Automatic surfacing method for low-deformation dry quenching fan blade

By employing precise temperature control and stress relief technology, the problems of large deformation and poor quality during the overlay welding process of dry quenching coke blower blades have been solved, achieving high-precision, low-deformation automated overlay welding and improving the wear resistance and service life of the blades.

CN123128768APending Publication Date: 2026-11-20CHONGQING GENERAL IND (GRP) LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611512061.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

The existing dry quenching fan blade overlay welding process has problems such as concentrated heat input, large amount of twisting deformation after blade overlay welding, poor quality of overlay layer, angular deviation after blade pressing, and high overall cost, making it impossible to achieve high-precision, low-deformation, and high-consistency automated overlay welding.

Method used

An automatic overlay welding method for low-deformation dry quenching fan blades is adopted. Through precise temperature control, segmented symmetrical staggered overlay welding, gradient heat input, and stress relief post-treatment integrated process, including stress relief groove processing, multi-point rigid clamping and positioning, real-time temperature monitoring, low-temperature stress relief heat treatment and precision grinding, the thermal stress and shrinkage deformation during the blade overlay welding process are controlled.

Benefits of technology

It significantly reduces blade torsion deformation and curvature offset, improves the stability and consistency of weld overlay quality, increases blade pass rate and service life, reduces repair costs, and is suitable for the manufacture of blades for dry quenching fans and other high-end ventilation fans in various industries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128768A_ABST
    Figure CN123128768A_ABST
Patent Text Reader

Abstract

The application discloses a kind of low deformation dry quenching fan blade automatic surfacing methods, comprising: blade is pretreated, stress relieving groove is processed in the area to be surfacing, positioning blade is prepositioned to reverse deformation, after clamping is completed, overall preheating is carried out;Blade is scanned modeling three-dimensionally, and generates surfacing path planning;Select transition welding wire, complete first layer backing surfacing of weld and relieving groove with surfacing path planning;Real-time monitoring weld and heat-affected zone temperature is cooled to preset temperature interval, with the welding wire of adaptation dry quenching operating condition is carried out surface layer surfacing and stress relieving, and diamond grinding wheel is used to blade surfacing area and overall profile grinding processing;Blade is low-temperature moulding shaping, detects the defect of formed blade and carries out local repair welding, and is polished to repair welding place and so on processing;Comprehensive inspection blade, so that it meets dry quenching extreme operating condition operation standard.The application can greatly reduce the deformation of blade mass production, ensure the stability and reliability of blade surfacing quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of wind power generation technology, and in particular to an automatic overlay welding method for low-deformation dry quenching wind turbine blades. Background Technology

[0002] Ventilation fans are core ventilation, dust removal, and air exchange equipment in industrial production, and are widely used in mining, power, metallurgy, coking, chemical and other fields. As the core load-bearing and flow-through components, the blades are subjected to dust, water vapor, corrosive media erosion, solid particle erosion, and alternating loads during operation. They are prone to failure defects such as blade wear, pitting, and edge damage, which directly cause the fan's air volume to decrease, operating vibration and noise to exceed the standard. In severe cases, they can lead to safety accidents such as blade breakage and equipment shutdown, which significantly increases the company's equipment operation and maintenance costs.

[0003] Among them, dry quenching coke circulating fans, as key core equipment in the coking industry, operate under more stringent conditions. They are subjected to extreme environments of high temperature, high dust, high-speed erosion by high-hardness coke powder, and coupling with trace amounts of corrosive media for extended periods. This places extremely high demands on the wear resistance, erosion resistance, high-temperature resistance, and fatigue resistance of the blade surface. To meet the long-term operation requirements of the equipment, the industry generally uses ultra-hard wear-resistant alloy materials with a hardness of 59-62 HRC and a hard phase content of over 50% to reinforce failed blades through welding. This significantly improves the wear resistance and erosion resistance of the blade surface and effectively extends the service life of the blades. At present, the mainstream welding method in the industry is still mainly manual welding, with gradual attempts to explore automated welding processes. However, the overall technical system is not yet mature, and there are many technical problems that urgently need to be solved.

[0004] Existing conventional welding processes for repairing ultrahard materials on dry quenching fan blades suffer from several key drawbacks, including large blade deformation, significant torsional deformation, unstable welding quality, and insufficient reliability. These are detailed below: First, the blades of dry quenching blowers are mostly 8-12mm large-arc curved steel structures. Traditional manual arc welding and conventional gas shielded welding have large heat inputs, concentrated heat-affected areas, and no precise temperature control strategy. The thermal stress distribution during the welding process is extremely uneven. The ultra-hard wear-resistant alloy material has poor plasticity, extremely high thermal sensitivity, and large residual welding stress, which easily leads to blade warping and edge twisting, resulting in large deformation of the blades after welding. At the same time, the cooling shrinkage stress of the ultra-hard material is concentrated, and defects such as microcracks, porosity, slag inclusions, and interlayer detachment are prone to occur in the weld and heat-affected zone. The blade qualification rate is low, and some blades are directly scrapped due to excessive deformation and stress cracking that cannot be corrected.

[0005] Secondly, traditional manual surfacing often uses continuous long weld seams without standardized path planning. The welding trajectory is highly random, the heat input area is messy, and the consistency and precision of the surfacing are poor. Furthermore, it cannot perform differentiated welding for the curved surface structure and wall thickness differences of the blades. This results in uneven thickness of the superhard surfacing layer, large dispersion of hard phase distribution, unstable wear resistance, and difficulty in adapting to the extreme working conditions of long-term high-speed coke powder scouring in dry quenching fans. The improvement effect on the service life of the blades after surfacing is limited, and the rework rate is high.

[0006] Third, existing improvement solutions have significant technical shortcomings, failing to balance deformation control and weld quality. Currently, a few technical solutions address deformation by reducing welding current and increasing welding speed, but this results in shallow penetration of the ultra-hard weld overlay, insufficient metallurgical bonding to the matrix, and problems such as weld overlay detachment and localized rapid wear.

