TC4 flux-cored wire, preparation method and application thereof
By using TC4 flux-cored welding wire with flux-cored powder inside the TC4 titanium alloy outer sheath, pre-oxidized hydrogenated titanium powder decomposes to form bubbles at the front end of the molten pool, combined with calcium oxide and rare earth oxides to stabilize the pores, boron powder to refine the grains, and calcium fluoride to purify the molten pool, the problem of porous titanium alloy preparation in the prior art has been solved, and efficient and uniform porous titanium alloy preparation has been achieved.
Patent Information
- Application Number
- CN202611632947.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-21
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies lack flux-cored welding wires for the TC4 titanium alloy system, making it impossible to achieve uniform flux filling and stable composition. Furthermore, it is difficult to achieve integrated preparation of porous titanium alloys through gradient segmentation via additive manufacturing.
TC4 flux-cored welding wire with a TC4 titanium alloy outer sheath and a flux-cored powder filling is used. The flux-cored powder composition includes TC4 alloy powder, pre-oxidized hydrogenated titanium powder, calcium oxide, rare earth oxides, boron powder, and calcium fluoride. The pre-oxidized hydrogenated titanium powder decomposes and releases hydrogen to form bubbles at the front end of the molten pool. Combined with calcium oxide and rare earth oxides, the pores are stabilized. The boron powder refines the grains, and the calcium fluoride purifies the molten pool, thus realizing the preparation of porous titanium alloy.
A porous titanium alloy with round and uniformly distributed pores was obtained, which significantly improved material utilization and forming efficiency. It can form large-size and suspended complex structures, and achieve continuous forming of dense load-bearing layer, transition layer and porous functional layer in additive manufacturing.
Smart Images

Figure CN123128784A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of additive manufacturing materials and welding material preparation technology, specifically relating to a TC4 flux-cored welding wire, its preparation method and application. Background Technology
[0002] Porous titanium alloys combine the high specific strength and corrosion resistance of titanium alloys with the low density, low elastic modulus, and high permeability of porous structures, making them important candidate materials for medical implants (bone ingrowth, vascularization), lightweight load-bearing structures, and energy-absorbing structures. Taking TC4 (Ti-6Al-4V) alloy as an example, dense TC4 has an elastic modulus of approximately 110 GPa, far exceeding the 10-30 GPa of human cortical bone, resulting in a stress-shielding effect after implantation. In contrast, porous TC4 with a porosity of 40%-60% can reduce its elastic modulus to 10-25 GPa, matching that of cortical bone. Simultaneously, the pores provide channels for bone tissue ingrowth, enabling long-term biological fixation. The service performance of porous titanium alloys is highly dependent on the controllability of porosity, pore size, open porosity, pore shape, and the metallurgical quality of the pore walls.
[0003] Traditional methods for preparing porous titanium alloys mainly involve powder metallurgy: titanium powder is mixed with spacer particles (such as sodium chloride or urea particles), pressed, sintered, and then the spacer particles are dissolved. This method has many steps, a long cycle, and is limited by molds, making it difficult to form complex shapes. Furthermore, the spacer particles are not completely dissolved, leaving impurities.
[0004] Existing technologies lack flux-cored wires for additive manufacturing that are designed for the TC4 titanium alloy system, use flux-cored wires as carriers, and create in-situ pores based on the hydrogen dissolution-precipitation mechanism. There is also a lack of flux-cored wire preparation methods that can ensure uniform flux filling, stable composition, and achieve integrated gradient segmentation. Summary of the Invention
[0005] The purpose of this invention is to provide a TC4 flux-cored welding wire, its preparation method, and its application. The provided TC4 flux-cored welding wire consists of a TC4 titanium alloy outer sheath and flux powder filling the TC4 titanium alloy outer sheath. The flux powder comprises TC4 alloy powder, pre-oxidized hydrogenated titanium powder, calcium oxide, rare earth oxides, boron powder, and calcium fluoride; wherein the pre-oxidized hydrogenated titanium powder acts as a foaming component to induce hydrogen pores, calcium oxide and rare earth oxides act as pore-stabilizing components, boron powder acts as a refining component, and calcium fluoride acts as a slag-forming and purifying component. In use, the pre-oxidized hydrogenated titanium powder decomposes and releases hydrogen at the front end of the molten pool. The hydrogen dissolves into the liquid titanium molten pool and, upon solidification, is supersaturated and precipitates as bubbles. These bubbles are captured by the solidification front to form spherical micropores, thereby obtaining a porous titanium alloy.
