A multi-frequency ultrasonic resistance closed-loop control method for lithium battery tab welding quality
By using a multi-frequency ultrasonic resistance closed-loop control method to adjust welding parameters in real time, the problem of poor welding quality consistency of lithium battery tabs was solved, and online monitoring and adaptive optimization were achieved, thereby improving welding quality and reliability.
Patent Information
- Application Number
- CN202611218230.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-12
- Publication Date
- 2026-11-20
AI Technical Summary
Existing lithium battery tab welding processes cannot effectively adapt to batch fluctuations in thickness tolerance, interlayer gap, and surface oxidation state of multi-layer tab materials, resulting in poor welding quality consistency, frequent occurrence of defects such as incomplete welding and over-welding, and traditional detection methods are highly lagging and cannot achieve online real-time control.
A multi-frequency ultrasonic resistance closed-loop control method is adopted. By combining multi-frequency ultrasonic vibration with dynamic resistance data acquisition, welding parameters are adjusted in real time, and the welding process is controlled in stages, including pre-compression, crushing, diffusion and homogenization stages. Closed-loop control is carried out by feedback of resistance characteristic parameters.
It improves the adaptability of welding quality, reduces the incidence of incomplete welds and over-welds, realizes real-time online monitoring and adaptive optimization of welding quality, and enhances the mechanical properties and long-term reliability of welded joints.
Smart Images

Figure CN123128697A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery tab welding technology, and in particular to a multi-frequency ultrasonic resistance closed-loop control method for lithium battery tab welding quality. Background Technology
[0002] Ultrasonic metal welding is a core technology for reliably connecting lithium battery tabs to terminals and adapters. Through the coupling of high-frequency mechanical vibration and welding pressure, it promotes diffusion bonding between metal atoms under solid-state conditions, effectively avoiding problems such as thermal damage, material embrittlement, and spatter caused by molten welding. It has become the mainstream technology for connecting tabs in square, pouch, and cylindrical power batteries. With the continuous improvement of energy density and safety performance requirements for power batteries, the number of welding layers on the tabs is constantly increasing, and the demand for consistent welding quality and precise process control in production lines is also rising.
[0003] Existing conventional ultrasonic welding processes for electrode tabs generally employ a single, fixed frequency and fixed process parameters. This approach cannot effectively adapt to batch variations in the thickness tolerances, interlayer gaps, and surface oxidation states of multi-layer electrode tabs, easily leading to poor consistency in welding quality within the same batch and frequent occurrences of incomplete welds and over-welds. Furthermore, current welding quality control relies on offline sampling methods such as post-weld tensile testing and metallographic sectioning. These methods have long inspection cycles and significant time lags, making it impossible to perceive the real-time bonding status of the welding interface online. Moreover, it is difficult to dynamically adjust process parameters based on actual welding results. By the time batch quality defects are discovered, a large number of battery cells have often already entered the next process, significantly increasing quality costs and rework risks in the production process. Summary of the Invention
[0004] In view of this, the present invention proposes a multi-frequency ultrasonic resistance closed-loop control method for the welding quality of lithium battery tabs, which can significantly improve the adaptability of the welding process to fluctuations in operating conditions, reduce the incidence of defects such as incomplete welding and over-welding, and effectively reduce quality losses and rework costs caused by batch defects.
[0005] The technical solution of this invention is implemented as follows: In a first aspect, the present invention provides a multi-frequency ultrasonic resistance closed-loop control method for the welding quality of lithium battery tabs, comprising the following steps: A set welding pressure is applied to the welding area of the lithium battery tab. According to the preset sequence of multiple welding stages, multi-frequency ultrasonic vibration including the main frequency and at least two auxiliary frequencies is used to input coupled vibration energy to the welding interface, which is the frequency combination and energy distribution ratio corresponding to each welding stage. Throughout the welding process, dynamic resistance data of the welding circuit is collected in real time. The welding circuit includes the welding head, lithium battery tabs, and bottom mold. The resistance characteristic parameters reflecting the bonding degree of the welding interface are extracted from the dynamic resistance data. The resistance characteristic parameters are compared with the preset resistance characteristic quality judgment threshold to generate quality deviation data. Based on the quality deviation data, the parameter adjustments for the ultrasonic energy distribution ratio, welding pressure, and welding time corresponding to the next welding cycle are calculated. The welding process parameters for the next welding cycle are updated based on the parameter adjustment amount, and the welding operation of the next lithium battery tab is performed according to the updated welding process parameters, so as to achieve closed-loop control of welding quality.
[0006] In one embodiment, the two auxiliary frequencies are a first auxiliary frequency and a second auxiliary frequency, and the execution sequence of the multiple welding stages includes a pre-compression stage, a crushing stage, a diffusion stage, and a homogenization stage, wherein, The pre-pressure stage performs the following steps: only inputting the vibration energy corresponding to the main frequency, applying a first set welding pressure to the lithium battery tab welding area, and completing the tab clamping positioning and initial contact establishment; The crushing stage performs the following steps: simultaneously inputting the vibration energy corresponding to the main frequency and the first auxiliary frequency, applying the second set welding pressure to the lithium battery tab welding area, and completing the crushing of the oxide layer at the welding interface and roughening of the interface. The diffusion stage performs the following steps: simultaneously inputting the vibration energy corresponding to the main frequency and the first auxiliary frequency, applying a third set welding pressure to the lithium battery tab welding area, and completing the interface atomic diffusion and metallurgical bonding formation. The homogenization stage performs the following steps: simultaneously inputting the vibration energy corresponding to the first auxiliary frequency and the second auxiliary frequency, applying a fourth set welding pressure to the lithium battery tab welding area, and completing the homogenization of the interface temperature field and the release of residual stress.
[0007] In one embodiment, the main frequency has a frequency range of 15-25kHz, the first auxiliary frequency has a frequency range of 35-45kHz, and the second auxiliary frequency has a frequency range of 55-65kHz.
[0008] In one embodiment, the dynamic resistance data of the welding circuit is obtained by the following steps: Apply a constant DC test current to the welding circuit; Real-time voltage signals at both ends of the welding interface are synchronously acquired at the voltage measurement end of the welding circuit, and the acquisition of the real-time voltage signals is synchronized with the ultrasonic vibration period of the main frequency. Based on the correspondence between constant DC test current and real-time voltage signal, the real-time dynamic resistance data of the welding circuit is calculated.
[0009] In one embodiment, the resistance characteristic parameters include initial contact resistance, minimum resistance, resistance decrease rate, steady-state resistance, and resistance recovery amount. Extracting the resistance characteristic parameters reflecting the bonding degree of the weld interface from dynamic resistance data specifically includes the following steps: The average resistance value within a set duration at the end of the pre-loading stage is extracted from the dynamic resistance data as the initial contact resistance. The minimum resistance is extracted from the dynamic resistance data throughout the welding process and recorded as the minimum resistance. Calculate the average slope of the resistance as it decreases from the initial contact resistance to the minimum resistance to obtain the resistance decrease rate. The average resistance within a set time period after welding is extracted from the dynamic resistance data as the steady-state resistance. Calculate the difference between the steady-state resistance and the minimum resistance to obtain the resistance recovery amount.
[0010] In one embodiment, the step of calculating the adjustment amounts of the ultrasonic energy distribution ratio, welding pressure, and welding time corresponding to the next welding cycle based on the quality deviation data specifically includes the following steps: The quality deviation data is input into the incremental PID control logic, and the calculation is performed by combining the quality deviation data of the current cycle with those of the previous two cycles. The initial adjustment values for three types of parameters—ultrasonic energy distribution ratio, welding pressure, and welding time—are output respectively. For each type of initial adjustment, a limit is applied to ensure that the absolute value of a single parameter adjustment does not exceed the preset percentage threshold of the current corresponding parameter value. If the adjustment exceeds the limit range, the parameter adjustment is output according to the limit value.