[0007] Fourth, the application of automated cladding technology is imperfect and lacks targeted process support. The industry has gradually introduced welding robots for assisted operations, but they generally only achieve simple trajectory replication. There is no dedicated gradient heat input process for superhard materials, and no overall temperature control and step-by-step stress relief system. Problems such as disordered heat input, severe stress accumulation, and poor deformation control still exist. It is impossible to achieve high-precision, low-deformation, and high-consistency automated cladding, which is difficult to meet the production needs of standardized and batch cladding of dry quenching coke blower blades.

[0008] Therefore, there is an urgent need for an automatic surfacing welding method for dry quenching fan blades with low deformation, in order to solve the problems of large surfacing deformation and high difficulty in straightening, and improve the reliability of the equipment. Summary of the Invention

[0009] The present invention aims to provide an automatic overlay welding method for low-deformation dry quenching fan blades, in order to solve the problems of concentrated heat input, large amount of twisting deformation after blade overlay welding, poor quality of overlay layer, blade curvature deviation after pressing, and high overall cost in the existing dry quenching fan blade overlay welding process. The present invention can effectively control the thermal stress and shrinkage deformation during the blade overlay welding process, and significantly reduce the amount of blade twisting deformation and blade curvature deviation.

[0010] To achieve the above objectives, the basic solution of the present invention is as follows: an automatic overlay welding method for low-deformation dry quenching fan blades, comprising the following steps: S1. Pre-treat the blades, the pre-treatment including non-destructive testing, grinding and surface treatment; S2. Perform stress relief groove processing in the area of ​​the blade to be welded; S3. Place the blade with the completed easing groove on the fixture, perform multi-point rigid clamping and positioning, perform reverse deformation pre-setting according to the blade thermal deformation law, press and fix it to fit the four-sided contour of the blade, and perform overall preheating after clamping. S4. Perform 3D scanning modeling on the blade after clamping and preheating, identify the boundary of the blade to be welded area and the position of the buffer groove, and generate a welding path plan. S5. Select transition welding wire and complete the first layer of root cladding welding of the weld seam and buffer groove in accordance with the cladding path planning. S6. Monitor the temperature of the weld and heat-affected zone in real time. After the temperature cools down to the preset temperature range naturally, use welding wire suitable for dry quenching conditions to perform surface layer welding. S7. After the welding is completed, a low-temperature stress-relieving heat treatment is performed, and a diamond grinding wheel is used to perform precision grinding on the welded area and the overall profile of the blade. S8. Use a blade curved surface molding die to perform low-temperature molding and shaping of the blade, detect defects in the molded blade, perform local repair welding on the defects, and perform overall fine grinding, polishing and smooth transition treatment on the repaired area. S9. Conduct a comprehensive re-inspection of the blades to ensure that all parameters meet the operating standards for extreme dry quenching conditions.

[0011] Further, step S2 includes: using a CNC milling integrated forming process to process stress relief grooves in the area of ​​the blade to be welded. The stress relief grooves are evenly and equidistantly distributed at both ends of the weld seam, with a groove depth of 1.0-3.0 mm and a groove width of 3.0-5.0 mm. The bottom and opening of the groove are both transitioned with an arc of R1.5-R2.5, and the stress relief grooves are longitudinally spaced with a segment interval of 15-20 mm.

[0012] Further, step S3 includes: placing a block of a set thickness at the center of the lower surface of the blade, and fastening the blade to the fixture with a long pressure plate to form a central protrusion structure for pre-setting the anti-deformation; preheating by manual flame heating to set the heating rate, and combining it with an infrared thermometer for real-time temperature control, wherein the temperature of the blade edge area is controlled at 80-100℃, and the temperature of the area to be welded is controlled at 100-120℃.

[0013] Further, step S4 includes: using a three-dimensional vision scanning system mounted on a six-axis linkage welding robot to perform three-dimensional scanning modeling on the blade after clamping and preheating, identifying the boundary of the area to be welded and the position of the buffer groove; dividing the area to be welded into standard short welding units of a set length, generating a standardized welding trajectory with intersecting segments, left and right symmetry, center first then edge, and weld layer first then buffer groove; and fine-tuning the welding gun posture, travel angle and swing amplitude according to the different anti-deformation preset angles of the blade to obtain the weld path planning.

[0014] Further, step S5 includes: performing root pass welding using CMT pulsed gas shielded welding process and controlling heat input parameters; wherein, the first layer of root pass welding is performed using a sinusoidal oscillating welding mode with a frequency and amplitude that meet the low stress effect, the height of the first layer of root pass welding in the buffer groove is 2 / 3 of the height of the buffer groove, and the thickness of subsequent single-layer root passes is controlled within the thickness range.

[0015] Further, step S6 includes: after the root pass welding is completed, interpass temperature control is performed, and the maximum temperature of the interpass temperature control does not exceed 100°C; during the cooling process, a flexible hammering process is used to uniformly and moderately hammer the root pass weld, the heat-affected zone and the area around the buffer tank until the temperature cools down to the preset temperature range.

[0016] Further, step S6 includes: using a welding wire adapted to dry quenching conditions for surface layer cladding, the welding wire having a diameter of 1.2-1.6 mm, the hardness of the formed layer after cladding being 59-62 HRC, and the hard phase content exceeding 50%; using a welding wire with a diameter of 1.2-1.6 mm and setting surface layer welding parameters, performing layered cladding according to the symmetrical staggered path in the cladding path planning, the thickness of a single layer cladding is controlled within 0.8-1.2 mm, the total thickness of the layered cladding is controlled within 5-10 mm, the last layer adopts an 8-shaped oscillating welding mode, and in the last layer of weld cladding in the buffer groove, the welding current and voltage are increased by setting a window to make the weld surface smooth and defect-free, the surface layer welding parameters are: welding current of 110-1150 A, welding voltage of 20-24 V, and welding speed of 7-9 cm / min.

[0017] Further, step S7 includes: after the welding is completed, the blade is naturally cooled to the room, the tooling fixture is removed, the blade is placed in the heat preservation furnace, the temperature is raised to 180-220℃ at a uniform rate, and the temperature is maintained for 2-3 hours before being slowly cooled with the furnace; the surface oxide layer, welding slag, fine protrusions and rough peaks of the blade after welding are removed by a surface grinder equipped with a diamond grinding wheel, and the local thickness deviation of the weld layer is corrected by uniform grinding.

