A method for processing a quartz glass substrate of an FPD mask

By introducing a synergistic technique of texture disturbance and directional polishing in the T-side processing of FPD mask quartz glass substrates, the problems of non-selective texture removal, hydrodynamic ineffective area and geometric accuracy contradiction in the existing technology are solved. This achieves efficient, texture-free surface quality and high-precision processing, improving production efficiency and product reliability.

CN123128983APending Publication Date: 2026-11-20JIANGSU HENGXIN QUARTZ TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611308526.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies for processing the T-side of quartz glass substrates in FPD photomasks suffer from problems such as non-selective texture removal, inefficiency and secondary defects caused by hydrodynamic ineffective regions, and a contradiction between the large amount of texture removal required for texture elimination and maintaining geometric accuracy, making it difficult to improve processing quality and efficiency.

Method used

By employing a synergistic technique of texture disturbance and directional polishing, after integral grinding with a shaped diamond grinding wheel, the vibration-assisted texture disturbance of a cylindrical diamond grinding head and the hydrodynamic optimization polishing of a brush wheel are combined to disrupt the continuity and directionality of the ordered texture, thereby achieving efficient material removal.

Benefits of technology

While reducing the total amount of material removed by polishing, it improves surface quality and geometric accuracy, shortens processing time, increases the yield and reliability of mass production, and reduces the risk of brittle fracture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128983A_ABST
    Figure CN123128983A_ABST
Patent Text Reader

Abstract

The application discloses a processing method of a quartz glass substrate of an FPD mask plate, and comprises the following steps: integrally forming and grinding a T surface of the substrate by using a forming diamond grinding wheel to obtain a substrate with a target geometric profile of the T surface; horizontally clamping the ground substrate on a tool platform capable of vertical vibration, and driving the tool platform to vertically vibrate through a driving mechanism; processing a side surface of the T surface of the substrate through a cylindrical diamond grinding head to realize texture disturbance; horizontally clamping the substrate with the texture disturbance on a workbench, and polishing the T surface of the substrate by using a brush wheel. The application introduces a texture disturbance and directional polishing cooperation technology, and expects to realize the unity of high surface quality and high processing efficiency of the T surface under the premise of basically using an existing equipment main body and controllable modification cost, simultaneously greatly reduces the total polishing removal amount required, so that the process window of geometric precision can be widened from the root, and the batch production yield can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of quartz glass substrate processing technology, and specifically to a method for processing FPD mask quartz glass substrates. Background Technology

[0002] A photomask is a core pattern transfer tool in the manufacturing process of FPDs (including LCD, OLED, Mini / MicroLED, etc.). Its function is similar to a photomask in semiconductor integrated circuit manufacturing, used to precisely transfer designed pixel circuits, driving lines, and other patterns onto the glass substrate of the display panel through photolithography. The substrate material of FPD photomasks is generally made of high-purity synthetic quartz glass, which has an extremely low coefficient of thermal expansion (CTE, approximately 5.5 × 10⁻⁶). -7 With its excellent deep ultraviolet (DUV) transmittance, high chemical stability, and high mechanical strength, it can meet the stringent requirements of high-precision photolithography processes.

[0003] Unlike semiconductor IC masks, which typically use small square sizes such as 152mm×152mm×6.4mm, FPD mask substrates exhibit larger sizes as display production lines upgrade. The mainstream substrate size for G6 lines is 520mm×800mm×10.55mm, while G8.5 lines can reach the 2200mm×2500mm range. The substrate thickness is generally over 10mm, making them large-size thin-plate precision optical components.

[0004] A complete FPD (Film Photomask) quartz glass substrate comprises six outer surfaces. The two large, flat surfaces at the top and bottom are the main surfaces (A-side / B-side), used for subsequent chrome plating, resist coating, and patterning exposure processes. The four sides surrounding the substrate (including the rounded corners at the four apex of the large surfaces, which are part of the side surfaces) and the chamfered surfaces connecting the side surfaces to the main surfaces are collectively referred to as "T-sides." Although the T-sides do not participate in pattern transfer, their processing quality directly determines the lifespan of the mask and the lithography yield. High-quality T-sides should be smooth and transparent, free of microcracks, sharp edges, and particle shedding. If the T-sides have grinding textures, microcracks, or chipped edges, particulate contaminants are easily generated and transferred to the patterned area of ​​the main surface during mask handling, cleaning, and lithography recycling, causing lithography defects. At the same time, sharp edges can cause stress concentration, significantly increasing the risk of substrate breakage under thermal shock or external force.

[0005] Furthermore, in the field of polishing the periphery of small-sized substrates for semiconductor IC photomasks, a common process is to clamp multiple substrates side-by-side and polish them simultaneously. This improves batch production efficiency by processing multiple products in a single clamping operation, and this technology is a well-known and conventional process in the field. However, due to the large substrate size and high added value per unit, FPD photomasks are mostly processed on a single-unit basis in the industry.

[0006] The current mainstream process adopts a two-stage process chain of "precision grinding + traditional brush wheel polishing", and the specific steps are as follows: (1) Precision forming grinding process The quartz glass substrate to be processed is clamped onto the worktable of a high-precision CNC engraving machine using vacuum adsorption. The spindle drives a shaped diamond grinding wheel with a cross-sectional profile complementary to the target T-face shape to rotate at high speed. Following a preset CNC path, the wheel moves along the perimeter of the substrate, performing one-piece grinding of the sides, chamfered surfaces, and rounded corners. During the grinding process, a water-based coolant is continuously sprayed to remove grinding heat and debris. After this process, the dimensional and positional accuracy of the T-face (side perpendicularity, chamfer width, corner radius, squareness, etc.) basically meets the design tolerances, but the surface has a frosted appearance and exhibits continuous groove-like grinding textures parallel to the feed direction, with a texture depth typically several micrometers.

[0007] (2) Traditional brush wheel polishing process The ground substrate is transferred to a dedicated T-surface polishing machine. A brush wheel composed of flexible polymer bristles (such as nylon or PBT) is used in conjunction with a polishing slurry containing free cerium oxide abrasive to perform contact polishing on the T-surface. The high-speed rotating bristles carry the abrasive to remove trace amounts of material from the surface. Combining mechanical wiping with chemical mechanical polishing (CMP) mechanisms, the grinding texture is gradually smoothed, ultimately resulting in a smooth T-surface surface.

[0008] However, the above-mentioned "precision grinding + traditional brush wheel polishing" process has the following problems: (1) Compliant polishing mechanism leads to non-selective removal of texture. Brush wheels are typical "compliant" machining tools. The flexible bristles bend under contact pressure, conforming to the existing macroscopic and microscopic contours of the workpiece. For regular grooves and textures on the surface after fine grinding, the contact pressure, relative speed, and abrasive concentration applied by the bristles and the polishing fluid they carry to the texture peaks and valleys are basically the same, and they do not have the "rigid correction" ability to preferentially remove the material at the peaks.