[0006] To achieve the above objectives, the present invention provides the following technical solution: One of the technical solutions of the present invention is to provide a TC4 flux-cored welding wire, which is composed of a TC4 titanium alloy outer sheath and flux powder filled in the TC4 titanium alloy outer sheath; the composition of the flux powder, in addition to TC4 alloy powder, includes, by mass percentage: 5%~20% pre-oxidized hydrogenated titanium powder, 1%~6% calcium oxide, 0.5%~3% rare earth oxides, 0.05%~0.3% boron powder and 0.5%~2% calcium fluoride; the flux powder accounts for 12%~25% of the total mass of the TC4 flux-cored welding wire.
[0007] In the core powder of the present invention, pre-oxidized titanium dioxide powder is used as a foaming component to induce hydrogen pores, calcium oxide and rare earth oxides are used as pore-stabilizing components, boron powder is used as a refining component, and calcium fluoride is used as a slag-forming and purification component.
[0008] A schematic diagram illustrating the mechanism of hydrogen-induced porosity in pre-oxidized titanium dioxide powder in the core powder is shown below. Figure 1 .
[0009] A schematic diagram illustrating the synergistic pore-stabilizing and strengthening mechanism of the components in the core powder is shown below. Figure 2 .
[0010] When the filling rate of the core powder is less than 12%, the core powder is prone to flow interruption and local powder absence after drawing. When it is higher than 25%, it is difficult to close the joint and the risk of wire breakage during drawing increases.
[0011] Preferably, the pre-oxidized titanium hydride powder is obtained by treating titanium hydride powder in air at 450~520℃ for 1~3 hours.
[0012] After titanium hydride powder is pre-oxidized in air at 450~520℃, a TiO2 shell is formed on its surface, which increases the decomposition initiation temperature from about 400℃ to 560~650℃, thus preventing the welding wire from decomposing and releasing hydrogen prematurely when it is fed into the heating section; at the same time, the pre-oxidized shell also has a passivation effect, improving the storage stability of the core powder.
[0013] Preferably, the rare earth oxide is selected from one or more of lanthanum oxide, cerium oxide, and yttrium oxide.
[0014] Preferably, the diameter of the TC4 flux-cored welding wire is 1.0~2.0mm; the diameter of the segmented TC4 flux-cored welding wire is 1.0~2.0mm; and the thickness of the TC4 titanium alloy outer sheath is 0.25~0.4mm.
[0015] Preferably, the pre-oxidized titanium dioxide powder has a mass percentage of 8% to 15% and a particle size of 20 to 120 μm.
[0016] The content of pre-oxidized hydrogenated titanium powder in the flux-cored wire primarily controls porosity, while particle size primarily controls pore size. Orthogonal control of these two parameters allows for the control of porosity in porous titanium alloys made with TC4 flux-cored wire to range from 14% to 65%, with an average pore size of 80 to 400 μm. The content and particle size of the pre-oxidized hydrogenated titanium powder are independently adjustable, and fine-tuning can be achieved with linear energy density assistance, resulting in a wide process window.