[0018] Further, step S8 includes: according to the standard surface parameters of the blade, using a molding process, the blade is molded and shaped under thermal stress-free conditions at 100-120℃; the blade after low-temperature molding is subjected to comprehensive appearance, size and surface defect inspection, matched with the original welding material parameters, the detected defects are locally repaired by welding, and the repaired area is subjected to overall fine grinding, polishing and smooth transition treatment.

[0019] Furthermore, step S9 includes: conducting a comprehensive re-inspection of the overall dimensional accuracy, surface profile, deformation, hardness of the weld overlay, and surface roughness of the blade, so that the overall deformation of the blade is ≤0.3mm / m, and all parameters meet the operating standards for extreme dry quenching conditions.

[0020] Compared with the prior art, the advantages and beneficial effects of the present invention are as follows: 1. This invention significantly reduces the mass production deformation of dry-quenched coke thin-walled blades through the dual guarantee of structural pressure relief and process control, resulting in a high yield rate.

[0021] 2. The ultra-hard surface layer formed by the blade overlay of the present invention has uniform properties and good batch quality consistency, which can ensure the stability of the overlay quality.

[0022] 3. The blades of this invention are precision-formed and have excellent aerodynamic performance, which makes the overall operation of the dry quenching coke unit highly stable.

[0023] 4. This invention realizes fully automated intelligent manufacturing of dry quenching fan blades, with high mass production efficiency and low overall cost.

[0024] 5. The blades produced by this invention have high reliability and wide adaptability. They can be adapted to the extreme working conditions of high temperature and high erosion of dry quenching fans, and can also be widely adapted to the precision manufacturing of high-end ventilation fan blades in many industries such as power, metallurgy, and chemical industry. Attached Figure Description

[0025] Figure 1 This is a schematic diagram of an automatic overlay welding method for low-deformation dry quenching fan blades in one embodiment.

[0026] Figure 2 This is a schematic diagram of the processed buffer groove in one embodiment.

[0027] Figure 3 This is a schematic diagram of the blade overlay welding partition in one embodiment.

[0028] Figure 4 This is a schematic diagram of the weld overlay path in one embodiment. Detailed Implementation

[0029] Before describing the specific embodiments of the present invention, the overall concept of the present invention will be explained as follows: This invention is mainly based on the surfacing process of dry quenching fan blades. Existing dry quenching fan blade surfacing processes have problems such as concentrated heat input, large amount of twisting deformation after blade surfacing, poor quality of surfacing layer, angular deviation after blade pressing, and high overall cost.

[0030] Therefore, this invention provides a low-deformation overlay welding method for dry quenching fan blades. Through precise temperature control, segmented symmetrical staggered overlay welding, gradient heat input, and stress relief post-treatment integrated process design, it effectively controls thermal stress and shrinkage deformation during blade overlay welding, significantly reduces blade torsional deformation and blade curvature offset, while ensuring a strong bond, uniform structure, and excellent wear and corrosion resistance of the overlay layer. This improves the blade overlay welding qualification rate and service life, simplifies subsequent correction procedures, reduces repair costs, and is suitable for batch overlay welding and strengthening operations of various thin-walled dry quenching fan blades.

[0031] Having introduced the overall concept of the present invention, to make the invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0032] like Figure 1 As shown, an automatic surfacing welding method for low-deformation dry quenching fan blades is provided, including the following steps: Step S110: Pre-treatment of the blade, including non-destructive testing, grinding and surface treatment.

[0033] Specifically, the microstructure of the substrate is inspected using an ultrasonic non-destructive testing instrument to eliminate rolling micro-defects. Then, the area of ​​the blade to be welded is cleaned by sandblasting combined with precision grinding to remove surface oxide scale, rust, oil, coke residue and fatigue hardening layer. The cleaning range is 20-30mm from the blade boundary to ensure that the substrate welding surface is clean and free of impurities and has uniform surface roughness, providing high-quality substrate conditions for subsequent processing and welding.

[0034] Step S120: Perform stress relief groove processing on the area of ​​the blade to be welded.

[0035] Specifically, considering the thin-walled structure of dry quenching coke blades and the high stress concentration coefficient and easy cracking characteristics of ultra-hard welding materials, a special stress relief groove structure is designed in the area of ​​the blade to be welded, and the corresponding relief groove is processed according to the design, so that the ultra-hard welding forming stress can be released in advance during subsequent welding to avoid blade deformation.

[0036] Step S120 includes: using CNC milling integrated forming process to process stress relief grooves in the area of ​​the blade to be welded. The stress relief grooves are evenly and equidistantly distributed at both ends of the weld seam. The dimensions are groove depth 1.0-3.0mm, groove width 3.0-5.0mm, groove bottom and groove opening are both transitioned with R1.5-R2.5 arc, and the stress relief groove is longitudinally set with a segment interval of 15-20mm.

[0037] Specifically, a CNC milling integrated forming process is adopted to machine stress relief grooves in the area of ​​the blade to be welded, eliminating the dimensional deviations and sharp edges of manual grooving. The stress relief grooves are evenly and equidistantly distributed at both ends of the weld seam, with a longitudinal interval of 15-20mm between the grooves. The resulting stress relief grooves are as follows: Figure 2 As shown, the specific dimensions of the stress relief groove can be designed according to the blade conditions, and it is ensured that the stress relief groove has no right-angle stress singularities, and that the groove body is continuous, smooth, and uniform in depth.

[0038] Step S130: Place the blade with the completed easing groove on the fixture, perform multi-point rigid clamping and positioning, perform reverse deformation pre-setting according to the blade thermal deformation law, press and fix it to fit the four-sided contour of the blade, and perform overall preheating after clamping.

