Performance strengthening method of selective laser melting Ti2AlNb alloy

By using a mixed gas of nitrogen and argon for protection during the selective laser melting of Ti2AlNb alloy, the in-situ solid solution of nitrogen atoms in the β phase and the cooling rate are improved, which solves the problem of improving the strength and plasticity of Ti2AlNb alloy and achieves efficient synergistic enhancement of strength and plasticity.

CN123128538APending Publication Date: 2026-11-20HARBIN INST OF TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611603088.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-16
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies struggle to effectively improve the room temperature strength and plasticity of selective laser melting Ti2AlNb alloys without altering the powder composition or introducing heterogeneous reinforcing phases. Furthermore, existing in-situ atmosphere strengthening techniques lack quantitative control over the content of active gases and the strengthening effect in Ti2AlNb-based alloys.

Method used

A mixture of nitrogen and argon is used as the forming protective atmosphere. Under the action of laser, nitrogen is decomposed into nitrogen atoms and dissolved into the molten pool. Fine grain strengthening is achieved through in-situ solid solution strengthening of nitrogen atoms in the β phase and cooling rate enhancement. The specific steps include atmosphere replacement, selective laser melting forming, uniform distribution of nitrogen atoms, and cooling removal.

Benefits of technology

Without changing the powder composition and process equipment, the room temperature strength and plasticity of Ti2AlNb alloy were significantly improved. The room temperature yield strength increased from 932MPa to 1080MPa, the tensile strength increased from 947MPa to 1099MPa, and the elongation remained above 11.0%, achieving a synergistic improvement in strength and plasticity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128538A_ABST
    Figure CN123128538A_ABST
Patent Text Reader

Abstract

Ti2AlNb base alloy is an ideal material for engine hot end components in aerospace field due to its low density, high specific strength and good high temperature performance, and its complex structure can be formed by selective laser melting technology. However, the room temperature strength of the printed Ti2AlNb alloy is still low, and the existing strengthening methods also have defects: when alloying elements or ceramic particles are added, composition segregation and unmelted defects are easily produced due to the difference in melting point, and the interface bonding between the reinforcing phase and the matrix is poor. The application discloses a performance strengthening method for selective laser melting Ti2AlNb alloy, and a mixed gas of nitrogen and argon is used as a forming protective atmosphere, the volume fraction of nitrogen is 1% to 5%, nitrogen is decomposed into nitrogen atoms under the action of laser and dissolved into the molten pool, nitrogen atoms are preferentially solid-solved in the interstitial space of beta phase octahedron to realize in-situ solid-solution strengthening; at the same time, nitrogen can improve the cooling rate of the molten pool as a diatomic gas, and the beta phase grains are refined. The method in the disclosure can improve the room temperature tensile strength of the alloy from 940MPa to 1100MPa without significantly losing the elongation, thereby promoting the application of selective laser melting Ti2AlNb alloy in aerospace hot end components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of laser additive manufacturing technology and relates to a method for performance enhancement of Ti2AlNb alloy by selective laser melting. It is particularly suitable for the manufacturing of hot-end structural components of engines in the aerospace field, such as complex thin-walled components like compressor disks, compressor casings, and turbine guide vanes. Background Technology

[0002] Ti2AlNb-based alloys are typical representatives of Ti-Al-Nb intermetallic compounds. Their microstructure consists of an ordered B2(β) phase matrix, orthorhombic O phase, and close-packed hexagonal α2 phase. They combine the high specific strength, good oxidation and creep resistance of intermetallic compounds with the low density of titanium alloys, making them ideal candidates for replacing nickel-based superalloys in the 600℃~750℃ temperature range and achieving weight reduction in aero-engines. These hot-end components often have complex surfaces, thin walls, and internal flow channels. Traditional forging, casting, and machining methods are cumbersome, have low material utilization, and long manufacturing cycles. Selective laser melting (laser powder bed melting) technology, with its high degree of design freedom, enables integrated forming of complex components, allowing for convenient and rapid near-net-shape forming. This provides a new approach for manufacturing Ti2AlNb-based alloy hot-end components.

[0003] However, the selective laser melting process involves extremely high cooling rates, resulting in a microstructure dominated by metastable β phases in the printed Ti2AlNb-based alloy. This leads to relatively low room-temperature strength, making it difficult to meet the load-bearing requirements of hot-end components. Furthermore, due to its ordered crystal structure, the alloy also faces the challenge of simultaneously improving both strength and plasticity. Therefore, how to further enhance the mechanical properties of the printed Ti2AlNb-based alloy while maintaining the forming density has become a key research focus in this field.

