Highly wear resistant titanium alloy parts and additive manufacturing methods thereof

By introducing C and Fe elements into the titanium alloy matrix and using laser powder bed melting technology to generate nanoscale TiC particles, a multi-scale microstructure is formed, which solves the problem of insufficient wear resistance of additively manufactured titanium alloys and realizes high wear-resistant titanium alloy parts with high hardness and good plastic deformation coordination.

CN123128540APending Publication Date: 2026-11-20BEIJING ZHONGKE HONGTAI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611550454.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-08
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing additively manufactured titanium alloys have insufficient wear resistance, especially under high contact loads and particle erosion conditions, they are prone to adhesive wear, abrasive wear and fatigue wear. Furthermore, traditional surface coatings and chemical heat treatments have problems with coating uniformity and interfacial bonding reliability.

Method used

By introducing C and Fe elements into the titanium alloy matrix, dispersed nanoscale TiC particles are generated in situ using laser powder bed melting technology. Furthermore, the β→α' phase transformation behavior is regulated by Fe to form a multi-scale microstructure, thereby improving the material's hardness and plastic deformation coordination.

Benefits of technology

This method achieves high hardness, high load-bearing capacity, and good plastic deformation coordination in high wear-resistant titanium alloy parts, improves the stability of the friction layer, broadens the application fields of titanium alloys, and avoids the problems of limited reinforcement layer thickness and interface bonding in traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128540A_ABST
    Figure CN123128540A_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of metal material preparation, and particularly relates to a high-wear-resistance titanium alloy part and an additive manufacturing method thereof, the high-wear-resistance titanium alloy part has a multi-scale structure composed of a micron-level alpha / alpha' phase, a micron-level beta phase and a nano-level TiC particle; the C element in the alpha / alpha' phase is in a supersaturated solid solution state; the beta phase is stably formed by Fe element and is distributed between the alpha / alpha' phase; the TiC particle is formed by in-situ reaction of C and Ti in the additive manufacturing process and is dispersedly distributed in the matrix structure composed of the alpha / alpha' phase and the beta phase. The high-wear-resistance titanium alloy part has high hardness, high bearing capacity and good plastic deformation coordination capacity, can improve the plastic deformation coordination capacity of the friction layer while improving the hardness and the ploughing resistance, and is helpful to widening the application field of the titanium alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of metal material preparation technology, and specifically relates to a high wear-resistant titanium alloy part and its additive manufacturing method. Background Technology

[0002] Titanium alloys possess high specific strength, excellent corrosion resistance, and biocompatibility, and have been widely used in aerospace, weaponry, biomedicine, and energy and chemical industries. However, their high melting point and low thermal conductivity present challenges when using traditional melting and forging methods, leading to difficulties in fabricating complex structures, low yield, low material utilization, and high production costs. In contrast, metal additive manufacturing technologies such as Laser Powder Bed Fusion (LPBF), which uses powder as raw material to form layers, offer significant advantages in optimizing product structure and function, achieving near-net-shape forming, and controlling microstructure and properties. These technologies enable lightweight titanium alloy components, integrated complex structures, and high-performance, low-cost manufacturing, making them an important method for fabricating complex titanium alloy components.

[0003] In recent years, additively manufactured titanium alloys have been applied in my country's C919 passenger aircraft and American F-22 and F / A-18E / F fighter jets. However, the low hardness, insufficient plastic deformation capacity, and poor wear resistance of additively manufactured titanium alloys make them prone to adhesive wear, abrasive wear, and fatigue wear under conditions such as sliding friction, high contact loads, and particle erosion, severely limiting their further application. Currently, the main methods to improve the wear resistance of titanium alloys include surface coating, surface chemical heat treatment, and in-situ generation of ceramic particles to reinforce the matrix. Surface coating can form a high-hardness wear-resistant layer on the surface of titanium alloys, but it involves additional coating preparation and interface treatment processes. For complex three-dimensional components, there are still problems such as difficulty in uniform coating coverage and insufficient reliability of interface bonding. Surface chemical heat treatment forms a reinforcing layer on the material surface through element diffusion and phase transformation reactions, which can improve surface hardness and wear resistance, but it is prone to problems such as uneven thickness and composition of the reinforcing layer and insufficient deformation coordination between the matrix and the reinforcing layer.

[0004] In contrast, in-situ generation of ceramic reinforcing phase particles within the titanium alloy matrix can improve the material's hardness and wear resistance while avoiding complex coating preparation and diffusion layer treatment processes, as well as the problem of insufficient matrix-diffusion layer coordination. Among many reinforcing phases, titanium carbide (TiC) is considered one of the most ideal reinforcing phases for titanium alloys due to its high hardness, high strength, good elastic modulus, and density and coefficient of thermal expansion similar to the titanium matrix. By introducing carbon into titanium alloys, fine TiC particles can be generated in-situ within the matrix using the rapid melting and solidification process characteristics of additive manufacturing, thereby improving the material's hardness, load-bearing capacity, and resistance to plastic ploughing. However, additively manufactured titanium alloys inherently possess a "high strength, low plasticity" microstructure dominated by α'martensite. When further TiC reinforcing phases are introduced, if the content, size, and distribution of the reinforcing phase are not properly controlled, local stress concentration can easily occur at the TiC / matrix interface under frictional loads, inducing microcrack nucleation and propagation, leading to surface fatigue spalling and reinforcing phase detachment, which in turn exacerbates abrasive wear.

[0005] Therefore, the wear resistance of existing additively manufactured titanium alloys still needs to be improved. Summary of the Invention

[0006] The purpose of this application is to provide a high wear-resistant titanium alloy part and its additive manufacturing method. The high wear-resistant titanium alloy part of this application has high hardness, high load-bearing capacity and good plastic deformation coordination ability. It can improve the plastic deformation coordination ability of the friction layer while improving hardness and anti-plowing ability, which helps to broaden the application fields of titanium alloy.