[0039] Specifically, the blade with the completed eccentric groove is placed on a fixture for multi-point rigid clamping and positioning. The blade is pre-deformed according to the thermal deformation law, and is pressed and fixed to fit the four-sided contour of the blade to constrain the free deformation of the blade and avoid free warping and twisting deformation during the welding process. After clamping, the whole is preheated.

[0040] Step S130 includes: placing a block of a set thickness at the center of the lower surface of the blade, and fastening the blade to the fixture with a long pressure plate to form a central protrusion structure for pre-setting the reverse deformation; preheating by manual flame heating to set the heating rate, and real-time temperature control by combining an infrared thermometer, wherein the temperature of the blade edge area is controlled at 80-100℃, and the temperature of the area to be welded is controlled at 100-120℃.

[0041] Specifically, the anti-deformation pre-set involves placing a block with a blade plate thickness of 0.5-1 mm at the center of the lower surface of the blade, and then using a long pressure plate to fasten the blade to the fixture, forming a central protrusion structure.

[0042] The blade is preheated by manual flame heating, combined with real-time precise temperature control by an infrared thermometer: 80-100℃ for the blade edge area and 100-120℃ for the welding area. The heating rate is strictly controlled at 3-5℃ / min to avoid local rapid heating and thermal stress, uniformly eliminate low-temperature residual stress in the blade, and significantly reduce the thermal stress caused by the superhard material welding.

[0043] Step S140: Perform a 3D scanning model of the blade after clamping and preheating, identify the boundary of the blade to be welded area and the position of the buffer groove, and generate a welding path plan.

[0044] Step S140 includes: using a three-dimensional vision scanning system mounted on a six-axis linkage welding robot to perform three-dimensional scanning modeling on the blade after clamping and preheating, identifying the boundary of the area to be welded and the position of the buffer groove, dividing the area to be welded into standard short welding units of a set length, generating a standardized welding trajectory with intersecting segments, left and right symmetry, center first and then edge, and weld layer first and then buffer groove; and fine-tuning the welding gun posture, walking angle and swing amplitude according to the different anti-deformation preset angles of the blade to obtain the weld path planning.

[0045] Specifically, relying on a six-axis linkage welding robot equipped with a 3D vision scanning system, the preheated blades are scanned and modeled in 3D to accurately identify the boundaries of the area to be welded and the location of the buffer groove. Combining the stress balance mechanism of dry-quenched coke blades and the welding deformation law of superhard materials, the robot system adaptively and intelligently plans the welding path: automatically dividing the welding area into standard short welding units of 100-150mm in length, generating standardized welding trajectories that are staggered, symmetrical, and follow a pattern of first the center and then the edge, and first the weld layer and then the buffer groove. At the same time, the welding gun posture, walking angle and swing amplitude are adaptively and finely adjusted according to the different anti-deformation preset angles of the blade to obtain the welding path planning. This can avoid stress concentration areas and eliminate the problems of messy manual welding trajectories and disordered heat input, providing precise path support for low-deformation automated welding.

[0046] Step S150: Select transition welding wire and complete the first layer of weld and buffer trench rooting welding in accordance with the weld overlay path planning.

[0047] Specifically, low-energy, high-toughness transition welding wire is selected to avoid affecting the strength and toughness of the blade and to reduce residual stress. Combined with robot welding path planning, the first layer of weld seam and buffer groove is completed. The toughness transition layer buffers the performance difference between the superhard material and the substrate, prevents the substrate stress from being transmitted to the superhard surface layer, effectively prevents the superhard weld layer from cracking and falling off, and lays a stable foundation for the subsequent superhard wear-resistant layer welding.

[0048] Step S150 includes: performing root pass welding using CMT pulsed gas shielded welding process and controlling heat input parameters; wherein, the first layer of root pass welding is performed using a sinusoidal oscillating welding mode with a frequency and amplitude that meet the low stress effect, the height of the first layer of root pass welding in the buffer groove is 2 / 3 of the height of the buffer groove, and the thickness of subsequent single-layer root passes is controlled within the thickness range.

[0049] Specifically, the root pass welding process employs CMT pulsed gas shielded welding, with strict control over low-stress heat input parameters: welding current 90-110A, welding voltage 18-20V, and welding speed 8-15cm / min. The first root pass welding uses a thin penetration depth, low-stress sinusoidal oscillating welding mode, achieved by increasing frequency and reducing amplitude, ensuring tensile strength while avoiding overheating fracture, and reducing residual stress in the weld to minimize deformation. The thickness of a single root pass is controlled at 0.8-1.0mm to ensure good metallurgical fusion between the root pass weld layer and the blade substrate, free from defects such as incomplete fusion, porosity, and microcracks. Furthermore, the first root pass welding height for the stress-relieving groove is 2 / 3 of the groove height, ensuring that the stress-relieving groove function is maintained during the second weld pass.

[0050] Step S160: Monitor the temperature of the weld and heat-affected zone in real time. After the temperature cools naturally to the preset temperature range, use welding wire suitable for dry quenching conditions to perform surface layer welding.

[0051] Specifically, welding is stopped immediately after the root pass is completed, and the process of precise temperature control and stress relief between layers begins. The temperature of the weld and heat-affected zone is monitored in real time. Only after the temperature of the area has naturally cooled to 80-100℃ can zonal cladding be performed using welding wire suitable for dry quenching conditions to achieve surface cladding. The zonal cladding of the blade is as follows: Figure 3 As shown, welding is performed sequentially according to the welding zone number.

[0052] Step S160 includes: after the root pass welding is completed, interpass temperature control is performed, and the maximum temperature of the interpass temperature control does not exceed 100°C; during the cooling process, a flexible hammering process is used to uniformly and moderately hammer the root pass weld, heat-affected zone and surrounding area of ​​the buffer tank until the temperature cools down to the preset temperature range.

[0053] Specifically, the interlayer temperature is controlled to not exceed 100℃ to prevent stress accumulation caused by continuous high-temperature welding. During the cooling process, a flexible hammering process is used to uniformly and moderately hammer the root weld, heat-affected zone, and surrounding area of ​​the buffer groove to refine the weld metallographic structure, release residual tensile stress generated by welding solidification shrinkage, suppress the accumulation of micro-deformation of the blade, and further avoid the risk of crack initiation in ultra-hard material welding.