[0011] In one embodiment, the calculation process of the parameter adjustment amount also matches a deviation type adjustment strategy, specifically including: When the quality deviation data reflects that the weld bond strength is lower than the target value, increase the proportion of the main frequency energy, extend the diffusion stage duration, and increase the parameter adjustment amount corresponding to the welding pressure. When the quality deviation data reflects that the thickness of the interface metallurgical layer is higher than the target value, the parameter adjustment amount corresponding to increasing the proportion of the first auxiliary frequency energy and shortening the diffusion stage duration is increased. When the quality deviation data reflects a resistance increase higher than the target value, the parameter adjustments should be made to reduce the total vibration energy input and shorten the total welding time.
[0012] Secondly, this invention provides a multi-frequency ultrasonic resistance closed-loop control system for lithium battery tab welding quality, comprising a multi-frequency ultrasonic welding module, a resistance acquisition module, a feature extraction and deviation generation module, an adjustment calculation module, and a closed-loop update control module, wherein... The multi-frequency ultrasonic welding module is used to apply a set welding pressure to the welding area of the lithium battery tab, and according to the preset sequence of multiple welding stages, it uses multi-frequency ultrasonic vibration including a main frequency and at least two auxiliary frequencies to input coupled vibration energy to the welding interface, which is the frequency combination and energy distribution ratio corresponding to each welding stage. The resistance acquisition module is used to acquire dynamic resistance data of the welding circuit in real time throughout the welding process. The welding circuit includes the welding head, lithium battery tabs, and bottom mold. The feature extraction and deviation generation module is used to extract resistance feature parameters reflecting the bonding degree of the welding interface from dynamic resistance data, compare the resistance feature parameters with a preset resistance feature quality judgment threshold, and generate quality deviation data. The adjustment calculation module is used to calculate the parameter adjustment amounts of the ultrasonic energy distribution ratio, welding pressure, and welding time corresponding to the next welding cycle based on the quality deviation data. The closed-loop update control module is used to update the welding process parameters for the next welding cycle according to the parameter adjustment amount, and control the multi-frequency ultrasonic welding module to perform the welding operation of the next lithium battery tab according to the updated welding process parameters, so as to realize closed-loop control of welding quality.
[0013] Thirdly, the present invention provides an electronic device, including a processor and a memory; the memory stores a computer program, wherein the computer program, when executed by the processor, implements the above-described multi-frequency ultrasonic resistance closed-loop control method for lithium battery tab welding quality.
[0014] Fourthly, the present invention provides a non-transitory computer-readable storage medium having a computer program stored thereon, wherein the computer program, when executed by a processor, implements the steps of the above-described multi-frequency ultrasonic resistance closed-loop control method for the welding quality of lithium battery tabs.
[0015] The multi-frequency ultrasonic resistance closed-loop control method for lithium battery tab welding quality of the present invention has the following advantages over the prior art: 1. Employing multi-frequency ultrasonic vibration including a main frequency and at least two auxiliary frequencies, coupled vibration energy with corresponding frequency combinations and energy distribution ratios is input to the welding interface according to a preset sequence of multiple welding stages. This allows for precise control of the entire process of plastic deformation, oxide layer breakage, and atomic diffusion at the welding interface, effectively adapting to fluctuations in the incoming material status of multi-layer tabs. Furthermore, by acquiring dynamic resistance data of the welding circuit in real time, the bonding process of the welding interface can be quantified online, replacing the traditional offline sampling inspection method and eliminating the lag in quality inspection at the source. Based on this, resistance characteristic parameters reflecting the degree of interface bonding are extracted, compared with preset judgment thresholds to generate quality deviation data, further calculate the parameter adjustment amount for the next welding cycle, and update the welding process parameters, forming a periodic adaptive closed-loop control of welding quality. 2. By dividing the welding process into four sequentially executed welding stages—pre-compression, crushing, diffusion, and homogenization—and matching each stage with a corresponding frequency combination and welding pressure gradient, the main frequency provides the basic energy input required for welding. The first auxiliary frequency enhances the microscopic plastic flow and atomic-level close contact at the interface, while the second auxiliary frequency achieves the homogenization of the interface temperature field and the release of residual stress at the end of the welding process. The functions of each stage are clearly defined, and the energy input rhythm is highly matched with the physical change process of the welding interface. This can improve the weld bonding strength while suppressing interface grain coarsening and residual stress accumulation, further improving the mechanical properties and long-term reliability of the welded joint. 3. An incremental PID control logic is used to calculate the adjustment amount of process parameters and is combined with amplitude limiting. At the same time, a directional parameter adjustment strategy is matched for three typical quality deviations: insufficient weld bonding strength, excessive metallurgical layer thickness at the interface, and excessive resistance rise. This can ensure the response speed of closed-loop control while avoiding system oscillations caused by large parameter fluctuations. It makes the adjustment of process parameters more in line with the physical change law of the welding interface, and further improves the stability of closed-loop control and the accuracy of quality control. Attached Figure Description
[0016] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0017] Figure 1 This is a flowchart illustrating the multi-frequency ultrasonic resistance closed-loop control method for lithium battery tab welding quality according to the present invention. Detailed Implementation
[0018] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0019] like Figure 1 As shown, the present invention provides a multi-frequency ultrasonic resistance closed-loop control method for the welding quality of lithium battery tabs, taking the ultrasonic stacking process of multi-layer tabs in power batteries as the application scenario. The multi-frequency ultrasonic resistance closed-loop control method for the welding quality of lithium battery tabs runs on a multi-frequency ultrasonic welding platform for lithium battery tabs, and is used to achieve cycle-by-cycle adaptive control of the welding quality of tabs.
[0020] Before starting a single-cycle welding operation, the welding platform first completes the positioning and clamping of the lithium battery tab stack to be welded, and applies a set welding pressure to the lithium battery tab welding area to make the tab stack form a stable contact state with the welding head and the bottom mold.
[0021] After welding is started, according to the preset sequence of multiple welding stages, multi-frequency ultrasonic vibration including the main frequency and at least two auxiliary frequencies is used to input coupled vibration energy to the welding interface with the frequency combination and energy distribution ratio corresponding to each welding stage. Through the synergistic effect of vibrations at different frequencies, the welding interface is driven to complete the complete welding process of contact establishment, surface oxide layer removal, interface plastic deformation and atomic diffusion bonding in sequence.
[0022] It is important to note that when starting the welding production line for the first time or changing the electrode material type, pre-calibrated baseline process parameters should be used as the welding parameters for the initial cycle. These baseline process parameters are determined in advance through process experiments for the corresponding material type and include the initial main and auxiliary frequency energy distribution ratio, welding pressure at each stage, duration of each stage, and total welding time. After completing at least three consecutive stable welding cycles, the closed-loop adjustment mechanism should be activated to avoid parameter misadjustments caused by insufficient data samples or an unstable state during the cold start phase.
[0023] Throughout the welding process, resistance monitoring and closed-loop control are initiated simultaneously, specifically through steps S100 to S400.
[0024] It should be noted that the multi-frequency ultrasonic vibration energy input process and the dynamic resistance acquisition process are synchronous and parallel in timing. The resistance acquisition unit starts working simultaneously with the start of welding vibration, and the resistance acquisition covers the entire welding stage, continuously recording the complete evolution of the interface resistance. Resistance feature extraction, quality deviation calculation, and parameter adjustment calculation are all performed after the current welding cycle is completely finished. The calculated parameter adjustment only applies to the next welding cycle, which is a closed-loop control mode of cycle-by-cycle iteration, rather than real-time parameter adjustment within a single welding cycle. This mode is adapted to the short cycle characteristics of ultrasonic welding at the millisecond level, ensuring the stability of the single-cycle welding process while achieving production line-level adaptive quality optimization through continuous iteration.
