A preheating-slow cooling-aging synergistic residual stress control process method for electron beam welding of Ti55531 titanium alloy

CN123128690APending Publication Date: 2026-11-20NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611557408.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-09
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In the existing technology, the electron beam welding of Ti55531 titanium alloy in the thick plate welding process suffers from insufficient control of residual stress and deformation, resulting in poor joint strength and toughness matching. There is a lack of systematic process methods to cover stress control throughout the entire welding process.

Method used

A preheating-slow cooling-aging synergistic residual stress control process is adopted, including preheating before welding, vacuum electron beam welding, vacuum slow cooling after welding, and aging treatment after welding. By matching parameters, the welding thermal response and residual stress are controlled throughout the process, and the peak residual stress of the joint is controlled to be below 20% of the yield strength of the base material, and the angular deformation of the welded plate is within 0.4°.

Benefits of technology

Effective control of residual stress peak in the joint was achieved, the joint strength matched that of the base material, welding deformation was kept within a controllable range, and the overall mechanical properties of the joint were improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128690A_ABST
    Figure CN123128690A_ABST
Patent Text Reader

Abstract

The application discloses a preheating-slow cooling-aging synergic residual stress control process method for Ti55531 titanium alloy electron beam welding. The method comprises the following steps: machining, pickling and butt assembly of the to-be-welded plate; preheating the welding area at 200-350 DEG C under vacuum; one-time penetration welding is carried out by maintaining the vacuum degree, accelerating voltage of 50-70 kV, electron beam current of 45-80 mA, welding speed of 400-700 mm / min and focusing current of 950-1050 mA; the welding part is cooled to below 100 DEG C at a cooling rate of 1-50 DEG C / min; and the welding part cooled to room temperature is subjected to aging heat treatment at 480-590 DEG C for 4-8 h. According to the application, the peak value of the joint residual stress can be controlled to be below 20% of the yield strength of the base material, the angular deformation of the tailor-welded plate is within 0.4 DEG, and the joint and the base material are matched in strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of titanium alloy beam welding technology, specifically relating to a preheating-slow cooling-aging synergistic process for controlling residual stress in electron beam welding of Ti55531 titanium alloy. Background Technology

[0002] Ti55531 (Ti-5Al-5V-5Mo-3Cr-1Zr) is a near-β-type ultra-high-strength titanium alloy with good hardenability, excellent strength-toughness balance, and a tensile strength typically not less than 1100 MPa. It has been used in aerospace main load-bearing structures, large forgings, and landing gear components. This alloy has a high β-stability coefficient, making it suitable for manufacturing large-section components; thick-plate welding is a key process in its engineering applications.

[0003] Vacuum electron beam welding offers advantages such as high energy density, rapid heating and cooling, small heat-affected zone, and pollution-free vacuum environment, making it a commonly used method for high-quality welding of titanium alloys. Previous research has demonstrated the successful welding of 60 mm thick Ti55531 plates into a full-penetration joint, followed by post-weld solution treatment and aging. The joint achieved a tensile strength of 1129 MPa, with the fusion zone composed of coarse β grains and fine intragranular α phases. In the as-welded fusion zone of homologous alloys, residual β phase dominates, resulting in a lower hardness than the base metal. Under tensile stress, localized strain concentrates in the weld, and fracture often originates here.

[0004] The welding thermal cycle has a significant impact on near-β alloys. Fine secondary phases precipitated during cooling reduce the joint's plasticity and toughness, and embrittled metastable phases may form in the weld microstructure, requiring post-weld heat treatment to eliminate them. On the other hand, the rapid heating and cooling of electron beam welding creates a steep temperature gradient in thick plate joints, leaving a residual stress field dominated by longitudinal tensile stress after the weld and near-weld zone cool. When the plate thickness exceeds 30 mm, the structural constraint increases significantly, and the peak residual stress can reach over 40% of the base metal's yield strength. Angular deformation and longitudinal deflection directly affect machining allowances and assembly accuracy. Currently, reports on residual stress and deformation control in electron beam welding of this alloy are far fewer than studies on microstructure characterization and conventional mechanical properties.

[0005] Preheating before welding helps reduce the hardness difference between the fusion zone, heat-affected zone, and base metal, improving joint strength and toughness while reducing residual stress levels. Its effect extends beyond simply raising the initial temperature; slower cooling also promotes the precipitation of secondary α-phase, preventing the concentrated precipitation of excessively fine dispersed phases. Slow cooling after welding alters the residual stress distribution characteristics, positively impacting stress concentration. Setting cooling rates in segments according to temperature ranges allows for controlled process cycles while ensuring stress relaxation. Post-weld aging treatment not only compensates for strength loss through precipitation strengthening but also further relaxes residual stress.

[0006] Each of the above methods, when used individually, has its own emphasis, but all only act on a specific stage of the residual stress formation process. Preheating determines the starting point of the thermal cycle, slow cooling determines the degree of stress relaxation from the high-temperature stage to the medium-temperature stage, and aging determines the stress release and microstructure recovery in the medium-temperature stage. In engineering, it is common practice to use preheating and aging in combination. The cooling process between the end of welding and entering the furnace is often uncontrolled, with the workpiece being directly air-cooled. However, it is precisely this period that determines the final magnitude of the residual stress.

[0007] Currently, published reports on electron beam welding of Ti55531 near-β type ultra-high strength titanium alloys mainly focus on joint microstructure characterization and control of conventional mechanical properties, lacking a systematic approach that integrates preheating, welding, slow cooling, and aging treatment into a unified design. Therefore, a composite process method is needed to cover the entire welding process and systematically control residual stress levels and welding deformation. Summary of the Invention

[0008] Technical problem solved: To address the above-mentioned technical problems, this invention provides a preheating-slow cooling-aging synergistic process for controlling residual stress in electron beam welding of Ti55531 titanium alloy. This process can control the peak residual stress of the joint to below 20% of the yield strength of the base material and control the angular deformation of the welded plate to within 0.4° without adding special equipment, thus achieving equal strength matching between the joint and the base material.