[0009] According to Archard's law of wear, the linear wear at each point on the contour is approximately equal under uniform contact pressure. During polishing, the overall texture is uniformly weakened. This processing mode determines that its material removal efficiency has a theoretical bottleneck, making it difficult to achieve efficient "peak shaving and valley filling". To achieve a surface quality without obvious texture, a very large total material removal volume and an extremely long processing time are required.

[0010] (2) Inefficiency and secondary defects caused by micro-hydrodynamic ineffective regions Conventional brush bristles are typically hundreds of micrometers in diameter, far exceeding the several micrometers of depth in grinding textures. When the bristles sweep across the textured surface, they "bridge" the peaks of adjacent textures, forming microscale bridging structures above the texture valleys. This structure results in extremely poor flowability of the polishing fluid in the valley areas, creating near-stagnant "dead water zones": fresh abrasive materials struggle to reach the bottom of the valleys, and abrasive debris and chemical reaction products cannot be discharged in a timely manner.

[0011] Computational fluid dynamics (CFD) simulation studies show that a stagnant vortex region with extremely low flow velocity is formed below the bridging region, making the material removal efficiency at the bottom of the valley much lower than at the top, further lengthening the polishing cycle; at the same time, the accumulation of grinding debris and abrasive agglomeration can easily produce secondary defects such as micro-scratches and pits on the surface, reducing the product yield.

[0012] (3) Texture removal requires a large amount of material removal, which contradicts the need to maintain geometric accuracy. The T-face of an FPD mask has specific tolerance requirements for geometric features such as chamfer width and corner radius (e.g., chamfer width tolerance zone approximately ±100μm, corner radius tolerance zone approximately ±500μm). In existing processes, the surface after fine grinding contains continuous groove textures several micrometers deep (e.g., Rz of 3-5μm) and a subsurface damage layer of a certain depth. To completely eliminate these and obtain a smooth surface, sufficient total material removal must be ensured. Due to the defects of traditional brush wheel polishing, such as non-selective removal and fluid dead zones, in actual production, it is often necessary to remove tens or even hundreds of micrometers of surface material to completely eliminate the texture. Such removal is uniformly applied to the entire T-face contour, inevitably leading to significant dimensional changes in chamfer width, corner radius, etc. (e.g., chamfer width decreases by 0.03mm~0.15mm on one side). Although these changes may still not exceed the product design tolerance, they severely compress the process window, making it easy for even slight fluctuations in process parameters to cause geometric feature deviations. Traditional processes have to find a fragile balance between "qualified surface texture" and "geometric accuracy and safety", making it difficult to guarantee the yield and consistency of mass production.

[0013] From a technological perspective, due to the "compliant" processing principle of traditional brush wheel polishing, even when polishing to a surface roughness Ra below 2nm, the material removal mode is essentially still "overall uniform weakening." This mode cannot eradicate the "directional skeleton" of ordered textures. Therefore, under strong light visual inspection, it is expected that faint texture traces remaining along the original grinding direction will be easily observed in the side areas, typically appearing as "slight texture" or "obvious texture." Even if the amount of material removed is significantly increased, leading to a deterioration in geometric accuracy, it is still difficult to ensure the complete removal of directional textures. This is a long-standing technical dilemma in this field.

[0014] In addition, existing shaped diamond grinding wheels generally suffer from poor chip removal and insufficient coolant supply in the grinding zone during the fine grinding process, which easily leads to the formation of micro-crack layers on the subsurface. These cracks are difficult to completely eliminate in subsequent polishing, becoming a long-term reliability hazard. Meanwhile, ordinary cylindrical grinding heads are prone to chip extrusion and scratches, and ordinary brush wheels have uneven contact at the bristle tips, all of which limit further improvement in processing quality to some extent. Summary of the Invention

[0015] This invention addresses the shortcomings of existing technologies by providing a processing method for FPD mask quartz glass substrates. By introducing a synergistic technique of texture disturbance and directional polishing, it aims to achieve a balance between high surface quality (completely eliminating processing lines and making the T-side smooth and transparent) and high processing efficiency on the T-side, while maintaining the basic existing equipment and controllable modification costs. At the same time, it significantly reduces the total amount of polishing removal required, thereby potentially broadening the process window for geometric accuracy from the root and improving the yield of mass production.

[0016] To address the aforementioned technical problems, this invention provides a method for processing an FPD mask quartz glass substrate, wherein the T-side of the substrate is processed, the T-side including a side surface and a chamfered surface, and the top corner of the side surface is rounded. The processing method includes the following steps: S1. The substrate T-side is integrally ground using a shaped diamond grinding wheel to obtain a substrate with the target geometric contour of the T-side. The ground surface of the substrate forms parallel groove-like textures. S2. The ground substrate is horizontally clamped on a vertically vibrating tooling platform, and the tooling platform is driven to vibrate vertically by a drive mechanism; the side surface of the T-side of the substrate is processed by a cylindrical diamond grinding head to achieve texture disturbance, and the groove-like texture is transformed into a non-directional interlaced texture. S3. The substrate with the texture disturbance completed is horizontally clamped on the worktable, and the T-side of the substrate is polished using a brush wheel.

[0017] This invention inserts a "vibration-assisted texture disruption" process between precision grinding and final polishing. Utilizing a three-axis CNC machine with a vibratory clamping fixture and a cylindrical diamond grinding head, the texture is disrupted only on the side surfaces (including rounded corners) of the T-surface. This transforms ordered parallel grooves into shallow textures with irregular directions, while preserving the original grinding texture of the chamfered edges to protect its geometric accuracy. Subsequently, a hydrodynamically optimized brush wheel is used. Through a workpiece dwell-rotation motion pattern, combined with the reciprocating movement of the brush wheel along the workpiece thickness direction, efficient contour polishing is performed. The texture is efficiently removed by relying on the perpendicular effect between the polishing direction and the texture direction.

[0018] Furthermore, in S1, the profile of the shaped diamond grinding wheel is complementary to the geometric profile of the T-face target. Material removal is achieved through CNC contour cutting, thus obtaining a T-face geometric profile consistent with the grinding wheel profile, and the dimensional accuracy can be controlled within the design tolerance range. Because the diamond abrasive grains move along the feed direction on the workpiece surface, the machined surface will exhibit continuous groove-like textures parallel to this movement direction. The shaped diamond grinding wheel has several micro-chip removal grooves evenly spaced circumferentially. The groove depth is 0.3-0.8 mm, the groove width is 0.2-0.5 mm, and the spacing between adjacent grooves is 5-10 mm. This structure enhances the ability of coolant to enter the grinding arc zone during grinding, accelerates chip removal, reduces grinding heat accumulation, and reduces the generation of micro-cracks on the subsurface of the quartz glass.

