A nano cobalt particle multi-scale synergistically modified lead-free composite solder paste and a preparation method thereof

By introducing nano-cobalt powder into the SnAgCu solder system, a lead-free composite solder paste with multi-scale synergistic modification of nano-cobalt particles is formed, which solves the problem of insufficient mechanical reliability of lead-free solder paste under high temperature, high power and extreme environment, and achieves high strength, oxidation resistance and uniform IMC layer of solder joint, which is suitable for reliable interconnection of high-end electronic devices.

CN123128779APending Publication Date: 2026-11-20YINGDE CHUANGZHI NEW MATERIAL TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611646319.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-23
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing lead-free solder pastes lack mechanical reliability under high temperature, high power and extreme environments. Solder joints are prone to strength reduction and fatigue resistance due to microstructural instability. Furthermore, the intermetallic compound layer at the solder interface is uneven, making it difficult to meet the high reliability interconnect requirements of high-end electronic devices.

Method used

Introducing nano-cobalt powder into the SnAgCu solder system forms a lead-free composite solder paste with multi-scale synergistic modification of nano-cobalt particles. Through the metallurgical bonding of nano-cobalt particles and tin alloy powder, a high-melting-point intermetallic compound is formed, which refines the grains, improves the mechanical properties and wettability of the solder joint, and prevents nano-cobalt agglomeration through synergistic vacuum stirring.

Benefits of technology

It improves the mechanical properties and reliability of solder joints, enhances high-temperature resistance, improves high-temperature oxidation resistance, forms a uniform and smooth IMC layer, reduces the risk of solder joint cracking, and is suitable for electronic packaging in high-temperature, high-power and extreme environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128779A_ABST
    Figure CN123128779A_ABST
Patent Text Reader

Abstract

A lead-free composite solder paste with multi-scale synergistic modification by nano-cobalt particles and its preparation method are disclosed, relating to the field of soldering materials technology. The lead-free composite solder paste of this invention comprises the following components: 0.1-0.5% nano-cobalt powder, 85-92% SnAgCu solder powder, and 7.5-14.9% flux. The lead-free composite solder paste of this invention introduces nano-cobalt powder into the SnAgCu solder system, exhibiting excellent wetting properties and forming a more stable IMC layer interface, improving the mechanical properties and reliability of the solder joint, enhancing high-temperature resistance, improving high-temperature oxidation resistance, and increasing conductivity. It is suitable for electronic packaging scenarios in high-temperature, high-power, and extreme environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of soldering materials technology, specifically to a lead-free composite solder paste modified by multi-scale synergistic modification of cobalt nanoparticles and its preparation method. Background Technology

[0002] With the rapid development of the electronics and information industry, electronic packaging technology has placed increasingly stringent demands on the performance of solder paste. As a core material for achieving electrical connections and mechanical fixation in electronic devices, solder paste's wetting properties, mechanical reliability (such as solder joint strength and fatigue resistance), and electrical properties (such as conductivity and electromigration) directly determine the quality and lifespan of electronic products. Traditional tin-lead eutectic solder has a low melting point, good wettability, and high soldering quality and reliability. However, lead-containing solder paste, due to the high toxicity of lead, poses serious harm to the environment and human health, and its use has been restricted by regulations in most countries worldwide. Lead-free solder paste has become an inevitable trend in its development.

[0003] Among existing lead-free solder systems, SnAgCu (SAC) solder paste has become one of the most widely used lead-free solders due to its relatively suitable melting point, good soldering compatibility, and certain comprehensive performance. However, SAC solder paste has significant shortcomings in electronic packaging scenarios with high temperature, high power, and extreme environments: First, its mechanical reliability is insufficient. When solder joints are used for a long time or subjected to harsh environments such as temperature cycling and vibration, their strength and fatigue resistance are easily reduced due to microstructural instability. Second, the electrical performance stability caused by microcracks is difficult to meet the high reliability interconnection requirements of high-end electronic devices.