[0009] Technical solution: A preheating-slow cooling-aging synergistic process for controlling residual stress in electron beam welding of Ti55531 titanium alloy, comprising the following steps: S1. Pre-welding surface treatment: Machining and pickling the butt joint surfaces of the plates to be welded to remove the oxide film; S2. Assembly and Fixing: The plates to be welded are assembled by butt welding with welding fixtures, and arc-starting plates and arc-ending plates are installed at both ends of the weld. S3. Preheating before welding: Preheat the welding area under vacuum conditions by electron beam defocusing scanning at a temperature of 200~350℃. S4. Vacuum electron beam welding: Maintain vacuum, use an accelerating voltage of 50~70 kV, an electron beam current of 45~80 mA, a welding speed of 400~700 mm / min, and a focusing current of 950~1050 mA to perform one-time penetration welding; S5. Post-weld vacuum slow cooling: Maintain the vacuum level, and after welding, cool the weldment to below 100°C in the vacuum chamber at a cooling rate of 1~50°C / min; S6. Post-weld aging: After vacuum slow cooling, the weldment is further cooled to room temperature and then subjected to aging heat treatment. The aging temperature is 480~590℃ and the time is 4~8h. When both plasticity and toughness need to be considered, the combination of the upper limit temperature and the lower limit time is used. When both strength need to be considered, the combination of the lower limit temperature and the upper limit time is used.

[0010] Preferably, the nominal composition of the plate to be welded is as follows by weight percentage: Al 4.5%~5.5%, V 4.5%~5.5%, Mo 4.5%~5.5%, Cr 2.5%~3.5%, Zr 0.5%~1.5%, with the balance being Ti and unavoidable impurities, and the impurity elements being no more than 0.03% O, no more than 0.05% Si, no more than 0.03% N, and no more than 0.008%.

[0011] Preferably, in step S1, the surface roughness Ra of the mating surface after machining is no greater than 1.6 μm; the pickling solution used in the pickling treatment includes 2%~4% HF and 30%~40% HNO3 by volume, with the remainder being deionized water, and the pickling time is 30~60s. Welding shall begin within 4 hours after the surface treatment is completed.

[0012] Preferably, in S2, the misalignment of the butt joint assembly does not exceed 0.1 mm, the assembly gap is not greater than 0.05 mm, and the clamping point of the welding fixture is located more than 20 mm away from the center line of the weld; the arc-starting plate and the arc-ending plate are made of the same material and have the same thickness as the plate to be welded, and the assembly gap with the formal weld is not greater than 0.1 mm; the clamping point of the fixture is arranged more than 20 mm away from the center line of the weld.

[0013] Preferably, the scanning preheating area in S3 is the weld and an area of ​​not less than 30 mm on both sides, the temperature deviation within the area does not exceed ±15℃, and the heat preservation time is not less than 2 min per 10 mm plate thickness.

[0014] Preferably, the preheating temperature of S3 and the welding line energy of S4 are matched according to the following rules: when the preheating temperature is 200~250℃, the accelerating voltage is 50~60 kV, the electron beam current is 45~60 mA, and the welding speed is 500~700 mm / min, corresponding to a line energy of 193~432 J / mm; when the preheating temperature is 250~350℃, the accelerating voltage is 60~70 kV, the electron beam current is 55~80 mA, and the welding speed is 400~600 mm / min, corresponding to a line energy of 330~840 J / mm.

[0015] Preferably, in step S4, the focal position of the vacuum electron beam welding is located 2-4 mm below the surface of the plate to be welded, the scanning waveform is circular or sine wave, the scanning frequency is 50-200 Hz, and the scanning amplitude is 0.3-1.0 mm. The electron beam current of the arc initiation and arc termination segments of the vacuum electron beam welding is controlled by a linear slope. When the arc is initiated, the beam current rises from zero to the set value in 2-5 seconds, and when the arc is terminated, it drops from the set value to zero in 3-8 seconds.

[0016] Preferably, the slow cooling of S5 is set with an upper limit for the cooling rate in segments according to temperature range: no more than 40℃ / min from the peak welding temperature to 500℃, no more than 10℃ / min in the 500~200℃ range, and no more than 5℃ / min in the 200~100℃ range.

[0017] Preferably, the vacuum degree in steps S3 to S5 is no higher than 5 × 10⁻⁶. -2 Pa.

[0018] Preferably, the aging temperature in S6 is 480~550℃, the aging is carried out in a vacuum or inert atmosphere, and the heating rate does not exceed 5℃ / min.

[0019] Beneficial Effects: The core of this invention lies in integrating preheating before welding, vacuum electron beam welding, post-weld vacuum gradient cooling, and post-weld aging treatment into a complete process route. Parameters across each step are matched to allow for relay regulation of welding thermal response and residual stress at different stages of the welding process. The magnitude of residual stress is determined by two factors: the peak temperature gradient during the thermal cycle and the material's stress relaxation ability at high temperatures during cooling. Preheating directly compresses the former, while slow cooling and aging improve the latter. Matching welding parameters with preheating temperature ensures that the two do not cancel each other out.