[0019] Furthermore, the shaped diamond grinding wheel is made of a metal-bonded or resin-bonded material, wherein the metal-bonded material is a bronze-based binder, and the resin-bonded material is a phenolic resin-based or polyimide resin-based binder.

[0020] Furthermore, the grinding zone of the shaped diamond grinding wheel corresponding to the side of the substrate has a grit size of D46-D64 to ensure grinding efficiency, and the grinding zone corresponding to the chamfered surface of the substrate has a grit size of D30-D46 to reduce the load for subsequent polishing.

[0021] Furthermore, the spindle speed of the shaped diamond grinding wheel is 20,000-30,000 rpm, the feed rate is 300-600 mm / min, the grinding depth is 0.02-0.04 mm per pass, and the final fine grinding is completed in 2-3 passes; the cooling method is continuous spraying of water-based coolant at a flow rate of 5-10 L / min, and the coolant temperature is controlled at 22℃±2℃; the tool path is a forward grinding method along the closed contour of the substrate, and the entire T-surface is machined in a single pass.

[0022] Furthermore, in S2, the vibration frequency f of the tooling platform is 50-120Hz, and the amplitude is 0.1-0.5mm; the feed rate Vf of the cylindrical diamond grinding head satisfies the following formula with respect to the vibration frequency: N = f / (Vf / 60) = 8 - 35, where Vf is in mm / min. This results in a dense and uniform cross-hatching pattern, ensuring consistency in subsequent polishing.

[0023] Furthermore, in S2, the working surface of the cylindrical diamond grinding head is provided with a helical chip-receiving groove. The groove depth is 0.1-0.3 mm, the lead is 10-20 mm, and the helix angle is 30°-60°. This structure can temporarily accommodate grinding chips and coolant during micro-grinding, preventing secondary micro-scratches caused by the extrusion of grinding chips between the grinding head and the workpiece, while improving the uniformity of texture disturbance.

[0024] Furthermore, the cylindrical diamond grinding head has an abrasive particle size of D64-D91 and a grinding head diameter of 3-6mm; the cylindrical diamond grinding head is made of bronze-based binder, phenolic resin-based binder, or polyimide resin-based binder.

[0025] Furthermore, in S2, the spindle speed of the cylindrical diamond grinding head is 10,000-20,000 rpm, the feed rate is 100-300 mm / min, the grinding depth is 1-3 μm, and the cooling method is: full spraying of coolant with a flow rate of 3-6 L / min.

[0026] The S2 process only performs texture disturbance processing on the four sides (including corner fillets) of the T-surface, deliberately avoiding the chamfered and beveled areas. The chamfered and beveled areas are the most geometrically sensitive areas; preserving their original grinding texture avoids disturbances to the chamfer width and straightness of the edges caused by micro-grinding, ensuring the accuracy of key geometric features from a process strategy perspective. Motion method: The grinding head is mounted on a CNC spindle and rotates at high speed, performing contour cutting along a direction parallel to the original grinding texture (i.e., the circumferential direction of the substrate); simultaneously, the workpiece vibrates up and down at high frequency with a vibration fixture. The circumferential motion of the rotating abrasive grains and the vibration of the workpiece superimpose each other, creating an approximately sinusoidal cross-shaped pattern on top of the original parallel texture. This change in motion causes the abrasive grains to produce dense micro-fragments on the original grooved texture surface, fundamentally disrupting the continuity and directionality of the texture. Therefore, after this process, the surface morphology of the side (including rounded corners) area will undergo a fundamental change: the original parallel groove texture will be transformed into interlaced shallow textures without obvious directionality, the orderliness of the texture will be significantly weakened, and the valley peak depth Rz will be reduced accordingly.

[0027] Furthermore, in S3, the rotating plane of the brush wheel remains perpendicular to the local cutting plane of the T-surface of the substrate, achieving an approximately perpendicular match between the polishing direction and the texture direction.

[0028] Furthermore, in S3, a dedicated T-face brush wheel polishing machine is used, which mainly consists of a precision rotating worktable and two sets of brush wheel systems symmetrically arranged on both sides of the workpiece; the axis of the brush wheel is parallel to the long side of the workpiece, and its axial length is greater than the long side dimension of the workpiece; during the polishing process, the brush wheel rotates at high speed, and according to the T-face contour of the current contact area of ​​the workpiece, the brush wheel is controlled to move closer to or further away from the workpiece in real time to maintain a constant contact pressure or position.

[0029] Furthermore, in S3, the polishing of the substrate T-surface by the brush wheel specifically includes: The substrate is rotated until one side is parallel to the axis of the brush wheel and then stopped. The flat area of ​​that side is polished. After the side is polished, the substrate is rotated at a constant speed. During this process, the brush wheel polishes the rounded corners of the top corners that the substrate passes through. After rotating 90°, the substrate stops again and the next side is polished. This process is repeated to complete the processing of all sides.

[0030] Furthermore, in S3, the brush wheel also performs the following movements during the polishing process: The brush wheel moves axially back and forth along its axis, with a stroke of 8-12mm and a cycle of 2-10 seconds per cycle. It reciprocates along the thickness direction of the workpiece, with a stroke of 2-5mm and a frequency of 5-20 times / minute.

[0031] Furthermore, in S3, the bristles of the brush wheel have at least one of the following characteristics: The cross-section of the brush bristles is an irregular cross-section, such as a cross-shaped, trilobal, star-shaped, or Y-shaped cross-section. Its outer surface naturally forms multiple axially continuous recessed channels. When the brush bristles bend in contact with the workpiece, the change in channel volume generates a "pumping effect", actively transporting the polishing liquid stored inside to the processing interface and enhancing the fluid exchange in the valley area. The free end of the brush bristles has a 30°-45° bevel, with a bevel length of 0.5-1mm. This allows the brush bristles to form line contact with the workpiece surface rather than point contact, enhancing the uniformity of the polishing cutting action. Simultaneously, it avoids brush bristle breakage caused by stress concentration at the end, extending the service life of the brush wheel. When the brush bristles bend and contact the workpiece surface under the polishing motion, the contact area of ​​the circular end face (without a bevel) is only a small spot on the edge of the end face, approximating a circular patch (a point contact mode in a macroscopic sense). This leads to stress concentration and uneven cutting. However, with a 30°-45° bevel, the brush bristle end forms a wedge-shaped slope. When bent, this slope undergoes elastic deformation, forming a strip-shaped contact area that elongates along the diameter of the brush bristles. This contact shape ensures uniform stress distribution, increases the effective contact area, and facilitates the entry of polishing fluid into the contact interface, thereby improving polishing efficiency and uniformity.

[0032] The surface of the bristles has microgrooves or a uniformly distributed array of micropits extending along the bristle axis. The depth of the microgrooves or micropits is 5-50 μm. This structure can significantly improve the bristles' ability to carry and release polishing fluid.