[0025] Step S100: During the entire welding process, the dynamic resistance data of the welding circuit is collected in real time. The welding circuit includes the welding head, lithium battery tabs and bottom mold.
[0026] The resistance acquisition action is triggered synchronously with the start of ultrasonic vibration and terminated synchronously with the welding process, continuously acquiring the time-domain resistance data of the welding circuit throughout the entire process.
[0027] The welding circuit uses the welding head as the upper conductive path and the bottom mold as the lower conductive path. The multi-layered electrode stack to be welded is connected in series in the circuit as the intermediate test object. The core of the change in the total resistance of the circuit comes from the change in the contact resistance at the welding interface.
[0028] As the welding process progresses, the interface contact area increases, the oxide layer breaks down, and metallurgical bonding is formed. The circuit resistance will show a corresponding continuous change pattern. The collected dynamic resistance data can fully reflect the real-time evolution of the welding interface bonding state, providing a data basis for subsequent quality judgment.
[0029] Step S200: Extract resistance characteristic parameters reflecting the bonding degree of the welding interface from the dynamic resistance data, compare the resistance characteristic parameters with the preset resistance characteristic quality judgment threshold, and generate quality deviation data.
[0030] Feature analysis is performed on the acquired continuous dynamic resistance time-domain data to extract multi-dimensional resistance feature parameters that can characterize the interface bonding process, bonding strength and interface state.
[0031] The preset resistance characteristic quality judgment threshold is a qualified range pre-defined by statistically analyzing the resistance characteristic data of a large number of qualified welding samples, corresponding to the reasonable value range of each characteristic parameter under standard welding quality. During the pre-production stage, a certain number of qualified welding samples are selected, and the resistance characteristic parameters of each sample are collected and statistically analyzed. Based on the normal distribution range of each characteristic parameter, and combined with the post-weld tensile test and metallographic inspection results of the corresponding samples, the qualified threshold range is determined. The threshold can be periodically calibrated according to changes in production line material batches and ambient temperature to ensure the adaptability of the judgment standard to actual working conditions.
[0032] Each resistance feature parameter extracted from the current welding cycle is compared with its corresponding quality judgment threshold. The direction and magnitude of each parameter's deviation from the qualified range are calculated. Each resistance feature parameter corresponds to an independent resistance feature quality judgment threshold, including the upper and lower limits of the qualified range. During the comparison process, it is determined whether each feature parameter falls within the qualified range, and the direction and magnitude of each parameter's deviation from the qualified range are calculated. Finally, a quality deviation dataset containing multi-dimensional feature deviation information is formed, rather than a single numerical deviation result, providing a multi-dimensional decision-making basis for subsequent categorized and directional parameter adjustments.
[0033] Step S300: Based on the quality deviation data, calculate the parameter adjustment amounts for the ultrasonic energy distribution ratio, welding pressure, and welding time corresponding to the next welding cycle.
[0034] Based on the generated quality deviation data, the adjustment amounts of three types of core process parameters are calculated according to preset control rules. These include adjusting the proportion of different frequency vibrations in the total welding energy for ultrasonic energy distribution to adapt to the required depth of interface bonding; adjusting the pressure output value during the welding process for welding pressure to change the tightness of interface contact and the intensity of friction; and adjusting the total welding time for welding time to control the total amount of interface energy input.
[0035] The magnitude of parameter adjustment is matched with the magnitude of quality deviation; the larger the deviation, the larger the corresponding adjustment, ensuring the targeted and effective control.
[0036] Step S400: Update the welding process parameters for the next welding cycle according to the parameter adjustment amount, and perform the next lithium battery tab welding operation according to the updated welding process parameters to achieve closed-loop control of welding quality.
[0037] The parameter update operation is completed within the interval of the next lithium battery tab loading and positioning. The calculated parameter adjustments are superimposed on the baseline process parameters of the current welding cycle to generate the target process parameter set for the next welding cycle, which is then sent to the ultrasonic generator unit, pressure control unit, and timing control unit of the welding platform. After the parameters are sent, parameter verification is performed to confirm that the parameter values are within the preset process safety range. Only after the verification is passed can the next welding cycle be started.
[0038] Once the next lithium battery tab to be welded is positioned and clamped, the welding platform directly calls the updated process parameters to perform welding, and simultaneously starts a new round of resistance acquisition, feature extraction, deviation calculation and parameter update process.
[0039] By implementing welding, monitoring status, judging quality, optimizing parameters, and then proceeding to the next welding cycle, this iterative mechanism enables cycle-by-cycle adaptive optimization of welding quality, forming a complete closed-loop control chain.
[0040] In some embodiments, the energy input process of multi-frequency ultrasonic vibration needs to be subdivided into time sequences. The two auxiliary frequencies are defined as the first auxiliary frequency and the second auxiliary frequency, respectively. The welding energy input process is divided into four continuously executed process stages according to the physical evolution law of the welding interface: pre-compression stage, crushing stage, diffusion stage and homogenization stage. Each stage is matched with different frequency combinations and welding pressure settings.
[0041] During the pre-compression stage, only the main frequency output vibration energy is used, and a first set welding pressure is applied to the lithium battery tab welding area. The control objective is to complete the clamping and positioning of the tab stack and establish initial contact.
[0042] Specifically, in the initial welding state, there are interlayer gaps between the multiple layers of electrode foil, the overall stack thickness has incoming material tolerances, and there are slight deviations in the relative positions of the electrode tabs, welding head, and bottom mold. Single-frequency vibration has the characteristics of large amplitude and strong macroscopic force. Combined with relatively low welding pressure, it can fully level the electrode tab stack and gradually eliminate the interlayer gaps without damaging the electrode foil, ultimately forming a stable and uniform initial contact interface, providing a reliable contact foundation for the subsequent high-energy welding stage.
[0043] If this stage setting is not adopted, high-frequency high-energy vibration and high pressure are applied at the beginning of welding. The electrode stack is prone to interlayer slippage, edge folding, and even electrode foil tearing due to incomplete positioning. This directly leads to welding scrap and causes poor consistency of the initial state of welding in the same batch, resulting in a significant increase in the final quality fluctuation.
[0044] During the crushing stage, vibration energy is simultaneously output by coupling the main frequency and the first auxiliary frequency, while a second set welding pressure is applied to the lithium battery tab welding area. The control objective is to complete the crushing of the oxide layer at the welding interface and the micro-roughening of the interface.
[0045] Specifically, after initial contact is established, the oxide layer and adsorbed contaminants covering the metal surface of the tabs are the core obstacles hindering the formation of metallurgical bonding. The dominant frequency vibration provides macroscopic friction with large displacement, which can quickly break down the thick oxide film and macroscopic contaminants at the interface; the first auxiliary frequency provides high-frequency micro-amplitude vibration, which can perform fine friction on the microscopic uneven interface, remove microscopic oxidation residues, and at the same time form a microscopic uneven structure at the interface, increasing the effective contact area for subsequent atomic diffusion.
[0046] A moderate increase in welding pressure compared to the pre-pressing stage can enhance the friction between interfaces and improve the efficiency and thoroughness of oxide layer breakage.
[0047] If this dual-frequency combination setting is not adopted, relying solely on a single main frequency for oxide layer breaking will not effectively remove the oxide film in the microscopic depressions, leaving a large number of local insulation areas at the interface, ultimately forming a false solder joint defect, and significantly increasing the dispersion of the solder joint strength; relying solely on the first auxiliary frequency for breaking will result in insufficient macroscopic energy input, low oxide layer breaking efficiency, and a significantly extended welding cycle, making it unsuitable for the cycle time requirements of mass production lines.