[0020] The role of preheating before welding is reflected in three aspects. First, it increases the initial temperature and reduces the temperature gradient, thereby reducing thermal stress caused by uneven thermal expansion and contraction. Second, the microstructure evolution characteristics of the fusion zone and heat-affected zone change under preheating conditions, reducing the hardness difference between the weld center and the heat-affected zone, and making the mechanical properties of each region more uniform. This is the microstructural basis for reducing the degree of residual stress concentration. Third, preheating raises the temperature level in the initial cooling stage, allowing the weld zone to remain in the temperature range with lower yield strength and stronger creep relaxation ability for a longer period. Some thermal stress is released during the cooling process, rather than being completely frozen to room temperature. The role of vacuum slow cooling after welding is to control the cooling path of the welded joint from a high temperature state to room temperature. During rapid cooling, the temperature differences and uneven contraction in different regions of the welded joint are locked as residual stress. However, the controlled slow cooling process allows the temperature differences between different regions of the welded joint to gradually decrease, allowing some thermal stress to be released during the cooling process, thereby changing the final distribution of residual stress. Slow cooling is not necessarily better the slower it is. Cooling at a constant rate of 1℃ / min would require over 20 hours for a 30 mm thick plate, making production efficiency unacceptable. Furthermore, prolonged exposure to 400-600℃ would promote continuous precipitation and coarsening of the α-phase at grain boundaries, actually reducing toughness. Setting the cooling rate in temperature segments balances both factors: rapid passage above 500℃ avoids the sensitive area of ​​significant α-phase precipitation at grain boundaries; slowing down between 500-200℃ allows for sufficient stress relaxation in the region where the material's yield strength has decreased. Post-weld aging treatment has three functions. Ti55531 is a near-β-type alloy that can be strengthened through heat treatment. Welding thermal cycles alter the original microstructure and reduce strength. In the weld zone, the residual β-phase dominates in the weld state, resulting in lower hardness than the base metal. During aging, the secondary α-phase precipitated from the β matrix restores strength, and the hardness of the weld zone, heat-affected zone, and base metal tends to be consistent. Simultaneously, holding at the aging temperature promotes residual stress relaxation and reduces stress peaks. Aging also homogenizes the microstructure in various areas of the joint, improving overall mechanical properties. However, aging has limited stress relaxation capabilities; the yield strength of the material decreases only slightly at 470-580℃, and the elastic strain released by heat preservation is limited. Aging cannot replace slow cooling at high temperatures; the two operate in different temperature ranges and must be used in series.

[0021] Matching preheating and welding parameters is equally crucial. Preheating alters the heat dissipation conditions of the molten pool; if welding parameters are not adjusted accordingly, the preheating effect will be partially negated, or even new defects may be introduced. Using low heat input and high welding speed at high preheating temperatures prevents the molten metal from filling the keyhole in time, resulting in spikes and chain-like porosity. Conversely, using high heat input and low welding speed at low preheating temperatures prolongs the high-temperature dwell time, leading to β-grain coarsening and a wider heat-affected zone. In both cases, the joint's plasticity and strength decrease, while the peak residual stress increases.

[0022] The above steps, used in combination, enable phased control of residual stress in electron beam welded joints of Ti55531 titanium alloy. This process can be implemented on existing vacuum electron beam welding machine platforms. Preheating and slow cooling are completed by the welding machine's own vacuum chamber and CNC system. The workpiece does not leave the vacuum chamber before and after welding, avoiding secondary contamination and temperature fluctuations caused by intermediate transfer. The aging process is completed using a conventional heat treatment furnace. Attached Figure Description

[0023] Figure 1 This is a flowchart of the composite process of electron beam welding preheating, welding and post-weld treatment of Ti55531 titanium alloy according to the present invention. Figure 2 This is a schematic diagram of the assembly of the welded joint in an embodiment of the present invention; Figure 3 This is a comparison diagram of post-weld cooling paths, showing the temperature-time relationship of three paths: air cooling, uniform slow cooling at 10 ℃ / min, and the segmented gradient slow cooling of the present invention. Figure 4 The figure shows the matching window between preheating temperature and welding line energy, and also indicates the parameter positions of each embodiment and comparative example. Figure 5 The distribution curves of longitudinal residual stress along the direction perpendicular to the weld are shown for Examples 1, Examples 2, and Control Groups 1 and 2. Figure 6 Scanning electron microscope (SEM) images of the fracture morphology of each embodiment and comparative example; In the figure: 1-First Ti55531 titanium alloy plate, 2-Second Ti55531 titanium alloy plate, 3-Arc initiation plate, 4-Arc termination plate, 5-Welding fixture, 6-Weld. Detailed Implementation

[0024] The measured chemical composition (mass fraction, %) of the Ti55531 titanium alloy sheet used below is as follows: Al 5.10, V 4.91, Mo 5.09, Cr 2.68, Zr 1.05, impurities O 0.01, Si 0.026, N 0.0056, H 0.0021, with the balance being Ti. After forging in the α+β two-phase region, the sheet underwent standard heat treatment according to the following procedure: holding at 872 ℃ for 2 h followed by air cooling, and then holding at 510 ℃ for 8 h followed by air cooling. The measured β phase transformation point was 857 ℃, and the microstructure was an equiaxed primary α and β transformation matrix.

[0025] Two plates measuring 100 mm (weld direction) × 60 mm × 30 mm are butted together along a 60 mm edge. The resulting welded plate has dimensions of 120 mm (width) × 100 mm (length) × 30 mm (thickness). The weld is located at the transverse center of the welded plate. Figure 2As shown. The arc-starting plate and arc-ending plate are both 40 mm × 40 mm × 30 mm in size, and the material is from the same batch as the plates to be welded. Unless otherwise specified, the pre-welding surface treatment, assembly and fixation, and vacuum conditions are exactly the same for the example and the control group.