[0033] Furthermore, the bristle substrate is made of flexible polymers such as nylon (PA), polybutylene terephthalate (PBT) or polypropylene (PP), and the bristle diameter is 0.1-0.5 mm.

[0034] Furthermore, the polishing slurry in S3 is a cerium oxide water-based polishing slurry with an average abrasive particle size of 0.5-3μm, a solid content of 5-20wt%, and a pH value controlled within the neutral range (6.5~7.5). The slurry is supplied continuously via a circulating spray method at a flow rate of 2-10L / min to ensure that the brush wheel is fully wetted throughout the process, and the temperature of the polishing slurry is kept stable at 22℃±2℃.

[0035] Furthermore, in S3, the brush wheel linear speed is 800-1200m / min, the nominal contact pressure is 0.5-1.5kgf, the reciprocating stroke in the workpiece thickness direction is 2-5mm, and the frequency is 5-20 times / minute; the total material removal amount is: the material removal depth on one side in this process is usually controlled at 0.02-0.05mm, which can completely eliminate residual texture and achieve a transparent and smooth surface; while traditional processes require a removal amount of 0.10mm-0.30mm to possibly eliminate texture.

[0036] Furthermore, after the polishing described in S3 is completed, the substrate is placed in a dark room and illuminated with a strong light with an illuminance of ≥100000lx at an incident angle of 30°-60°. When visually observed from the direction of the reflected light, there are no visible directional processing lines.

[0037] Furthermore, after the polishing described in S3 is completed, the roughness Ra of the substrate T surface is ≤10nm, and the variation in the chamfering and bevel processing is within 1 / 10 of the tolerance zone.

[0038] The beneficial effects of this invention are: This invention introduces vibration-assisted texture disturbance, fundamentally disrupting the continuity and directionality of the ordered texture in the side region, eliminating the conditions for the formation of fluid dead zones, and enabling isotropic material removal in subsequent polishing. Furthermore, in the polishing process: the chamfered surface utilizes its geometric position closest to the T-surface edge, contacting the brush wheel first and bearing relatively higher contact pressure. Texture peaks are preferentially removed, forming an efficient "peak-shaving and valley-filling" effect. Therefore, even while preserving the original regular texture, this area can still achieve rapid texture smoothing with a small removal amount. Even if the side surface is in a relatively concave position resulting in lower contact pressure, texture removal is still effective. Therefore, the side region relies on texture disturbance to break the fluid dead zone, and the chamfered surface relies on the contact priority due to its geometric position. Only a minimal material removal amount is needed to process the entire T-surface to a "texture-free" level where no visible texture is visible throughout the entire area. Geometric accuracy loss can be controlled to a very small range, fundamentally resolving the contradiction in traditional processes of "sacrificing accuracy safety margin for smoothness," and significantly widening the process window.

[0039] This invention disrupts the ordered groove structure through a texture disturbance process, and combined with the "pumping effect" of the vertical polishing direction and irregularly shaped brush bristles, it can essentially eliminate microscopic fluid dead zones. Under this efficient mass transfer mechanism, material removal is more selective; combined with the workpiece dwell-rotation processing mode, the total polishing time to achieve the same surface quality is expected to be significantly shortened compared to traditional processes, with the polishing cycle time for a single G6 substrate T-side compressed to less than 40 minutes.

[0040] This invention greatly expands the process window, eliminating the need for process engineers to compromise between surface quality and geometric accuracy. It also allows for higher tolerance in parameter adjustments and better consistency in batch production. Furthermore, the optimization of the grinding wheel chip removal groove and the grinding head chip containment groove reduces subsurface damage and secondary scratches, thereby improving the overall product yield.

[0041] The present invention effectively reduces cutting and polishing forces, and significantly reduces the depth of subsurface damage layer after T-side processing. It is expected to effectively improve the bending strength of quartz glass substrates, reduce the risk of brittle fracture in subsequent processes, and improve the reliability of the product throughout its entire life cycle. Attached Figure Description

[0042] To more clearly illustrate the technical solution of the present invention, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0043] Figure 1 This is a schematic diagram of the structure of the FPD mask quartz glass substrate of the present invention; Figure 2 This is a cross-sectional view of the side surface region of the substrate of the present invention; Figure 3 This is a schematic diagram of the molded diamond grinding wheel structure of the present invention; Figure 4 This is a schematic diagram of the cylindrical diamond grinding head structure of the present invention; Figure 5 This is a schematic diagram of the cross-section of the bristles of the brush wheel of the present invention; Figure 6 This is a front view of the bristles of the brush wheel of the present invention; Figure 7 This is a schematic diagram showing the contact state between the brush bristles of the brush wheel of the present invention and the workpiece. Figure 8 This is a schematic diagram of the tooling platform capable of vertical vibration of the present invention, which clamps the base plate. Figure 9 This is a front view of the brush wheel polishing the substrate according to the present invention; Figure 10 This is a top view of the substrate polishing state of the brush wheel of the present invention; Explanation of the labels in the figure: 1. Substrate, 101. Upper main surface, 102. Lower main surface, 103. Side surface, 1031. Rounded corner, 104. Beveled edge; 2. Shaped diamond grinding wheel, 201, side grinding profile section, 202, chamfered bevel grinding profile section, 203, micro chip removal channel; 3. Diamond grinding head, 301, spiral chip groove; 4. Brush wheel, 401. Brush bristles, 402. Recessed channel, 403. Beveled chamfer, 404. Microgroove; 5. Vertically vibrating tooling platform; 501. Vacuum adsorption platform; 502. Vibration platform plate; 503. Drive mechanism; 504. Vibration damping base; 505. Machine tool worktable. Detailed Implementation

[0044] The technical solution of the present invention will be clearly and completely described below with reference to specific embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0045] refer to Figure 1-8 This embodiment provides a method for processing an FPD mask quartz glass substrate, wherein, as... Figure 1-2 As shown, substrate 1 includes an upper main surface 101, a lower main surface 102, and a T-surface. The T-surface includes a side surface 103 and a chamfered bevel 104. The apex corner of the side surface is rounded 1031. The T-surface of substrate 1 is processed by the following steps: S1. The substrate 1 is integrally ground on the T-side using a shaped diamond grinding wheel 2 to obtain the substrate 1 with the target geometric contour of the T-side. The ground surface of the substrate 1 forms parallel groove-like textures. S2. The ground substrate 1 is horizontally clamped onto a vertically vibrating fixture platform, and the fixture platform is driven to vibrate vertically by a drive mechanism. The cylindrical diamond grinding head 3 processes the side surface of the substrate 1's T-plane to achieve texture disturbance, transforming the groove-like texture into a non-directional interlaced texture. Specifically, a schematic diagram of the vertically vibrating fixture platform 5 clamping the substrate 1 is shown below. Figure 8 As shown, the vertically vibrating tooling platform 5 includes a vacuum adsorption platform 501, a vibration platform plate 502, a drive mechanism 503 (electromagnetic vibrator or mechanical eccentric vibration mechanism), a shock-absorbing base 504, and a machine tool worktable 505. The vacuum adsorption platform 501 adsorbs and fixes the substrate, and the drive mechanism 503 drives the substrate 1 to reciprocate in the direction of the arrow.