[0004] Currently, the main methods for strengthening the mechanical properties of titanium alloys include in-situ alloying, ceramic particle strengthening, and in-situ atmosphere strengthening. Among these, in-situ alloying and ceramic particle strengthening both require the introduction of second-phase particles or alloying elements into the powder. Due to the difference in melting points between the added components and the original powder, component segregation and incomplete fusion defects are prone to occur during the forming process. Furthermore, the interfacial bonding between the reinforcing phase, such as ceramic particles, and the matrix is ​​poor, often resulting in a significant sacrifice of plasticity while improving strength. Moreover, it requires changes to the original powder preparation process and powder system, making the process complex and costly. In-situ atmosphere strengthening is achieved by decomposing and dissolving active gases in the forming protective atmosphere into the molten pool under laser action. It does not require changing the powder composition or introducing heterogeneous reinforcing phases. However, in the existing technology, this type of method is mainly used for pure titanium and titanium alloys such as TC4. For Ti2AlNb-based alloys, the type and content range of active gases in the atmosphere and their influence on β-phase lattice distortion, grain size and mechanical properties are still unclear. If the atmosphere content is too low, the strengthening effect is insufficient. If the content is too high, the solute atoms exceed the solid solubility limit and a large number of brittle compounds precipitate, resulting in a significant decrease in plasticity and making it difficult to achieve a synergistic improvement in strength and plasticity.

[0005] In summary, current methods for strengthening Ti2AlNb-based alloys largely rely on the addition of alloying elements or the introduction of ceramic particles, which suffer from problems such as compositional segregation, incomplete fusion defects, and poor interfacial bonding, and are difficult to effectively improve strength without sacrificing plasticity. Furthermore, existing in-situ atmosphere strengthening techniques lack quantitative control over the content of active gases and the strengthening effect in Ti2AlNb-based alloys. There is an urgent need for a method to strengthen Ti2AlNb alloys that does not alter the powder composition, does not introduce heterogeneous reinforcing phases, is simple in process, and is fully compatible with existing selective laser melting processes. Summary of the Invention

[0006] To address the shortcomings of existing technologies, this invention aims to propose a method for enhancing the performance of Ti2AlNb alloys through selective laser melting. This method utilizes a mixture of nitrogen and argon as the forming protective atmosphere, allowing nitrogen to decompose into nitrogen atoms under laser irradiation and dissolve into the molten pool. Through in-situ solid solution strengthening of nitrogen atoms in the β phase and grain refinement resulting from the increased cooling rate brought by nitrogen, a synergistic improvement in the room-temperature strength and plasticity of the printed Ti2AlNb-based alloy is achieved without altering the powder composition or introducing heterogeneous reinforcing phases. This method only requires increasing the nitrogen ratio in the gas supply system of existing selective laser melting equipment, without changing the powder preparation process or forming equipment. The process is simple, low-cost, and suitable for large-scale application.

[0007] The technical solution of this invention to solve the above-mentioned technical problems is as follows: A method for enhancing the performance of Ti2AlNb alloy by selective laser melting, characterized by comprising the following steps: Step 1, Atmosphere Replacement and Proportioning: Replace the atmosphere in the forming chamber with a mixture of nitrogen and argon, wherein the volume fraction of nitrogen in the mixture is 1% to 5% (preferably 1% to 3%), and the remainder is argon. Introduce high-purity gas until the oxygen content in the forming chamber is below 100 ppm. Step 2, Selective Laser Melting and Forming: Under the protection of the mixed gas, the Ti2AlNb alloy powder is melted and formed layer by layer using a laser powder bed melting process. The laser energy density is 50J / mm3~80J / mm3 and the interlayer rotation angle is 67°. Step 3, In-situ solid solution of nitrogen atoms: Under the action of laser, nitrogen in the mixed gas decomposes into nitrogen atoms and dissolves into the molten pool. The nitrogen atoms dissolved on the surface of the molten pool are transported to the interior of the molten pool and uniformly distributed under the action of surface tension and molten pool convection. Since the bonding strength of nitrogen atoms in the octahedral interstices of the β phase is higher than that in the O phase, nitrogen atoms preferentially dissolve in the β phase, causing β phase lattice distortion. At the same time, nitrogen gas, as a diatomic gas, can transfer more energy to the molten pool, thereby increasing the temperature gradient and cooling rate at the liquid-solid interface, thus refining the β phase grains. Step 4, Cooling and Removal: After the forming process is completed, the component is removed after cooling to room temperature in the forming chamber, resulting in a Ti2AlNb alloy component with in-situ solid solution strengthening of nitrogen atoms.