[0026] The welding line energy for each embodiment and the control group was calculated based on E = 60·U·I / v. Where U is the accelerating voltage (kV), I is the electron beam current (mA), v is the welding speed (mm / min), and E is in J / mm. Welding parameters are matched with the preheating temperature according to the following rules: at a preheating temperature of 200~250℃, an accelerating voltage of 50~60 kV, an electron beam current of 45~60 mA, and a welding speed of 500~700 mm / min are used, corresponding to a linear energy of 193~432 J / mm; at a preheating temperature of 250~350℃, an accelerating voltage of 60~70 kV, an electron beam current of 55~80 mA, and a welding speed of 400~600 mm / min are used, corresponding to a linear energy of 330~840 J / mm.

[0027] The basis for proposing the above matching relationship is as follows. When the preheating temperature is 200~250℃, the temperature difference between the base material and the molten pool is large, heat dissipation is rapid, and the molten pool solidifies quickly. If the heat input is increased and the welding speed is decreased at this time, the high-temperature dwell time is prolonged, β-grain coarsening occurs, and the heat-affected zone widens, thus offsetting the effect of preheating in reducing the temperature gradient. Therefore, this range is matched with high welding speed and low heat input. After the preheating temperature rises to 250~350℃, heat dissipation from the base material slows down, and the molten pool and keyhole duration are prolonged. If high welding speed and low heat input are continued, the backfill time of the liquid metal behind the keyhole is insufficient, easily forming spike defects, chain-like pores, and humps. Therefore, this range is matched with lower welding speed and medium heat input to prolong the molten pool duration and facilitate gas escape and backfilling. There is an overlap area (330~432 J / mm) between the two windows in terms of heat input. When in the overlap area, the window assignment is determined by the preheating temperature. The invention will be further described below with specific embodiments and accompanying drawings. Example

[0028] In this embodiment, the two Ti55531 titanium alloy plates mentioned above are used to form a welded plate by vacuum electron beam butt welding.

[0029] A preheating-slow cooling-aging synergistic residual stress control process for electron beam welding of Ti55531 titanium alloy includes the following steps: Step 1: Surface treatment before welding The mating surfaces are machined to a Ra value not exceeding 1.6 μm. The straightness of the mating surfaces is controlled within 0.05 mm / m to ensure uniform gap along the weld length after assembly. The oxide film on the mating surfaces and surrounding areas is removed using a pickling solution composed of 3% HF, 35% HNO3, and the remainder deionized water, with a pickling time of 45 seconds. After rinsing with deionized water and drying, the surfaces are wiped with anhydrous ethanol for degreasing and then dried with hot air. A 2.5-hour interval is allowed between pickling and furnace loading to prevent surface contamination (if the waiting time is longer, the workpieces should be stored in a dry and clean environment, and the mating surfaces should not be touched by bare hands).

[0030] Step Two: Assembly and Fixing The special fixtures are used for butt welding, with a misalignment of 0.06 mm and a gap of 0.03 mm. The arc-starting and arc-ending plates are installed at both ends of the weld, with a gap of 0.05 mm from the main weld. The thickness of the arc-starting and arc-ending plates is the same as that of the plate to be welded, and their mating surfaces are treated as in step one. The clamping points of the fixtures are located at least 20 mm away from the weld centerline to prevent excessive local heat dissipation from altering the solidification conditions of the molten pool.

[0031] Step 3: Preheating treatment before welding Vacuum degree better than 5×10 -3 After Pa, electron beam defocusing scanning preheating is performed at a temperature of 250℃, a scanning width of 80mm (40mm on each side of the weld), a scanning frequency of 300 Hz, and a preheating beam current of 40% of the welding beam current. The holding time is 8 min, and the temperature deviation in the preheating zone is ±11℃ to ensure that the energy is evenly distributed within the scanning width and to avoid local overheating. Welding begins immediately after preheating.

[0032] Step 4: Vacuum electron beam welding Maintaining a vacuum level in the vacuum chamber better than 5×10 -3 Under the conditions of Pa, vacuum electron beam welding was performed on the workpiece. The welding parameters were as follows: accelerating voltage 60kV, electron beam current 60mA, welding speed 500mm / min, focusing current 1000mA, focal point located 3mm below the workpiece surface, scanning waveform circular scan, scanning frequency 100Hz, scanning amplitude 0.5 mm, corresponding to a linear energy of 432 J / mm. The scanning amplitude was set to the upper limit as the plate thickness increased, and 0.8~1.0 mm was used when the plate thickness exceeded 40 mm to widen the upper opening of the molten pool and facilitate gas escape. Welding was performed using a one-time penetration welding method, with the welding direction entering from the arc-starting plate, passing through the entire formal weld, and terminating at the arc-ending plate. The arc-starting beam slope time was 3 s, and the arc-ending beam slope time was 5 s, used to fill the arc crater and suppress arc-ending cracks and shrinkage cavities. After welding, the workpiece remained in the vacuum chamber.

[0033] Step 5: Post-weld vacuum gradient slow cooling treatment After welding, the workpiece is cooled in a vacuum chamber at a controlled rate in stages from the highest welding temperature to below 100°C before being removed. The average cooling rate is 32°C / min from the peak temperature to 500°C, 8°C / min from 500°C to 200°C, and 4°C / min from 200°C to 100°C, taking approximately 76 minutes in total. Throughout the slow cooling process, the vacuum level in the vacuum chamber is maintained at a level better than 5 × 10⁻⁶. -3 When the vacuum level is insufficient, gas intrusion will cause pores to form in the weld, and at the same time, it will accelerate the evaporation loss of volatile elements such as Al, resulting in more obvious softening of the fusion zone. The cooling rate is controlled by feedback from a sheathed thermocouple fixed at a distance of 30 mm from the weld on the workpiece surface. This is achieved by adjusting the convection intensity of the residual gas in the vacuum chamber and the contact heat conduction of the workpiece support platform. Forced air cooling or water cooling must not be used. When the weld length exceeds 400 mm, the plate thickness exceeds 40 mm, or the joint consists of multiple intersecting welds, the cooling rate should be 1~10℃ / min. At this time, the cumulative heat input of welding is large and the restraint is high, requiring slower cooling to fully release stress.

