A method for welding a girth weld of a nuclear power pipeline B sleeve in service repair

The angular arc-shaped oscillating welding method using a CMT and GTA composite heat source solves the problem of heat input control in the welding of the B-shaped sleeve circumferential fillet weld of nuclear power pipelines, achieves high-quality weld welding, reduces non-fusion defects and embrittlement risks, and is suitable for in-service repair of nuclear power pipelines.

CN123128673APending Publication Date: 2026-11-20CHINA NUCLEAR IND MAINTENANCE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611228051.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-13
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

The heat input is difficult to control during the welding of the circumferential fillet weld of the B-type sleeve of nuclear power pipeline, which easily leads to non-fusion defects. In addition, the large heat input of automated welding leads to the risk of weld embrittlement and low-stress cracking.

Method used

By employing a composite heat source of cold metal transfer (CMT) and gas non-consumable electrode inert gas (GTA), and through angular arc-shaped oscillating welding, combined with the low heat input of CMT and the remelting of the weld bead by GTA, the contact angle at the weld toe is reduced, incomplete fusion defects are reduced, and the deposition rate is improved.

Benefits of technology

It effectively reduces welding heat input, prevents weld embrittlement, improves weld quality, reduces incomplete fusion defects, and increases production efficiency. It is suitable for in-service repair of nuclear power pipelines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128673A_ABST
    Figure CN123128673A_ABST
Patent Text Reader

Abstract

A kind of nuclear power pipeline B type sleeve in-service repair ring corner weld welding method, solve the problem that traditional B type sleeve ring corner weld welding heat input is difficult to control, easy to produce interpass lack of fusion defects.Utilize CMT and GTA arc complex heat source, through swing multilayer multi-pass welding, complete sleeve ring corner weld welding.Compared with prior art, the method has good process stability, small welding heat input, excellent defect control ability, can effectively improve the quality of nuclear power pipeline repair and operation safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of in-service pipeline repair technology, specifically relating to a welding method for in-service repair of circumferential fillet welds on B-shaped sleeves of nuclear power pipelines. Background Technology

[0002] Nuclear power plant pipelines are critical pressure-bearing components of the nuclear island and conventional island, carrying various media. They bear the primary coolant, secondary steam and water, circulating water, chemicals, and emergency injection media, directly constituting a nuclear safety barrier. Failure of these pipelines can easily lead to significant safety risks such as leaks, radiation leaks, and unplanned shutdowns. Nuclear power plant pipelines operate under harsh conditions for extended periods, making them susceptible to localized damage and defects caused by single or coupled factors such as media corrosion, alternating operating pressures, geological disturbances, external human-induced loads, and material aging. This damage not only significantly shortens the pipeline's service life but can also trigger major nuclear safety accidents in severe cases. In-service repair, as a crucial technical means for the operation and maintenance of nuclear power plant pipelines, allows for defect remediation without shutting down the reactor or interrupting system media transport, maximizing continuous energy supply and stable power generation. It has become the core method for the safe maintenance and life-extending operation and maintenance of nuclear power plant pipelines.

[0003] Type B sleeve welding is a mature process for repairing nuclear power pipelines. This method involves covering the defective area with a pair of semi-circular protective plates, first forming a monolithic sleeve through longitudinal butt welds, and then fixing the ends of the sleeve to the main pipe using circumferential fillet welds, thus repairing the pipeline defect. In the longitudinal weld of the sleeve, a backing plate is often used for support, minimizing the impact of the arc heat on the pipeline itself. However, the circumferential fillet weld requires direct heating of both the sleeve and the outer surface of the pipeline. Poor heat input control can easily lead to joint embrittlement, potentially causing low-stress cracking under operating pressure, and in severe cases, leading to pipe rupture. Currently, the welding method for circumferential fillet welds is gradually transitioning from inefficient and labor-intensive manual arc welding to efficient and high-quality automated gas metal arc welding (MAG). However, automated MAG welding has a high heat input, and multiple passes can easily lead to severe weld overheating, requiring strict control of the upper limit of heat input. On the other hand, due to the large thickness of the pipes and matching sleeves, the circumferential fillet welds mainly employ multi-layer, multi-pass welding. Improper control of process parameters can easily lead to excessively large contact angles at the weld toe, resulting in incomplete fusion defects at weld overlaps. Therefore, developing a high-quality welding process that balances low heat input and high deposition rate is of significant engineering value for the welding of circumferential fillet welds during the repair of nuclear power plant pipe sleeves. Summary of the Invention

[0004] To overcome the shortcomings of the prior art, the present invention aims to provide a welding method for in-service repair of circumferential fillet welds on B-type sleeves of nuclear power pipelines. Addressing the problems of difficult heat input control and easy formation of interpass incomplete fusion in the circumferential fillet welds of B-type sleeves during in-service repair of nuclear power pipelines, the present invention is based on cold metal transfer (CMT) and gas non-consumable electrode inert gas (GTA) welding of circumferential fillet welds on B-type sleeves of nuclear power pipelines. First, a composite heat source is formed using CMT and GTA arcs. CMT is a low-heat-input welding method, and by coordinating wire feeding monitoring and process control, the alternation of "cold" and "hot" in the welding process is achieved, reducing the welding heat input while maintaining a high deposition rate. The composite post-GTA heat source remelts the weld toe area, reducing the weld contact angle and increasing the coverage area of ​​the weld toe area when heated by the subsequent arc, thereby reducing the probability of interpass incomplete fusion defects.