[0046] S3. The substrate 1 with the texture disturbance completed is horizontally clamped on the worktable, and the T-side of the substrate 1 is polished using a brush wheel 4.

[0047] This invention inserts a "vibration-assisted texture disruption" process between precision grinding and final polishing. Using a three-axis CNC machine with a vibratory clamping fixture and a cylindrical diamond grinding head 3, the texture is disrupted only on the side surface (including the rounded corners) of the T-surface. The orderly parallel grooves are transformed into shallow textures with irregular directions, while the original grinding texture of the chamfered surface is preserved to protect its geometric accuracy. Subsequently, a hydrodynamically optimized brush wheel 4 is used to perform efficient contour polishing by using a workpiece dwell-rotation motion mode and coordinating the reciprocating movement of the brush wheel 4 in the workpiece thickness direction. The texture is efficiently removed by relying on the perpendicular effect between the polishing direction and the texture direction.

[0048] In a preferred embodiment, in S1, the profile of the shaped diamond grinding wheel 2 is complementary to the target geometric profile of the T-face. Material removal is achieved through CNC contour cutting, thus obtaining a T-face geometric profile consistent with the grinding wheel profile, and the dimensional accuracy can be controlled within the design tolerance range. Because the diamond abrasive grains perform cutting motion along the feed direction on the workpiece surface, the machined surface will exhibit continuous groove-like textures parallel to this motion direction. (Reference) Figure 3 The abrasive working layer of the shaped diamond grinding wheel includes a side grinding profile section 201 and a chamfered bevel grinding profile section 202. The shaped diamond grinding wheel 2 has several micro-chip removal grooves 203 evenly spaced circumferentially. The groove depth of each micro-chip removal groove 203 is 0.3-0.8 mm, the groove width is 0.2-0.5 mm, and the spacing between adjacent grooves is 5-10 mm. This structure enhances the ability of coolant to enter the grinding arc zone during grinding, accelerates chip removal, reduces grinding heat accumulation, and minimizes the generation of micro-cracks on the subsurface of the quartz glass.

[0049] Furthermore, the shaped diamond grinding wheel 2 is made of a metal binder or a resin binder, wherein the metal binder is a bronze-based binder, and the resin binder is a phenolic resin-based or polyimide resin-based binder.

[0050] Furthermore, the grinding grit size of the shaped diamond grinding wheel 2 corresponding to the side surface of the substrate is D46-D64 to ensure grinding efficiency, and the grinding grit size corresponding to the chamfered surface of the substrate is D30-D46 to reduce the load for subsequent polishing.

[0051] Furthermore, the spindle speed of the shaped diamond grinding wheel 2 is 20,000-30,000 rpm, the feed rate is 300-600 mm / min, the grinding depth is 0.02-0.04 mm per pass, and the final fine grinding is completed in 2-3 passes; the cooling method is continuous spraying of water-based coolant at a flow rate of 5-10 L / min, and the coolant temperature is controlled at 22℃±2℃; the tool path is a forward grinding method along the closed contour of the substrate 1, and the entire T-surface is machined in a single pass.

[0052] Furthermore, in S2, the vibration frequency f of the tooling platform is 50-120Hz, and the amplitude is 0.1-0.5mm; the feed rate Vf of the cylindrical diamond grinding head 3 satisfies the following formula with respect to the vibration frequency: N = f / (Vf / 60) = 8 - 35, where Vf is in mm / min. This results in a dense and uniform cross-hatching pattern, ensuring consistency in subsequent polishing.

[0053] Furthermore, in S2, refer to Figure 4 As shown, the cylindrical diamond grinding head 3 has a spiral chip groove 301 on its working surface. The groove depth of the spiral chip groove 301 is 0.1-0.3 mm, the lead is 10-20 mm, and the helix angle is 30°-60°. This structure can temporarily accommodate grinding chips and coolant during micro-grinding, avoiding secondary micro-scratches caused by the extrusion of grinding chips between the grinding head and the workpiece, while improving the uniformity of texture disturbance.

[0054] Furthermore, the cylindrical diamond grinding head 3 has an abrasive particle size of D64-D91 and a grinding head diameter of 3-6mm; the cylindrical diamond grinding head 3 is made of bronze-based binder, phenolic resin-based binder, or polyimide resin-based binder.

[0055] Furthermore, in S2, the spindle speed of the cylindrical diamond grinding head 3 is 10000-20000 rpm, the feed rate is 100-300 mm / min, the grinding depth is 1-3 μm, and the cooling method is: full spraying of coolant with a flow rate of 3-6 L / min.

[0056] The S2 process only performs texture disturbance processing on the four sides (including corner fillets) of the T-surface, deliberately avoiding the chamfered and beveled areas. The chamfered and beveled areas are the most geometrically sensitive areas; preserving their original grinding texture avoids disturbances to the chamfer width and straightness of the edges caused by micro-grinding, ensuring the accuracy of key geometric features from a process strategy perspective. Motion method: The grinding head is mounted on a CNC spindle and rotates at high speed, following the contour of the material along a direction parallel to the original grinding texture (i.e., the circumferential direction of substrate 1); simultaneously, the workpiece vibrates up and down at high frequency with the vibration fixture. The circumferential motion of the rotating abrasive grains and the vibration of the workpiece superimpose each other, creating an approximately sinusoidal cross-pattern on the original parallel texture. This change in motion causes the abrasive grains to produce dense micro-fragments on the original grooved texture surface, fundamentally disrupting the continuity and directionality of the texture. Therefore, after this process, the surface morphology of the side (including rounded corners) area will undergo a fundamental change: the original parallel groove texture will be transformed into interlaced shallow textures without obvious directionality, the orderliness of the texture will be significantly weakened, and the valley peak depth Rz will be reduced accordingly.