[0034] Step Six: Post-weld aging treatment After slow cooling to room temperature, the weldments were subjected to aging heat treatment at 520℃ for 6 hours in a vacuum furnace with a heating rate of 4℃ / min and a furnace temperature uniformity of ±4℃. After aging, the weldments were air-cooled to room temperature. For plate thicknesses exceeding 40 mm, the holding time was at least 6 hours to ensure uniform cross-sectional temperature. When the aging temperature exceeded 550℃, the holding time was set to the lower limit to avoid excessive coarsening of the secondary α phase. Example

[0035] All parameter settings not mentioned in this embodiment are the same as in Embodiment 1.

[0036] A preheating-slow cooling-aging synergistic residual stress control process for electron beam welding of Ti55531 titanium alloy includes the following steps: Step 1 and Step 2 are the same as in Example 1.

[0037] Step 3: Preheating treatment. The preheating temperature is set to 300℃, with a temperature deviation of ±13℃ within the preheating zone. Step 4: Vacuum electron beam welding. The welding parameters are as follows: accelerating voltage 65kV, electron beam current 70mA, welding speed 450mm / min, focusing current 1020mA, focal point 3.5mm below the workpiece surface, circular scanning waveform, scanning frequency 120Hz, scanning amplitude 0.6 mm, corresponding linear energy 607 J / mm, arc initiation slope time 3 s, and arc termination slope time 6 s.

[0038] Step 5: Post-weld vacuum gradient slow cooling treatment. The average cooling rate is 28℃ / min from the peak temperature to 500℃, 5℃ / min from 500 to 200℃, and 3℃ / min from 200 to 100℃, with a total time of approximately 112 minutes.

[0039] Step Six: Post-weld aging treatment. Aging temperature 510℃, aging time 8 hours. Example

[0040] This embodiment is used to verify the upper limit condition of the range defined in the claims, namely, a high preheating temperature combined with a moderately high upper limit energy, a slow cooling rate at the lower limit, and an aging time combining the lower limit temperature and the upper limit time. Parameter settings not mentioned in this embodiment are the same as in Embodiment 1.

[0041] Step 1 and Step 2 are the same as in Example 1.

[0042] Step 3: Preheating treatment before welding. The preheating temperature is set to 350 ℃, and the preheating beam current is 45% of the welding beam current. The temperature deviation in the preheating zone is ±14 ℃.

[0043] Step 4: Vacuum electron beam welding. Welding parameters are: accelerating voltage 70kV, electron beam current 80mA, welding speed 400mm / min, focusing current 1050mA, focal point located 4mm below the workpiece surface, scanning waveform is sine wave scanning, scanning frequency 200Hz, scanning amplitude 1.0mm, corresponding linear energy 840J / mm, arc initiation slope time 4s, and arc termination slope time 8s.

[0044] Step 5: Post-weld vacuum gradient slow cooling treatment. The average cooling rate is 36℃ / min from the peak temperature to 500℃, 10℃ / min from 500 to 200℃, and 5℃ / min from 200 to 100℃, with a total time of approximately 65 minutes.

[0045] Step Six: Post-weld aging treatment. Aging temperature 480 ℃, aging time 8 hours.

[0046] Comparative Example The comparison ratio was set according to the single-factor principle. Except for the process to be investigated, the other conditions were kept the same as in Example 1 so that the differences in the test results could be attributed to specific process steps.

[0047] Control group 1: Conventional process (no preheating → electron beam welding → air cooling → aging) No preheating was performed before welding. The workpiece was directly welded at room temperature (25°C), and the welding parameters were exactly the same as in Example 1 (60kV, 60mA, 500mm / min, linear energy 432J / mm). No vacuum slow cooling was performed after welding. The workpiece was cooled to approximately 300°C in a vacuum chamber before being removed and air-cooled to room temperature. The measured average cooling rate from the peak temperature to 300°C was approximately 82°C / min. Subsequently, the workpiece was aged at 520°C for 6 hours, followed by air cooling.

[0048] Control group 2: Preheating was provided, but a vacuum slow cooling section was missing. Preheating to 250℃ before welding, welding parameters were the same as in Example 1, and vacuum gradient slow cooling was not performed after welding. The cooling method was the same as in control group 1, followed by aging at 520℃ for 6 hours. The only difference from Example 1 was the post-weld cooling process.

[0049] Control group 3: Preheating temperature and welding parameters do not match (heat input is too low) The preheating temperature was mismatched with the welding parameters (heat input was too low). The preheating temperature was 320℃. According to the matching rules, 60~70kV, 55~80mA, and 400~600mm / min should have been selected. However, this group used 55kV, 50mA, and 650mm / min, with a linear energy of 254 J / mm, which is lower than the lower limit of the window of 330 J / mm. The focusing current was 980mA, the focal point was located 2.5mm below the surface, and the circular scan was 150Hz. Gradual cooling was performed after welding, followed by aging at 520℃ for 6 hours.

[0050] Control group 3′: Preheating temperature and welding parameters do not match (heat input is too high) Preheating temperature 220℃. According to the matching rules, 50~60kV, 45~60mA, 500~700mm / min should be selected. This group changed to 65kV, 70mA, 430mm / min, with a linear energy of 605 J / mm, exceeding the upper limit of the window by 432 J / mm. Focusing current 1020mA, focal point located 3.5mm below the surface, circular scan 120Hz. Gradient slow cooling after welding, aging at 520℃ for 6h.