[0054] The surface layer is cladding using welding wire adapted to dry quenching conditions. The wire diameter is 1.2-1.6mm, and the hardness of the cladding layer is 59-62HRC with a hard phase content exceeding 50%. Using welding wire of 1.2-1.6mm diameter and setting the surface layer welding parameters, layered cladding is performed according to the symmetrical staggered path in the cladding path planning. The thickness of a single layer is controlled within 0.8-1.2mm, and the total thickness of the layered cladding is controlled within 5-10mm. The last layer uses an 8-shaped oscillating welding mode. For the last weld layer in the buffer groove, a set window is used to increase the welding current and voltage, ensuring a smooth and defect-free weld surface. The surface layer welding parameters are: welding current 110-1150A, welding voltage 20-24V, and welding speed 7-9cm / min.

[0055] Specifically, after the interlayer stress relief is completed, an ultra-hard wear-resistant alloy welding wire adapted to the extreme working conditions of dry quenching is used for surface layer welding; the surface layer welding follows a pre-set symmetrical staggered path of the robot for layered welding, as shown in the welding path. Figure 4 As shown, welding parameters are gradually increased during the overlay welding process; the total thickness of the layered overlay welding is controlled within the set range, and the last layer adopts an 8-shaped oscillating welding mode, resulting in a beautiful weld surface and uniform metal filling. For the last layer of the tempering groove overlay welding, the welding current and voltage need to be appropriately increased to ensure a smooth and defect-free weld surface. Uniform heat input is maintained throughout the overlay welding process to ensure a uniform thickness of the ultra-hard overlay layer, a dense distribution of the hard phase, and no overlay defects, meeting the high-temperature resistance and high-speed erosion resistance requirements of the dry quenching fan.

[0056] Step S170: After the welding is completed, a low-temperature stress-relieving heat treatment is performed, and a diamond grinding wheel is used to perform precision grinding on the welded area and the overall profile of the blade.

[0057] Specifically, after the entire blade welding process is completed, the blade is allowed to cool naturally to room temperature. The tooling fixtures are then removed, and the blade undergoes a low-temperature stress-relieving heat treatment. After the stress-relieving treatment is completed, a diamond grinding wheel is used to perform precision grinding on the welded area and the overall surface of the blade.

[0058] Step 170 includes: after the welding is completed, the blade is naturally cooled to the room, the tooling fixture is removed, the blade is placed in the heat preservation furnace, the temperature is raised to 180-220℃ at a uniform rate, and the temperature is maintained for 2-3 hours before being slowly cooled with the furnace; the surface oxide layer, welding slag, fine protrusions and rough peaks of the blade after welding are removed by a surface grinder equipped with a diamond grinding wheel, and the local thickness deviation of the weld layer is corrected by uniform grinding.

[0059] Specifically, during stress relief treatment, the blade is placed in a heat-preserving furnace and heated at a uniform rate to 180-220℃. After holding at this temperature for 2-3 hours, it is slowly cooled with the furnace. This completely eliminates the multi-layered residual stress generated during the entire process of root welding and super-hard layer welding, solves the stress cracking problem in the subsequent pressing process of the blade, significantly improves the structural stability and service reliability of the blade, and provides a stress-free substrate state for subsequent precision grinding and molding.

[0060] During precision grinding, the advantages of diamond grinding wheels—high hardness, high cutting accuracy, and good grinding uniformity—are utilized. A surface grinder is used to remove the oxide layer, weld slag, fine protrusions, and rough peaks from the surface of the blades after welding. This precisely optimizes the microstructure of the blade surface, significantly reducing surface roughness and improving surface flatness and smoothness. Simultaneously, uniform grinding corrects local thickness deviations in the weld overlay layer, ensuring uniform stress during subsequent molding and avoiding indentations and localized deformation caused by surface hard spots and protrusions. This provides a high-precision, highly consistent surface foundation for low-temperature molding.

[0061] Step S180: The blade is formed by low-temperature molding using a blade curved surface molding die. Defects in the molded blade are detected, and the defects are repaired by local welding. The repaired area is then finely ground, polished, and smoothed.

[0062] Specifically, after precision grinding, the blades are precisely shaped by cryogenic molding using a specialized blade surface molding die. The cryogenically molded blades undergo comprehensive inspection for appearance, dimensions, and surface defects. Minor defects such as missing material, molding depressions, and grinding residue are precisely repaired by localized welding. The repaired areas are then finely ground, polished, and smoothed to eliminate machining edges and stress concentration points.

[0063] Step S180 includes: according to the standard curved surface parameters of the blade, using a molding process, the blade is molded and shaped under thermal stress-free conditions at 100-120℃; the blade after low-temperature molding is subjected to comprehensive appearance, size and surface defect inspection, matched with the original welding material parameters, the detected defects are locally repaired by welding, and the repaired area is subjected to overall fine grinding, polishing and smooth transition treatment.

[0064] Specifically, based on the original standard surface parameters of the blade, a molding process is adopted under the condition of 100-120℃ without thermal stress, so that the overall surface curvature, flatness, and contour of the blade fully meet the design standards. Moreover, there is no additional welding thermal stress during the low-temperature molding process, which effectively ensures the structural integrity of the superhard weld overlay layer.

[0065] After cryogenic molding, the blades undergo comprehensive appearance, dimensional and surface defect inspection. Precise local repair welding is performed for minor defects such as missing material, molding depressions and grinding residue. The repair welding process follows the principle of low line energy and short intermittent welding, matching the parameters of the original superhard welding material to ensure seamless integration and consistent performance between the repaired area and the original weld overlay. Subsequently, the repaired area is finely ground, polished and smoothed to eliminate machining edges and stress concentration points.

[0066] Step S190: Conduct a comprehensive re-inspection of the blades to ensure that all parameters meet the operating standards for extreme dry quenching conditions.

[0067] Step S190 includes: conducting a comprehensive re-inspection of the overall dimensional accuracy, surface profile, deformation, hardness of the weld overlay, and surface roughness of the blade, so that the overall deformation of the blade is ≤0.3mm / m, and all parameters meet the operating standards for extreme dry quenching conditions.