[0007] The first aspect of this application provides a high wear-resistant titanium alloy part, which has a multi-scale microstructure composed of micron-sized α / α' phase, micron-sized β phase, and nano-sized TiC particles; the C element in the α / α' phase is in a supersaturated solid solution state; the β phase is stably formed by Fe element and distributed between the α / α' phase; the TiC particles are formed by the in-situ reaction of C and Ti during additive manufacturing and are dispersed in the matrix structure composed of the α / α' phase and the β phase.

[0008] In some embodiments, the high wear-resistant titanium alloy part has a hardness ≥434HV and an average coefficient of friction ≤0.46.

[0009] The second aspect of this application provides a method for preparing the high wear-resistant titanium alloy part described in the first aspect, comprising the following steps: mixing and ball milling titanium alloy powder, carbon source powder and iron source powder to obtain mixed powder; sieving and vacuum drying the mixed powder to obtain dry mixed powder; using the dry mixed powder as raw material, and using laser powder bed melting to obtain the high wear-resistant titanium alloy part.

[0010] In some embodiments, the titanium alloy powder includes at least one of TC4, TA15, TC11, and TC21 powders.

[0011] In some embodiments, the carbon source powder includes at least one of carbon black or graphite.

[0012] In some embodiments, the iron source powder includes at least one of pure iron and iron oxide powder.

[0013] In some embodiments, the added mass of the carbon source powder is calculated as 0.2 wt.% to 1 wt.% of the total mass of the mixed powder, and the added mass of the iron source powder is calculated as 0.25 wt.% to 3.5 wt.% of the total mass of the mixed powder; wherein, the total mass of the mixed powder is the sum of the masses of the titanium alloy powder, the carbon source powder, and the iron source powder.

[0014] In some embodiments, the ball milling and mixing adopts an atmosphere-protected double-roller ball milling method, and is set with a cycle mode of rotating for 10 minutes and pausing for 5 minutes. The ball milling speed is 100 r / min to 300 r / min, the ball milling time is 4 h to 8 h, and the ball-to-material ratio is 2:1 to 6:1.

[0015] In some embodiments, the protective atmosphere is high-purity argon.

[0016] In some embodiments, the ball milling mixture uses zirconium oxide grinding balls, which are prepared in a ratio of φ3mm:φ5mm=2:1, where φ is the diameter of the grinding ball.

[0017] In some embodiments, the particle size of the dried mixed powder is 15 μm to 53 μm.

[0018] In some embodiments, the drying temperature is 80℃~100℃ and the drying time is 5h~10h.

[0019] In some embodiments, the parameters for laser powder bed melting include: laser power of 175W~300W, scanning speed of 900mm / s~1500mm / s, scanning spacing of 0.08mm~0.16mm, and powder layer thickness of 25μm~35μm.

[0020] In some embodiments, the laser powder bed melting process is carried out under the protection of high-purity argon gas, and the oxygen content in the forming chamber is controlled to be less than 500 ppm, and the substrate preheating temperature is 200°C to 300°C.

[0021] In some embodiments, the preparation method further includes grinding and mechanical polishing the resulting high wear-resistant titanium alloy parts.

[0022] In some embodiments, the high wear-resistant titanium alloy parts are sequentially polished with SiC sandpaper of 240#, 800#, 1500#, 2000# and 3000#; then mechanically polished to a mirror finish, the high wear-resistant titanium alloy parts are ultrasonically cleaned in anhydrous ethanol for 15 minutes and then dried.

[0023] The beneficial effects of this application are: (1) This application provides a multi-scale strengthening structure synergistically regulated by C and Fe. Utilizing the ultra-high cooling rate and extreme temperature gradient characteristics of the additive manufacturing process, C reacts in situ with Ti to form diffusely distributed nanoscale TiC particles, while some C exists in the matrix in the form of supersaturated interstitial solid solution; Fe, a strong β-stabilizing element, regulates the β→α' phase transformation behavior, so that the room temperature structure retains an appropriate amount of β phase, thereby achieving the synergistic effect of TiC particle reinforcement, C interstitial solid solution strengthening and matrix structure plasticity regulation.

[0024] (2) This application provides a wear-resistant additive manufacturing titanium alloy with high hardness, high load-bearing capacity and good plastic deformation coordination ability, with a hardness ≥434HV. The dispersed nano-sized TiC particles and interstitial solid solution C effectively improve the material hardness and resistance to plastic deformation, and reduce the plowing and adhesion effects during the friction process; the appropriate amount of β phase formed by Fe regulation improves the plastic deformation coordination ability and stability of the friction layer, reduces the shedding of wear debris and the formation of secondary abrasive particles, which is conducive to the stable formation of the friction film and inhibits the initiation, propagation and shedding of microcracks and reinforcing phase, thereby achieving improved wear resistance.

[0025] (3) This application has the advantage of low-cost manufacturing of complex wear-resistant components. By synergistic alloying of C and Fe elements, a wear-resistant and reinforced structure is constructed inside the titanium alloy matrix, thereby improving the overall wear resistance of the material and avoiding the problems of limited reinforcement layer thickness, interface bonding and local failure in traditional surface coating and diffusion layer technologies. Even if the surface wears, the internal material still maintains the same wear-resistant structure and properties, thereby improving the service stability and service life of the wear-resistant components.

[0026] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Attached Figure Description

[0027] To more clearly illustrate the technical solutions in the specific embodiments of this application or the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0028] Figure 1 This is a SEM image of the dried mixed powder after sieving and drying in Example 1 of this application; Figure 2 This is a curve showing the change in the friction coefficient of the titanium alloy part prepared in Example 1 of this application over time. Detailed Implementation

[0029] Exemplary embodiments of this application will now be described in more detail with reference to the accompanying drawings. While exemplary embodiments of this application are shown in the drawings, it should be understood that this application may be implemented in various forms and should not be limited to the embodiments set forth herein. Rather, these embodiments are provided to enable a more thorough understanding of this application and to fully convey the scope of this application to those skilled in the art.

