A method for uniformly planting abrasive grains on abrasive paper
By using a partitioned collaborative control architecture with multiple sets of independently adjustable high-voltage electric fields and conductive grids, combined with dual closed-loop thickness adjustment, the problems of lateral drift and uneven density of abrasives in electrostatic sand planting are solved, enabling precise sand planting and stable production of high-end products.
Patent Information
- Application Number
- CN202611245979.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-17
- Publication Date
- 2026-11-20
AI Technical Summary
In existing electrostatic sand-coating processes, abrasive particles are prone to lateral drift, resulting in uneven sand density, difficulty in precisely controlling local deviations, and insufficient batch stability, which fails to meet the production requirements of high-end products.
A zoned control architecture is adopted, which is matched with multiple sets of independent adjustable high-voltage electric fields and quantitative feeding points. Combined with the same polarity biased conductive grid between adjacent electric fields, and the feedforward and feedback double closed-loop thickness adjustment before and after sand planting, precise zoned control is achieved.
It improves the uniformity of the abrasive density across the entire sheet and the batch stability of continuous production, ensuring the uniform implantation of abrasive and the precision of electric field control.
Smart Images

Figure CN123129055A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of coated abrasive manufacturing technology, and more specifically, it relates to a method for uniformly coating abrasive into sandpaper. Background Technology
[0002] Electrostatic sanding is a core process in the preparation of coated abrasives. It relies on an electric field to drive the abrasive to move in a directional manner and be vertically implanted into the adhesive layer. The uniformity of the sanding density in the finished sandpaper directly determines the grinding accuracy, cutting efficiency, and service life of the product. With the continuous development of applications such as precision grinding and high-end polishing, the downstream market has placed higher demands on the consistency of sanding and batch stability of sandpaper products. The control precision of conventional sanding processes is no longer sufficient to meet the production needs of high-end products.
[0003] Currently, the electrostatic sand-planting process commonly used in the industry mostly adopts a production mode of single-group full-width high-voltage electric field combined with unified material supply. There is a lack of effective separation means between adjacent deposition zones, and the abrasive is prone to lateral drift, which can lead to local density deviation. Moreover, the production process mostly relies on manual sampling after sand planting for delayed adjustment, which cannot accurately correct local deviations. There is still room for improvement in the uniformity of sand planting density and batch stability during continuous production. Summary of the Invention
[0004] To address the problems of poor uniformity of electrostatic sand deposition density, difficulty in accurately controlling local deviations, and insufficient batch stability in existing technologies, this application provides a method for uniformly depositing sand into sandpaper abrasives.
[0005] A method for uniformly applying abrasive to sandpaper includes the following steps: S1. Parameter preset: Select abrasives of different particle sizes and mix them according to a preset mass ratio to obtain mixed abrasives. Preset the fluidization and pre-charge operation parameters. Arrange multiple sets of independent adjustable high-voltage electric fields along the material feeding direction of the substrate. Each set of electric fields is matched with a corresponding quantitative feeding point. A conductive grid is arranged horizontally between two adjacent sets of electric fields and a bias voltage consistent with the polarity of the abrasive charge is passed through the grid. Thickness detection process is set before and after the sand planting process. S2, Fluidized homogenized material: The mixed abrasive is fed into a horizontal insulated fluidized chamber, and clean and dry compressed air is introduced to make the abrasive in a fully fluidized state. A DC electric field is applied to make the fluidized abrasive acquire surface charge, and the electric field strength and fluidized gas velocity are synergistically controlled. S3. Grouped sand planting: The substrate coated with base adhesive passes through the sand planting electric field area at a uniform speed. Each feeding point will uniformly transport the charged abrasive to the corresponding electric field interval. Under the action of the Coulomb force of the electric field, the abrasive is vertically implanted into the base adhesive layer along the direction of the electric field line. The output voltage of each group of electric fields and the feeding rate of the corresponding point are adjusted synchronously. S4. Grid-based drift limiting: A conductive grid applies a repulsive force of like charges to the abrasive, separating the deposition regions corresponding to adjacent electric fields. S5. Pre-drying and shaping: The substrate with sand-coated material is sent into a segmented drying tunnel for drying.