[0017] The second technical solution of the present invention provides a segmented TC4 flux-cored welding wire, which is composed of a TC4 titanium alloy outer sheath and flux powder segmented and filled within the TC4 titanium alloy outer sheath; the flux powder is divided into dense segments, transition segments and porous segments along the wire length direction. In addition to TC4 alloy powder, the core powder of the dense section also includes, by mass percentage: no more than 1% pre-oxidized titanium dioxide powder, 1%~6% calcium oxide, 0.5%~3% rare earth oxides, 0.05%~0.3% boron powder, and 0.5%~2% calcium fluoride; In addition to TC4 alloy powder, the core powder of the transition section, by mass percentage, also includes: 1%~8% pre-oxidized titanium dioxide powder, 1%~6% calcium oxide, 0.5%~3% rare earth oxides, 0.05%~0.3% boron powder, and 0.5%~2% calcium fluoride; In addition to TC4 alloy powder, the porous core powder composition, by mass percentage, includes: 8%~20% pre-oxidized titanium dioxide powder, 1%~6% calcium oxide, 0.5%~3% rare earth oxides, 0.05%~0.3% boron powder, and 0.5%~2% calcium fluoride; The flux-cored powder in each segment accounts for 12% to 25% of the total mass of the segmented TC4 flux-cored welding wire.
[0018] In this invention, the length of each segment of the segmented TC4 flux-cored welding wire is determined according to the part slicing path planning.
[0019] A schematic diagram of the cross-sectional structure of the segmented TC4 flux-cored welding wire in this invention is shown below. Figure 3 ; where (a) is the cross section and (b) is the longitudinal section.
[0020] In the figure, 1-TC4 metal outer skin, 2-TC4 alloy powder, 3-pre-oxidized TiH2 powder, 4-pore-stabilizing component (CaO / rare earth oxide), 5-refining / purifying component (B / CaF2).
[0021] Preferably, the pre-oxidized titanium hydride powder is obtained by treating titanium hydride powder in air at 450~520℃ for 1~3 hours.
[0022] Preferably, the rare earth oxide is selected from one or more of lanthanum oxide, cerium oxide, and yttrium oxide.
[0023] Preferably, the diameter of the segmented TC4 flux-cored welding wire is 1.0~2.0mm; and the thickness of the TC4 titanium alloy outer sheath is 0.25~0.4mm.
[0024] The third technical solution of the present invention provides a method for preparing the above-mentioned TC4 flux-cored welding wire or the above-mentioned segmented TC4 flux-cored welding wire, comprising the following steps: The flux-cored powder prepared according to the specified ratio is filled into a U-shaped tube made of TC4 titanium alloy strip, the tube is closed, and it is drawn to the target welding wire diameter through multiple passes to obtain the TC4 flux-cored welding wire or the segmented TC4 flux-cored welding wire.
[0025] Preferably, the single-pass diameter reduction rate of the multi-pass drawing is 10%~15%.
[0026] Preferably, a wire drawing lubricant is used during drawing, and the ellipticity of the welding wire after drawing is not greater than 0.05 mm.
[0027] The fourth technical solution of the present invention provides an application of the above-mentioned TC4 flux-cored welding wire or the above-mentioned segmented TC4 flux-cored welding wire in the preparation of porous titanium alloys.
[0028] The beneficial technical effects of the present invention are as follows: The TC4 flux-cored welding wire of this invention utilizes a hydrogen dissolution-precipitation pore-forming mechanism to achieve superior pore shape. Pre-oxidized TiH2 powder decomposes and releases hydrogen in an atomic state into the liquid titanium molten pool. During solidification, the solubility of the solid phase drops sharply, leading to supersaturation and precipitation. The resulting bubbles are small, dispersed, and have rounded pores (sphericity not less than 0.85) with uniform distribution, significantly different from the large bubbles formed by direct gas generation from foaming agents in steel and aluminum systems. The decomposition product, elemental titanium, is homogeneous with the matrix and free from inclusions and contamination. Calcium oxide increases melt viscosity, inhibiting bubble escape and merging; rare earth oxides purify grain boundaries and refine pore wall structure; boron forms TiB, refining β-grains; and calcium fluoride adsorbs inclusions and floats them upwards. The pore wall exhibits high metallurgical quality and a compressive strength not less than 180 MPa.
[0029] The TC4 flux-cored welding wire of the present invention can be integrated for hole creation, eliminating the need for powder mixing and powder laying. The utilization rate of laser wire feeding deposition material is not less than 95%, and it can form large-size and suspended complex structures. The forming efficiency is significantly higher than that of the powder route.