[0048] During the diffusion stage, the dual-frequency coupled vibration output of the main frequency and the first auxiliary frequency is maintained, while a third set welding pressure is applied to the lithium battery tab welding area. The control objective is to promote the diffusion of interfacial atoms and the formation of metallurgical bonding.
[0049] Specifically, after the oxide layer is removed, the welding enters the core stage of solid-state metallurgical bonding. In this stage, by adjusting the energy distribution ratio between the main frequency and the first auxiliary frequency, the energy input of the two tends to be balanced. The main frequency vibration continuously drives the interface material to produce macroscopic plastic flow, so that the interface concave and convex structures are fully interlocked, expanding the effective bonding area. The high-frequency micro-vibration of the first auxiliary frequency can intensify the thermal motion and collision probability of interface atoms, significantly improve the atomic diffusion rate, and promote the formation of large-area continuous metallurgical bonding.
[0050] The welding pressure is raised to the highest value in the entire cycle, which can ensure that the interface reaches atomic-level close contact and provide the necessary pressure conditions for solid-state diffusion bonding.
[0051] If this dual-frequency equalization setting is not adopted, if the main frequency energy ratio is too high and the first auxiliary frequency ratio is insufficient, excessive macroscopic plastic deformation of the interface will cause excessive thinning of the tabs. At the same time, the interface grains are prone to coarsening, resulting in embrittlement of the weld joint and a decrease in fatigue resistance. If the first auxiliary frequency energy ratio is too high and the main frequency ratio is insufficient, the macroscopic plastic flow of the interface will be insufficient, the effective bonding area will be insufficient, and the overall welding strength will not meet the requirements for the use of power batteries.
[0052] For the homogenization stage, the vibration energy is output by coupling the first auxiliary frequency and the second auxiliary frequency. At the same time, a fourth set welding pressure is applied to the lithium battery tab welding area. The control objective is to achieve uniformity of the interface temperature field and release of welding residual stress.
[0053] After the diffusion stage, a basic metallurgical bond has formed at the interface. At this point, ceasing the input of high-energy main frequency avoids interface overheating and material embrittlement caused by continuous high-energy input. The combination of the first and second auxiliary frequencies in a medium-to-high frequency micro-amplitude vibration serves two purposes: firstly, it homogenizes the interface temperature field through high-frequency micro-stirring, eliminating localized high-temperature zones formed during the diffusion stage and preventing thermal stress cracks caused by excessive temperature differences during cooling; secondly, it excites dislocation movement at the interface through micro-amplitude vibration, releasing residual stress accumulated during welding, reducing the risk of joint failure during subsequent service, and improving the long-term reliability of the welded joint. The welding pressure is appropriately reduced compared to the diffusion stage to prevent excessive compression and deformation of the interface in a softened state at high temperatures.
[0054] If this stage setting is not adopted, and all vibrations are stopped directly after welding, uneven interface temperature distribution will lead to large residual stress and microcracks during the cooling process, resulting in a decrease in the mechanical properties of the welded joint and a high risk of connection failure during long-term battery cycling. If the main frequency vibration is retained in this stage, excessive total energy input can easily cause over-welding at the interface and excessive growth of intermetallic compounds, which will reduce the mechanical and electrical properties of the joint.
[0055] In some embodiments, the frequency range of the main frequency is 15-25kHz, the frequency range of the first auxiliary frequency is 35-45kHz, and the frequency range of the second auxiliary frequency is 55-65kHz.
[0056] The main frequency range is 15-25kHz, with 20kHz being the preferred value. The main frequency serves as the core energy input for welding, primarily driving macroscopic plastic deformation at the interface, breaking thick oxide films, and achieving macroscopic material bonding. The 15-25kHz frequency band is chosen because its ultrasonic vibrations possess large amplitude and high power density, providing sufficient macroscopic frictional energy for welding 20-120 layer electrode stacks, thus meeting the thick-thickness welding requirements of multi-layer electrode stacks in power batteries. If the main frequency is below 15kHz, the vibration wavelength is too long and the macroscopic displacement of the welding head is too large, which can easily cause excessive deformation and tearing of the electrode foil. At the same time, the mechanical resonance design of the transducer and the welding head becomes much more difficult, the stability of equipment operation decreases, and low-frequency vibration can easily cause resonance of the whole machine structure, resulting in greater operating noise and mechanical loss. If the main frequency is above 25kHz, the single-cycle vibration displacement decreases, the macroscopic friction effect is significantly weakened, and it is impossible to effectively break the thick oxide film and achieve macroscopic plastic deformation of large-thickness stacks. This will lead to insufficient welding bonding area, increased probability of poor welding, and difficulty in adapting to the welding conditions of multi-layer electrodes.
[0057] The first auxiliary frequency ranges from 35 to 45 kHz, with 40 kHz being the preferred value. The first auxiliary frequency functions as a microscopic plasticity enhancer and promotes atomic diffusion. It primarily works in conjunction with the main frequency to remove the microscopic oxide layer at the interface, improve microscopic contact tightness, and accelerate the thermal motion and diffusion of atoms at the interface. The core reason for choosing the 35-45 kHz frequency band is that the high-frequency micro-amplitude vibrations in this band can excite material flow at the microscopic scale of the interface, filling microscopic uneven areas that the main frequency vibration cannot cover, without causing excessive macroscopic deformation of the material. If the first auxiliary frequency is below 35 kHz, the vibration scale is close to the main frequency range, the microscopic refinement effect is significantly weakened, and it cannot effectively remove oxide residues in microscopic depressions, nor can it significantly promote grain refinement and atomic diffusion. The process gain effect of dual-frequency coupling is significantly reduced. If the first auxiliary frequency is above 45 kHz, the vibration penetration depth is insufficient, only acting on the outermost layer of the interface, failing to promote the interlayer bonding of the multilayer tabs. Furthermore, high-frequency energy tends to concentrate on the surface, causing localized overheating and increasing the risk of over-soldering at the interface.
[0058] The second auxiliary frequency ranges from 55 to 65 kHz, with 60 kHz being the preferred value. This second auxiliary frequency is responsible for temperature field homogenization and residual stress release, primarily used in the homogenization stage at the end of welding. It eliminates residual welding stress by stimulating thermal homogenization and dislocation movement in the interfacial micro-regions through ultra-high frequency micro-amplitude vibration. The core reason for choosing the 55-65 kHz frequency band is that ultra-high frequency vibration in this band exhibits uniform thermal effects and high stress release efficiency, without causing macroscopic damage to the formed metallurgical interface. If the second auxiliary frequency is below 55 kHz, the macroscopic effect of the vibration is enhanced, easily causing secondary frictional damage to the formed metallurgical interface at the end of welding. It also inputs excessive energy, exacerbating the interface temperature rise, which is detrimental to temperature field homogenization and stress release. If the second auxiliary frequency is above 65 kHz, the vibration decays rapidly, resulting in a very shallow effective depth, failing to reach the internal interface of the multi-layer tabs. This limits the range of stress release and temperature homogenization, resulting in insignificant process gains, and significantly increases the manufacturing cost and maintenance difficulty of the high-frequency transducer.
[0059] In some embodiments, the process of acquiring dynamic resistance data of the welding circuit in step S100 can be implemented through sub-steps S101-S103.
[0060] Step S101: Apply a constant DC test current to the welding circuit.
[0061] A constant DC test current is applied to the welding circuit consisting of the welding head, lithium battery tabs, and bottom mold. Specifically, a precision constant current source can be used, connected to the welding circuit through two independent current leads to form an independent current excitation circuit. The amplitude of the constant DC test current remains stable throughout the process without periodic fluctuations.