[0006] By adopting the above technical solution, multiple sets of independently adjustable high-voltage electric fields are arranged in zones along the material feeding direction of the substrate and matched with corresponding quantitative feeding points. The sand planting force and material supply can be individually adjusted for different material feeding zones, breaking through the limitation of traditional single electric field full-width control that cannot correct local deviations. The conductive grids arranged between adjacent electric fields are supplied with a bias voltage of the same polarity as the abrasive. The repulsive barrier formed by the same charge constrains the lateral diffusion of the abrasive, clearly separating the corresponding deposition range of each zone and avoiding deposition interference caused by the distortion of adjacent electric field edges. With the thickness detection process set before and after sand planting, the zoned precise control of the sand planting process can be achieved, gradually correcting the density deviation in the material feeding direction and improving the uniformity of sand planting and the stability of continuous production.
[0007] Preferably, in step S1, the high-voltage electric field is set up in 3 to 5 groups, and each group of high-voltage electric fields is arranged in a one-to-one correspondence with the quantitative feeding point.
[0008] By adopting the above technical solution, the number of electric field groups in the corresponding interval is adapted to the width and feeding speed of conventional sandpaper substrate. Each group of high-voltage electric fields is arranged one-to-one with the quantitative feeding point, which can ensure that the feeding amount and electric field strength of each group of electric fields form a precise matching relationship, avoiding the problem of uneven local feeding caused by multiple feeding points sharing the same electric field. This number of groups can not only completely cover the sand planting processing area and achieve sufficiently fine zoning control, but also avoid the system control complexity, increased interference between adjacent electric fields and increased production line costs caused by too many electric field groups, thus balancing the sand planting control accuracy and the economic efficiency of production line operation.
[0009] Preferably, in step S1, the mixed abrasive is composed of two to three abrasives with different particle sizes. The abrasive is pre-treated with a surface-modifying component, which includes a silane coupling agent and nano-fumed silica. The abrasive is one or more of corundum, silicon carbide, zirconium corundum, or ceramic corundum, and the particle size range of the mixed abrasive does not exceed four particle size numbers.
[0010] By adopting the above technical solutions, limiting the particle size types and spans of the mixed abrasives can ensure that the particle size differences of the mixed abrasives are within a controllable range, reducing the risk of particle size stratification in the subsequent charging and sand-planting processes. Nano-sized fumed silica can be uniformly attached to the abrasive surface, finely adjusting the surface resistivity of the particles, reducing the differences in electrostatic properties between abrasives of different sizes and materials, and significantly reducing the dispersion of the particle charge-to-mass ratio during fluidized charging. Silane coupling agents can form an organic functionalized transition layer on the abrasive surface, enhancing the interfacial bonding force between the abrasive and the resin adhesive layer through chemical bonding. The two work together to complete the dry conditioning of the abrasive surface, adapting to the process requirements of subsequent electrostatic sand-planting from the raw material end.
[0011] Preferably, in step S2, the initial fluidizing gas velocity of the fluidizing pre-charge is 0.5 m / s to 1.2 m / s, the initial DC charging voltage applied in the cavity is 2 kV to 8 kV, and the electric field is applied in a vertically parallel arrangement.
[0012] By adopting the above technical solution, the initial fluidizing gas velocity matched with the fluidization characteristics of the abrasive can maintain the abrasive of different particle sizes in a stable and fully fluidized state, avoiding abrasive deposition and agglomeration due to excessively low gas velocity or abrasive entrainment and loss due to excessively high gas velocity; the electric field arranged in parallel above and below can form a uniform DC electric field environment in the fluidization cavity, and with a suitable initial DC charging voltage, all surfaces of the suspended and tumbling abrasive can fully contact the electric field and uniformly carry surface charge, avoiding the problem of uneven single-sided charging in falling charging, and providing a stable charging basis for the subsequent sand planting process.