[0030] The segmented TC4 flux-cored welding wire of the present invention is filled with flux powder in segments along the wire length, including dense segment, transition segment and porous segment. The segment boundaries remain clear after drawing, which can realize the continuous forming of dense bearing layer, transition layer and porous functional layer in one additive manufacturing process.
[0031] This invention enables continuous and uninterrupted flow of the core material through a process of U-shaped coiling + quantitative filling + joining + multi-pass drawing, meeting the stable use requirements of continuous wire feeding additive manufacturing. Attached Figure Description
[0032] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0033] Figure 1 This is a schematic diagram illustrating the mechanism of hydrogen-induced porosity in the pre-oxidized titanium dioxide powder of the TC4 flux-cored wire of the present invention.
[0034] Figure 2 This is a schematic diagram illustrating the synergistic pore-stabilizing and strengthening mechanism of the components in the core powder of the TC4 flux-cored welding wire of the present invention.
[0035] Figure 3 This is a schematic diagram of the cross-sectional structure of the segmented TC4 flux-cored welding wire in this invention; where (a) is the cross-section and (b) is the longitudinal section.
[0036] Figure 3 In the composition, 1-TC4 metal outer skin, 2-TC4 alloy powder, 3-pre-oxidized TiH2 powder, 4-pore-stabilizing component (CaO / rare earth oxide), 5-refining / purifying component (B / CaF2).
[0037] Figure 4 This is a schematic diagram illustrating the principle of preparing TC4 porous titanium alloy using laser-directed energy deposition.
[0038] Figure 5 SEM image (a) and EDS scan image (b) of Ti element in the SEM image of the porous titanium alloy prepared in Example 1 of the present invention.
[0039] Figure 6 The relationship between the content of pre-oxidized hydrogenated titanium powder and the porosity of porous titanium alloy in the TC4 flux-cored wire of the present invention (a) and the relationship between the particle size of pre-oxidized hydrogenated titanium powder and the pore size of porous titanium alloy (b) are shown. Detailed Implementation
[0040] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention. It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the present invention.
[0041] It should be noted that any aspects not described in detail in this invention are conventional practices in the field and are not the focus of this invention.
[0042] Furthermore, regarding the numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Any stated value or intermediate value within a stated range, as well as each smaller range between any other stated value or intermediate value within said range, are also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0043] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar to or equivalent to those described herein may be used in the implementation or testing of this invention.
[0044] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0045] This invention provides a method for preparing TC4 flux-cored welding wire, the steps of which are as follows: Select TC4 titanium alloy strip with a thickness of 0.25~0.4mm, clean and degrease it, and then cut it longitudinally. Weigh each component according to the proportions in Table 1, and mix them in a powder mixer for 0.5~2h to obtain the core powder. Among them, the titanium hydride powder is pre-oxidized in air atmosphere before use (pre-oxidation conditions can be within the range of 450~520℃ and 1~3h), and the calcium oxide is dried at 800℃ for 2h before use to remove water. After the strip is formed into a U-shape by the coiling roll, the core powder is quantitatively filled into the tube (filling rate 12%~25%). After the joint is closed, it is drawn and reduced in diameter in 3~8 passes (single pass reduction rate 10%~15%, using wire drawing lubricant) to a diameter of 1.0~2.0mm and then wound up. The ellipticity of the obtained welding wire is not greater than 0.05mm, and the core filling is continuous and without interruption.
[0046] This invention also provides a method for preparing segmented TC4 flux-cored welding wire. The only difference from the preparation steps of TC4 flux-cored welding wire is that the flux powder is filled in segments, and the content of titanium hydride powder in each segment of the flux powder is different. During filling, the dense segment (titanium hydride powder not exceeding 1 wt%), the transition segment (titanium hydride powder 1 wt%~8 wt%), and the porous segment (titanium hydride powder 8 wt%~20 wt%) of flux powder are sequentially filled along the wire length. The length of each segment is determined according to the part slicing path planning.