[0068] Specifically, the overall dimensional accuracy, surface profile, deformation, hardness of the weld overlay, and surface roughness of the blades are comprehensively re-inspected to ensure that the overall deformation of the blades is ≤0.3mm / m, the ultra-hard weld overlay has uniform performance, regular shape, and excellent surface quality, and that all parameters meet the operating standards for extreme dry quenching conditions.

[0069] In this embodiment, the blade undergoes pretreatment such as non-destructive testing, grinding, and surface treatment. Stress-relieving grooves are machined in the area to be welded to release the stress during the ultra-hard weld overlay process. The blade is placed on a fixture for multi-point rigid clamping and positioning. Anti-deformation is pre-set according to the blade's thermal deformation characteristics, and the blade is pressed and fixed to fit the four-sided contour. Overall preheating is performed to prevent free warping and twisting deformation during welding. A 3D scanning model of the blade is created to identify the boundaries of the area to be welded and the location of the stress-relieving grooves, generating a weld overlay path plan to provide a precise path for subsequent welding. A transition welding wire is selected, and the weld overlay path plan is configured for the first layer of weld and stress-relieving groove overlay, effectively preventing cracking and peeling of the ultra-hard weld overlay layer. The temperature of the weld and heat-affected zone is monitored in real time. After the temperature naturally cools to the preset temperature range, an adaptive dry quenching process is employed. The welding wire used in coke quenching operations undergoes surface layer welding to gradually relieve stress and prevent deformation and end cracking during mass production of ultra-hard welded blades. After welding, low-temperature stress-relieving heat treatment is performed to significantly improve the structural stability and service reliability of the blades. Diamond grinding wheels are used to precisely grind the welded areas and the overall surface of the blades to eliminate weld peaks, oxide hard layers, and local stress concentration points, effectively ensuring the operational stability of the blades. Low-temperature molding and shaping of the blades is performed using blade curved surface molding molds to effectively ensure the structural integrity of the ultra-hard welded layer. Defects in the formed blades are detected and repaired locally. The repaired areas are then finely ground, polished, and smoothed. The blades undergo comprehensive re-inspection to ensure that all parameters meet the operating standards for extreme dry quenching conditions, ensuring the quality of the finished blades and making them suitable for large-scale, precision mass production of dry quenching fan blades.

[0070] In one embodiment, to verify the technical effect of the present invention, the above-mentioned automatic overlay welding method for low-deformation dry quenching fan blades was applied to the mass production of high-end dry quenching circulating fan blades in the coking industry. The blade substrate is made of Q460ME high-strength steel and is molded. The specific mass production specifications of the blades are: total length 829.5mm, wall thickness 12mm, blade width 277 / 171mm, arc R1541, overlay layer thickness 7mm, and 12 blades. After the blades are overlaid with an ultra-hard wear-resistant layer, they are molded. The specific manufacturing process is as follows: S1. Blade substrate pretreatment: Select qualified Q460ME blade substrate and use a sandblasting + precision grinding composite process to clean the entire working surface of the blade. The cleaning range is 25mm from the boundary to thoroughly remove surface oxide scale, rolling oil stains, burrs and surface impurities, ensuring that the welding surface of the substrate is clean and the structure is uniform and stable.

[0071] S2. Stress easing groove machining: The arc-shaped stress easing groove is machined by CNC milling; the groove depth is 3.0mm, the groove width is 5mm, the longitudinal groove spacing is 20mm, the groove opening and bottom are uniformly transitioned with R1.5 arc, without sharp edges, and the groove body is smooth and continuous.

[0072] S3. Blade clamping and preheating: Place the 6mm high 5*5mm square blade at the center of the lower surface of the blade, then perform multi-point rigid clamping and positioning, and finally use manual flame preheating with the blade edge area at 90℃ and the weld overlay area at 110℃, with a heating rate of 4℃ / min.

[0073] S4. Adaptive Intelligent Path Planning: The six-axis linkage welding robot is equipped with a 3D vision scanning system to scan and model the entire blade area, accurately identifying the surface curvature, wall thickness distribution, and the position of the buffer groove. The robot adaptively generates a symmetrical staggered welding path with a single welding length of 50mm. It adopts a staggered welding trajectory with longitudinal first and transverse second, and welding layer first and buffer groove second. At the same time, it adaptively fine-tunes the welding gun swing amplitude and walking posture according to the preset arc of anti-deformation to avoid stress concentration areas.

[0074] S5. Root pass welding: Use Φ1.4mm high toughness transition welding wire and pulsed gas shielded welding process. First pass welding parameters: welding current 100A, welding voltage 19V, welding speed 9cm / min, single pass thickness 0.9mm.

[0075] S6. Interlayer temperature control and stress relief: After the single-segment, single-layer root pass welding is completed, it is naturally cooled to 80℃ before the ultra-hard wear-resistant layer welding is carried out. At the same time, during the cooling process, a flexible hammering process is used to uniformly hammer the weld, heat-affected zone and the periphery of the buffer groove to refine the metallographic structure, release the solidification residual tensile stress and suppress the accumulation of micro-deformation.

[0076] S7. Superhard wear-resistant layer welding: Φ1.4mm dry quenching coke special superhard wear-resistant alloy welding wire is used, and the layer welding is carried out in layers following the robot's preset symmetrical staggered path; surface layer welding parameters: current 120A, voltage 22V, welding speed 8cm / min, single layer welding thickness 1.0mm, total superhard welding thickness 6.0mm, after welding, the surface hardness is measured to be 60HRC, the hard phase is evenly distributed, and there are no defects such as pores, slag inclusions, or microcracks.

[0077] S8. Stress relief treatment: After the overlay welding is completed, the blade is allowed to cool naturally to room temperature. The tooling is removed, and the blade is placed in a heat preservation furnace and heated to 200°C at a uniform rate. After heat preservation for 2.5 hours, the blade is slowly cooled with the furnace to completely eliminate the residual stress superimposed by the multi-layer overlay welding and stabilize the blade substrate structure.