[0030] It should be understood that the terminology used herein is for the purpose of describing particular exemplary embodiments only and is not intended to be limiting. Unless the context clearly indicates otherwise, the singular forms “a,” “an,” and “described” as used herein may also include the plural forms. The terms “comprising,” “including,” “containing,” and “having” are inclusive and therefore indicate the presence of the stated features, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, steps, operations, elements, components, and / or combinations thereof. The method steps, processes, and operations described herein are not construed as requiring them to be performed in a particular order described or illustrated unless the order of performance is explicitly indicated. It should also be understood that additional or alternative steps may be used.

[0031] In the description of the embodiments of this application, technical terms such as "first" and "second" are used only to distinguish different objects and should not be construed as indicating or implying relative importance or implicitly specifying the number, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, "multiple" means two or more, unless otherwise explicitly defined.

[0032] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0033] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this document generally indicates that the preceding and following related objects have an "or" relationship.

[0034] In the description of the embodiments of this application, the term "multiple" refers to two or more (including two), similarly, "multiple sets" refers to two or more (including two sets), and "multiple pieces" refers to two or more (including two pieces).

[0035] The first aspect of this application provides a high wear-resistant titanium alloy part, which has a multi-scale microstructure composed of micron-sized α / α' phase, micron-sized β phase and nano-sized TiC particles; the C element in the α / α' phase is in a supersaturated solid solution state; the β phase is stably formed by Fe element and distributed between the α / α' phase; the TiC particles are formed by the in-situ reaction of C and Ti during the additive manufacturing process and are dispersed in the matrix microstructure composed of the α / α' phase and the β phase.

[0036] In the embodiments of this application, by introducing C and Fe elements, and utilizing the high chemical reactivity between Ti and C, as well as the high cooling rate and large temperature gradient characteristics of the additive manufacturing process, C elements are dispersed in situ to form ultrafine nano-TiC and achieve partial supersaturated solid solution of C. At the same time, the β-stabilizing effect of Fe is used to regulate the β→α' phase transformation behavior and β phase content, thereby improving the plastic deformation coordination ability of the matrix. This achieves a multi-scale synergistic strengthening effect of ultrafine nano-scale TiC reinforcement, C interstitial solid solution strengthening, and matrix deformation coordination, resulting in a wear-resistant titanium alloy with high hardness, high load-bearing capacity, and good plastic deformation coordination ability. This improves the hardness and anti-ploughing ability while enhancing the plastic deformation coordination ability of the friction layer, which helps to broaden the application fields of titanium alloys.

[0037] In some embodiments of this application, the hardness of the high-wear-resistant titanium alloy part is ≥434HV, and the average coefficient of friction is ≤0.46. As an example, the hardness of the high-wear-resistant titanium alloy part can be one of 434HV, 451HV, 464HV, 470HV, 475HV, and 478HV, or any value satisfying the above range. As an example, the average coefficient of friction of the high-wear-resistant titanium alloy part can be one of 0.46, 0.45, 0.43, 0.41, and 0.40, or any value satisfying the above range.

[0038] The second aspect of this application provides an additive manufacturing method for high wear-resistant titanium alloy parts, which mainly includes the following steps: mixing and ball milling titanium alloy powder, carbon source powder and iron source powder to obtain mixed powder; sieving and vacuum drying the mixed powder to obtain dry mixed powder; using the dry mixed powder as raw material, and using laser powder bed melting to obtain high wear-resistant titanium alloy parts.

[0039] In this embodiment, the preparation method introduces C and Fe elements during additive manufacturing. C reacts in situ with Ti in a high-temperature molten pool to form a TiC reinforcing phase. The rapid solidification and extremely high temperature gradient of the additive manufacturing process suppress the coarsening and aggregation of TiC particles, allowing them to be dispersed in the matrix as ultrafine nanoparticles, resulting in significant second-phase reinforcement. Simultaneously, rapid solidification causes C to exist in the matrix as a supersaturated interstitial solid solution, generating solid solution reinforcement through lattice distortion. Furthermore, Fe, a strong β-stabilizing element, regulates the β→α' transformation behavior and β-phase stability, forming an appropriate amount of β-phase in the room-temperature microstructure. This improves the plastic deformation coordination of the matrix, alleviates local stress concentration at the TiC reinforcing phase-matrix interface under frictional loads, thereby inhibiting microcrack nucleation and propagation, and promoting the formation and stabilization of the friction film. Through the synergistic regulation of C and Fe, a multi-scale synergistic reinforcement structure is constructed, improving both the material's hardness and load-bearing capacity while enhancing plastic deformation coordination, thus significantly improving the wear resistance of additively manufactured titanium alloys.

[0040] In some embodiments of this application, the additive manufacturing method for high wear-resistant titanium alloy parts is mainly carried out according to the following steps.

[0041] S1, Prepare mixed powder.

[0042] In some embodiments, the raw material powders used to prepare the mixed powder include titanium alloy powder, carbon source powder, and iron source powder.

[0043] In some embodiments, the titanium alloy powder includes at least one of TC4, TA15, TC11, and TC21 powders.

[0044] In some embodiments, the carbon source powder includes at least one of carbon black or graphite.

[0045] In some embodiments, the iron source powder includes at least one of pure iron and iron oxide powder.