[0004] The morphology of the intermetallic compound (IMC) layer at the weld interface has a significant impact on the quality of the weld. Due to the special properties of welding materials, a coarse-grained and uneven IMC layer formed at the weld interface often reduces the reliability of the weld joint. Therefore, obtaining a weld interface of moderate thickness and uniform smoothness, and achieving precise control over the interface morphology, has become a core objective in the field of solder development.

[0005] Studies have shown that adding nano-metal particles can improve the wettability, mechanical properties, and electrical properties of solder. However, this approach often focuses on highlighting a single property such as mechanical properties or wettability, making it difficult to comprehensively solve the problems of existing technologies. Patent CN104014947A discloses a composite lead-free solder paste reinforced with nano-Ag3Sn particles and its preparation method. The solder paste is composed of nano-Ag3Sn particles and low-Ag lead-free solder paste. It focuses on the dispersion strengthening and suppression of coarsening of nano-Ag3Sn in the low-silver SnAgCu system to improve the mechanical properties of the solder joint. However, it does not address the regulation of the intermetallic compound layer at the copper substrate interface by nano-cobalt, nor does it address the high-temperature oxidation resistance of the solder joint. Therefore, it is necessary to develop a lead-free solder material with good wettability, capable of forming a uniform and smooth IMC layer interface, and improving the mechanical properties and reliability of the solder joint, suitable for electronic packaging applications in high-temperature, high-power, and extreme environments. Summary of the Invention

[0006] To address the technical problems in the prior art, this invention provides a lead-free composite solder paste modified by multi-scale synergistic modification of cobalt nanoparticles, forming a uniform and smooth IMC layer interface, thereby improving the mechanical properties and reliability of the solder joint.

[0007] Another object of the present invention is to provide a method for preparing the above-mentioned lead-free composite solder paste.

[0008] Another object of the present invention is to provide the application of the above-mentioned lead-free composite solder paste in the packaging of microelectronic devices.

[0009] This invention provides a lead-free composite solder paste modified by multi-scale synergistic modification of cobalt nanoparticles, comprising the following components by mass fraction: Nano cobalt powder 0.1~0.5%, SnAgCu solder powder 85~92%, flux 7.5~14.9%.

[0010] The lead-free composite solder paste of this invention introduces nano-cobalt powder into the SnAgCu solder system, which enhances mechanical properties, reduces surface tension, improves high-temperature resistance, enhances high-temperature oxidation resistance, and increases conductivity. It can suppress the excessive growth of brittle IMC layers (such as Cu6Sn5) at the copper substrate interface, forming a more stable (Cu,Co)6Sn5 compound, effectively reducing the risk of solder joint cracking. In temperature cycling (-40℃~150℃) impact tests, no microcracks were observed in the solder joints after 1000 cycles. It can be used in scenarios requiring compliance with automotive-grade AEC-Q100 standards and is suitable for wide-temperature cycling applications such as new energy vehicle motor controllers and SiC / GaN power modules.

[0011] Specifically, the lead-free composite solder paste of the present invention has the following advantages: (1) Enhanced mechanical properties: The nano-sized particles of the cobalt nanopowder have a large specific surface area and high activity. In solder paste, they can form a good metallurgical bond with tin alloy powder (SnAgCu solder powder). During the soldering process, the cobalt particles are dispersed in the tin alloy matrix as a reinforcing phase to form high-melting-point intermetallic compounds (such as CoSn2 and CoSn3), which hinder grain boundary movement and dislocation movement, thereby improving the strength and hardness of the solder joint. In addition, the nano-cobalt particles act as heterogeneous nucleation points, refine the tin grains, and improve the toughness of the solder joint, thereby enhancing the mechanical properties of the solder joint such as shear strength and tensile strength, making the solder joint more robust and reliable.

[0012] (2) Reduce surface tension: Nano-cobalt particles have high surface energy, which can reduce the surface tension of solder paste, making it easier for the solder paste to spread and wet the soldering surface. Good wettability helps to form uniform and dense solder joints, reduce the generation of defects such as cold solder joints and false solder joints, thereby improving the quality and reliability of soldering.