[0057] In S2, the micro-chipping removal mechanism assisted by high-frequency vibration is as follows: In traditional ductile grinding, the aim is to avoid brittle fracture to obtain a smooth surface; this invention utilizes "controlled micro-chipping" to solve the texture problem. According to fracture mechanics theory, the brittle fracture of quartz glass depends on the propagation of indentation cracks. When a cylindrical diamond grinding head rotates at a speed n, and the workpiece vibrates vertically at a frequency f (50-120Hz) and an amplitude A (0.1-0.5mm), the relative motion trajectory between a single diamond abrasive grain and the workpiece is no longer a smooth curve, but a high-frequency oscillating waveform. The instantaneous impact velocity V_impact of the abrasive grain cutting into the workpiece can be approximately expressed as: V_impact≈V_rot+2πfA·cos(2πft); where V_rot is the linear velocity of the grinding head rotation. This high-frequency impact causes the force F exerted by the abrasive grain on the workpiece surface to exhibit pulse-like changes. When the instantaneous impact force exceeds the micro-fracture threshold F_c of quartz glass, micro-chipping occurs in the material. Due to the extremely high vibration frequency, this micro-fragmentation is extremely small and dense. The continuous deep grooves (depth Rz≈1-5μm) left by the fine grinding are "interrupted" and "covered" by the micro-pits (depth <1μm) generated by this high-frequency micro-fragmentation. This micro-fragmentation removal mainly occurs in the shallow surface layer, and due to its complex distribution direction, it is significantly different from the original fine-grinding grooves. It eliminates the "directionality" and "continuity" of the original texture, completely destroying the geometric basis for the formation of "hydrodynamic dead zones" during subsequent polishing. Unlike the original continuous groove structure, these irregular, dimensionally limited discrete micro-pits cannot geometrically provide long-distance stable support for the brush bristles, making it difficult to form continuous "bridging" closed cavities. Instead, due to their openness, they become micro-vortex pools that facilitate fluid exchange under the dynamic pressure fluctuations of the brush bristles.

[0058] Furthermore, in S3, the rotating plane of the brush wheel 4 is perpendicular to the local cutting plane of the T-surface of the substrate 1, achieving an approximately perpendicular match between the polishing direction and the texture direction.

[0059] Furthermore, in S3, a dedicated T-face brush wheel 4 polishing machine is used, mainly composed of a precision rotary worktable and two sets of brush wheel 4 systems symmetrically arranged on both sides of the workpiece, such as... Figure 9-10 As shown; the axis of brush wheel 4 is parallel to the long side of the workpiece, and its axial length is greater than the long side dimension of the workpiece; during the polishing process, brush wheel 4 rotates at high speed, and according to the T-surface contour of the current contact area of ​​the workpiece, the brush wheel 4 is controlled in real time to move closer to or away from the workpiece to maintain a constant contact pressure or position; at the same time, the following movements are performed: axial reciprocating motion along the axis of brush wheel 4, with a stroke of 8-12mm and a cycle of 2-10 seconds / time; reciprocating motion along the thickness direction of the workpiece, with a stroke of 2-5mm and a frequency of 5-20 times / minute, as shown. Figure 9-10 As shown by the double-headed arrow.

[0060] Furthermore, in S3, the polishing of the substrate 1T surface by the brush wheel 4 specifically includes: The substrate 1 is rotated until one side is parallel to the axis of the brush wheel 4, and then stopped. The flat area of ​​that side is polished. After polishing that side, the substrate 1 rotates at a constant speed, during which the brush wheel 4 polishes the rounded corners of the apex that it passes through. After rotating 90°, it stops again and polishes the next side. This cycle is repeated until all sides are processed. The rotation state is as follows. Figure 10 The rotating arrow on the middle substrate is shown.

[0061] Furthermore, in S3, such as Figure 5-6 As shown, the bristles 401 of the brush wheel 4 have at least one of the following characteristics: The cross-section of the bristles 401 is an irregular cross-section, such as a cross-shaped, trilobal, star-shaped, or Y-shaped cross-section. Its outer surface naturally forms multiple axially continuous recessed channels 402. When the bristles 401 bend in contact with the workpiece, the change in channel volume generates a "pumping effect", actively transporting the polishing liquid stored inside to the processing interface and enhancing the fluid exchange in the valley area. The free end of the brush bristles 401 has a 30°-45° bevel chamfer 403 with a chamfer length of 0.5-1mm, which allows the brush bristles 401 to form line contact with the workpiece surface (e.g., Figure 7 (As shown) Instead of point contact, it enhances the uniformity of the polishing cutting action, while avoiding the breakage of the brush bristles 401 caused by stress concentration at the end, thus extending the service life of the brush wheel 4. When the brush bristles 401 bend and contact the workpiece surface under the polishing motion, the contact area of ​​the circular end face (without chamfer) is only a small spot on the edge of the end face, which is approximately a circular patch (belonging to the point contact mode in a macroscopic sense). The contact stress is concentrated, which can easily lead to uneven cutting. However, after adopting a 30°-45° bevel, the end of the brush bristles 401 forms a wedge-shaped bevel. When bending, this bevel undergoes elastic deformation, forming a strip-shaped contact area that is stretched along the diameter of the brush bristles 401 with the workpiece surface. This contact form makes the contact stress evenly distributed, increases the effective contact area, and facilitates the entry of polishing fluid into the contact interface, thereby improving polishing efficiency and uniformity.

[0062] The surface of the bristles 401 has microgrooves 404 extending along the axial direction of the bristles 401 or a uniformly distributed array of micro-pits. The depth of the microgrooves or micro-pits is 5-50 μm. This structure can significantly improve the ability of the bristles 401 to carry and release polishing fluid.

[0063] Furthermore, the substrate of the brush bristles 401 is made of flexible polymers such as nylon (PA), polybutylene terephthalate (PBT) or polypropylene (PP), and the diameter of the brush bristles 401 is 0.1-0.5 mm.

[0064] Furthermore, the polishing slurry in S3 is a cerium oxide water-based polishing slurry with an average abrasive particle size of 0.5-3μm, a solid content of 5-20wt%, and a pH value controlled within the neutral range (6.5~7.5). The slurry is supplied continuously via a circulating spray method at a flow rate of 2-10L / min to ensure that the brush wheel 4 is fully wetted throughout the process, and the temperature of the polishing slurry is kept stable at 22℃±2℃.

[0065] Furthermore, in S3, the brush wheel has a linear speed of 800-1200 m / min, a nominal contact pressure of 0.5-1.5 kgf, a reciprocating stroke of 2-5 mm in the workpiece thickness direction, and a frequency of 5-20 times / minute. The total material removal amount is typically controlled at 0.02-0.05 mm on one side in this process, which is sufficient to completely eliminate residual texture and achieve a transparent and smooth surface. In contrast, traditional processes require a removal amount of 0.10 mm to 0.30 mm to potentially eliminate texture.