[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A welding method for repairing the circumferential fillet weld of a B-type sleeve in a nuclear power plant pipeline, characterized by comprising the following steps: Step 1: Mechanically grind the end face of the B-shaped sleeve that has completed longitudinal seam welding and the surface of the pipe that is paired with it to clean the oil, oxides and other impurities in the weld area. Step 2: Move the CMT and GTA composite welding torch to the starting position of the circumferential fillet weld at one end of the sleeve, and use angular arc-shaped oscillation to complete the welding of the root layer weld. Step 3: Move the composite welding torch to the starting point of the second weld bead and complete the second weld bead welding by angular oscillation; Step 4: Repeat step (3) to complete the welding of the single-sided circumferential weld of the type B sleeve; Step 5: Move the composite welding torch to the circumferential weld at the other end of the sleeve, and repeat steps (1) to (4) in sequence to complete the welding of the B-shaped sleeve.

[0006] Furthermore, the structure of the composite welding torch is that the CMT and GTA welding torches are arranged side by side, with the GTA welding torch positioned at the rear, and the distance between the centers of the two welding torches is adjustable, ranging from 10 to 20 mm.

[0007] Furthermore, the aforementioned angular arc swing refers to the CMT welding torch only moving along the welding direction during the welding process, while the GTA welding torch simultaneously moves longitudinally along the welding direction and swings angularly around the CMT welding torch, with an amplitude of 0~45°, a frequency of 2~10Hz, and a dwell time of 0.2~0.8s on both sides.

[0008] Furthermore, the GTA welding torch employs a self-fusion welding mode without filler wire.

[0009] Furthermore, the CMT welding torch initiates the arc welding first, and the GTA welding torch begins arc welding when it moves to the starting point of the CMT weld.

[0010] Furthermore, the welding parameters are as follows: CMT welding current is 150~280A, arc voltage is 18~26V, and gas flow rate is 15~22L / min; GTA welding current is 120~150A, arc length is 3~6mm, and gas flow rate is 9~13L / min. The welding speed of the composite welding torch is 30~50cm / min.

[0011] The beneficial effects of this invention are: 1. The CMT welding method can reduce the heat input during sleeve welding, avoiding the problem of weld embrittlement caused by excessive heat input.

[0012] 2. By using a specially designed angular arc-shaped trajectory oscillation welding method, the contact angle at the weld toe can be reduced, preventing incomplete fusion defects in subsequent welds. This also increases weld width and improves production efficiency. Furthermore, the periodic movement of the electric arc during oscillation stirs the molten pool, refining grains and improving weld microstructure.

[0013] 3. Compared with composite heat source welding processes such as laser-GTA and laser-Gas Magnetic Arc Welding (GMA), CMT and GTAW composite heat sources have wider adaptability, especially for root penetration of fillet welds in pipelines, and have lower equipment costs, better portability, and are more suitable for in-service pipeline repair. Attached Figure Description

[0014] Figure 1 This is a schematic diagram of the composite welding torch structure.

[0015] Figure 2 This is a schematic diagram of an angular arc-shaped swing.

[0016] Figure 3 A schematic diagram illustrating the welding principle for repairing circumferential fillet welds on in-service B-type sleeves of nuclear power plant pipelines.

[0017] Figure 4 This is a schematic diagram of an embodiment. Detailed Implementation

[0018] The following detailed description, in conjunction with the accompanying drawings and specific embodiments, provides a method for welding in-service circumferential fillet welds of B-type sleeves for nuclear power plant pipelines, as proposed by the present invention. The advantages and features of the present invention will become clearer from the following detailed embodiments. It should be noted that the accompanying drawings are all in a very simplified form and use non-precise proportions, intended only to facilitate and clarify the illustration of the embodiments of the present invention; furthermore, the structures shown in the drawings are often part of the actual structures.

[0019] like Figures 1-4 As shown, a welding method for repairing the circumferential fillet weld of a B-type sleeve for nuclear power pipelines in service is characterized by comprising the following steps: Step 1: Mechanically grind the end face of the B-shaped sleeve that has completed longitudinal seam welding and the surface of the pipe that is paired with it to clean the oil, oxides and other impurities in the weld area. Step 2: Move the CMT and GTA composite welding torch to the starting position of the circumferential fillet weld at one end of the sleeve, and use angular arc-shaped oscillation to complete the welding of the root layer weld. Step 3: Move the composite welding torch to the starting point of the second weld bead and complete the second weld bead welding by angular oscillation; Step 4: Repeat step (3) to complete the welding of the single-sided circumferential weld of the type B sleeve; Step 5: Move the composite welding torch to the circumferential weld at the other end of the sleeve, and repeat steps (1) to (4) in sequence to complete the welding of the B-shaped sleeve.

