa, and the average elongation was approximately 8.0%. In contrast, the strength of Example 1 after adding Fe increased to 1306-1349 MPa, an increase of over 220 MPa, while the elongation (approximately 8.4%-8.5%) remained essentially the same as the original TC4, achieving a significant increase in strength without a decrease in plasticity. Figure 3 As shown. The microstructure reveals that the sample without added Fe consists of coarse columnar β grains that penetrate multiple molten pool layers, as shown. Figure 2 As shown, this is the fundamental reason for anisotropy.
[0085] Comparative Example 2 (only 3 wt.% fine Fe powder added, no coarse Fe powder added)
[0086] Only 3 wt.% of 15-53 μm fine Fe powder was added, without adding 53-75 μm coarse Fe powder, and other conditions were the same as in Example 1.
[0087] The tensile test results of the samples in Comparative Example 2 (TC4-3Fe-transverse and TC4-3Fe-longitudinal) are as follows: tensile strengths are 1349 MPa and 1360 MPa, yield strengths are 1284 MPa and 1287 MPa, and elongation is 3.3% and 5.0% (average 4.15%).
[0088] The difference in elongation between the transverse and longitudinal directions was 1.7%, with a relatively small difference in strength, indicating improved anisotropy, but there is still room for improvement. Microscopic observation revealed the continued presence of columnar crystal characteristics. This clearly demonstrates that while adding fine Fe powder alone improves anisotropy, it cannot achieve equiaxed microstructure; coarse Fe powder (53-75 μm) must be added in combination as a heterogeneous nucleation core to effectively eliminate anisotropy and achieve a better plasticity match while maintaining high strength.
[0089] Comparative Example 3 (only 53-75 μm coarse Fe powder added)
[0090] Only 3 wt.% of 53-75 μm coarse Fe powder was added, without adding fine Fe powder, and other conditions were the same as in Example 1.
[0091] The results show that due to the large size of the coarse Fe powder particles, it is difficult to fully dissolve during the rapid laser melting process, resulting in uneven Fe element distribution. The tensile strength is 1426 MPa, but the large unmelted particles act as defects, worsening the plasticity. This method cannot simultaneously meet the requirements of high strength and isotropy.
[0092] While the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the invention. Those skilled in the art can make other changes within the spirit of the invention and apply it to fields not mentioned in the invention. Of course, all such changes made in accordance with the spirit of the invention should be included within the scope of protection claimed by the invention.
Claims
1. A method for preparing isotropic TC4 titanium alloy parts with equiaxed grain structure by selective laser melting forming technology, characterized in that: It includes the following steps: Step 1: Raw material preparation; Step 11: Spherical TC4 alloy powder prepared by gas atomization method is selected as the matrix material; Steps 1 and 2: Select two types of pure Fe powder with a particle size range and a purity of ≥99.5% as additives: the first type is fine Fe powder with a particle size of 15-53μm, and the second type is coarse Fe powder with a particle size of 53-75μm. Step 13: Place spherical TC4 alloy powder, 2 wt.% fine Fe powder and 1 wt.% coarse Fe powder in a powder mixer and mix them evenly for 4 hours; Step 14: After mixing, place the mixed powder in a drying oven and dry it. Set the oven temperature to 60 ℃ and keep it at that temperature for 2 hours. Step 2: Establish a structural model of the target part, then perform two-dimensional slicing on the established three-dimensional model of the target part, and import the two-dimensional slices into a selection area laser melting forming equipment; Step 3: Set the processing parameters for the selective laser melting process and perform selective laser melting. The processing parameters are as follows: The substrate is made of TC4 titanium alloy, the substrate preheating temperature is 200 ℃, the laser power is 350 W, the powder layer thickness is 30 μm, the scanning rate is 1400 mm / s, the scanning spacing is 90 μm, the scanning strategy is cross scanning and each layer scanning path is rotated 67° relative to the previous layer. Throughout the manufacturing process, high-purity argon gas is continuously introduced into the equipment's working chamber to control the oxygen content inside the working chamber to be below 300 ppm; Step 4: Perform wire cutting and surface treatment on the machined parts in sequence: After separating the part from the substrate and removing the support, surface treatment is performed to obtain an isotropic TC4 titanium alloy part with an equiaxed crystal structure.
2. The method for preparing isotropic TC4 titanium alloy parts with equiaxed grain structure by selective laser melting forming technology according to claim 1, characterized in that: The TC4 titanium alloy powder in step one mainly consists of powder with a particle size of less than 15 μm ≤ 5 wt%, powder with a particle size of greater than 53 μm ≤ 5 wt%, and the balance being powder with a particle size of 15 μm ~ 53 μm.
3. The method for preparing isotropic TC4 titanium alloy parts with equiaxed grain structure by selective laser melting forming technology according to claim 2, characterized in that: The loose packing density of the TC4 alloy powder prepared by the gas atomization method in step one is 2.3 g / cm³ ~ 2.6 g / cm³, and the tap density is 2.8 g / cm³ ~ 3.1 g / cm³.
4. The method for preparing isotropic TC4 titanium alloy parts with equiaxed grain structure by selective laser melting forming technology according to claim 3, characterized in that: The powder mixer in step one or three is a V-type powder mixer.
5. A method for preparing isotropic TC4 titanium alloy parts with equiaxed grain structure by selective laser melting forming technology according to claim 4, characterized in that: In step two, a structural model of the target part is constructed using 3D software and saved as an STL file. Supports are added to the constructed model using additive manufacturing processing software, followed by 2D slicing. The 2D slices are then imported into a selective laser melting device.
6. A method for preparing isotropic TC4 titanium alloy parts with equiaxed grain structure by selective laser melting forming technology according to claim 5, characterized in that: In step two, the thickness of the two-dimensional slice is 30 μm.
7. A method for preparing isotropic TC4 titanium alloy parts with equiaxed grain structure by selective laser melting forming technology according to claim 6, characterized in that: In step three, before starting selective laser melting, the selective laser melting equipment is first purged with high-purity argon gas to reduce the oxygen content inside the equipment to below 300 ppm before processing begins.
8. A method for preparing isotropic TC4 titanium alloy parts with equiaxed grain structure by selective laser melting forming technology according to claim 7, characterized in that: In step three, the laser used for selective laser melting is a fiber laser with a laser spot diameter of 60 ± 5 μm and a strip scanning strategy with a strip width of 10 mm.
9. A method for preparing isotropic TC4 titanium alloy parts with equiaxed grain structure by selective laser melting forming technology according to claim 8, characterized in that: In step three, the flow rate of the high-purity argon gas is 15-20 L / min.
10. A method for preparing isotropic TC4 titanium alloy parts with equiaxed grain structure by selective laser melting forming technology according to claim 9, characterized in that: The surface treatment in step four consists of surface cleaning and surface polishing. The surface cleaning process is as follows: ultrasonic cleaning is performed using anhydrous ethanol as the cleaning medium for 10 to 30 minutes. The surface polishing process is as follows: the surface is polished on sandpaper of #400, #800, #1000, #2000 and #3000 in sequence until it is flat and smooth.