[0062] The principle of using independent constant current excitation in this step is to provide a unified and stable electrical excitation reference for the welding interface, so that the change in interface contact resistance can be linearly converted into the change in voltage signal, providing a constant reference for subsequent resistance calculation.
[0063] If constant DC excitation is not used, but instead current or AC excitation with amplitude fluctuations, the change in current amplitude will be directly superimposed on the voltage measurement results, resulting in a systematic deviation in the resistance calculation results, which cannot accurately reflect the true trend of the interface contact state.
[0064] Step S102: Real-time voltage signals at both ends of the welding interface are synchronously acquired at the voltage measurement terminal of the welding circuit. The acquisition of the real-time voltage signals is synchronized with the ultrasonic vibration period of the main frequency.
[0065] Two independent voltage leads are arranged close to the upper and lower sides of the welding interface to form an independent voltage measurement circuit. The voltage measurement circuit does not carry excitation current and is only used to collect voltage signals at both ends of the interface.
[0066] The sampling trigger signal is synchronous with the main frequency vibration period. The zero velocity phase of the main frequency vibration is used as the fixed sampling trigger point. Sampling is performed once every set number of main frequency vibration periods, and finally a continuous real-time voltage signal sequence is obtained.
[0067] The principle of phase-synchronous sampling is that ultrasonic vibration causes the interface contact pressure to fluctuate periodically with the vibration cycle, which in turn causes the contact resistance to oscillate at the same frequency. At the zero point of vibration velocity, the welding head displacement is the largest and the interface contact state is the most stable. At this time, sampling can filter out the resistance fluctuation noise caused by vibration from the signal source, which can greatly improve the signal-to-noise ratio of the measurement data.
[0068] If phase synchronization sampling is not used, the sampling points are randomly distributed at different phases of the vibration cycle. The measured voltage signal will be superimposed with a large amount of vibration noise, and the data fluctuation amplitude will be large. It is impossible to accurately extract the overall trend and key characteristics of the resistance change. The error of subsequent quality deviation calculation will increase significantly, directly reducing the stability of closed-loop control.
[0069] Step S103: Calculate the real-time dynamic resistance data of the welding circuit based on the correspondence between the constant DC test current and the real-time voltage signal.
[0070] Based on Ohm's law, the amplitude of the real-time voltage signal acquired at each sampling moment is divided by the amplitude of the constant DC test current to obtain the dynamic resistance value of the welding circuit at the corresponding moment. After point-by-point calculation, a complete dynamic resistance time-domain data sequence is formed.
[0071] The formula for calculating real-time dynamic resistance is as follows: Where R(t) is the real-time dynamic resistance of the welding circuit at time t, U(t) is the real-time voltage signal at both ends of the welding interface acquired at time t, and T0 is the amplitude of the applied constant DC test current.
[0072] This step employs a four-wire measurement architecture that separates the current loop and the voltage loop. The core principle is that no excitation current flows through the voltage measurement loop, which can completely eliminate the interference of lead resistance and external electrode contact resistance on the measurement results. This ensures that the calculated resistance value only reflects the actual contact resistance change at the welding interface, making it suitable for high-precision measurement requirements ranging from milliohms to microohms.
[0073] In some embodiments, the extraction process of resistance characteristic parameters in step S200 is specifically implemented through sub-steps S201-S205. The resistance characteristic parameters include initial contact resistance, minimum resistance, resistance decrease rate, steady-state resistance, and resistance recovery amount.
[0074] Step S201: Extract the average resistance value within the set duration at the end of the pre-pressure stage from the dynamic resistance data as the initial contact resistance.
[0075] Using the end of the pre-pressure stage as the time endpoint, a resistance data segment of a set duration is extracted forward. The arithmetic mean of all sampling points within this data segment is then calculated to obtain the initial contact resistance R0. The set duration is typically 10ms, covering multiple sampling periods to ensure the stability of the average value.
[0076] At the end of the pre-pressing stage, the tab stack has completed leveling, positioning and initial contact establishment. The interface contact state is stable and has not yet entered the oxide layer breakage stage. At this time, the resistance value can accurately reflect the initial interface contact state before welding and can be used as the benchmark value for subsequent resistance change rate calculation and quality judgment.
[0077] If data from the early stage of preloading is selected, the tab stack has not yet been leveled, the interlayer gap fluctuates greatly, and the resistance value is highly discrete. This data cannot be used as a stable calculation benchmark and will lead to a significant increase in the calculation error of subsequent derived parameters such as the resistance decrease rate and resistance ratio.
[0078] Step S202: Extract the minimum resistance value from the dynamic resistance data throughout the welding process as the minimum resistance, and record the time when the minimum resistance occurs.
[0079] A sliding window method was used to traverse the dynamic resistance data throughout the entire welding cycle. Each window width was set to 20ms. The minimum resistance value within each window was compared to obtain the minimum resistance R for the entire cycle. min And simultaneously record the time point t corresponding to the minimum value. Rmin .
[0080] During welding, as the oxide layer breaks down, the interfacial contact area increases, and metallurgical bonding forms, the loop resistance continuously decreases. The minimum resistance corresponds to the moment when the interfacial bonding area is largest and the contact is most complete. Its value directly reflects the sufficiency of the interfacial metallurgical bonding and is a core characteristic parameter for judging the quality of the weld bond. Using a sliding window to take the minimum value can avoid extreme value misjudgment caused by single-point sampling noise and improve the stability of feature extraction.
[0081] Step S203: Calculate the average slope of the resistance as it decreases from the initial contact resistance to the minimum resistance, and obtain the resistance decrease rate.
[0082] The average slope of the resistance decrease process, i.e. the resistance decrease rate, is calculated by using the difference between the initial contact resistance and the minimum resistance as the numerator and the difference between the time when the minimum resistance occurs and the time corresponding to the initial contact resistance as the denominator.
[0083] The formula for calculating the rate of decrease in resistance is as follows: Where R0 is the initial contact resistance, R min For the minimum resistance, t Rmin t represents the time when the minimum resistance occurs. R0 This is the moment corresponding to the initial contact resistance, i.e., the end of the pre-pressure stage.
[0084] The rate of resistance decrease can directly reflect the efficiency of oxide layer breakage and the speed of interface bonding at the welding interface. The faster the rate, the more fully the oxide layer is broken and the smoother the interface bonding process. It can be used to identify abnormal working conditions such as excessive oxide layer or insufficient energy input.
[0085] Step S204: Extract the average resistance value within a set time period after the welding is completed from the dynamic resistance data as the steady-state resistance.
[0086] After welding is completed, the vibration energy input stops, the interface temperature gradually drops, and the contact state tends to stabilize. At this time, the resistance value can reflect the final interface bonding state after welding is completed, which is the direct basis for judging the final welding quality.
[0087] Starting from the moment welding vibration stops, a resistance data segment of a set duration is extracted. The arithmetic mean of the sampling points within this data segment is then taken to obtain the steady-state resistance R. end The set duration can be 50ms to ensure the interface cools down to a relatively stable state, while covering a sufficient number of sampling points to improve data stability.
[0088] Step S205: Calculate the difference between the steady-state resistance and the minimum resistance to obtain the resistance recovery amount.
[0089] Subtracting the minimum resistance from the steady-state resistance yields the resistance recovery ΔR after the welding process ends.
[0090] The formula for calculating the resistance recovery is as follows: ΔR=R end -R min The amount of resistance recovery can reflect the degree of springback and microcrack formation during the cooling process of the weld interface: the smaller the recovery, the smaller the residual stress at the interface and the more stable the metallurgical bond; the larger the recovery, the greater the risk of over-welding softening, cooling shrinkage cracks or residual stress concentration at the interface, which is a key feature for identifying over-welding defects.