[0047] Table 1 Table 2 Explanation of the hole-forming mechanism during welding wire use: Pre-oxidized titanium hydride decomposes into hydrogen (TiH2→Ti+H2↑) at the front of the molten pool in the temperature range of 560~650℃. The decomposition product, elemental titanium, is homogeneous with the matrix. The solubility of hydrogen in liquid titanium is more than 10 times that in solid titanium. Atomic hydrogen is uniformly dissolved into the molten pool. During solidification, the solubility of the solid phase drops sharply, and hydrogen precipitates as H2 bubbles at the supersaturation front of solidification. These bubbles are captured by the dendritic network and form spherical micropores. Explanation of the stabilization mechanism: Calcium oxide increases the viscosity of the melt, reduces the bubble rising speed, and prolongs the bubble residence time in the molten pool. Rare earth oxides agglomerate at grain boundaries, purifying the grain boundaries and acting as heterogeneous nucleation cores to refine the pore wall structure. Boron forms TiB, refining β grains and strengthening the pore walls. Calcium fluoride adsorbs oxide inclusions in the molten pool and floats them to the surface, ensuring the metallurgical quality of the pore walls. In use, laser-guided energy deposition can be used to melt and deposit flux-cored welding wire to form porous titanium alloy structural parts. Exemplary process parameters are: laser power 800~2000W, spot diameter 1~3mm, scanning speed 4~15mm / s, wire feed speed 0.6~2.5m / min, linear energy density 80~350J / mm, and interlayer temperature not exceeding 200℃. If the linear energy density is too low, the foaming agent will not be fully activated and incomplete fusion defects are likely to occur. If it is too high, the molten pool will overheat, and bubbles will grow and escape, both of which will cause the pore structure to become uncontrolled.
[0048] A schematic diagram illustrating the principle of preparing TC4 porous titanium alloy using laser-directed energy deposition is shown below. Figure 4 .
[0049] Example 1 Preparation and application effects of TC4 flux-cored welding wire: A 0.35mm thick TC4 strip is used as the outer sheath. The core powder, by mass percentage, consists of: 12% TiH2 powder (particle size 45~75μm) pre-oxidized in air at 500℃ for 2 hours, 3% CaO (dried at 800℃ for 2 hours before use), 1.5% La2O3, 0.1% B, 1% CaF2, and the balance being TC4 alloy powder. The core powder is mixed in a powder mixer for 1 hour. After the strip is formed into a U-shaped tube by a coiling roller, the core powder is quantitatively filled (the core powder accounts for 18% of the total mass of the welding wire). After the joint is closed, the wire is drawn in 6 passes to reduce the diameter to 1.6mm (the diameter reduction rate per pass is approximately 12%), and then wound up to obtain the flux-cored welding wire. The ellipticity of the obtained welding wire is 0.03mm, and longitudinal section inspection shows that the core filling is continuous and uniform. Laser-guided energy deposition (LAD) was performed using this welding wire (laser power 1200W, spot diameter 2mm, scanning speed 6mm / s, wire feed speed 1.2m / min, argon protection) to form cylindrical specimens with a diameter of 10mm and a height of 15mm. Testing revealed that the formed porous titanium alloy had a porosity of 45%, pore size of 120~280μm (average 180μm), pore sphericity of 0.87, open porosity of 55%, compressive strength of 195MPa, elastic modulus of 18GPa, and the pore wall microstructure consisted of fine acicular α′ martensite and dispersed TiB phases, indicating good metallurgical quality. The SEM image (a) and EDS scan image (b) of the Ti element in the SEM image of the prepared porous titanium alloy are shown below. Figure 5 .
[0050] Example 2 The effect of pre-oxidized hydrogenated titanium powder content on porosity control: Using the same outer sheath, wire diameter, core powder ratio, preparation method, and application process as Example 1, only the content of pre-oxidized TiH2 powder in the core powder was changed (the remainder was supplemented with TC4 alloy powder): when the TiH2 content was 5%, 8%, 12%, 15%, and 20%, the porosity was 14%, 26%, 45%, 56%, and 63%, respectively (see Table 3). The porosity showed an approximately linear relationship with the TiH2 content (porosity ≈ 3.2 × TiH2 content % + 1). This indicates that the porosity is mainly controlled by the TiH2 content.