[0013] (3) Enhanced high-temperature resistance: Nano-cobalt particles can improve the high-temperature strength of solder joints. In some high-temperature working environments, the solder joint strength of ordinary solder paste will decrease significantly, while the solder joint formed by solder paste with added nano-cobalt particles can maintain good strength and stability at higher temperatures. The addition of Co can increase the recrystallization temperature of tin alloys and delay the softening and creep process of solder joints at high temperatures, thereby enhancing the high-temperature mechanical properties of solder joints.

[0014] (4) Improved high-temperature oxidation resistance: Nano-cobalt particles can form a protective layer in solder paste, preventing direct contact between the solder joint and the external environment, and slowing down the oxidation rate of the solder joint at high temperatures. Experiments show that the oxide layer thickness of SAC solder paste with added nano-Co is significantly reduced after aging at 150℃. The CoSn3 IMC layer inhibits further oxidation of Sn, thereby reducing the degree of oxidation of the solder joint at high temperatures and extending the service life of the solder joint.

[0015] (5) Improved conductivity: Cobalt is a good conductive metal. The addition of nano-cobalt particles can increase the conductive phase content in solder paste, thereby improving the conductivity of the solder paste. In the soldering of some electronic components with high conductivity requirements, such as the packaging and interconnection of integrated circuits and chips, the use of solder paste containing nano-cobalt powder can reduce the resistance of the solder joint and improve the efficiency and quality of signal transmission. Nano-cobalt particles can fill the tiny gaps and pores between the solder paste and the soldering surface during the soldering process, improve the microstructure of the solder joint, reduce defects and discontinuities in the solder joint, and thus reduce the contact resistance of the solder joint.

[0016] Preferably, the nano-cobalt powder is pre-dispersed in the flux and blended with SnAgCu solder powder in the lead-free composite solder paste. Pre-dispersing the nano-cobalt powder in the flux to form a nano-cobalt paste effectively prevents the agglomeration of nano-cobalt, allowing the nano-cobalt powder particles to be more uniformly dispersed in the composite solder paste. This facilitates the filling of tiny gaps and pores between the solder paste and the soldering surface during the soldering process, improving the microstructure of the solder joint and enhancing its reliability.

[0017] In some embodiments, the nano-cobalt powder is 0.1-0.45%, SnAgCu solder powder is 86-90%, and flux is 10-13%.

[0018] In some embodiments, the particle size of the cobalt nanoparticles is 1~100 nm.

[0019] In some embodiments, the chemical composition of the SnAgCu solder powder, by mass fraction, includes: 0.1%~4% Ag, 0.1%~1.2% Cu, with the balance being Sn and unavoidable impurities.

[0020] In some embodiments, the SnAgCu solder powder is selected from any one of SnAg3.0Cu0.5 solder powder (Ag 3.0 wt%, Cu 0.5 wt%, balance Sn), SnAg1.0Cu0.5 solder powder (Ag 1.0 wt%, Cu 0.5 wt%, balance Sn), and SnAg0.3Cu0.7 solder powder (Ag 0.3 wt%, Cu 0.7 wt%, balance Sn).

[0021] In some embodiments, the SnAgCu solder powder is spherical or near-spherical with a major-to-minor axis ratio of <1.2; the particle size is Type 4-7, such as Type 4, Type 5, Type 6 or Type 7, and the particle size refers to the industry standard IPC J-STD-005B.

[0022] In some embodiments, the flux is not particularly limited and can be a conventional flux in the field of soldering materials; for example, lead-free flux CPT-1001HF-S4 from Yingde Chuangzhi New Material Technology Co., Ltd. can be used.

[0023] This invention provides a method for preparing lead-free composite solder paste, comprising the following steps: S1, mix the nano-cobalt powder and flux evenly to obtain nano-cobalt slurry; S2, the nano-cobalt paste is mixed with SnAgCu solder powder and stirred evenly under vacuum to obtain the lead-free composite solder paste.