[0051] Control group 4: Base material standard Base material benchmark. Ti55531 plates from the same batch, without welding, were subjected to standard heat treatments of 857℃ / 2h air cooling and 510℃ / 8h air cooling. This group is used to evaluate the performance retention rate of the welded joint relative to the base material.

[0052] Performance testing methods Each embodiment and comparative example was sampled and tested using the same method, and the arithmetic mean of 3 samples (3 plates) was taken for each test item.

[0053] Tensile properties at room temperature were determined according to GB / T228.1 "Metallic materials, tensile testing—Part 1: Test at room temperature". Rectangular cross-section specimens were used, with a parallel section width of 12.5 mm and a thickness of 6 mm (wire-cut from the middle of the plate thickness, each specimen including the weld, heat-affected zone, and base material). The initial gauge length L0 = 50 mm, with the weld located at the center of the gauge length and perpendicular to the tensile axis. A strain rate of 0.00025 s⁻¹ was applied before yielding. -1 Control, switch to 0.0067s after yielding. -1 The location of the fracture was determined using a stereomicroscope, and the distance between the fracture surface and the fusion line was measured.

[0054] Residual stress was measured in two steps. The longitudinal residual stress on the surface was measured according to GB / T 7704 "Non-destructive Testing - X-ray Stress Measurement Method," using Mn Kα radiation, Ti(213) crystal plane, and the sin²ψ method. The ψ angle was taken as 0°, ±15°, ±25°, ±35°, and ±45°, with a collimator diameter of 1 mm. Measurement points were arranged perpendicular to the weld direction, with a spacing of 1 mm in the near-weld zone (within 10 mm of the weld center), 2 mm in the 10-30 mm zone, and 4 mm in the remaining zones, extending to the plate edge. The longitudinal residual stress in the thickness direction was measured using the profile method: a line cut was made along the middle of the weld cross-section, and the profile of the cut surface was scanned using a coordinate measuring machine (GB / T 16857.2) to invert the stress distribution. The blind hole method (GB / T 31310) was used to cross-calibrate the measurement points near the surface. The deviation between the two methods was less than 25 MPa.

[0055] Welding deformation was measured using a coordinate measuring machine (GB / T 16857.2). The zero point was the grid points (10 mm × 10 mm grid) on the upper and lower surfaces measured before welding, and the same set of points was measured again after welding. Angular deformation was taken as the arctangent value of the ratio of the relative height difference Δh between the two ends of the transverse section to the half-plate width L, and longitudinal deflection was taken as the maximum out-of-plane displacement in the length direction of the plate.

[0056] Microhardness testing was performed according to GB / T 4340.1 "Metallic Materials - Vickers Hardness Test - Part 1: Test Methods", with a load of HV0.2 and a holding time of 10 s. Tests were conducted at 0.5 mm intervals along the weld direction, and the average values ​​for the weld zone, heat-affected zone, and base material were recorded. Metallographic specimens were prepared according to GB / T 13298 "Metallic Materials - Microstructure Examination Methods", etched with Kroll etchant (2 mL HF + 6 mL HNO3 + 92 mL deionized water) for 8–15 s. The average β-grain intercept was determined using the intercept method in GB / T 6394 "Method for Determination of Average Grain Size of Metals", with at least 200 intercepts recorded for each weld. Fracture morphology and microstructure were observed using a field emission scanning electron microscope (FET) at an accelerating voltage of 15 kV.

[0057] Test results The process parameters for each embodiment and comparative example are summarized in Table 1, the room temperature tensile properties are shown in Table 2, the residual stress and welding deformation are shown in Table 3, and the microhardness and microstructure characteristics are shown in Table 4. In the table, control group 4 is the base material reference, i.e., Ti55531 plate that has not been welded and has only undergone standard heat treatment.

[0058] Table 1. Process parameters for each embodiment and comparative example

[0059] Table 2. Room temperature tensile properties of welded joints (average of 3 pieces)

[0060] Note: The strength factor is the ratio of the tensile strength of the joint to the tensile strength of the base material.

[0061] Table 3 Residual stress and welding deformation (average values ​​of 3 plates)

[0062] Note: The peak longitudinal stress on the surface occurs at the center of the weld; the extreme compressive stress occurs at a distance of about 30-40 mm from the center of the weld; the core stress is measured by the profile method, taking the value along the center of the weld at 1 / 2 of the plate thickness; the peak value / base material yield strength is normalized to the base material yield strength of 1065 MPa.

[0063] Table 4 Microhardness and Weld Microstructure Characteristics

[0064] Note: The microstructure of the control group 4 base material is an equiaxed primary α and β transformation matrix, without the distinction between weld zone and heat-affected zone.