[0051] Table 3 Example 3 Control of pore size by pre-oxidized hydrogenated titanium powder particle size: Similar to Example 1, the content of pre-oxidized TiH2 powder was fixed at 12 wt%, with only the TiH2 particle size changed: for particle sizes of 20~45 μm, 45~75 μm, and 75~120 μm, the average pore sizes were 90 μm, 180 μm, and 290 μm, respectively, while the porosity remained basically unchanged (43%~46%, see Table 4). This indicates that the pore size is mainly controlled by the TiH2 particle size, and the content and particle size parameters achieve orthogonal regulation of porosity and pore size.
[0052] Table 4 The relationship between the content of pre-oxidized hydrogenated titanium powder and the porosity of porous titanium alloy in the TC4 flux-cored welding wire of the present invention (a) and the relationship between the particle size of pre-oxidized hydrogenated titanium powder and the pore size of porous titanium alloy (b) are shown in [reference needed]. Figure 6 .
[0053] Example 4 Preparation and application effects of segmented TC4 flux-cored welding wire: A 0.35mm thick TC4 tape was used as the outer skin. During filling, the core powder was sequentially and quantitatively filled along the filament length into the dense section (0.5wt% pre-oxidized TiH2 content), the transition section (6wt% pre-oxidized TiH2 content), and the porous section (12wt% pre-oxidized TiH2 content). The pre-oxidation treatment of TiH2 content was the same as in Example 1, and the other components were the same as in Example 1. The length of each section was determined according to the part slicing path planning. In this case, a single-wall simulation part with a length of 150mm and a width of 20mm was used for slicing path planning. The single-layer deposition path length was 150mm, and the single-layer deposition height was 1.5mm. The bottom dense bearing layer was set to 8 layers, the middle transition layer to 4 layers, and the top porous functional layer to 8 layers, for a total of 20 layers and a total height of about 30mm. Based on a wire feed speed of 1.0 m / min and a scanning speed of 5 mm / s, the ratio of wire consumption length to deposition path length is (1.0 × 1000 / 60) / 5 ≈ 3.33, meaning that approximately 3.33 mm of wire is consumed for every 1 mm of deposition path. Therefore, each layer consumes approximately 150 × 3.33 = 500 mm of wire. Theoretically, the dense section requires 8 × 500 = 4000 mm of wire, the transition section requires 4 × 500 = 2000 mm, and the porous section requires 8 × 500 = 4000 mm, for a theoretical total consumption of 10000 mm. Considering arc initiation, arc termination, clamping, and a 10% process allowance, the actual total length of the segmented TC4 flux-cored wire prepared in this study is 11000 mm, including 4400 mm for the dense section, 2200 mm for the transition section, and 4400 mm for the porous section. The total filler content of the flux-cored powder in each segment is 18 wt%, consistent with Example 1. The dense section of the flux-cored wire contains 0.5 wt% pre-oxidized TiH2, the transition section contains 6 wt%, and the porous section contains 12 wt%. The remaining components are the same as in Example 1, namely 3 wt% CaO, 1.5 wt% La2O3, 0.1 wt% B, 1 wt% CaF2, with the balance being TC4 alloy powder. The pre-oxidized TiH2 powder has a particle size of 45–75 μm, and the pre-oxidation conditions are air treatment at 500℃ for 2 hours. After joining, the wire is drawn in 6 passes to reduce the diameter to 1.6 mm, and then wound into segmented flux-cored wires. Longitudinal section inspection shows clear segment boundaries and no cross-contamination of the core powder. Laser-directed energy deposition (laser power 1100 W, spot diameter 2 mm, scanning speed 5 mm / s, wire feed speed 1.0 m / min) is performed using this wire to continuously form a bottom dense support layer, a middle transition layer, and a top porous functional layer in a single deposition process. Testing revealed that the dense layer of the fabricated porous titanium alloy has a porosity of 1.2% and a compressive strength of 985 MPa; the porous layer has a porosity of 45% and a compressive strength of 195 MPa; the porosity of the transition layer varies continuously along the thickness direction; the dense layer and the porous layer are metallurgically bonded; and metallographic examination of the interface revealed no cracks or lack of fusion defects. This structure is suitable for interbody fusion devices, femoral stem implants, and other implants that combine load-bearing and bone ingrowth functions.