[0091] In some embodiments, the comparison of the resistance characteristic parameters with a preset resistance characteristic quality judgment threshold in step S200 to generate quality deviation data can be achieved through sub-steps S206-S207.
[0092] Step S206: Input the extracted resistance feature parameters into the pre-trained welding quality prediction model to predict the welding tensile strength and intermetallic compound thickness of the current weld in real time.
[0093] Relying solely on single-parameter threshold comparison cannot comprehensively address the coupled effects of multiple features. When a nonlinear operating condition occurs where a single parameter meets the standard but the overall performance fails to meet the standard, quality misjudgment is likely to occur, causing the closed-loop control direction to deviate from the actual needs and significantly reducing the control effect. Therefore, in a further embodiment, a welding quality prediction model can be used for judgment.
[0094] The welding quality prediction model employs a multi-layer neural network architecture. It uses the resistance characteristics of a large number of welding samples from historical production as input features, and supervises training using the post-weld measured tensile strength and metallographic measured IMC thickness of the corresponding samples as label data. The input features include all five resistance characteristics: initial contact resistance, minimum resistance, resistance decrease rate, steady-state resistance, and resistance recovery amount. The model outputs continuous predicted tensile strength and IMC thickness values.
[0095] There is a nonlinear mapping relationship between resistance characteristic parameters and welding mechanical properties and microstructure. Simple single-parameter threshold comparison cannot accurately fit this nonlinear relationship. By using a pre-trained model, multi-dimensional resistance characteristics can be integrated to achieve high-precision regression prediction of the final welding quality, making the quality deviation judgment closer to the actual post-weld performance and improving the accuracy of closed-loop control.
[0096] Step S207: Compare the predicted weld tensile strength and intermetallic compound thickness with the corresponding preset quality target values to generate quality deviation data for the corresponding weld bonding strength deviation and intermetallic layer thickness deviation.
[0097] The preset quality target values include the target lower limit for weld tensile strength and the target upper limit for the thickness of the intermetallic compound at the interface. The predicted values output by the model are subtracted from the corresponding target values to obtain deviation values with positive and negative directions. Positive deviation indicates that the performance is better than the target, and negative deviation indicates that the performance is worse than the target. Finally, a multi-dimensional quality deviation dataset containing strength deviation and thickness deviation is formed, which is directly used as the input for subsequent parameter adjustment calculations.
[0098] In some embodiments, step S300 calculates the parameter adjustment amounts for the ultrasonic energy distribution ratio, welding pressure, and welding time corresponding to the next welding cycle based on the quality deviation data, specifically through sub-steps S301-S303.
[0099] Step S301: Input the quality deviation data into the incremental PID control logic and perform calculations by combining the quality deviation data of the current cycle with those of the previous two cycles.
[0100] The current welding cycle's quality deviation value is used as the control input, while historical quality deviation values from the previous two consecutive welding cycles are retrieved and input into the incremental PID control logic for calculation, outputting the parameter adjustment increment for the current cycle. The core principle of using incremental PID control logic is that this control method only outputs the parameter adjustment amount between adjacent cycles, without needing to accumulate historical deviations, effectively avoiding integral saturation problems and adapting to welding closed-loop control scenarios with cycle-by-cycle iterative optimization; at the same time, by introducing historical deviations from the previous two cycles, the current magnitude, trend, and rate of change of the deviation can be taken into account simultaneously, making the parameter adjustment both responsive and stable.
[0101] The calculation formula for incremental PID control is as follows: Where Δu(k) is the initial parameter adjustment for the k-th welding cycle, e(k) is the quality deviation data for the k-th welding cycle, e(k-1) is the quality deviation data for the (k-1)-th welding cycle, e(k-2) is the quality deviation data for the (k-2)-th welding cycle, and K p K is a proportionality coefficient used to match the relationship between the deviation magnitude and the adjustment amount. i K is the integral coefficient used to eliminate steady-state deviation. d The differential coefficient is used to suppress rapid fluctuations in the deviation.
[0102] If conventional positional PID control is used, the control output is the absolute value of the parameter. Historical deviations need to be continuously accumulated, which can easily lead to integral saturation when the quality deviation continues to be in the same direction, resulting in excessive parameter adjustment and severe system overshoot. If only the deviation of the current single cycle is used for calculation, it is impossible to predict the trend of deviation changes, and the control response is prone to lag and oscillation, and the stability of closed-loop control is significantly reduced.
[0103] Step S302: Output the initial adjustment values corresponding to the three types of parameters: ultrasonic energy distribution ratio, welding pressure, and welding time.
[0104] For the three types of process parameters—ultrasonic energy distribution ratio, welding pressure, and welding time—independent PID coefficient groups are configured. The control calculations for the three types of parameters are independent of each other, and the corresponding initial adjustment amounts are calculated based on the same quality deviation data.
[0105] The principle of using independent tuning coefficients for each parameter is that the three types of parameters have different sensitivities, adjustment inertia, and effective adjustment ranges in their influence on welding quality: the influence of welding pressure on the interface contact state is fast and sensitive, so a smaller control coefficient needs to be configured; the influence of total welding time on total energy input is linear and has a large inertia, so a relatively large control coefficient can be configured.
[0106] Independent tuning ensures that the adjustment range of each parameter matches its own regulation characteristics, achieving coordinated and stable control.
[0107] Step S303: Perform amplitude limiting processing on each type of initial adjustment amount to ensure that the absolute value of a single parameter adjustment amount does not exceed the preset percentage threshold of the current corresponding parameter value. If it exceeds the amplitude limit range, output the parameter adjustment amount according to the amplitude limit value.
[0108] There is a nonlinear relationship between welding quality and process parameters, and the welding process has a certain degree of process inertia. When a sudden large deviation occurs, if the single adjustment is too large, it is easy to cause reverse overshoot of the quality in the next cycle, causing parameter fluctuations and system oscillations, which will exacerbate the dispersion of welding quality.
[0109] The preset percentage threshold is preferably 10%, meaning that within a single welding cycle, the adjustment range of any process parameter shall not exceed 10% of its current set value. After calculating the initial adjustment amount, the ratio of the initial adjustment amount to the current parameter value is first calculated. If the absolute value of the ratio is less than or equal to the preset percentage threshold, the initial adjustment amount is directly output as the final parameter adjustment amount; if the absolute value of the ratio exceeds the preset percentage threshold, the final adjustment amount after the limit is output according to ±10% of the current parameter value.
[0110] By limiting the amplitude, parameter adjustments can be constrained within the stable range of the process, achieving gradual and stable optimization and avoiding system instability.
[0111] In some embodiments, the calculation process of the parameter adjustment amount in step S300 is also matched with the deviation type adjustment strategy. Based on the deviation results of the resistance characteristic parameters, the quality deviation is divided into three typical types: insufficient welding bond strength, excessive interface metallurgical layer thickness, and excessive resistance recovery amount.
[0112] For each type of deviation, corresponding core control parameters and adjustment directions are pre-matched. Before incremental PID calculation, the control weights of each process parameter are configured in a targeted manner, so that the parameter adjustment direction corresponds one-to-one with the defect formation mechanism, avoiding secondary quality problems caused by blindly adjusting all parameters. Specifically, it can be divided into the following three types.
[0113] When the quality deviation data reflects that the weld bonding strength is lower than the target value, the parameter adjustment amount corresponding to increasing the main frequency energy ratio, extending the diffusion stage duration, and increasing the welding pressure is increased.