[0008] Under the above process parameters, selective laser melting forming of Ti2AlNb alloy powder in a nitrogen-containing mixed atmosphere resulted in significantly improved room temperature mechanical properties compared to those obtained under a pure argon atmosphere: when the nitrogen gas fraction increased from 0% to 5%, the nitrogen content in the printed alloy increased from 0.015 wt.% to 0.068 wt.%, the room temperature yield strength increased from 932 MPa to 1080 MPa, the room temperature tensile strength increased from 947 MPa to 1099 MPa, while the room temperature elongation remained above 11.0%; when the nitrogen gas fraction was 1% to 3%, no obvious nitrides were detected in the printed alloy, the room temperature tensile strength was 1005 MPa to 1066 MPa, and the elongation was 12.3% to 13.1%, achieving a synergistic improvement in strength and plasticity.

[0009] Preferably, the volume fraction of nitrogen in the mixed gas is 1% to 3%, with the balance being argon. Within this range, nitrogen atoms exist in the β phase in solid solution form, without obvious nitride precipitation, resulting in increased strength and minimal loss of plasticity.

[0010] Preferably, the volume fraction of nitrogen in the mixed gas is 3%, with the balance being argon; at this point, the room temperature yield strength of the alloy is 1051 MPa, the tensile strength is 1066 MPa, and the elongation is 12.3%, achieving the best match between strength and plasticity.

[0011] Preferably, the laser energy density of the laser powder bed melting process is 65 J / mm3 to ensure the forming density of the component; the interlayer rotation angle is 67°.

[0012] Preferably, the oxygen content in the forming chamber is less than 100 ppm, and the purity of the nitrogen and argon is not less than 99.99%, in order to avoid the adverse effects of oxygen on the alloy properties.

[0013] Preferably, the Ti2AlNb alloy powder has an Al content of 20%–24% and a Nb content of 23%–27% by atomic percentage, with the balance being Ti and unavoidable impurities, and the powder particle size distribution is 15μm–53μm.

[0014] Preferably, the mass fraction of nitrogen in the obtained Ti2AlNb alloy component is 0.026% to 0.068%, and the average grain size of the β phase is 42.6 μm to 49.5 μm.

[0015] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: This invention utilizes in-situ solid solution of nitrogen atoms in the interstices of the β-phase octahedrons for strengthening. First-principles calculations show that the interaction energies of nitrogen atoms in the interstices of the O phase and β phase are -6.876 eV and -8.233 eV, respectively. This indicates that the bonding strength between nitrogen atoms and surrounding atoms in the β phase is higher. Therefore, during laser powder bed melting, nitrogen atoms tend to dissolve more readily in the β phase, causing lattice distortion, microstrain, and dislocation density in the β phase, thereby increasing the resistance to dislocation movement. Quantitative calculations show that when the nitrogen gas integral is 1%, 3%, and 5%, the contribution of nitrogen atom solid solution strengthening to the yield strength is 42 MPa, 75 MPa, and 148 MPa, respectively, which is one of the main sources of strength improvement in this invention.

[0016] This invention utilizes the characteristic of nitrogen as a diatomic gas to transfer more energy to the molten pool and increase the cooling rate under laser irradiation, thereby significantly refining the β-phase grains. Experimental results show that when the volume fraction of nitrogen in the protective atmosphere increases from 0% to 5%, the average grain size of the β-phase decreases from 68.4 μm to 42.6 μm, and the contribution of grain refinement to yield strength increases from 96 MPa to 106 MPa, further enhancing the strength of the alloy.

[0017] This invention does not change the powder composition or introduce heterogeneous reinforcing phases, thus avoiding problems such as component segregation, incomplete fusion defects, and poor interfacial bonding between the reinforcing phase and the matrix caused by differences in the melting points of added components and ceramic particle strengthening methods. At the same time, it does not require changes to the original powder preparation process and forming equipment. It only requires increasing the nitrogen ratio in the gas supply system and controlling the ratio through a mass flow controller. The process is simple, low-cost, and fully compatible with existing selective laser melting processes, making it suitable for large-scale promotion.