[0013] Preferably, in step S2, the coordinated control is achieved by collecting the average charge-to-mass ratio data of the discharged abrasive at the discharge position in real time, comparing the measured value with the preset target value, and then dynamically adjusting the output voltage of the charged electric field and the fluidizing gas velocity.
[0014] By adopting the above technical solution, the average charge-to-mass ratio data is collected in real time at the abrasive discharge position. After comparing the measured value with the preset target value, the output voltage of the charging electric field and the fluidizing gas velocity are adjusted in linkage. The charging conditions can be dynamically corrected according to the fluctuation of the abrasive fluidization state, and the influence of external disturbances such as batch differences of abrasive, fluctuations in gas source pressure, and changes in ambient temperature and humidity can be offset. This ensures that the charge-to-mass ratio of the discharged abrasive is always maintained within the target range, improves the stability and uniformity of the charging process, and provides a prerequisite for the precise control of subsequent sand planting density.
[0015] Preferably, in step S3, the charged abrasive is transported to each unloading point through a sealed, insulated channel with an inner wall covered by polytetrafluoroethylene. The air source for transport is dry compressed air with a relative humidity of no more than 40%, and the abrasive is kept charged throughout the process.
[0016] By adopting the above technical solution, the sealed channel with the inner wall covered with insulating material has excellent insulation performance, which can reduce the charge leakage caused by contact with the wall surface during the abrasive transportation process. With the low humidity dry compressed air as the transportation air source, it can avoid the rapid charge decay and particle agglomeration caused by the formation of conductive water film on the surface of the abrasive by ambient water vapor. This ensures that the abrasive maintains a stable charged state throughout the entire process from the fluidization chamber to the feeding point, ensuring the consistency of the charged state when entering the sand planting electric field, and supporting the uniformity and controllability of the sand planting process.
[0017] Preferably, in step S1, the bias voltage amplitude of the conductive grid is 10% to 15% of the corresponding main electric field voltage, and the grid aperture is 3 to 5 times the maximum particle size of the mixed abrasive.
[0018] By adopting the above technical solution, the bias voltage amplitude of the conductive grid is matched with the main electric field voltage. This not only constrains the lateral movement of the abrasive through the repulsion of like charges and clearly separates the deposition boundaries of adjacent electric fields, but also does not interfere with the electric field line distribution of the main electric field, thus avoiding affecting the vertical implantation posture of the abrasive. The grid aperture is matched with the maximum particle size of the abrasive, ensuring that abrasive particles of different sizes can pass through the grid structure normally without the problem of grid blockage. At the same time, it maintains the continuity of the overall electric field of the grid, taking into account both abrasive passage and interval separation effect.
[0019] Preferably, in step S1, the thickness detection process includes detecting the thickness of the base adhesive before sand planting and detecting the thickness of the abrasive layer after sand planting; before sand planting, the thickness of the wet film of the base adhesive is detected in real time and the initial voltage of the corresponding electric field group is adjusted forward; after sand planting, the thickness of the abrasive layer is detected in real time and the electric field voltage and feeding rate are adjusted in feedback, forming a double closed-loop adjustment circuit of feedforward and feedback.
[0020] By adopting the above technical solution, the thickness detection of the base adhesive before sand planting can collect the wet film thickness of the base adhesive in real time and feedforward to adjust the initial voltage of the corresponding electric field group, predict the impact of adhesive layer fluctuations on the sand planting depth in advance, and adjust the electric field force in advance to offset the adhesive thickness deviation. This is a predictive adjustment with fast response speed and small lag. The thickness detection of the abrasive layer after sand planting can collect thickness data in real time and feed back to adjust the electric field voltage and feeding rate to correct the sand planting density deviation that has been generated. The two adjustment loops work together to form a complete closed-loop control system, which can quickly respond to known disturbances and correct unknown deviations, thereby improving sand planting accuracy and batch stability.
[0021] Preferably, in step S3, the specific method for synchronously adjusting the voltage of each group of electric fields and the feeding rate of the corresponding point is as follows: when the sand density of the corresponding interval is lower than the target value, the output voltage of the electric field group and the feeding rate of the corresponding point are increased synchronously; when the sand density of the corresponding interval is higher than the target value, the output voltage of the electric field group and the feeding rate of the corresponding point are decreased synchronously.