[0046] Carbon black or graphite is used as the carbon source, and pure iron and iron oxides are used as the iron source. C reacts with Ti in situ to form TiC, while the β-phase stabilizing effect of Fe is utilized to form an appropriate amount of β phase. By rationally controlling the content of C and Fe elements, as well as key forming process parameters such as laser power, scanning speed, scanning spacing and layer thickness, the size and distribution of TiC particles are regulated, so that they are dispersed in the matrix at the nanoscale. The amount of TiC particle precipitation and the volume fraction of β phase are controlled within a reasonable range to avoid excessive second phase leading to a decrease in plasticity. Finally, a multi-scale structure composed of micron-sized α / α′ phase, micron-sized β phase and nano-TiC particles is formed.

[0047] In some embodiments, the total mass of the mixed powder is the sum of the masses of titanium alloy powder, carbon source powder, and iron source powder; wherein, the mass of carbon source powder is calculated as 0.2wt.% to 1wt.% of the total mass of the mixed powder, and the mass of iron source powder is calculated as 0.25wt.% to 3.5wt.% of the total mass of the mixed powder.

[0048] As an example, the mass of carbon source powder added can be calculated as one of the following: 0.2 wt.%, 0.3 wt.%, 0.4 wt.%, 0.5 wt.%, 0.6 wt.%, 0.7 wt.%, 0.8 wt.%, 0.9 wt.%, 1 wt.%, or any value within the above range, based on the mass of C element as a percentage of the total mass of the mixed powder.

[0049] As an example, the added mass of iron source powder can be calculated as follows: the mass of Fe element accounts for 0.25 wt.%, 0.3 wt.%, 0.4 wt.%, 0.5 wt.%, 0.6 wt.%, 0.7 wt.%, 0.8 wt.%, 0.9 wt.%, 1 wt.%, 1.1 wt.%, 1.2 wt.%, 1.3 wt.%, 1.4 wt.%, 1.5 wt.%, 1.6 wt.%, 1.7 wt.%, 1.8 wt.%, 1.9 wt.%, 2 wt.%, 2.1 wt.%, 2.2 wt.%, 2.3 wt.%, 2.4 wt.%, 2.5 wt.%, 2.6 wt.%, 2.7 wt.%, 2.8 wt.%, 2.9 wt.%, 3 wt.%, 3.1 wt.%, 3.2 wt.%, 3.3 wt.%, 3.4 wt.%, and 3.5 wt.%, or any value within the above range, of the total mass of the mixed powder.

[0050] In some embodiments, titanium alloy powder, carbon source powder, and iron source powder are ball-milled and mixed in a desired ratio to obtain a mixed powder.

[0051] In some embodiments, titanium alloy powder, carbon source powder and iron source powder are prepared in the required proportions, and then ball-milled and mixed using a two-roll ball milling process protected by high-purity argon gas to obtain mixed powder.

[0052] In some embodiments, the rotational speed during ball milling is set to 100 r / min to 300 r / min. As an example, the rotational speed can be one of 100 r / min, 120 r / min, 150 r / min, 180 r / min, 200 r / min, 220 r / min, 250 r / min, 280 r / min, 300 r / min, or any value within the range described above.

[0053] In some implementations, the ball-to-material ratio is 2:1 to 6:1. As an example, the ball-to-material ratio can be one of 2:1, 3:1, 4:1, 5:1, 6:1, or any value that satisfies the above range.

[0054] In some implementations, the ball milling time is 4 to 8 hours. As an example, the ball milling time can be one of 4 hours, 5 hours, 6 hours, 7 hours, or 8 hours, or any value within the range described above.

[0055] In some implementations, a cyclic ball milling mode of rotating for 10 minutes and pausing for 5 minutes is used.

[0056] In some embodiments, the grinding balls are zirconia balls, prepared in a ratio of φ3mm:φ5mm=2:1, where φ is the diameter of the grinding ball.

[0057] S2, pretreatment of mixed powders.

[0058] In some embodiments, the mixed powder obtained in step S1 is subjected to sieving and vacuum drying, and then cooled to room temperature after drying to obtain dried mixed powder.

[0059] In some embodiments, the mixed powder obtained in step S1 is sieved to select mixed powder with a particle size in the range of 15μm to 53μm; then it is vacuum dried at a temperature of 80℃ to 100℃ for 5h to 10h, and then cooled to room temperature after drying to obtain dried mixed powder.

[0060] As an example, the particle size of the dry mixed powder can be one of 15μm, 18μm, 20μm, 22μm, 25μm, 28μm, 30μm, 32μm, 35μm, 38μm, 40μm, 42μm, 45μm, 48μm, 50μm, 53μm or any value that satisfies the above range.

[0061] As an example, the drying temperature can be one of 80°C, 85°C, 90°C, 95°C, 100°C or any value that meets the above range.

[0062] As an example, the drying time can be one of 5h, 6h, 7h, 8h, 9h, 10h or any value that meets the above range.

[0063] It is worth noting that "room temperature" in this application generally refers to a state without active heating or cooling. In some embodiments, room temperature refers to a temperature of 20°C to 35°C. For example, it could be 25°C.

[0064] S3, LPBF formed titanium alloy parts.

[0065] In some embodiments, the dried mixed powder obtained in step S2 is used as raw material to prepare titanium alloy parts using the LPBF process. Before printing begins, the substrate is preheated to 200°C to 300°C. The printing process is carried out under the protection of high-purity argon gas, and the oxygen content in the forming chamber is controlled to be less than 500 ppm.

[0066] As an example, the substrate preheating temperature can be one of 200°C, 220°C, 250°C, 280°C, 300°C, or any value that meets the above range.

[0067] In some implementations, the LPBF process parameters include: laser power of 175W~300W, scanning speed of 900mm / s~1500mm / s, scanning spacing of 0.08mm~0.16mm, and powder layer thickness of 25μm~35μm.

[0068] As an example, the laser power can be one of 175W, 180W, 185W, 190W, 195W, 200W, 210W, 220W, 230W, 240W, 250W, 260W, 270W, 275W, 280W, 290W, 300W or any value that meets the above range.