[0018] This invention, by controlling the volume fraction of nitrogen in the mixed gas, can quantitatively regulate the contribution of nitrogen atom solid solution strengthening and grain refinement strengthening, thereby achieving a synergistic improvement in room temperature strength and plasticity: when the nitrogen gas fraction is 1% to 3%, the room temperature tensile strength increases from 947 MPa to 1005 MPa to 1066 MPa, while the elongation only decreases from 15.1% to 12.3% to 13.1%, with no obvious nitrides appearing; when the nitrogen gas fraction is 5%, the room temperature tensile strength reaches 1099 MPa, while the elongation remains at 11.0%, achieving a significant increase in room temperature strength without significantly sacrificing plasticity.

[0019] The present invention limits the nitrogen gas integral to 5% as follows: when the nitrogen gas integral exceeds 5%, the solid solubility of nitrogen atoms in the β phase reaches saturation and more TiN particles precipitate. Furthermore, with the further increase of the cooling rate, the precipitation of the O phase is suppressed, and its volume fraction decreases from 4.3% to 0.1%, which significantly reduces the room temperature elongation of the alloy. At the same time, the ability to stabilize the β phase at high temperatures is weakened. Therefore, an excessively high nitrogen gas integral is actually detrimental to the strength-plasticity balance of the alloy. Attached image description: Figure 1 This is a schematic diagram showing the crystallographic characteristics of the β phase in Ti2AlNb alloys under different atmospheric conditions. Figure 2 This is a schematic diagram of the XRD patterns of Ti2AlNb alloys with different N2 contents. Figure 3 This is a schematic diagram showing the mechanical properties of Ti2AlNb alloys with different N2 contents. Detailed implementation method: Example 1 This embodiment describes a method for enhancing the performance of a Ti2AlNb alloy using selective laser melting. The alloy used has the following atomic percentage composition: Al: 22%, Nb: 25%, with the balance being Ti and unavoidable impurities. All percentages are atomic percentages, and the powder particle size ranges from 15 to 53 μm.

[0020] In this embodiment, the protective atmosphere inside the forming chamber is a mixture of 99 vol.%Ar + 1 vol.%N2 gas, the oxygen content inside the forming chamber is less than 100 ppm, the laser energy density is 64.81 J / mm³, and the interlayer rotation angle is 67°.

[0021] Because nitrogen in the mixed atmosphere decomposes into nitrogen atoms and dissolves into the molten pool under laser irradiation, the nitrogen content in the printed alloy prepared in this embodiment is 0.026 wt.%, which is significantly higher than that under pure argon atmosphere. However, no obvious nitrides were detected by XRD and TEM analysis, indicating that nitrogen atoms exist in the β phase in solid solution form. Since nitrogen atoms are dissolved in the octahedral interstices of the β phase and increase the cooling rate of the molten pool, the average grain size of the β phase decreases from 68.4 μm under pure argon atmosphere to 49.5 μm. The resistance to dislocation movement increases. After processing into tensile specimens, tensile performance tests were performed, and the room temperature yield strength was 990 MPa, the tensile strength was 1005 MPa, and the elongation was 13.1%, all of which are significantly improved compared with the specimen under pure argon atmosphere, and the elongation loss is small.

[0022] Example 2 This embodiment is a method for enhancing the performance of Ti2AlNb alloy by selective laser melting. The composition, particle size range, and forming process of the alloy used are the same as those in Example 1.

[0023] In this embodiment, the protective atmosphere inside the forming chamber is a mixture of 97 vol.% Ar + 3 vol.% N2, the oxygen content inside the forming chamber is less than 100 ppm, the laser energy density is 64.81 J / mm³, and the interlayer rotation angle is 67°.

[0024] Due to the further increase in the nitrogen content in the mixed atmosphere, the nitrogen content in the printed alloy prepared in this embodiment increased to 0.047 wt.%, and no obvious nitrides were detected by XRD and TEM analysis. Nitrogen atoms existed in the β phase in solid solution form. The average grain size of the β phase was further reduced to 47.6 μm, and the degree of lattice distortion was intensified, thus further improving the strength of the alloy. After processing into tensile specimens, tensile property tests were performed, and the room temperature yield strength was 1051 MPa, the tensile strength was 1066 MPa, and the elongation was 12.3%, achieving a synergistic improvement in strength and plasticity.

[0025] Example 3 This embodiment is a method for enhancing the performance of Ti2AlNb alloy by selective laser melting. The composition, particle size range, and forming process of the alloy used are the same as those in Example 1.

[0026] In this embodiment, the protective atmosphere in the forming chamber is a mixture of 95 vol.% Ar + 5 vol.% N2, the oxygen content in the forming chamber is less than 100 ppm, the laser energy density is 64.81 J / mm³, and the interlayer rotation angle is 67°.