[0024] In some embodiments, step S1 specifically includes: premixing nano-cobalt powder with a first amount of flux, ultrasonically dispersing the mixture to obtain a premixed nano-cobalt slurry, and then mixing the premixed nano-cobalt slurry with a second amount of flux evenly to obtain a nano-cobalt slurry; wherein the mass ratio of the nano-cobalt powder to the first amount of flux is 1:(8~15), and the sum of the first amount and the second amount is the total amount of flux in the composite solder paste.

[0025] Preferably, the mass ratio of the nano-cobalt powder to the first amount of flux is 1:(9~12).

[0026] In some embodiments, the ultrasound duration is 10-30 minutes and the power is 200-400 W.

[0027] In some embodiments, in step S2, the vacuum degree of the vacuum stirring is ≤0.06MPa, preferably 0.02~0.06 MPa, the stirring speed is 20~35rpm, the stirring temperature is 23~26℃, and the stirring time is 20~30 min.

[0028] This invention provides the application of the lead-free composite solder paste or the lead-free composite solder paste prepared by the method thereof in the packaging of microelectronic devices.

[0029] The present invention has, but is not limited to, the following beneficial technical effects: The lead-free composite solder paste modified by multi-scale synergistic modification of nano-cobalt particles of the present invention introduces nano-cobalt powder into the SnAgCu solder system, which improves wettability and forms a more stable IMC layer interface, thereby improving the mechanical properties and reliability of the solder joint, enhancing high-temperature resistance, improving high-temperature oxidation resistance, and improving conductivity.

[0030] The preparation method of lead-free composite solder paste of the present invention involves pre-mixing nano-cobalt powder with flux to form nano-cobalt slurry, which effectively prevents the agglomeration of nano-cobalt and makes the nano-cobalt powder particles more uniformly dispersed in the composite solder paste; synergistic vacuum stirring can enhance the coating properties of flux, improve uniformity, and at the same time eliminate air bubbles, reduce voids inside the solder joint, and improve the reliability of the solder joint. Attached Figure Description

[0031] To clearly illustrate the specific embodiments of the present invention and certain detection techniques used in the experiments, the implementation schemes and the techniques used will be described below, mainly through the accompanying drawings.

[0032] Figure 1 The images show the solder creep and wetting patterns of the QFNPQFN pins of the composite solder paste prepared in Embodiment 1 and Comparative Example 1 of this invention; wherein, Figure 1 Figure a shows the solder creep and wetting pattern of the solder joint in Example 1. Figure 1 Figure b shows the solder creep and wetting diagram of the solder joint in Comparative Example 1.

[0033] Figure 2 Metallographic images of the IMC layer of the composite solder paste solder joints prepared in Example 1 and Comparative Example 1 of this invention; wherein, Figure 2 a is the metallographic image of the IMC layer of the solder joint in Example 1; Figure 2 b is the metallographic image of the IMC layer of the solder joint in Comparative Example 1.

[0034] Figure 3 These are comparative images showing solder joint voids in the ball grid array (BGA) packages of composite solder paste prepared in Example 1 and Comparative Example 1 of this invention; wherein, Figure 3 'a' is a diagram of the BGA solder joint void in Example 1. Figure 3 Figure b is a comparison image of the voids in the BGA solder joint of Comparative Example 1.

[0035] Figure 4 These are comparative cross-sectional images of the solder joints prepared in Example 1 and Comparative Example 1 of the present invention after 1000 temperature cycles (-40℃ to 150℃); wherein, Figure 4 'a' is a cross-sectional view of the weld joint after temperature cycling shock in Example 1. Figure 4 b is a cross-sectional view of the weld point after temperature cycling shock in Comparative Example 1.