[0054] Comparative Example 1 Titanium hydride-free flux-cored welding wire: The preparation method and usage process were the same as in Example 1, except that TiH2 was not included in the core powder (it was replaced with an equal amount of TC4 alloy powder). The resulting porous titanium alloy had a porosity of only 1.5% and a compressive strength of 970 MPa, exhibiting a dense structure, indicating that the pores were mainly decomposed by titanium hydride to explain the hydrogen contribution.
[0055] Comparative Example 2 Titanium hydride without pre-oxidation treatment: Similar to Example 1, the only difference is that the TiH2 was not pre-oxidized. Since the decomposition initiation temperature of the unoxidized TiH2 is approximately 400°C, lower than the 560-650°C after pre-oxidation, it decomposes and releases hydrogen prematurely as soon as the welding wire enters the heating section. The hydrogen gas escapes outside the molten pool, resulting in a porous titanium alloy with a porosity of only 7% and uneven distribution. This demonstrates the crucial role of pre-oxidation treatment in matching the decomposition temperature window with the molten pool temperature field.
[0056] Comparative Example 3 Excessive titanium hydride content: Similar to Example 1, the only difference was that the TiH2 content was increased to 25% (exceeding the upper limit of 20%). Although the porosity of the prepared porous titanium alloy reached 72%, a large number of bubbles merged and connected in the molten pool, with pore sizes ranging from 500 to 2500 μm and uncontrolled distribution, causing the compressive strength to plummet to 42 MPa. This indicates that the TiH2 content needs to be controlled below 20%.
[0057] Comparative Example 4 Unstable hole components: Similar to Example 1, the only difference is that the core powder does not contain CaO and La2O3 (it is replaced with an equal amount of TC4 alloy powder). Due to insufficient melt viscosity, a large number of bubbles escape and merge, resulting in a porosity of only 28% for the porous titanium alloy (due to bubble escape losses), a pore sphericity reduced to 0.58, and a compressive strength of 120 MPa. This demonstrates the necessity of stabilizing components for bubble stabilization and pore sphericity.
[0058] Comparative Example 5 Insufficient filler powder content: Similar to Example 1, the only difference is that the flux-cored powder accounts for 8% of the total mass of the welding wire (below the lower limit of 12%). After drawing and reducing the diameter, the flux-cored powder flow is interrupted, and longitudinal section inspection reveals multiple localized cavities without flux. The porous titanium alloy deposited with this welding wire exhibits uneven pore distribution (nominal porosity 45%, actual measured local porosity 8%~72%), making it impossible to stably form a porous structure. This demonstrates the necessity of a lower limit for flux-cored filling rate for welding wire quality and operational stability.
[0059] Compared with the lattice structure design route (CN110369724A, etc.): the flux-cored wire of the present invention can obtain random spherical pores in laser additive manufacturing, without the need for support and powder cleaning, and achieves integrated forming of dense-porous structure through segmented flux-cored wire.
[0060] Compared with the Ti-TiH2 mixed powder laser powder bed melting route, the flux-cored welding wire of the present invention eliminates the need for powder mixing and powder laying, resulting in high material utilization. After pre-oxidation treatment, the decomposition window of titanium hydride matches the temperature field of the molten pool, avoiding the problem of narrow window where the foaming agent cannot be effectively activated under powder bed technology. The flux filling rate and component uniformity are guaranteed by the preparation method of the present invention (quantitative filling + multi-pass drawing), resulting in good batch-to-batch consistency.
[0061] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.