[0069] As an example, the scanning speed can be one of 900mm / s, 950mm / s, 1000mm / s, 1100mm / s, 1200mm / s, 1300mm / s, 1400mm / s, 1500mm / s or any value that meets the above range.

[0070] As an example, the scanning interval can be one of 0.08mm, 0.09mm, 0.10mm, 0.11mm, 0.12mm, 0.13mm, 0.14mm, 0.15mm, or 0.16mm, or any value within the range mentioned above.

[0071] As an example, the powder layer thickness can be one of 25μm, 26μm, 27μm, 28μm, 29μm, 30μm, 31μm, 32μm, 33μm, 34μm, 35μm or any value that meets the above range.

[0072] S4, Pretreatment of titanium alloy parts.

[0073] In some embodiments, the titanium alloy parts obtained in step S3 are subjected to grinding and mechanical polishing.

[0074] In some embodiments, the titanium alloy parts are polished sequentially using SiC sandpaper of 240#, 800#, 1500#, 2000# and 3000#; then mechanical polishing is performed until a mirror finish is achieved, and the titanium alloy parts are ultrasonically cleaned in anhydrous ethanol for 15 minutes and then dried.

[0075] Unless otherwise defined, the technical terms used in the following embodiments have the same meaning as commonly understood by those skilled in the art to which this application pertains. Unless otherwise specified, the experimental reagents used in the following embodiments are all conventional biochemical reagents; the raw materials, instruments, and equipment used in the following embodiments can all be obtained through commercial purchase or by existing methods; the amounts of experimental reagents used are, unless otherwise specified, the amounts used in conventional experimental operations; and the experimental methods used are, unless otherwise specified, conventional methods. It should be further noted that the following descriptions are merely exemplary and not intended to limit the scope of this application. Moreover, the comparative examples below are selected to compare with the technical solutions of this application to demonstrate the advancement of the technical solutions of this application, and do not necessarily represent prior art in this technical field.

[0076] Example 1 Taking the design and preparation of the wear-resistant additive manufacturing TC4-0.4C-3Fe alloy with synergistic C and Fe control as an example, the preparation process is described in detail; where 0.4C represents a C element mass percentage of 0.4 wt.% and 3Fe represents a Fe element mass percentage of 3 wt.%, the specific steps are as follows: 1) Weigh carbon black particles, Fe powder, and TC4 alloy powder according to a C content of 0.4 wt.% and an Fe content of 3 wt.%. Simultaneously, weigh grinding balls with diameters of 3 mm and 5 mm according to a grinding ball mass to total powder mass ratio (sum of carbon black particles, Fe powder, and TC4 alloy powder) of 4:1 and a φ3mm:φ5mm ratio of 2:1. Add the weighed carbon black particles, Fe powder, TC4 alloy powder, and zirconia grinding balls to the grinding jar. Powder weighing, grinding ball weighing, and filling and sealing of the grinding jar are all completed in a glove box. The grinding jar is filled with high-purity argon as a protective atmosphere. Place the grinding jar on a two-roll ball mill and mix the carbon black particles, Fe powder, and Ti-6Al-4V alloy powder. Set the grinding speed to 300 r / min and the grinding time to 4 hours, cycling through the mill in a 10-minute rotation, 5-minute pause pattern until the program ends.

[0077] 2) Remove the grinding balls and mixed powder from the ball mill jar. Use a sieve to separate the mixed powder from the grinding balls, and further screen out the mixed powder with a particle size of 15μm~53μm. The screened mixed powder is then dried in a vacuum drying oven at 80℃ for 8 hours. After the process is complete, allow the mixed powder to cool to room temperature before removing it for later use. The morphology of the mixed powder is as follows: Figure 1 As shown.

[0078] 3) The mixed powder after drying is used to prepare the part using LPBF technology. The substrate preheating temperature is 200℃, the laser power is 275W, the scanning speed is 1100mm / s, the scanning spacing is 0.16mm, the powder layer thickness is 30μm, and the entire printing process is carried out under the protection of high-purity argon gas. The oxygen content in the forming chamber is always less than 500ppm.

[0079] 4) The prepared LPBF titanium-based alloy parts were pretreated by grinding the titanium-based alloy parts with SiC sandpaper of 240#, 800#, 1500#, 2000# and 3000# in sequence; then mechanical polishing was performed until the surface was mirror-finished. After that, the titanium-based alloy parts were ultrasonically cleaned in anhydrous ethanol for 15 minutes and then dried.

[0080] Performance testing 1. Hardness test.

[0081] The hardness of titanium alloy parts after grinding and mechanical polishing was tested using a microhardness tester.

[0082] Hardness tests were conducted using a microhardness tester under an applied load of 0.5 kg and a holding time of 15 s. Ten points were tested on each titanium alloy part, and the average value of the ten points was taken as the hardness test result.

[0083] 2. Tribological property characterization.

[0084] The friction performance of titanium alloy parts after grinding and mechanical polishing was tested using a multi-functional friction and wear testing machine to obtain the average friction coefficient.

[0085] Tribological properties were tested using a multi-functional friction and wear testing machine to obtain the average coefficient of friction. The friction method was ball-plane reciprocating sliding, with a reciprocating stroke of 4 mm and a time of 30 min. The friction pair consisted of silicon nitride ceramic balls.

[0086] The test results show that the average friction coefficient of the titanium-based alloy part in Example 1 is 0.46 and the average hardness is 434 HV. The results are shown in Table 1. Figure 2 The graph showing the change in the friction coefficient of the titanium alloy part over time in Example 1 is shown.