[0022] By adopting the above technical solution and using the synchronous adjustment of electric field voltage and feeding rate, it is possible to ensure that the abrasive feed rate and electric field driving force are matched during the sand planting density adjustment process, avoiding process imbalance caused by adjusting only one parameter. If only the electric field voltage is adjusted while the feeding rate remains unchanged, the abrasive may be implanted too deeply or fall over. If only the feeding rate is adjusted while the electric field voltage remains unchanged, the abrasive may accumulate or the electric field force may be excessive. Synchronous adjustment can make the sand planting density in each interval smoothly adjusted to the target range. During the adjustment process, the implantation posture and bonding depth of the abrasive remain stable, ensuring the uniformity of sand planting quality.
[0023] Preferably, in step S5, the dried substrate undergoes a series of processes including adhesive coating, main drying, high-temperature curing, flexible humidification, slitting, and winding to obtain the finished product.
[0024] By adopting the above technical solution, after the sand is pre-dried, it goes through multiple post-processing steps to gradually complete the solvent evaporation and resin cross-linking curing of the adhesive layer, firmly anchoring the abrasive to the substrate surface; the re-adhesion process can further wrap the tail of the abrasive to improve the overall bonding force; high-temperature curing can make the resin reach the final bonding strength; flexible humidification can adjust the internal stress of the finished substrate to avoid the substrate from becoming brittle and easy to break after curing; slitting and winding can obtain finished products of corresponding specifications; the entire post-processing process is smoothly connected with the front-end sand planting process, ensuring the integrity of product preparation and industrial feasibility.
[0025] In summary, this application has the following beneficial effects: 1. Because this application adopts a zoned collaborative control architecture with multiple sets of independent adjustable high-voltage electric fields and quantitative feeding points, combined with the separation effect of the deposition zone of the same polarity biased conductive grid between adjacent electric fields, and supplemented by the feedforward plus feedback double closed-loop thickness adjustment mechanism before and after sand planting, it can realize the fine independent control of the sand planting density in each material feeding zone, effectively improve the uniformity of the sand planting density of the whole width, and improve the batch stability of continuous production.
[0026] 2. In this application, a horizontal insulated fluidization chamber is preferred for fluidized pre-charging. Combined with a mechanism for real-time acquisition and dynamic adjustment of the charge-to-mass ratio at the abrasive discharge position, the mixed abrasive obtains a uniform and stable surface charge in a fully fluidized suspension state. This can reduce the dispersion of the charge-to-mass ratio of abrasives with different particle sizes and provide a stable and controllable charging basis for the subsequent electric field sand planting process.
[0027] 3. The method of this application uses silane coupling agent and nano-fumed silica to perform composite surface conditioning treatment on the mixed abrasive, which can finely adjust the surface resistivity of the particles to adapt to the subsequent electrostatic discharge process. At the same time, an organic transition layer is built on the surface of the abrasive to enhance the interfacial bonding force with the base adhesive, thus optimizing the uniformity of sand planting and the adhesion strength of abrasive particles from the raw material end.
[0028] 4. In this application, a closed, insulated channel with an inner wall covered by polytetrafluoroethylene is used to transport charged abrasive materials with dry compressed air of controlled relative humidity. The charged state of the abrasive materials is maintained throughout the process, which can reduce charge leakage and particle agglomeration during the transportation process, ensure that the charged state of the abrasive materials is stable and consistent when they enter the sand planting electric field, and ensure that the sand planting process is uniform and controllable. Attached Figure Description
[0029] Figure 1 This is a flowchart of the preparation process of a uniform sanding abrasive method provided in this application; Figure 2This is a comparison diagram of the uniformity test results of the sand layer thickness of the various embodiments and comparative examples provided in this application; Figure 3 This is a comparison diagram of the abrasive adhesion test results of the various embodiments and comparative examples provided in this application; Figure 4 This is a comparison chart of the sandpaper abrasion resistance test results of the various embodiments and comparative examples provided in this application. Detailed Implementation
[0030] The present application will be further described in detail below with reference to embodiments and comparative examples. Unless otherwise specified, the experimental methods used below are conventional methods. Unless otherwise specified, the materials, reagents, methods and instruments used are all conventional materials, reagents, methods and instruments in the art, which can be obtained by those skilled in the art through commercial channels or prepared according to literature methods.