[0036] Specific implementation methods The specific embodiments of the present invention are explained with the aid of examples. Except for the detection technology, which does not limit the present invention in any way, some of the solutions in the described embodiments are part of the embodiments of the invention. All embodiments obtained by ordinary people in the art without creative results are within the protection scope of the present invention. Example

[0037] A lead-free composite solder paste, comprising the following components by mass fraction: Nano cobalt powder 0.26%, SnAgCu solder powder 88.24%, flux 11.5%.

[0038] The particle size range of the nano-cobalt powder is 1~100 nm.

[0039] The SnAgCu solder powder is SnAg3.0Cu0.5 solder powder, with spherical or near-spherical particles, an aspect ratio of <1.2, and a particle size grade of Type 4. The flux is lead-free flux CPT-1001HF-S4 from Yingde Chuangzhi New Material Technology Co., Ltd.

[0040] The preparation method of lead-free composite solder paste in this embodiment includes the following steps: S1, 1.3g of nano cobalt powder is added to 13g of flux for premixing (the mass ratio of flux to nano cobalt powder is 10:1), and further ultrasonically dispersed (ultrasonic power 300 W, time 20 min) to form a premixed nano cobalt slurry; the premixed nano cobalt slurry is mixed and stirred evenly with 44.5g of flux to obtain nano cobalt slurry.

[0041] S2, add 441.2 g of SnAg3.0Cu0.5 solder powder to the nano-cobalt slurry and perform vacuum stirring at 23℃, vacuum degree 0.04 MPa, stirring speed 20 rpm, and stirring time 35 min. After stirring stops, open the vacuum valve. Once the pressure inside the stirrer reaches atmospheric pressure, open the lid to obtain 500 g of SnAgCu-Co composite solder paste. Store under refrigeration conditions of 0~10℃ and warm to 25℃ before use. Example

[0042] A lead-free composite solder paste, comprising the following components by mass fraction: Nano cobalt powder 0.1%, SnAgCu solder powder 88.4%, flux 11.5%.

[0043] The particle size range of the nano-cobalt powder is 1~100 nm.

[0044] The SnAgCu solder powder is SnAg1.0Cu0.5 solder powder, with spherical or near-spherical particles, an aspect ratio of <1.2, and a particle size grade of Type 5. The flux is lead-free flux CPT-1001HF-S4 from Yingde Chuangzhi New Material Technology Co., Ltd.

[0045] The preparation method of lead-free composite solder paste in this embodiment includes the following steps: S1, 0.5g of nano cobalt powder is added to 5g of flux for premixing (the mass ratio of flux to nano cobalt powder is 10:1), and further ultrasonically dispersed (ultrasonic power 300 W, time 20 min) to form a premixed nano cobalt slurry; the premixed nano cobalt slurry is mixed and stirred evenly with 52.5g of flux to obtain nano cobalt slurry.

[0046] S2, add 442g of SnAg1.0Cu0.5 solder powder to the nano-cobalt slurry and vacuum stir at 25℃, vacuum degree 0.06 MPa, stirring speed 30 rpm, and stirring time 25 min. After stirring stops, open the vacuum valve. Once the pressure inside the stirrer reaches atmospheric pressure, open the lid to obtain 500g of SnAgCu-Co composite solder paste. Store under refrigeration conditions of 0~10℃ and warm to 25℃ before use. Example

[0047] A lead-free composite solder paste, comprising the following components by mass fraction: Nano cobalt powder 0.44%, SnAgCu solder powder 88.06%, flux 11.5%.

[0048] The particle size range of the nano-cobalt powder is 1~100 nm. The SnAgCu solder powder is SnAg0.3Cu0.7 solder powder, with spherical or near-spherical particles, an aspect ratio of <1.2, and a particle size grade of Type 6. The flux is lead-free flux CPT-1001HF-S4 from Yingde Chuangzhi New Material Technology Co., Ltd.

[0049] The preparation method of lead-free composite solder paste in this embodiment includes the following steps: S1, 2.2g of nano cobalt powder is added to 22g of flux for premixing (the mass ratio of flux to nano cobalt powder is 10:1), and further ultrasonically dispersed (ultrasonic power 300 W, time 20 min) to form a premixed nano cobalt slurry; the premixed nano cobalt slurry is mixed with 35.5g of flux and stirred evenly to obtain a nano cobalt slurry.