[0066] In S3, the principle of vertical polishing and hydrodynamic pumping effect is as follows: In traditional polishing, the brush bristles move parallel to the texture, easily forming a hydrodynamic lubricating film, preventing the abrasive from contacting the pits. In this invention, the brush wheel's rotation plane is perpendicular to the T-plane, meaning the bristle movement direction V_brush is perpendicular to the grinding texture direction V_grinding (for undisturbed chamfered surfaces) or perpendicular to the pit arrangement direction. According to the simplified form of the Reynolds Equation, the hydrodynamic effect P is related to the velocity gradient and the film thickness h. / x(h³· P / x)=6ηU· h / x. Rate of change of film thickness h when the brush filaments perpendicularly cross the texture or pits. h / The extreme magnitude of x generates strong hydrodynamic pressure fluctuations. These fluctuations disrupt the stable lubricating film, making it easier for the polishing slurry to be "squeezed" into the bottom of the micro-pits. Furthermore, the irregularly shaped brush bristles (such as star-shaped, Y-shaped, and trilobal bristles) create a "pumping effect" through their grooved cross-sections when they bend and deform upon contact with the workpiece. This active fluid transport mechanism forces the abrasive-rich polishing slurry into the micro-pits formed by S2 and carries away the abrasive debris, thus achieving extremely high material removal efficiency.

[0067] Furthermore, after the polishing described in S3 is completed, the substrate 1 is placed in a dark room and illuminated with a strong light with an illuminance of ≥100000lx at an incident angle of 30°-60°. When visually observed from the direction of the reflected light, there are no visible directional processing lines.

[0068] Furthermore, after the polishing described in S3 is completed, the surface roughness Ra of the substrate 1T is ≤10nm, and the variation in the chamfering and bevel processing is within 1 / 10 of the tolerance zone.

[0069] This invention employs a zoned differentiated processing strategy, dividing the T-surface into a "side surface (including rounded corners of the large surface) area" and a "beveled surface area." The side surface area has relatively loose geometric tolerances but is prone to stress concentration and particle residue. Therefore, "vibration disturbance" is used to degrade its surface, followed by efficient removal using vertical polishing. The beveled surface area is a critical region for mask alignment and stress distribution, requiring high straightness and width uniformity of the edges. Typically, the processing variation is controlled within 1 / 10 of the tolerance zone (approximately ±10~20μm). This area skips the vibration disturbance in S2, retaining its original, regular grinding texture. During S3 polishing, when the brush moves perpendicular to the texture direction, the brush acts like a "scraper," precisely scraping the peaks of the texture, unlike parallel polishing which "flattens" the entire surface. This "vertical scraping" mode has inherently high geometric retention, achieving a significant leap in surface finish with minimal material removal.

[0070] S2 only disturbs the texture of the side areas, while deliberately preserving the original texture of the chamfered surfaces, based on the following geometric-mechanical analysis: During polishing, the brush wheel approaches the T-face of the workpiece radially. The chamfered surface, as the area closest to the edge of the T-face, is the first part of the entire T-face contour to contact the brush bristles. Because the brush bristles bend and deform upon contact with the workpiece, the contact pressure is greatest at the moment of contact, and then gradually decreases as the degree of bending increases. Therefore, the chamfered surface experiences relatively higher contact pressure and more thorough brush cutting action with each brush stroke. In contrast, the side areas are located in relatively concave positions between the chamfered surfaces. After the brush bristles pass over the chamfered surfaces, the degree of bending has changed, and the effective contact pressure upon reaching the side areas has decreased. When the surface of the side areas still has an ordered parallel groove texture, due to the fluid bridging effect and the presence of dead zones, the decreased contact pressure is difficult to effectively act on the texture valleys, resulting in low material removal efficiency and incomplete texture elimination. Therefore, the textural disturbance of the side areas in S2 is indispensable: by transforming ordered grooves into disordered micro-pits, it eliminates the conditions for the formation of fluid dead zones at the source, allowing the polishing slurry to effectively penetrate the valleys in S3 even with relatively low contact pressure, achieving thorough material removal. Furthermore, the chamfered edges, due to their positional contact priority, can achieve effective texture smoothing through vertical polishing, even while preserving the original ordered texture. Simultaneously, in S3, the two brush wheels rotate in opposite directions, ensuring that the chamfered edges on both sides of the substrate can preferentially contact the brush bristles, with each side preferentially contacting the bristles of one of the brush wheels.

[0071] Example 1 This embodiment relates to a processing method for the T-side of an FPD mask quartz glass substrate (G6 generation quartz glass substrate). The processing object has dimensions of 520mm × 800mm × 10.55mm, and the target requirements are: chamfer width 0.8~1mm, corner radius R5±0.5mm, squareness 90°±5′, and final T-side surface roughness Ra≤10nm. The method includes the following steps: (1) Precision forming grinding A high-precision three-axis CNC engraving machine was used, equipped with a bronze-based bonded diamond grinding wheel with circumferential chip removal grooves. The wheel grit size was D54 on the side area and D30 on the chamfered area. The chip removal grooves were 0.5mm deep, 0.3mm wide, and spaced 8mm apart. The process parameters were set as follows: spindle speed 26000rpm, feed rate 450mm / min, two passes, single pass depth of cut 0.03mm, and coolant flow rate 8L / min. After this process, the chamfer width was controlled at approximately 0.9mm, and the corner radius was approximately R5.0mm. The surface had a frosted finish. White light interferometer measurements showed a surface roughness Ra of approximately 0.32μm and Rz of approximately 3.2μm, with parallel continuous groove-like textures along the feed direction.

[0072] (2) Vibration-assisted texture disturbance An electromagnetic vibration fixture was added to the same CNC engraving machine, and a cylindrical diamond grinding head with a spiral chip flute was installed. The grinding head diameter was 4mm, the grit size was D76, the chip flute depth was 0.2mm, and the lead was 15mm. Only the side surfaces (including the rounded corners) were machined, avoiding the chamfered surfaces. The process parameters were set as follows: grinding head speed 15000rpm, feed rate 200mm / min, grinding depth 2μm, vibration frequency 105Hz, amplitude 0.25mm, and coolant flow rate 5L / min. This process utilizes high-frequency vibration superimposed grinding to transform the surface texture of the side surfaces and rounded corners into a non-directional, interwoven pattern, destroying the original texture directionality, significantly reducing texture order, and lowering the Rz value; the chamfered surface areas, being unprocessed, retained their texture and geometric accuracy.

[0073] (3) Brush wheel hydrodynamic polishing A dedicated T-surface polishing machine is used, equipped with a 900mm long three-lobed PBT bristle brush wheel. The bristles are 0.3mm in diameter with a 45° beveled end, and the bevel length is 0.8mm. The brush wheel's rotation plane remains perpendicular to the T-surface. The process parameters are set as follows: the workpiece is processed in a dwell-rotation mode, with a dwell polishing time of 8 minutes for each side, and a workpiece rotation speed of 1 rpm during the R-angle rotation polishing stage. The brush wheel linear speed is 1000m / min, the contact pressure is 1.0kgf, the radial reciprocating stroke is 3mm, the frequency is 10 times / minute, and the axial reciprocating stroke is 10mm, with a cycle of 5 seconds / cycle. The total removal amount is controlled so that the removal depth on one side of the beveled area is approximately 0.03mm. With the above combination of process parameters, the T-surface can be processed to a "texture-free" level with no visible texture in approximately 40 minutes per piece, resulting in a uniform, smooth, and bright surface. Thanks to the combined use of texture disturbance and directional polishing techniques, the removal amount on one side can be controlled to around 0.03mm. The variation in chamfer width and fillet radius is expected to be limited to a very small range (e.g., within 0.05mm), thus ensuring high surface quality while achieving excellent geometric accuracy retention. When the substrate is placed in a dark room and illuminated with a strong light of ≥100,000 lx at an incident angle of 30°-60°, no visible directional processing lines are observed when viewed from the direction of reflected light. The substrate T-surface roughness Ra≤10nm, and the variation in chamfer bevel processing is within 1 / 10 of the tolerance band.