[0114] Specifically, the core causes of insufficient weld bonding strength are usually incomplete breakage of the interface oxide layer, insufficient macroscopic plastic deformation leading to a small effective bonding area, or insufficient atomic diffusion time leading to discontinuity of the metallurgical bonding layer.
[0115] Dominant frequency vibration is the core source of macroscopic frictional energy and the driving force for large-scale plastic deformation of the interface. Increasing the proportion of dominant frequency energy can enhance the macroscopic frictional effect at the interface, further breaking down residual oxide layers and expanding the effective bonding area of the interface. Extending the duration of the diffusion stage can increase the duration of atomic diffusion, promoting the formation of a continuous metallurgical bonding layer. Increasing the welding pressure can enhance the tightness of the interface contact, providing more sufficient pressure conditions for atomic-level diffusion bonding. The coordinated adjustment of these three types of parameters can specifically strengthen the weld bonding strength without causing excessive temperature rise at the interface.
[0116] When the quality deviation data reflects that the thickness of the interface metallurgical layer is higher than the target value, the parameter adjustment amount corresponding to increasing the proportion of the first auxiliary frequency energy and shortening the diffusion stage duration is increased.
[0117] Specifically, the core cause of excessive interfacial metallurgical layer thickness is excessive energy input during the diffusion stage, excessively high interfacial temperature, and excessively long atomic diffusion time, which leads to excessive coarsening growth of intermetallic compounds, ultimately causing embrittlement of the weld joint and a decline in mechanical and fatigue resistance.
[0118] The high-frequency micro-amplitude vibration of the first auxiliary frequency can promote the microscopic plastic flow of the interface, refine the interface grains, and inhibit the coarse growth of intermetallic compounds. Shortening the diffusion stage duration can directly reduce the total action time of atomic diffusion, thus limiting the excessive growth of the metallurgical layer from the time dimension. The combination of the two can control the thickness of the metallurgical layer within the optimal range while ensuring the basic bonding strength.
[0119] When the quality deviation data reflects a resistance increase higher than the target value, the parameter adjustments should be made to reduce the total vibration energy input and shorten the total welding time.
[0120] Specifically, an excessive increase in resistance corresponds to a large amount of springback and a high level of residual stress during the interface cooling process after welding, and there is even a risk of microcrack formation. The core cause is usually excessive total vibration energy input, excessively high interface peak temperature, and large thermal stress and residual stress generated during the cooling and contraction process.
[0121] Reducing the total vibration energy input can directly reduce the total heat generated by interfacial friction, lower the peak welding temperature, and reduce the temperature difference and thermal stress during the cooling process. Shortening the total welding time can reduce the energy accumulation time, avoid excessive softening of the interface, and reduce the probability of cooling rebound and microcrack formation. The synergistic effect of these two factors can fundamentally reduce residual stress at the interface, inhibit microcrack initiation, and improve the long-term service reliability of the welded joint.
[0122] The three types of directional adjustment rules mentioned above all match the formation mechanisms of their respective defects. The core cause of insufficient weld bonding strength is insufficient macroscopic plastic deformation and a small effective bonding area. Therefore, reinforcement is achieved through three macroscopic energy-related parameters: main frequency, diffusion time, and pressure. The core cause of excessive interfacial metallurgical layer thickness is excessive diffusion and grain coarsening. Therefore, fine-tuning is achieved through high-frequency auxiliary frequency and diffusion time. The core cause of excessive resistance rise is excessive total energy input and excessive residual stress. Therefore, total energy and total time are used for total quantity control. This directional adjustment mode can quickly correct quality deviations while avoiding secondary quality problems caused by blindly adjusting all parameters.
[0123] The lithium battery tab welding quality multi-frequency ultrasonic resistance closed-loop control system of the present invention includes a multi-frequency ultrasonic welding module, a resistance acquisition module, a feature extraction and deviation generation module, an adjustment calculation module and a closed-loop update control module.
[0124] The multi-frequency ultrasonic welding module is used to apply a set welding pressure to the welding area of the lithium battery tab. According to the preset sequence of multiple welding stages, it uses multi-frequency ultrasonic vibration, including the main frequency and at least two auxiliary frequencies, to input coupled vibration energy to the welding interface, which is the frequency combination and energy distribution ratio corresponding to each welding stage.
[0125] The resistance acquisition module is used to acquire dynamic resistance data of the welding circuit in real time throughout the welding process. The welding circuit includes the welding head, lithium battery tabs, and bottom mold.
[0126] The feature extraction and deviation generation module is used to extract resistance feature parameters reflecting the bonding degree of the welding interface from dynamic resistance data, compare the resistance feature parameters with the preset resistance feature quality judgment threshold, and generate quality deviation data.
[0127] The adjustment calculation module is used to calculate the parameter adjustment amounts for the ultrasonic energy distribution ratio, welding pressure, and welding time corresponding to the next welding cycle based on the quality deviation data.
[0128] The closed-loop update control module is used to update the welding process parameters for the next welding cycle based on the parameter adjustment amount. Based on the updated welding process parameters, the multi-frequency ultrasonic welding module is controlled to perform the welding operation of the next lithium battery tab, thereby realizing closed-loop control of welding quality.
[0129] The electronic device of the present invention includes a processor and a memory; the memory stores a computer program, wherein the computer program, when executed by the processor, implements the above-described multi-frequency ultrasonic resistance closed-loop control method for lithium battery tab welding quality.
[0130] The present invention provides a non-transitory computer-readable storage medium having a computer program stored thereon, which, when executed by a processor, implements the steps of the above-described multi-frequency ultrasonic resistance closed-loop control method for lithium battery tab welding quality.
[0131] It should be noted that, for the sake of simplicity, the foregoing method embodiments are all described as a series of actions. However, those skilled in the art should understand that this application is not limited to the described order of actions, as some steps may be performed in other orders or simultaneously according to this application. Furthermore, those skilled in the art should also understand that the embodiments described in the specification are preferred embodiments, and the actions and modules involved are not necessarily essential to this application.
[0132] In the above embodiments, the descriptions of each embodiment have different focuses. For parts not described in detail in a certain embodiment, please refer to the relevant descriptions in other embodiments.
[0133] In the several embodiments provided in this application, it should be understood that the disclosed apparatus can be implemented in other ways. For example, the apparatus embodiments described above are merely illustrative; for instance, the division of units is only a logical functional division, and in actual implementation, there may be other division methods. For example, multiple units or components may be combined or integrated into another system, or some features may be ignored or not executed. Furthermore, the shown or discussed mutual couplings or direct couplings or communication connections may be through some service interfaces; indirect couplings or communication connections between apparatuses or units may be electrical or other forms.
[0134] The units described as separate components may or may not be physically separate. The components shown as units may or may not be physical units; that is, they may be located in one place or distributed across multiple network units. Some or all of the units can be selected to achieve the purpose of this embodiment, depending on actual needs.
[0135] Furthermore, the functional units in the various embodiments of this application can be integrated into one processing unit, or each unit can exist physically separately, or two or more units can be integrated into one unit. The integrated unit can be implemented in hardware or as a software functional unit.
[0136] If the integrated unit is implemented as a software functional unit and sold or used as an independent product, it can be stored in a computer-readable storage device (CMD). Based on this understanding, the technical solution of this application, in essence, or the part that contributes to the prior art, or all or part of the technical solution, can be embodied in the form of a software product. This computer software product is stored in a memory and includes several instructions to cause a computer device (which may be a personal computer, server, or network device, etc.) to execute all or part of the steps of the methods of the various embodiments of this application. The aforementioned memory includes various media capable of storing program code, such as USB flash drives, portable hard drives, magnetic disks, or optical disks.