[0078] S9. Precision grinding with diamond wheels: Diamond wheels are used to perform surface grinding on the weld overlay area of ​​the blade to remove the surface oxide layer, weld beads and micro protrusions, correct the thickness deviation of the weld overlay layer, achieve a blade surface roughness of R3.2, ensure uniform surface flatness, and eliminate local stress concentration hard points.

[0079] S10. Low-temperature molding of blades: After grinding, blades are molded at 120℃ using a special curved mold.

[0080] S11. Grinding, Welding Repair, and Finished Product Inspection: After molding, the blades are fully inspected. For minor dents and missing parts, the same type of ultra-hard welding wire is used for precise welding repair. Then, the whole blades are finely ground and chamfered to eliminate stress concentration at the edges. Finally, a full-size re-inspection is carried out.

[0081] After the above treatment, the test results of the blade were as follows: the overall deformation of the blade was 0.22 mm / m, there were no warping or twisting defects, the weld overlay layer had no cracks or pores, the bonding strength met the standard, the wear resistance was 2.8 times higher than that of the substrate, and the vibration and noise of the equipment during operation met the standards.

[0082] As can be seen from the above specific implementation, the present invention can produce dry quenching fan blades with a strong weld overlay layer, uniform structure, and excellent wear and corrosion resistance.

[0083] In summary, the present invention has the following advantages over the prior art: First, the invention provides dual protection through structural stress relief and process control, resulting in extremely low deformation and high yield in mass production. This invention innovatively designs a pre-fabricated stress-relieving groove for structural stress relief, releasing the stress from the ultra-hard welding process in advance at the structural level. Combined with a robotic intelligent path for precise heat control, preheating, symmetrical staggered low-stress welding, and step-by-step stress relief in an integrated mass production process, it achieves bidirectional synergy between structural pre-control and process stability, completely solving the problems of deformation, end cracking, and surface defects in the mass production of ultra-hard welded thin-walled blades using dry-quenched coke. The overall deformation of blades produced using this invention is ≤0.3mm / m, far superior to the 1.5mm / m deformation index of traditional mass production processes. It also boasts high flatness accuracy, eliminating the need for extensive subsequent corrections and rework. The mass production yield is increased from approximately 70% to over 99%, significantly reducing mass production scrap costs.

[0084] Secondly, the ultra-hard surface layer exhibits uniform and stable performance, with excellent batch quality consistency: Utilizing automated robotic gradient heat input welding mass production technology, the ultra-hard wear-resistant layer of the blade is metallurgically fused to the substrate, resulting in a dense bond without mass production defects such as porosity, slag inclusions, microcracks, or interlayer delamination. The bonding strength is high, the hard phase is evenly distributed, and the surface hardness is stably maintained at 59~62HRC. It exhibits excellent high-temperature resistance, resistance to high-speed erosion by coke powder, and wear resistance, perfectly adapting to the extreme operating conditions of dry quenching blowers. The performance dispersion of single-batch mass-produced blades is extremely small, completely solving the problem of inconsistent quality in traditional manual mass production. The overall service life of the blades is 2-3 times longer than that of traditionally mass-produced blades.

[0085] Third, it features precision forming and excellent aerodynamic performance, resulting in high overall operational stability: The surface roughness and flatness of the blades are optimized through full-area precision grinding with diamond grinding wheels, eliminating welding peaks, oxide hard layers, and local stress concentration points. Combined with low-temperature static pressure molding for precision shaping, it thoroughly corrects minor surface deviations during mass production, resulting in regular aerodynamic shape and uniform wind resistance. The stability of fan operation vibration, noise, and air volume is significantly improved, effectively ensuring the long-term efficient and stable operation of the dry quenching coke unit.

[0086] Fourth, fully automated intelligent manufacturing with high mass production efficiency and low overall cost: It integrates fully automated production line processes such as substrate pretreatment, structured decompression, robotic intelligent welding, precision grinding, and low-temperature molding. The process linkage is strong and the parameter standardization is high, which greatly reduces manual correction, grinding, and rework processes, shortens the mass production cycle of a single blade, and ensures high consistency and standardization in batch production. The overall manufacturing cost is reduced by more than 30%, making it suitable for large-scale, precision intelligent manufacturing mass production of high-end dry quenching fan blades.

[0087] Fifth, the product has high reliability and wide adaptability: the mass-produced blades produced by this process have high dimensional accuracy, low structural stress, and excellent surface wear resistance. They are suitable for the extreme working conditions of dry quenching coke blowers with high temperature and high erosion, and can also be widely used in the precision manufacturing of high-end ventilation fan blades in many industries such as power, metallurgy, and chemical industry. The product has extremely strong versatility and market adaptability.

[0088] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.

[0089] The above descriptions are merely embodiments of the present invention. Commonly known structures and characteristics are not described in detail here. Those skilled in the art are aware of all common technical knowledge in the field prior to the application date or priority date, are aware of all existing technologies in that field, and have the ability to apply conventional experimental methods prior to that date. Those skilled in the art can, under the guidance of this application, improve and implement this solution in combination with their own capabilities. Some typical known structures or methods should not be obstacles for those skilled in the art to implement this application. It should be noted that those skilled in the art can make several modifications and improvements without departing from the structure of the present invention. These should also be considered within the scope of protection of the present invention, and will not affect the effectiveness of the implementation of the present invention or the practicality of the patent. The scope of protection claimed in this application should be determined by the content of its claims, and the specific embodiments described in the specification can be used to interpret the content of the claims.