[0074] Example 2 The difference between this embodiment and Embodiment 1 is that in the vibration-assisted texture disturbance process, the vibration frequency is adjusted to 110Hz, the amplitude to 0.15mm, the feed speed to 150mm / min, and the grinding depth to 1.5μm. In the brush wheel hydrodynamic polishing process, the side dwell time is adjusted to 6 minutes, the R-angle rotation speed is adjusted to 0.8rpm, and the removal amount is controlled to approximately 0.025mm. Ultimately, the surface roughness Ra reaches below 1nm.

[0075] Comparative Example 1 The difference between this comparative example and Example 1 is that step (2) vibration-assisted texture disturbance process is omitted, and in step (3), the brush wheel is processed in a conventional parallel posture: the workpiece rotates continuously at a constant low speed (about 2 rpm), the rotation plane of the brush wheel is parallel to the rotation plane of the workpiece, pressure is maintained for contour polishing, the single-sided removal amount is set to about 0.12 mm, and the total polishing time is about 2 hours.

[0076] In Comparative Example 1, due to the lack of a texture disturbance process, the brush bristles easily form a "hydrodynamic dead zone" at the bottom of the grinding texture during polishing, resulting in a material removal efficiency at the bottom of the valley being much lower than at the top. Even with a longer polishing time (approximately 2 hours) and a larger material removal amount (0.12 mm), due to the limitations of the conformal polishing mechanism, it is expected that the parallel texture traces extending along the original fine grinding direction will still be difficult to completely eliminate in the T-side area. Visual inspection will determine it to be at the "obvious texture" level, making it difficult to achieve the "texture-free" smooth and transparent finish. Using a larger material removal amount (0.12 mm) to pursue surface quality leads to significant changes in the chamfer width and fillet radius. Although this may barely be within the tolerance range, the process window is extremely narrow, making it very easy to exceed tolerances in mass production.

[0077] The present invention has been described in detail above with reference to specific embodiments and exemplary examples; however, these descriptions should not be construed as limiting the present invention. Those skilled in the art will understand that various equivalent substitutions, modifications, or improvements can be made to the technical solutions and embodiments of the present invention without departing from the spirit and scope of the invention, and all such modifications and improvements fall within the scope of the present invention. The scope of protection of the present invention is defined by the appended claims.

Claims

1. A method for processing an FPD mask quartz glass substrate, characterized in that, The T-surface of the substrate is processed, the T-surface including a side surface and a chamfered surface, the top corner of the side surface being rounded, the processing method including the following steps: S1. The substrate T-side is integrally ground using a shaped diamond grinding wheel to obtain a substrate with the target geometric contour of the T-side. The ground surface of the substrate forms parallel groove-like textures. S2. The ground substrate is horizontally clamped on a vertically vibrating tooling platform, and the tooling platform is driven to vibrate vertically by a drive mechanism; the side surface of the T-side of the substrate is processed by a cylindrical diamond grinding head to achieve texture disturbance, and the groove-like texture is transformed into a non-directional interlaced texture. S3. The substrate with the texture disturbance completed is horizontally clamped on the worktable, and the T-side of the substrate is polished using a brush wheel.

2. The processing method of the FPD mask quartz glass substrate as described in claim 1, characterized in that, In S1, the profile of the shaped diamond grinding wheel is complementary to the geometric profile of the T-face target, and the shaped diamond grinding wheel is uniformly provided with several micro chip removal grooves along the circumference. The groove depth of the micro chip removal groove is 0.3-0.8mm, the groove width is 0.2-0.5mm, and the distance between adjacent grooves is 5-10mm.

3. The method for processing an FPD mask quartz glass substrate as described in claim 1, characterized in that, The grinding grit size of the shaped diamond grinding wheel corresponding to the side surface of the substrate is D46-D64, and the grinding grit size corresponding to the chamfered surface of the substrate is D30-D46.

4. The method for processing an FPD mask quartz glass substrate as described in claim 1, characterized in that, In S2, the vibration frequency f of the tooling platform is 50-120Hz, and the amplitude is 0.1-0.5mm; the feed rate Vf of the cylindrical diamond grinding head satisfies the following formula with respect to the vibration frequency: N = f / (Vf / 60) = 8 - 35, where Vf is in mm / min.

5. The method for processing an FPD mask quartz glass substrate as described in claim 1, characterized in that, In S2, the working surface of the cylindrical diamond grinding head is provided with a spiral chip-receiving groove. The groove depth is 0.1-0.3mm, the lead is 10-20mm, and the helix angle is 30°-60°.

6. The method for processing an FPD mask quartz glass substrate as described in claim 1, characterized in that, In S3, the polishing of the substrate T-surface by the brush wheel specifically includes: The substrate is rotated until one side is parallel to the axis of the brush wheel and then stopped. The flat area of ​​that side is polished. After the side is polished, the substrate is rotated at a constant speed. During this process, the brush wheel polishes the rounded corners of the top corners that the substrate passes through. After rotating 90°, the substrate stops again and the next side is polished. This process is repeated to complete the processing of all sides.

7. The method for processing an FPD mask quartz glass substrate as described in claim 1, characterized in that, In S3, the brush wheel also performs the following movements during the polishing process: The brush wheel moves axially back and forth along its axis, with a stroke of 8-12mm and a cycle of 2-10 seconds per cycle. It reciprocates along the thickness direction of the workpiece, with a stroke of 2-5mm and a frequency of 5-20 times / minute.

8. The method for processing an FPD mask quartz glass substrate as described in claim 1, characterized in that, In S3, the bristles of the brush wheel have at least one of the following characteristics: The cross-section of the brush bristles is an irregular shape. The free end of the bristles has a 30°-45° beveled angle; The surface of the brush bristles has microgrooves or a uniformly distributed array of micropits extending along the axial direction of the brush bristles, and the depth of the microgrooves or micropits is 5-50 μm.

9. The method for processing an FPD mask quartz glass substrate as described in claim 1, characterized in that, After polishing as described in S3, the substrate is placed in a dark room and illuminated with a strong light with an illuminance of ≥100000lx at an incident angle of 30°-60°. When visually observed from the direction of the reflected light, there are no visible directional processing lines.