[0065] The results of scanning electron microscopy (SEM) observation of the fracture morphology are as follows: Example 1 Tensile fracture ( Figure 6 a) Tensile fracture surface compared to Example 2 ( Figure 6 b) All fractures are located in the parent material region, with obvious necking visible macroscopically. Scanning electron microscopy reveals typical micropore aggregation-type ductile fracture: dimples are predominantly equiaxed, with considerable depth and relatively uniform size distribution. Numerous tear ridges and a small number of secondary cracks are visible between the dimples. Some dimples show α-phase particles or micro-pits left by their debonding at the bottom, indicating that micropores mainly nucleate, grow, and aggregate at the α / β phase interface. Fracture in the parent material indicates that the joint's load-bearing capacity is not lower than that of the parent material. Example 3: Tensile fracture surface ( Figure 6 c) The partial phase transformation / over-aging softening zone located near the base metal side of the heat-affected zone. This zone is still dominated by micropore aggregate dimples, but the dimple depth is significantly shallower than that of the base metal, and the size distribution is uneven. Locally, flat intergranular facets appear along β grain boundaries or α cluster interfaces, and a small number of secondary cracks are visible. This indicates that under the action of welding thermal cycling, the secondary α grains in this zone have undergone coarsening and partial dissolution, and the grain boundary bonding force has decreased, making it the second weakest link in the joint. Control group 1 fracture surface ( Figure 6 d) Located at the center of the weld, the surface is macroscopically smooth with no obvious necking. Under scanning electron microscopy, it exhibits a "candy-like" intergranular fracture: the crack extends along coarse columnar β grain boundaries, the grain boundaries are smooth with few dimples, secondary cracks branch along grain boundaries and connect to adjacent grains, and only a few shallow dimples are visible locally within grains and at grain boundary junctions. This morphology indicates that the columnar β grains in the weld zone are coarse, the grain boundary bonding is weak, and the crack rapidly and unstablely propagates along the grain boundaries after nucleation, resulting in extremely low plasticity. Control group 2 fracture surface ( Figure 6 e) The partially fused / coarse-grained region near the fusion line exhibits a mixed morphology of intergranular fracture along columnar β grain boundaries and shallow transgranular dimples. The dimples are small and shallow, and the tear edges are short and sparse, indicating that the microstructure and properties of this region change drastically, serving as a channel for deformation concentration and preferential crack propagation. Control group 3 fracture surface ( Figure 6 f) At the root of the weld (near the back side), in the nail tip / incomplete penetration area, a free surface without fusion is visible: the surface is smooth, without traces of plastic deformation, and clearly separated from the surrounding fracture by a step, retaining the characteristics of the original assembly surface / dendritic free growth surface; chain-like pores are distributed near it along the welding direction, the pores are round to elliptical with smooth inner walls, which should be caused by the trapping of bubbles in the molten pool under the condition of rapid solidification at the root. The pores and lack of fusion constitute a strong stress concentration source, inducing premature crack nucleation and rapid unstable propagation along the coarse columnar β grain boundaries. Intergranular facets and a small number of shallow dimples are visible around it, and locally there are quasi-cleavage pattern flat surfaces connected by short tear edges without obvious river patterns.

[0066] The contribution of preheating before welding: The only difference between control group 1 and control group 2 was whether preheating was used before welding; all other conditions were identical. After preheating to 250℃, the peak residual stress decreased from 468 MPa to 342 MPa, a reduction of 126 MPa (27%); angular deformation decreased from 1.86° to 1.14°; longitudinal deflection decreased from 1.24 mm to 0.76 mm; elongation after fracture increased from 4.1% to 6.3%; the fracture location shifted from the weld center to the fusion line; and the hardness difference between the weld zone and the base metal decreased from 56 HV to 40 HV. Preheating compressed the thermal cycling temperature range and improved the uniformity of microstructure in each region; both effects are reflected in the data.

[0067] Post-weld vacuum gradient slow cooling has the largest marginal contribution: The only difference between Example 1 and Control Group 2 was whether or not vacuum gradient cooling was performed after welding; all other conditions were identical (including the same preheating at 250°C and aging at 520°C for 6 hours). After gradient cooling, the peak residual stress decreased from 342 MPa to 176 MPa, a reduction of 166 MPa (49%), which was the largest marginal contribution among the three factors; angular deformation decreased from 1.14° to 0.32°, and longitudinal deflection decreased from 0.76 mm to 0.18 mm; elongation after fracture increased from 6.3% to 9.0%, the fracture location shifted from the fusion line to the base material, and the joint strength coefficient reached 93.6%.

[0068] Although control group 2 underwent aging at 520℃ for 6 hours, the peak residual stress was still 1.94 times that of Example 1. This is because the aging temperature range of 470-580℃ limits the decrease in the material's yield strength, resulting in minimal elastic strain release through heat preservation. Gradient cooling, on the other hand, releases stress more efficiently when the material is still at a higher temperature and its yield strength has significantly decreased. Since the two methods operate within different temperature ranges, they cannot be substituted for each other.

[0069] The preheating temperature and linear energy must be determined simultaneously: Control group 3, preheated at 320℃ with a heat input of 254 J / mm, exhibited discontinuous incomplete fusion and chain-like porosity at the weld root, with a cumulative length of 11.3%. The tensile strength was only 962 MPa, and the elongation was 2.5%. Control group 3′, preheated at 220℃ with a heat input of 605 J / mm, showed no macroscopic defects in the weld, but the average β-grain intercept reached 312 μm, and the heat-affected zone nearly doubled in width. The tensile strength was 1084 MPa, and the elongation was 5.5%, both significantly lower than Example 2 (preheated at 300℃ with a heat input of 607 J / mm, tensile strength 1085 MPa, elongation 8.5%). Both groups deviated from the expected performance, resulting in lower performance than the Example 2. The different directions of deviation led to different failure modes: insufficient heat input manifested as forming defects, while excessive heat input manifested as grain coarsening. Compared with Example 2, it is clear that the joint performance is not determined by either the heat input or the preheating temperature alone, but rather by whether the combination of both falls within the specified window.

[0070] Degree of compatibility with the base material: Example 2 exhibits a tensile strength of 92.5% of the base material, a residual stress peak of 138 MPa (13% of the base material's yield strength), and an angular deformation of 0.21°. Example 2 shows the best overall result among the three examples. Example 3 falls within the upper limit of the claim range (preheating at 350°C, linear energy of 840 J / mm), maintaining a strength modulus of 85.8%, but the average β-grain intercept increases to 348 μm, and the maximum hardness difference increases to 18 HV, indicating a significant grain coarsening trend. In actual production, the parameter ranges of Examples 1 and 2 should be prioritized.

[0071] Based on the above data, this invention controls the peak residual stress of a 30 mm thick Ti55531 welded joint to 13%~17% of the yield strength of the base material, keeps the angular deformation within 0.32°, and maintains the joint strength coefficient above 85% by combining preheating, gradient slow cooling, and aging. If any of the three steps is missing or the parameters are mismatched, the peak residual stress will rise back to more than 30% of the yield strength of the base material, and the tensile strength and elongation will decrease significantly.