[0050] S2, add 440.3g of SnAg0.3Cu0.7 solder powder to the nano-cobalt paste and perform vacuum stirring at 26℃, vacuum degree 0.02 MPa, stirring speed 20 rpm, and stirring time 30min. After stirring stops, open the vacuum valve. Once the pressure inside the stirrer reaches atmospheric pressure, open the lid to obtain 500g of SnAgCu-Co composite solder paste. Store under refrigeration conditions of 0~10℃ and warm to 25℃ before use. Example

[0051] A lead-free composite solder paste, comprising the following components by mass fraction: Nano cobalt powder 0.35%, SnAgCu solder powder 88.15%, flux 11.5%.

[0052] The particle size range of the nano-cobalt powder is 1~100 nm. The SnAgCu solder powder is SnAg0.3Cu0.7 solder powder, with spherical or near-spherical particles, an aspect ratio of <1.2, and a particle size grade of Type 6. The flux is lead-free flux CPT-1001HF-S4 from Yingde Chuangzhi New Material Technology Co., Ltd.

[0053] The preparation method of lead-free composite solder paste in this embodiment includes the following steps: S1, 1.75g ​​of nano cobalt powder is added to 17.5g of flux for premixing (the mass ratio of flux to nano cobalt powder is 10:1), and further ultrasonically dispersed (ultrasonic power 300 W, time 20 min) to form a premixed nano cobalt slurry; the premixed nano cobalt slurry is mixed with 40.0g of flux and stirred evenly to obtain nano cobalt slurry.

[0054] S2, add 440.75g of SnAg0.3Cu0.7 solder powder to the nano-cobalt slurry and vacuum stir at 26℃, vacuum degree 0.02 MPa, stirring speed 20 rpm, and stirring time 30min. After stirring stops, open the vacuum valve. Once the pressure inside the stirrer reaches atmospheric pressure, open the lid to obtain 500g of SnAgCu-Co composite solder paste. Store under refrigeration conditions of 0~10℃ and warm to 25℃ before use.

[0055] Comparative Example 1 A lead-free composite solder paste, which differs from Example 1 in that: this comparative example does not contain nano-cobalt powder.

[0056] Specifically, the lead-free composite solder paste of this comparative example comprises the following components by mass fraction: SnAg3.0Cu0.5 solder powder 88.5%, flux 11.5%.

[0057] The method for preparing the lead-free composite solder paste includes the following steps: 57.5g of flux and 442.5g of SnAg3.0Cu0.5 solder powder were stirred at 23℃, under a vacuum of 0.04 MPa, at a stirring speed of 20 rpm for 35 minutes. After stirring was stopped, the vacuum valve was opened, and the lid was opened once the pressure inside the stirrer reached atmospheric pressure. 500g of SnAgCu composite solder paste was obtained and stored at 0~10℃. It should be warmed to 25℃ before use.

[0058] Performance testing The lead-free composite solder pastes of Examples 1-4 and Comparative Example 1 were subjected to the following performance tests, and the results were as follows: Figure 1-4 As shown in Table 1.

[0059] Table 1

[0060] 1. Welding quality inspection See Figure 1 The solder crawling and wetting diagrams of the QFN pins in Example 1 show that the QFN pins of the chip are completely wetted in the composite SnAgCu-Co solder paste, with no solder shrinkage. Figure 1a). In Comparative Example 1, the root of the QFN pin of the SnAgCu solder paste exhibits poor wetting ( Figure 1 b).

[0061] 2. Metallographic characterization of the IMC layer See Figure 2 The metallographic images of the IMC layer show that the IMC layer interface of the composite SnAgCu-Co solder paste in Example 1 is more uniform and smooth, with finer grains and a thickness ranging from 0.693 to 1.98 μm; while the IMC layer interface of the composite SnAgCu solder paste in Comparative Example 1 is uneven in thickness, with coarser grains and a thickness ranging from 0.891 to 4.55 μm.