Claims
1. A TC4 flux-cored welding wire, characterized in that, The TC4 flux-cored welding wire consists of a TC4 titanium alloy outer sheath and flux powder filling the TC4 titanium alloy outer sheath. In addition to TC4 alloy powder, the flux powder, by mass percentage, also includes: 5%~20% pre-oxidized hydrogenated titanium powder, 1%~6% calcium oxide, 0.5%~3% rare earth oxides, 0.05%~0.3% boron powder, and 0.5%~2% calcium fluoride. The flux powder accounts for 12%~25% of the total mass of the TC4 flux-cored welding wire.
2. A segmented TC4 flux-cored welding wire, characterized in that, The segmented TC4 flux-cored welding wire consists of a TC4 titanium alloy outer sheath and flux powder segmented and filled within the TC4 titanium alloy outer sheath; the flux powder is divided into dense segments, transition segments and porous segments along the wire length direction. In addition to TC4 alloy powder, the core powder of the dense section also includes, by mass percentage: no more than 1% pre-oxidized titanium dioxide powder, 1%~6% calcium oxide, 0.5%~3% rare earth oxides, 0.05%~0.3% boron powder, and 0.5%~2% calcium fluoride; In addition to TC4 alloy powder, the core powder of the transition section, by mass percentage, also includes: 1%~8% pre-oxidized titanium dioxide powder, 1%~6% calcium oxide, 0.5%~3% rare earth oxides, 0.05%~0.3% boron powder, and 0.5%~2% calcium fluoride; In addition to TC4 alloy powder, the porous core powder composition, by mass percentage, includes: 8%~20% pre-oxidized titanium dioxide powder, 1%~6% calcium oxide, 0.5%~3% rare earth oxides, 0.05%~0.3% boron powder, and 0.5%~2% calcium fluoride; The flux-cored powder in each segment accounts for 12% to 25% of the total mass of the segmented TC4 flux-cored welding wire.
3. The TC4 flux-cored welding wire according to claim 1 or the segmented TC4 flux-cored welding wire according to claim 2, characterized in that, The pre-oxidized hydride titanium powder is obtained by treating hydride titanium powder in air at 450~520℃ for 1~3 hours.
4. The TC4 flux-cored welding wire according to claim 1 or the segmented TC4 flux-cored welding wire according to claim 2, characterized in that, The rare earth oxide is selected from one or more of lanthanum oxide, cerium oxide, and yttrium oxide.
5. The TC4 flux-cored welding wire according to claim 1 or the segmented TC4 flux-cored welding wire according to claim 2, characterized in that, The diameter of the TC4 flux-cored welding wire is 1.0~2.0mm; the diameter of the segmented TC4 flux-cored welding wire is 1.0~2.0mm; and the thickness of the TC4 titanium alloy outer sheath is 0.25~0.4mm.
6. The TC4 flux-cored welding wire according to claim 1, characterized in that, The pre-oxidized hydrogenated titanium powder has a mass percentage of 8% to 15% and a particle size of 20 to 120 μm.
7. A method for preparing the TC4 flux-cored welding wire according to any one of claims 1, 3-6 or the segmented TC4 flux-cored welding wire according to any one of claims 2-5, characterized in that, Includes the following steps: The flux-cored powder prepared according to the specified ratio is filled into a U-shaped tube made of TC4 titanium alloy strip, the tube is closed, and it is drawn to the target welding wire diameter through multiple passes to obtain the TC4 flux-cored welding wire or the segmented TC4 flux-cored welding wire.
8. The preparation method according to claim 7, characterized in that, The single-pass diameter reduction rate of the multi-pass drawing is 10%~15%.
9. The preparation method according to claim 7, characterized in that, Use wire drawing lubricant during drawing, and the ellipticity of the wire after drawing should not exceed 0.05mm.
10. The application of the TC4 flux-cored wire according to any one of claims 1, 3 to 6 or the segmented TC4 flux-cored wire according to any one of claims 2 to 5 in the preparation of porous titanium alloys.
Citation Information
Patent Citations
3D printing preparation method for high-strength titanium alloy part of porous structure
CN110369724A