[0072] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Those skilled in the art can modify or make equivalent substitutions to the technical solutions without departing from the scope of the present invention. The scope of protection of the present invention should be determined by the claims.

Claims

1. A preheating-slow cooling-aging synergistic process for controlling residual stress in electron beam welding of Ti55531 titanium alloy, characterized in that, The steps include the following: S1. Pre-welding surface treatment: Machining and pickling the butt joint surfaces of the plates to be welded to remove the oxide film; S2. Assembly and Fixing: The plates to be welded are assembled by butt welding with welding fixtures, and arc-starting plates and arc-ending plates are installed at both ends of the weld. S3. Preheating before welding: Preheat the welding area under vacuum conditions by electron beam defocusing scanning at a temperature of 200~350℃. S4. Vacuum electron beam welding: Maintain vacuum, use an accelerating voltage of 50~70 kV, an electron beam current of 45~80 mA, a welding speed of 400~700 mm / min, and a focusing current of 950~1050 mA to perform one-time penetration welding; S5. Post-weld vacuum slow cooling: Maintain the vacuum level, and after welding, cool the weldment to below 100°C in the vacuum chamber at a cooling rate of 1~50°C / min; S6. Post-weld aging: After vacuum slow cooling, the weldment is further cooled to room temperature and then subjected to aging heat treatment at an aging temperature of 480~590℃ for 4~8h.

2. The preheating-slow cooling-aging synergistic residual stress control process for electron beam welding of Ti55531 titanium alloy according to claim 1, characterized in that, The nominal composition of the plate to be welded is as follows by weight percentage: Al 4.5%~5.5%, V 4.5%~5.5%, Mo 4.5%~5.5%, Cr 2.5%~3.5%, Zr 0.5%~1.5%, with the balance being Ti and unavoidable impurities, and the impurity elements being no more than 0.03% O, no more than 0.05% Si, no more than 0.03% N, and no more than 0.008% H.

3. The preheating-slow cooling-aging synergistic residual stress control process for electron beam welding of Ti55531 titanium alloy according to claim 1, characterized in that, The surface roughness Ra of the mating surface after machining in S1 is no greater than 1.6 μm; the pickling solution used for pickling includes 2%~4% HF and 30%~40% HNO3 by volume, with the balance being deionized water, and the pickling time is 30~60s. Welding shall begin within 4 hours after the surface treatment is completed.

4. The preheating-slow cooling-aging synergistic residual stress control process for electron beam welding of Ti55531 titanium alloy according to claim 1, characterized in that, In S2, the misalignment of the butt joint assembly shall not exceed 0.1 mm, the assembly gap shall not exceed 0.05 mm, and the clamping point of the welding fixture shall be located more than 20 mm away from the center line of the weld. The arc-starting plate and the arc-ending plate shall be made of the same material and have the same thickness as the plate to be welded, and the assembly gap with the formal weld shall not exceed 0.1 mm. The clamping point of the fixture shall be arranged more than 20 mm away from the center line of the weld.

5. The preheating-slow cooling-aging synergistic residual stress control process for electron beam welding of Ti55531 titanium alloy according to claim 1, characterized in that, The scanning preheating area in S3 is the weld and an area of ​​not less than 30 mm on both sides, with a temperature deviation of no more than ±15℃ within the area, and a holding time of not less than 2 min per 10 mm plate thickness.

6. The preheating-slow cooling-aging synergistic residual stress control process for electron beam welding of Ti55531 titanium alloy according to claim 1, characterized in that, The preheating temperature of S3 and the welding line energy of S4 are matched according to the following rules: when the preheating temperature is 200~250℃, the accelerating voltage is 50~60 kV, the electron beam current is 45~60 mA, and the welding speed is 500~700 mm / min, corresponding to a line energy of 193~432 J / mm; when the preheating temperature is 250~350℃, the accelerating voltage is 60~70 kV, the electron beam current is 55~80 mA, and the welding speed is 400~600 mm / min, corresponding to a line energy of 330~840 J / mm.

7. The preheating-slow cooling-aging synergistic residual stress control process for electron beam welding of Ti55531 titanium alloy according to claim 1, characterized in that, In S4, the focal position of the vacuum electron beam welding is located 2-4 mm below the surface of the plate to be welded. The scanning waveform is circular or sine wave, the scanning frequency is 50-200 Hz, and the scanning amplitude is 0.3-1.0 mm. The electron beam current of the arc initiation and arc termination segments of the vacuum electron beam welding is controlled by a linear slope. When the arc is initiated, the beam current rises from zero to the set value in 2-5 seconds, and when the arc is terminated, it drops from the set value to zero in 3-8 seconds.

8. The preheating-slow cooling-aging synergistic residual stress control process for electron beam welding of Ti55531 titanium alloy according to claim 1, characterized in that, The slow cooling of S5 is set with upper limits for cooling rate in segments according to temperature range: no more than 40℃ / min from the peak welding temperature to 500℃, no more than 10℃ / min in the 500~200℃ range, and no more than 5℃ / min in the 200~100℃ range.

9. The preheating-slow cooling-aging synergistic residual stress control process for electron beam welding of Ti55531 titanium alloy according to claim 1, characterized in that, The vacuum degree in S3~S5 is no higher than 5×10⁻⁶. -2 Pa.

10. The preheating-slow cooling-aging synergistic residual stress control process for electron beam welding of Ti55531 titanium alloy according to claim 1, characterized in that, The aging temperature in S6 is 480~550℃, and the aging is carried out in a vacuum or inert atmosphere with a heating rate not exceeding 5℃ / min.