[0062] 3. Internal defect detection See Figure 3 The solder paste BGA solder joint diagram shows that the BGA solder joints of the composite SnAgCu-Co solder paste in Example 1 have almost no voids (void rate <0.1%) as detected by X-ray; while the BGA solder joints of the SnAgCu solder paste in Comparative Example 1 have small voids, with a BGA solder joint void rate of 3.9%.

[0063] 4. Reliability Testing See Figure 4 Cross-sectional images of solder joints after 1000 temperature cycling (-40℃~150℃) were observed using a crystal microscope. No microcracks were observed in the solder joints of the composite SnAgCu-Co solder paste in Example 1 after 1000 high and low temperature cycles of -40℃~150℃. However, obvious cracks appeared in the solder joints of the SnAgCu solder paste in Comparative Example 1 after 1000 high and low temperature cycles of -40℃~150℃.

[0064] The above description is only a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A lead-free composite solder paste with multi-scale synergistic modification by cobalt nanoparticles, characterized in that, By mass fraction, it includes the following components: Nano cobalt powder 0.1~0.5%, SnAgCu solder powder 85~92%, flux 7.5~14.9%.

2. The lead-free composite solder paste according to claim 1, characterized in that, Nano cobalt powder 0.1~0.45%, SnAgCu solder powder 86-90%, flux 10~13%.

3. The lead-free composite solder paste according to claim 1, characterized in that, The chemical composition of the SnAgCu solder powder, by mass fraction, includes: Ag 0.1%~4%, Cu 0.1%~1.2%, with the balance being Sn and unavoidable impurities.

4. The lead-free composite solder paste according to claim 1, characterized in that, The SnAgCu solder powder is selected from any one of SnAg3.0Cu0.5 solder powder, SnAg1.0Cu0.5 solder powder, and SnAg0.3Cu0.7 solder powder.

5. The lead-free composite solder paste according to any one of claims 1, 3-4, characterized in that, The SnAgCu solder powder is spherical or near-spherical with a major-to-minor axis ratio of <1.2; the particle size grade is Type 4-7, which refers to the industry standard IPC J-STD-005B.

6. A method for preparing lead-free composite solder paste with multi-scale synergistic modification of cobalt nanoparticles as described in any one of claims 1-5, characterized in that, Includes the following steps: S1, mix the nano-cobalt powder and flux evenly to obtain nano-cobalt slurry; S2, the nano-cobalt paste is mixed with SnAgCu solder powder and stirred evenly under vacuum to obtain the lead-free composite solder paste.

7. The preparation method according to claim 6, characterized in that, Step S1 specifically includes: premixing nano-cobalt powder with a first amount of flux, ultrasonically dispersing to obtain a premixed nano-cobalt slurry, and then mixing the premixed nano-cobalt slurry with a second amount of flux evenly to obtain a nano-cobalt slurry; wherein, the mass ratio of the nano-cobalt powder to the first amount of flux is 1:(8~15), and the sum of the first amount and the second amount is the total amount of flux in the composite solder paste.

8. The preparation method according to claim 7, characterized in that, The ultrasound duration is 10-30 minutes, and the power is 200-400 W.

9. The preparation method according to claim 6, characterized in that, In step S2, the vacuum degree of the vacuum stirring is ≤0.06MPa, the stirring speed is 20~35rpm, the stirring temperature is 23~26℃, and the stirring time is 20~30min.

10. The application of a lead-free composite solder paste prepared by the method of preparing the lead-free composite solder paste with multi-scale synergistic modification of cobalt nanoparticles as described in any one of claims 1-5 or claims 6-9 in the packaging of microelectronic devices.

Citation Information

Patent Citations

  • Nanometer Ag3Sn particle reinforced composite lead-free soldering paste and preparation method thereof

    CN104014947A