[0020] Furthermore, the structure of the composite welding torch is that the CMT and GTA welding torches are arranged side by side, with the GTA welding torch positioned at the rear, and the distance between the centers of the two welding torches is adjustable, ranging from 10 to 20 mm.

[0021] Furthermore, the aforementioned angular arc swing refers to the CMT welding torch only moving along the welding direction during the welding process, while the GTA welding torch simultaneously moves longitudinally along the welding direction and swings angularly around the CMT welding torch, with an amplitude of 0~45°, a frequency of 2~10Hz, and a dwell time of 0.2~0.8s on both sides.

[0022] Furthermore, the GTA welding torch employs a self-fusion welding mode without filler wire.

[0023] Furthermore, the CMT welding torch initiates the arc welding first, and the GTA welding torch begins arc welding when it moves to the starting point of the CMT weld.

[0024] Furthermore, the welding parameters are as follows: CMT welding current is 150~280A, arc voltage is 18~26V, and gas flow rate is 15~22L / min; GTA welding current is 120~150A, arc length is 3~6mm, and gas flow rate is 9~13L / min. The welding speed of the composite welding torch is 30~50cm / min. Example

[0025] The B-type sleeve method was used to repair a 304L nuclear power plant pipeline. The pipeline wall thickness was 6.02 mm, the outer diameter was 114.3 mm, the sleeve material was 304L, the welding material was ER308L, and the welding wire diameter was 1.2 mm. The shielding gas for the CMT arc in the composite heat source was 97.5% Ar and 2.5% CO. 2 The protective gas for GTA arcs is pure Ar.

[0026] A composite welding torch was used to weld the circumferential fillet weld between a type B sleeve and a pipe. The process parameters were as follows: CMT welding current 230A, arc voltage 22V, gas flow rate 20L / min; GTA welding current 130A, arc voltage 13V, gas flow rate 10L / min; composite welding torch moving speed 40cm / min; angular oscillation amplitude 30°, frequency 5Hz, and dwell time on both sides 0.2s.

[0027] By oscillating and welding with an angular arc trajectory of 30° angular oscillation, the contact angle at the weld toe is reduced, preventing incomplete fusion defects in subsequent welds. At the same time, the weld width is increased. In addition, the periodic movement of the electric arc during oscillation will stir the molten pool, which will refine the grains and improve the weld structure.

[0028] The welded joints are of good quality, effectively overcoming the problems of incomplete fusion between passes, stress deformation, and intergranular corrosion that are prone to occur in GMA welding with high heat input.

Claims

1. A welding method for in-service repair of circumferential fillet welds on a B-type sleeve of a nuclear power plant pipeline, characterized in that, Includes the following steps: Step 1: Mechanically grind the end face of the B-shaped sleeve that has completed longitudinal seam welding and the surface of the pipe that is paired with it to clean the oil, oxides and other impurities in the weld area. Step 2: Move the CMT and GTA composite welding torch to the starting position of the circumferential fillet weld at one end of the sleeve, and use angular arc-shaped oscillation to complete the welding of the root layer weld. Step 3: Move the composite welding torch to the starting point of the second weld bead and complete the second weld bead welding by angular oscillation; Step 4: Repeat step (3) to complete the welding of the single-sided circumferential weld of the type B sleeve; Step 5: Move the composite welding torch to the circumferential weld at the other end of the sleeve, and repeat steps (1) to (4) in sequence to complete the welding of the B-shaped sleeve.

2. The welding method for in-service repair of circumferential fillet welds on a B-type sleeve for nuclear power pipelines according to claim 1, characterized in that, The structure of the composite welding torch is that the CMT and GTA welding torches are arranged side by side, with the GTA welding torch positioned at the rear. The distance between the centers of the two welding torches is adjustable, ranging from 10 to 20 mm.

3. The welding method for in-service repair of circumferential fillet welds on a B-type sleeve for nuclear power pipelines according to claim 1, characterized in that, The aforementioned angular arc swing refers to the CMT welding torch only moving along the welding direction during the welding process, while the GTA welding torch simultaneously moves longitudinally along the welding direction and swings angularly around the CMT welding torch as the center. The swing amplitude is 0~45°, the frequency is 2~10Hz, and the dwell time on both sides is 0.2~0.8s.

4. The welding method for in-service repair of circumferential fillet welds on a B-type sleeve for nuclear power pipelines according to claim 1, characterized in that, The GTA welding torch described above adopts a self-fusion welding mode without filler wire.

5. The welding method for in-service repair of circumferential fillet welds on a B-type sleeve for nuclear power pipelines according to claim 1, characterized in that, The CMT welding torch initiates the arc welding first, and the GTA welding torch begins arc welding when it moves to the starting point of the CMT weld.

6. The welding method for in-service repair of circumferential fillet welds on a B-type sleeve for nuclear power pipelines according to claim 1, characterized in that, The welding parameters are as follows: CMT welding current is 150~280A, arc voltage is 18~26V, and gas flow rate is 15~22L / min; GTA welding current is 120~150A, arc length is 3~6mm, and gas flow rate is 9~13L / min. The welding speed of the composite torch is 30~50cm / min.