[0137] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A multi-frequency ultrasonic resistance closed-loop control method for the welding quality of lithium battery tabs, characterized in that, Includes the following steps: A set welding pressure is applied to the welding area of the lithium battery tab. According to the preset sequence of multiple welding stages, multi-frequency ultrasonic vibration including the main frequency and at least two auxiliary frequencies is used to input coupled vibration energy to the welding interface, which is the frequency combination and energy distribution ratio corresponding to each welding stage. Throughout the welding process, dynamic resistance data of the welding circuit is collected in real time. The welding circuit includes the welding head, lithium battery tabs, and bottom mold. The resistance characteristic parameters reflecting the bonding degree of the welding interface are extracted from the dynamic resistance data. The resistance characteristic parameters are compared with the preset resistance characteristic quality judgment threshold to generate quality deviation data. Based on the quality deviation data, the parameter adjustments for the ultrasonic energy distribution ratio, welding pressure, and welding time corresponding to the next welding cycle are calculated. The welding process parameters for the next welding cycle are updated based on the parameter adjustment amount, and the welding operation of the next lithium battery tab is performed according to the updated welding process parameters, so as to achieve closed-loop control of welding quality.
2. The multi-frequency ultrasonic resistance closed-loop control method for lithium battery tab welding quality as described in claim 1, characterized in that, The two auxiliary frequencies are the first auxiliary frequency and the second auxiliary frequency, respectively. The execution sequence of the multiple welding stages includes the pre-compression stage, the crushing stage, the diffusion stage, and the homogenization stage. The pre-pressure stage performs the following steps: only inputting the vibration energy corresponding to the main frequency, applying a first set welding pressure to the lithium battery tab welding area, and completing the tab clamping positioning and initial contact establishment; The crushing stage performs the following steps: simultaneously inputting the vibration energy corresponding to the main frequency and the first auxiliary frequency, applying the second set welding pressure to the lithium battery tab welding area, and completing the crushing of the oxide layer at the welding interface and roughening of the interface. The diffusion stage performs the following steps: simultaneously inputting the vibration energy corresponding to the main frequency and the first auxiliary frequency, applying a third set welding pressure to the lithium battery tab welding area, and completing the interface atomic diffusion and metallurgical bonding formation. The homogenization stage performs the following steps: simultaneously inputting the vibration energy corresponding to the first auxiliary frequency and the second auxiliary frequency, applying a fourth set welding pressure to the lithium battery tab welding area, and completing the homogenization of the interface temperature field and the release of residual stress.
3. The multi-frequency ultrasonic resistance closed-loop control method for lithium battery tab welding quality as described in claim 2, characterized in that, The main frequency has a frequency range of 15-25kHz, the first auxiliary frequency has a frequency range of 35-45kHz, and the second auxiliary frequency has a frequency range of 55-65kHz.
4. The multi-frequency ultrasonic resistance closed-loop control method for lithium battery tab welding quality as described in claim 1, characterized in that, The dynamic resistance data of the welding circuit is obtained through the following steps: Apply a constant DC test current to the welding circuit; Real-time voltage signals at both ends of the welding interface are synchronously acquired at the voltage measurement end of the welding circuit, and the acquisition of the real-time voltage signals is synchronized with the ultrasonic vibration period of the main frequency. Based on the correspondence between constant DC test current and real-time voltage signal, the real-time dynamic resistance data of the welding circuit is calculated.
5. The multi-frequency ultrasonic resistance closed-loop control method for lithium battery tab welding quality as described in claim 2, characterized in that, The resistance characteristic parameters include initial contact resistance, minimum resistance, resistance decrease rate, steady-state resistance, and resistance recovery. Extracting the resistance characteristic parameters reflecting the bonding strength of the weld interface from the dynamic resistance data specifically includes the following steps: The average resistance value within a set duration at the end of the pre-loading stage is extracted from the dynamic resistance data as the initial contact resistance. The minimum resistance is extracted from the dynamic resistance data throughout the welding process and recorded as the minimum resistance. Calculate the average slope of the resistance as it decreases from the initial contact resistance to the minimum resistance to obtain the resistance decrease rate. The average resistance within a set time period after welding is extracted from the dynamic resistance data as the steady-state resistance. Calculate the difference between the steady-state resistance and the minimum resistance to obtain the resistance recovery amount.
6. The multi-frequency ultrasonic resistance closed-loop control method for lithium battery tab welding quality as described in claim 1, characterized in that, The step of calculating the adjustment amounts of the ultrasonic energy distribution ratio, welding pressure, and welding time for the next welding cycle based on the quality deviation data specifically includes the following steps: The quality deviation data is input into the incremental PID control logic, and the calculation is performed by combining the quality deviation data of the current cycle with those of the previous two cycles. The initial adjustment values for three types of parameters—ultrasonic energy distribution ratio, welding pressure, and welding time—are output respectively. For each type of initial adjustment, a limit is applied to ensure that the absolute value of a single parameter adjustment does not exceed the preset percentage threshold of the current corresponding parameter value. If the adjustment exceeds the limit range, the parameter adjustment is output according to the limit value.
7. The multi-frequency ultrasonic resistance closed-loop control method for lithium battery tab welding quality as described in claim 2, characterized in that, The calculation process for the parameter adjustment amount also matches the deviation type adjustment strategy, specifically including: When the quality deviation data reflects that the weld bond strength is lower than the target value, increase the proportion of the main frequency energy, extend the diffusion stage duration, and increase the parameter adjustment amount corresponding to the welding pressure. When the quality deviation data reflects that the thickness of the interface metallurgical layer is higher than the target value, the parameter adjustment amount corresponding to increasing the proportion of the first auxiliary frequency energy and shortening the diffusion stage duration is increased. When the quality deviation data reflects a resistance increase higher than the target value, the parameter adjustments should be made to reduce the total vibration energy input and shorten the total welding time.
8. A multi-frequency ultrasonic resistance closed-loop control system for lithium battery tab welding quality, characterized in that, It includes a multi-frequency ultrasonic welding module, a resistance acquisition module, a feature extraction and deviation generation module, an adjustment calculation module, and a closed-loop update control module. The multi-frequency ultrasonic welding module is used to apply a set welding pressure to the welding area of the lithium battery tab, and according to the preset sequence of multiple welding stages, it uses multi-frequency ultrasonic vibration including a main frequency and at least two auxiliary frequencies to input coupled vibration energy to the welding interface, which is the frequency combination and energy distribution ratio corresponding to each welding stage. The resistance acquisition module is used to acquire dynamic resistance data of the welding circuit in real time throughout the welding process. The welding circuit includes the welding head, lithium battery tabs, and bottom mold. The feature extraction and deviation generation module is used to extract resistance feature parameters reflecting the bonding degree of the welding interface from dynamic resistance data, compare the resistance feature parameters with a preset resistance feature quality judgment threshold, and generate quality deviation data. The adjustment calculation module is used to calculate the parameter adjustment amounts of the ultrasonic energy distribution ratio, welding pressure, and welding time corresponding to the next welding cycle based on the quality deviation data. The closed-loop update control module is used to update the welding process parameters for the next welding cycle according to the parameter adjustment amount, and control the multi-frequency ultrasonic welding module to perform the welding operation of the next lithium battery tab according to the updated welding process parameters, so as to realize closed-loop control of welding quality.
9. An electronic device, characterized in that, It includes a processor and a memory; the memory stores a computer program, wherein the computer program, when executed by the processor, implements the multi-frequency ultrasonic resistance closed-loop control method for lithium battery tab welding quality as described in any one of claims 1 to 7.
10. A non-transitory computer-readable storage medium having a computer program stored thereon, characterized in that, When the computer program is executed by the processor, it implements the steps of the multi-frequency ultrasonic resistance closed-loop control method for the welding quality of lithium battery tabs as described in any one of claims 1-7.