[0087] Example 2 Taking the design and preparation of the wear-resistant additive manufacturing TC4-0.6C-2.5Fe alloy with synergistic C and Fe control as an example, the preparation process is described in detail; where 0.6C represents a C element mass percentage of 0.6 wt.% and 2.5Fe represents a Fe element mass percentage of 2.5 wt.%, the specific steps are as follows: 1) Weigh carbon black particles, Fe powder, and TC4 alloy powder according to a C content of 0.6 wt.% and an Fe content of 2.5 wt.%. Simultaneously, weigh grinding balls with diameters of 3 mm and 5 mm according to a grinding ball mass to total powder mass ratio (sum of carbon black particles, Fe powder, and TC4 alloy powder) of 5:1 and a φ3mm:φ5mm ratio of 2:1. Add the weighed carbon black particles, Fe powder, TC4 alloy powder, and zirconia grinding balls to the grinding jar. Powder weighing, grinding ball weighing, and filling and sealing of the grinding jar are all completed in a glove box. The grinding jar is filled with high-purity argon as a protective atmosphere. Place the grinding jar on a two-roll ball mill and mix the carbon black particles, Fe powder, and TC4 alloy powder. Set the grinding speed to 100 r / min and the grinding time to 8 hours, cycling through the mill in a 10-minute rotation, 5-minute pause pattern until the program ends.

[0088] 2) Remove the grinding balls and mixed powder from the ball mill jar. Use a sieve to separate the mixed powder from the grinding balls, and further screen out the mixed powder with a particle size of 15μm~53μm. The screened mixed powder is dried in a vacuum drying oven at 100℃ for 5 hours. After the program is completed, allow the mixed powder to cool to room temperature before taking it out for use.

[0089] 3) The mixed powder after drying is used to prepare the part using LPBF technology. The substrate preheating temperature is 200℃, the laser power is 300W, the scanning speed is 1500mm / s, the scanning spacing is 0.12mm, the powder layer thickness is 30μm, and the entire printing process is carried out under the protection of high-purity argon gas. The oxygen content in the forming chamber is always less than 500ppm.

[0090] 4) The prepared LPBF titanium alloy parts were pretreated by grinding them with SiC sandpaper of 240#, 800#, 1500#, 2000# and 3000# in sequence; then mechanical polishing was performed until the surface was mirror-finished. The titanium alloy parts were then ultrasonically cleaned in anhydrous ethanol for 15 minutes and dried.

[0091] The test results show that the average friction coefficient of the titanium alloy part in Example 2 is 0.45 and the average hardness is 451 HV. The results are shown in Table 1.

[0092] Example 3 Taking the design and preparation of the wear-resistant additive manufacturing TA15-0.3C-3.5Fe alloy with synergistic regulation of C and Fe as an example, the preparation process is described in detail; where 0.3C represents 0.3 wt.% of C element and 3.5Fe represents 3.5 wt.% of Fe element. The specific steps are as follows: 1) Weigh carbon black particles, Fe powder, and TA15 alloy powder according to a C content of 0.3 wt.% and an Fe content of 3.5 wt.%. Simultaneously, weigh grinding balls with diameters of 3 mm and 5 mm according to a grinding ball mass to total powder mass ratio (sum of carbon black particles, Fe powder, and TA15 alloy powder) of 6:1 and a φ3mm:φ5mm ratio of 2:1. Add the weighed carbon black particles, Fe powder, TA15 alloy powder, and zirconia grinding balls to the grinding jar. Powder weighing, grinding ball weighing, and filling and sealing of the grinding jar are all completed in a glove box. The grinding jar is filled with high-purity argon as a protective atmosphere. Place the grinding jar on a two-roll ball mill and mix the carbon black particles, Fe powder, and TA15 alloy powder. Set the grinding speed to 200 r / min and the grinding time to 6 hours, cycling through the mill in a 10-minute rotation, 5-minute pause pattern until the program ends.

[0093] 2) Remove the grinding balls and mixed powder from the ball mill jar. Use a sieve to separate the mixed powder from the grinding balls, and further screen out the mixed powder with a particle size of 15μm~53μm. The screened mixed powder is dried in a vacuum drying oven at 80℃ for 10 hours. After the program is completed, allow the mixed powder to cool to room temperature before taking it out for use.

[0094] 3) The mixed powder after drying is used to prepare the part using LPBF technology. The substrate preheating temperature is 250℃, the laser power is 250W, the scanning speed is 1200mm / s, the scanning spacing is 0.12mm, the powder layer thickness is 30μm, and the entire printing process is carried out under the protection of high-purity argon gas. The oxygen content in the forming chamber is always less than 500ppm.

[0095] 4) The prepared LPBF titanium alloy parts were pretreated by grinding them with SiC sandpaper of 240#, 800#, 1500#, 2000# and 3000# in sequence; then mechanical polishing was performed until the surface was mirror-finished. The titanium alloy parts were then ultrasonically cleaned in anhydrous ethanol for 15 minutes and dried.

[0096] The test results show that the average friction coefficient of the titanium alloy part in Example 3 is 0.40 and the average hardness is 478 HV. The results are shown in Table 1.

[0097] Example 4 Taking the design and preparation of the wear-resistant additive manufacturing TC4-0.8C-3.5Fe alloy with synergistic C and Fe control as an example, the preparation process is described in detail; where 0.8C represents 0.8 wt.% of C element mass and 3.5Fe represents 3.5 wt.% of Fe element mass percentage. The specific steps are as follows: 1) Weigh graphite powder, Fe powder, and TC4 alloy powder according to a C content of 0.3 wt.% and an Fe content of 3.5 wt.%. Simultaneously, weigh grinding balls with diameters of 3 mm and 5 mm according to a grinding ball mass to total powder mass ratio (sum of graphite powder, Fe powder, and TC4 alloy powder) of 2:1 and a φ3mm:φ5mm ratio of 2:1. Add the weighed graphite powder, Fe powder, TC4 alloy powder, and zirconia grinding balls to the grinding jar. Powder weighing, grinding ball weighing, and filling and sealing of the grinding jar are all completed in a glove box. The grinding jar is filled with high-purity argon as a protective atmosphere. Place the grinding jar on a two-roll ball mill and mix the graphite powder, Fe powder, and TC4 alloy powder. Set the grinding speed to 150 r / min and the grinding time to 6 hours, cycling through the mill in a 10-minute rotation, 5-minute pause pattern until the program ends.