[0027] In this embodiment, the nitrogen content in the printed alloy is 0.068 wt.%, at which point the solid solubility of nitrogen atoms in the β phase reaches saturation. A small amount of TiN nanoparticles were detected in the printed sample, and the contribution of TiN precipitation strengthening to the yield strength was 3.40 MPa. Due to the further enhancement of solid solution strengthening and grain refinement strengthening effects of nitrogen atoms, tensile property tests were conducted after processing into tensile specimens. The room temperature yield strength was 1080 MPa, the tensile strength was 1099 MPa, and the elongation was 11.0%, which is the highest room temperature strength embodiment in this invention. However, at the same time, due to the increased cooling rate suppressing the precipitation of the O phase, the volume fraction of the O phase decreased from 4.3% under pure argon atmosphere to 0.1%, and the number of TiN particles increased, further reducing the elongation of the alloy. This indicates that the nitrogen gas integral should not exceed 5%.

[0028] Comparative Example 1 This comparative example is a selective laser melting forming method for Ti2AlNb alloy. The composition, particle size range, and forming process of the alloy used are the same as those in Example 1.

[0029] In this comparative example, the protective atmosphere inside the forming chamber is pure argon, i.e., no mixture of nitrogen and argon is used. The oxygen content inside the forming chamber is less than 100 ppm, the laser energy density is 64.81 J / mm³, and the interlayer rotation angle is 67°.

[0030] The nitrogen content in the printed alloy prepared in this comparative example is only 0.015 wt.%, all of which comes from residual nitrogen in the powder and raw materials. The average grain size of the β phase is 68.4 μm, which is the largest among all samples. Due to the lack of in-situ solid solution strengthening and grain refinement strengthening effects of nitrogen atoms, the tensile properties were tested after processing into tensile specimens. The room temperature yield strength was 932 MPa and the tensile strength was 947 MPa, which is lower than the strength of the specimens prepared in the other examples.

Claims

1. A method for enhancing the performance of Ti2AlNb alloy by selective laser melting, characterized in that, Includes the following steps: Atmosphere replacement: The atmosphere in the forming chamber is replaced with a mixture of nitrogen and argon, wherein the volume fraction of nitrogen in the mixture is 1% to 5%, and the remainder is argon. Selective laser melting forming: Under the protection of the mixed gas, the Ti2AlNb alloy powder is melted and formed layer by layer using a laser powder bed melting process. The nitrogen in the mixed gas is decomposed into nitrogen atoms under the action of the laser and dissolved into the molten pool. The nitrogen atoms are dissolved in the β phase. After cooling and solidification, a Ti2AlNb alloy component with in-situ solid solution strengthening of nitrogen atoms is obtained.

2. The method for enhancing the performance of Ti2AlNb alloy by selective laser melting according to claim 1, characterized in that: The volume fraction of nitrogen in the mixed gas is 1% to 3%, with the remainder being argon.

3. The method according to claim 1, characterized in that: The oxygen content in the forming chamber is less than 100 ppm; the purity of both nitrogen and argon is not less than 99.99%.

4. The method according to claim 1, characterized in that: The laser energy density of the laser powder bed melting process is 50 J / mm². 3 ~80J / mm 3 .

5. The method according to claim 4, characterized in that: The laser energy density is 65 J / mm². 3 Furthermore, the interlayer rotation angle of the laser powder bed melting process is 67°.

6. The method according to claim 1, characterized in that: The Ti2AlNb alloy powder, by atomic percentage, contains 20%–24% Al, 23%–27% Nb, with the balance being Ti and unavoidable impurities, and has a particle size distribution of 15 μm–53 μm.

7. The method according to claim 1, characterized in that: The mixed gas is continuously introduced into the forming chamber in proportion through a mass flow controller, and the volume fraction of nitrogen in the mixed gas fluctuates by no more than ±0.5% during the forming process.

8. The method according to claim 1, characterized in that: The mass fraction of nitrogen in the obtained Ti2AlNb alloy components is 0.026% to 0.068%.

9. The method according to claim 1, characterized in that: The average grain size of the β phase in the obtained Ti2AlNb alloy components is 42.6 μm to 49.5 μm.

10. A Ti2AlNb alloy component prepared by the method according to any one of claims 1 to 10, characterized in that: The component contains 0.026% to 0.068% nitrogen by mass, the average grain size of the β phase is 42.6 μm to 49.5 μm, and the component has a room temperature tensile strength of not less than 1000 MPa and a room temperature elongation of not less than 11.0%.