Claims

1. An automatic surfacing welding method for low-deformation dry quenching fan blades, characterized in that, Includes the following steps: S1. Pre-treat the blades, the pre-treatment including non-destructive testing, grinding and surface treatment; S2. Perform stress relief groove processing in the area of ​​the blade to be welded; S3. Place the blade with the completed easing groove on the fixture, perform multi-point rigid clamping and positioning, perform reverse deformation pre-setting according to the blade thermal deformation law, press and fix it to fit the four-sided contour of the blade, and perform overall preheating after clamping. S4. Perform 3D scanning modeling on the blade after clamping and preheating, identify the boundary of the blade to be welded area and the position of the buffer groove, and generate a welding path plan. S5. Select transition welding wire and complete the first layer of root cladding welding of the weld seam and buffer groove in accordance with the cladding path planning. S6. Monitor the temperature of the weld and heat-affected zone in real time. After the temperature cools down to the preset temperature range naturally, use welding wire suitable for dry quenching conditions to perform surface layer welding. S7. After the welding is completed, a low-temperature stress-relieving heat treatment is performed, and a diamond grinding wheel is used to perform precision grinding on the welded area and the overall profile of the blade. S8. Use a blade curved surface molding die to perform low-temperature molding and shaping of the blade, detect defects in the molded blade, perform local repair welding on the defects, and perform overall fine grinding, polishing and smooth transition treatment on the repaired area. S9. Conduct a comprehensive re-inspection of the blades to ensure that all parameters meet the operating standards for extreme dry quenching conditions.

2. The automatic surfacing welding method for low-deformation dry quenching fan blades according to claim 1, characterized in that, Step S2 includes: The stress relief grooves are machined in the area of ​​the blade to be welded using a CNC milling integrated forming process. The stress relief grooves are evenly and equidistantly distributed at both ends of the weld seam, with a groove depth of 1.0-3.0mm and a groove width of 3.0-5.0mm. The bottom and opening of the groove are both transitioned with an arc of R1.5-R2.5, and the stress relief grooves are longitudinally spaced with a segment interval of 15-20mm.

3. The automatic overlay welding method for low-deformation dry quenching fan blades according to claim 1, characterized in that, Step S3 includes: A block of a set thickness is placed at the center of the lower surface of the blade, and the blade is fastened to the fixture with a long pressure plate to form a central protrusion structure for presetting the reverse deformation. Preheating is performed manually with a flame to set the heating rate, and real-time temperature control is achieved using an infrared thermometer. The temperature of the blade edge area is controlled at 80-100℃, and the temperature of the area to be welded is controlled at 100-120℃.

4. The automatic surfacing welding method for low-deformation dry quenching fan blades according to claim 1, characterized in that, Step S4 includes: A three-dimensional vision scanning system mounted on a six-axis linkage welding robot is used to perform three-dimensional scanning modeling on the blade after clamping and preheating, and to identify the boundary of the area to be welded and the position of the buffer groove. The area to be welded is divided into standard short welding units of a set length, generating a standardized welding trajectory that is intersecting, symmetrical, from the middle to the edge, and from the weld layer to the buffer groove. The welding torch posture, travel angle and swing amplitude are finely adjusted according to the different anti-deformation preset angles of the blades to obtain the welding path planning.

5. The automatic surfacing welding method for low-deformation dry quenching fan blades according to claim 1, characterized in that, Step S5 includes: The CMT pulsed gas shielded welding process was used for the root pass, and the heat input parameters were controlled. Among them, the first layer of underlay welding is carried out using a sinusoidal oscillating welding mode with a frequency and amplitude that meet the low stress effect. The height of the first layer of underlay welding in the buffer groove is 2 / 3 of the height of the buffer groove, and the thickness of subsequent single-layer underlay is controlled within the thickness range.

6. The automatic surfacing welding method for low-deformation dry quenching fan blades according to claim 1, characterized in that, Step S6 includes: After the root pass welding is completed, interpass temperature control is performed, and the maximum temperature of the interpass temperature control shall not exceed 100°C. During the cooling process, a flexible hammering process is used to uniformly and moderately hammer the root weld, heat-affected zone, and surrounding area of ​​the buffer tank until the temperature cools down to the preset temperature range.

7. The automatic surfacing welding method for low-deformation dry quenching fan blades according to claim 1, characterized in that, Step S6 includes: The surface layer is clad with welding wire adapted to dry quenching conditions. The diameter of the welding wire is 1.2-1.6 mm. After cladding, the hardness of the formed layer is 59-62 HRC, and the hard phase content exceeds 50%. Using welding wire with a diameter of 1.2-1.6mm and setting the surface layer welding parameters, layered welding is performed according to the symmetrical staggered path in the welding path planning. The thickness of a single layer is controlled within 0.8-1.2mm, and the total thickness of the layered welding is controlled within 5-10mm. The last layer adopts an 8-shaped oscillating welding mode. In the last layer of weld in the buffer groove, the welding current and voltage are increased by setting a window to make the weld surface smooth and defect-free. The surface layer welding parameters are: welding current of 110-1150A, welding voltage of 20-24V, and welding speed of 7-9cm / min.

8. The automatic surfacing welding method for low-deformation dry quenching fan blades according to claim 1, characterized in that, Step S7 includes: After the welding is completed, the blade is allowed to cool naturally indoors. The tooling fixtures are removed, and the blade is placed in a heat preservation furnace. The temperature is raised to 180-220℃ at a uniform rate and kept at that temperature for 2-3 hours before being slowly cooled in the furnace. A surface grinder equipped with a diamond grinding wheel is used to remove the surface oxide layer, weld slag, fine protrusions and rough peaks of the blade after welding, and the local thickness deviation of the weld layer is corrected by uniform grinding.

9. The automatic surfacing welding method for low-deformation dry quenching fan blades according to claim 1, characterized in that, Step S8 includes: Based on the standard surface parameters of the blade, the blade is molded and shaped under thermal stress-free conditions at 100-120℃ using a compression molding process. After low-temperature molding, the blades are subjected to comprehensive appearance, size and surface defect inspection. The original welding material parameters are matched, and the detected defects are locally repaired by welding. The repaired areas are then finely ground, polished and smoothed.

10. The automatic surfacing welding method for low-deformation dry quenching fan blades according to claim 1, characterized in that, Step S9 includes: The overall dimensional accuracy, surface profile, deformation, hardness of the weld overlay, and surface roughness of the blades were comprehensively re-inspected to ensure that the overall deformation of the blades was ≤0.3mm / m and that all parameters met the operating standards for extreme dry quenching conditions.