[0098] 2) Remove the grinding balls and mixed powder from the ball mill jar. Use a sieve to separate the mixed powder from the grinding balls, and further screen out the mixed powder with a particle size of 15μm~53μm. The screened mixed powder is dried in a vacuum drying oven at 80℃ for 10 hours. After the program is completed, allow the mixed powder to cool to room temperature before taking it out for use.

[0099] 3) The mixed powder after drying is used to prepare the part using LPBF technology. The substrate preheating temperature is 200℃, the laser power is 250W, the scanning speed is 1200mm / s, the scanning spacing is 0.12mm, the powder layer thickness is 35μm, and the entire printing process is carried out under the protection of high-purity argon gas. The oxygen content in the forming chamber is always less than 500ppm.

[0100] 4) The prepared LPBF titanium alloy parts were pretreated by grinding them with SiC sandpaper of 240#, 800#, 1500#, 2000# and 3000# in sequence; then mechanical polishing was performed until the surface was mirror-finished. The titanium alloy parts were then ultrasonically cleaned in anhydrous ethanol for 15 minutes and dried.

[0101] The test results show that the average friction coefficient of the titanium alloy part in Example 4 is 0.43 and the average hardness is 464 HV. The results are shown in Table 1.

[0102] Example 5 Taking the design and preparation of the wear-resistant additive manufacturing TC4-1C-0.25Fe alloy with synergistic C and Fe control as an example, the preparation process is described in detail; where 1C represents 1 wt.% of C element mass and 0.25Fe represents 0.25 wt.% of Fe element mass percentage. The specific steps are as follows: 1) Weigh graphite powder, Fe powder, and TC4 alloy powder according to a C content of 1 wt.% and an Fe content of 0.25 wt.%. Simultaneously, weigh grinding balls with diameters of 3 mm and 5 mm according to a grinding ball mass to total powder mass ratio (sum of graphite powder, Fe powder, and TC4 alloy powder) of 4:1 and a φ3mm:φ5mm ratio of 2:1. Add the weighed graphite powder, Fe powder, TC4 alloy powder, and zirconia grinding balls to the grinding jar. Powder weighing, grinding ball weighing, and filling and sealing of the grinding jar are all completed in a glove box. The grinding jar is filled with high-purity argon as a protective atmosphere. Place the grinding jar on a two-roll ball mill and mix the graphite powder, Fe powder, and TC4 alloy powder. Set the grinding speed to 200 r / min and the grinding time to 5 hours, cycling through the mill in a 10-minute rotation, 5-minute pause pattern until the program ends.

[0103] 2) Remove the grinding balls and mixed powder from the ball mill jar. Use a sieve to separate the mixed powder from the grinding balls, and further screen out the mixed powder with a particle size of 15μm~53μm. The screened mixed powder is dried in a vacuum drying oven at 80℃ for 8 hours. After the program is completed, allow the mixed powder to cool to room temperature before taking it out for use.

[0104] 3) The mixed powder after drying is used to prepare the part using LPBF technology. The substrate preheating temperature is 200℃, the laser power is 175W, the scanning speed is 900mm / s, the scanning spacing is 0.1mm, the powder layer thickness is 25μm, and the entire printing process is carried out under the protection of high-purity argon gas. The oxygen content in the forming chamber is always less than 500ppm.

[0105] 4) The prepared LPBF titanium alloy parts were pretreated by grinding them with SiC sandpaper of 240#, 800#, 1500#, 2000# and 3000# in sequence; then mechanical polishing was performed until the surface was mirror-finished. The titanium alloy parts were then ultrasonically cleaned in anhydrous ethanol for 15 minutes and dried.

[0106] The test results show that the average friction coefficient of the titanium alloy part in Example 5 is 0.45 and the average hardness is 470 HV. The results are shown in Table 1.

[0107] Example 6 Taking the design and preparation of wear-resistant additive manufacturing TA15-0.2C-1.5Fe alloy with synergistic C and Fe control as an example, the preparation process is described in detail; where 0.2C represents 0.2 wt.% of C element and 1.5Fe represents 1.5 wt.% of Fe element. The specific steps are as follows: 1) Weigh graphite powder, Fe2O3 powder, and TC4 alloy powder according to a C content of 0.2 wt.% and an Fe content of 1.5 wt.%. Simultaneously, weigh grinding balls with diameters of 3 mm and 5 mm according to a grinding ball mass to total powder mass ratio (sum of graphite powder, Fe powder, and TC4 alloy powder) of 4:1 and a φ3mm:φ5mm = 2:1 ratio. Add the weighed graphite powder, Fe2O3 powder, TA15 alloy powder, and zirconia grinding balls to the grinding jar. Powder weighing, grinding ball weighing, and filling and sealing of the grinding jar are all completed in a glove box. The grinding jar is filled with high-purity argon as a protective atmosphere. Place the grinding jar on a two-roll ball mill and mix the graphite powder, Fe powder, and TC4 alloy powder. Set the grinding speed to 200 r / min and the grinding time to 5 h, cycling through the mill in a 10-minute rotation, 5-minute pause pattern until the program ends.

[0108] 2) Remove the grinding balls and mixed powder from the ball mill jar. Use a sieve to separate the mixed powder from the grinding balls, and further screen out the mixed powder with a particle size of 15μm~53μm. The screened mixed powder is dried in a vacuum drying oven at 80℃ for 8 hours. After the program is completed, allow the mixed powder to cool to room temperature before taking it out for use.

[0109] 3) The mixed powder after drying is used to prepare the part using LPBF technology. The substrate preheating temperature is 250℃, the laser power is 175W, the scanning speed is 1300mm / s, the scanning spacing is 0.08mm, the powder layer thickness is 30μm, and the entire printing process is carried out under the protection of high-purity argon gas. The oxygen content in the forming chamber is always less than 500ppm.

[0110] 4) The prepared LPBF titanium alloy parts were pretreated by grinding them with SiC sandpaper of 240#, 800#, 1500#, 2000# and 3000# in sequence; then mechanical polishing was performed until the surface was mirror-finished. The titanium alloy parts were then ultrasonically cleaned in anhydrous ethanol for 15 minutes and dried.

[0111] The test results show that the average friction coefficient of the titanium alloy part in Example 6 is 0.41 and the average hardness is 475 HV. The results are shown in Table 1.

[0112] Comparative Example 1 Except that the powder used for LPBF printing was TC4 alloy powder, the powder pretreatment, printing preparation, part pretreatment and performance testing were carried out in the same way as in Example 1. The test results are shown in Table 1.

[0113] Comparative Example 2 Except that the powder used for LPBF printing was a mixture of TC4 alloy powder and carbon black (TC4-0.4C), the mixed powder preparation, powder pretreatment, printing preparation, part pretreatment and performance testing were carried out in the same way as in Example 1. The test results are shown in Table 1.

[0114] Table 1

[0115] As can be seen from the data in Table 1, this application has the advantage of low-cost manufacturing of complex wear-resistant components. By constructing a wear-resistant and reinforced structure within the titanium alloy matrix through synergistic alloying of C and Fe elements, the overall wear resistance of the material is improved, avoiding problems such as limited reinforced layer thickness, interface bonding, and localized failures that exist in traditional surface coating and diffusion layer technologies. Even if the surface layer wears, the internal material still maintains the same wear-resistant structure and properties, thereby improving the service stability and service life of the wear-resistant components.

[0116] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application.

Claims

1. A high wear-resistant titanium alloy component, characterized in that, The titanium alloy component has a multi-scale microstructure composed of micron-scale α / α' phase, micron-scale β phase and nano-scale TiC particles; The C element in the α / α' phase is in a supersaturated solid solution state; The β phase is stably formed by Fe element and is distributed between the α / α' phases; The TiC particles are formed by the in-situ reaction of C and Ti during additive manufacturing and are dispersed in the matrix structure composed of the α / α' phase and the β phase.

2. The high wear-resistant titanium alloy part as described in claim 1, characterized in that, The high wear-resistant titanium alloy part has a hardness ≥434HV and an average friction coefficient ≤0.

46.

3. A method for preparing a high wear-resistant titanium alloy part as described in claim 1 or 2, characterized in that, The preparation method includes the following steps: Titanium alloy powder, carbon source powder and iron source powder are mixed and ball-milled to obtain mixed powder; The mixed powder is sieved and vacuum dried to obtain a dry mixed powder. The high wear-resistant titanium alloy parts are obtained by using the dry mixed powder as raw material and laser powder bed melting forming.

4. The preparation method according to claim 1, characterized in that, The titanium alloy powder includes at least one of TC4, TA15, TC11, and TC21 powders; And / or, the carbon source powder includes at least one of carbon black or graphite; And / or, the iron source powder includes at least one of pure iron and iron oxide powder.

5. The preparation method according to claim 1, characterized in that, The mass of the added carbon source powder is calculated based on the mass of C element accounting for 0.2 wt.% to 1 wt.% of the total mass of the mixed powder. And / or, the mass of the added iron source powder is calculated based on the mass of Fe element accounting for 0.25wt.% to 3.5wt.% of the total mass of the mixed powder; The total mass of the mixed powder is the sum of the masses of the titanium alloy powder, the carbon source powder, and the iron source powder.

6. The preparation method according to claim 1, characterized in that, The ball milling and mixing adopts a two-roller ball milling method under atmosphere protection, and is set with a cycle mode of rotating for 10 minutes and pausing for 5 minutes. The ball milling speed is 100 r / min to 300 r / min, the ball milling time is 4 h to 8 h, and the ball-to-material ratio is 2:1 to 6:

1. Optionally, the protective atmosphere is high-purity argon; Optionally, the ball milling mixture uses zirconium oxide grinding balls, which are prepared in a ratio of φ3mm:φ5mm=2:1, where φ is the diameter of the grinding ball.

7. The preparation method according to claim 1, characterized in that, The particle size of the dried mixed powder is 15μm~53μm; Optionally, the drying temperature is 80℃~100℃ and the drying time is 5h~10h.

8. The preparation method according to claim 1, characterized in that, The parameters for laser powder bed melting and forming include: laser power of 175W~300W, scanning speed of 900mm / s~1500mm / s, scanning spacing of 0.08mm~0.16mm, and powder layer thickness of 25μm~35μm; Optionally, the laser powder bed melting and forming process is carried out under the protection of high-purity argon gas, and the oxygen content in the forming chamber is controlled to be less than 500 ppm, and the substrate preheating temperature is 200℃~300℃.

9. The preparation method according to claim 1, characterized in that, The preparation method also includes grinding and mechanical polishing the obtained high wear-resistant titanium alloy parts.

10. The preparation method according to claim 9, characterized in that, The high wear-resistant titanium alloy parts were sequentially polished using SiC sandpaper of grades 240#, 800#, 1500#, 2000# and 3000#. Then, they were mechanically polished to a mirror finish. After polishing, the high wear-resistant titanium alloy parts were ultrasonically cleaned in anhydrous ethanol for 15 minutes and then dried.