[0031] Technical Concept: Electrostatic sanding is a core process in the preparation of coated abrasives. The uniformity of sanding density directly determines the grinding accuracy and service life of the finished sandpaper. Current conventional electrostatic sanding processes mostly employ a single-set, full-width high-voltage electric field combined with a uniform material supply. On the one hand, there is a natural field strength distortion at the edge of the electric field, causing the abrasive to easily diffuse laterally under the influence of the electric field, blurring the boundaries between adjacent deposition zones and making it impossible to accurately correct local density deviations. On the other hand, mixed abrasives often use a falling corona charging method, resulting in significant differences in the surface charge state of particles of different sizes. Furthermore, the production process relies heavily on manual sampling and parameter adjustment after sanding, making it impossible to predict and offset fluctuations in previous processes such as the thickness of the base coat. Ultimately, this leads to insufficient sanding uniformity, and the batch stability of continuous production needs improvement.
[0032] This solution involves synergistic optimization across multiple dimensions, including system layout, charging process, control logic, and raw material pretreatment. Multiple sets of independent high-voltage electric fields and quantitative feeding points are set along the substrate feeding direction to achieve independent and precise adjustment of sand-planting parameters in each feeding zone. Conductive grids with the same polarity bias voltage are deployed at the boundaries of adjacent electric fields, relying on the repulsion of like charges to constrain the lateral diffusion of the abrasive and precisely separate the deposition zones of each electric field. A fluidized pre-charging and online charge-to-mass ratio synergistic control mechanism ensures uniform and stable abrasive charging. Combined with a feedforward and feedback dual-closed-loop thickness control system before and after sand planting, and supplemented by abrasive surface conditioning treatment to optimize particle electrostatic properties, a complete control link is formed from the raw material end to the production end, effectively improving sand planting uniformity and batch production stability.
[0033] Example 1: This example provides a method for uniformly applying abrasive to sandpaper, including the following steps: S1. Parameter preset: Select abrasives of different particle sizes and mix them according to a preset mass ratio to obtain mixed abrasives. Preset the fluidization and pre-charge operation parameters. Arrange multiple sets of independent adjustable high-voltage electric fields along the material feeding direction of the substrate. Each set of electric fields is matched with a corresponding quantitative feeding point. A conductive grid is arranged horizontally between two adjacent sets of electric fields and a bias voltage consistent with the polarity of the abrasive charge is passed through the grid. Thickness detection process is set before and after the sand planting process. The system includes four sets of high-voltage electric fields, each corresponding to a specific feeding point. The mixed abrasive is composed of two different particle sizes. The abrasive is pre-treated with a modified component for surface conditioning. For every 100 parts of abrasive mass, 0.5 parts of silane coupling agent and 0.2 parts of nano-fumed silica are added. The silane coupling agent used is γ-aminopropyltriethoxysilane. The abrasive is corundum, and the mixed abrasive has a particle size span of three sizes. The surface conditioning process employs a high-speed dry mixing process with a mixing speed of 1350 r / min, a mixing time of 6.5 min, and a mixing temperature controlled at 45℃, ensuring uniform coating of the modified component on the surface. The abrasive particle surface can reduce the difference in electrostatic properties between abrasive particles of different sizes and improve the uniformity of subsequent charging. The conductive grid is arranged perpendicular to the material feeding direction of the substrate and is located at the boundary between two adjacent high-voltage electric fields. The bias voltage amplitude is 12.5% of the corresponding main electric field voltage, and the grid aperture is 4 times the maximum particle size of the mixed abrasive. The thickness detection process includes the detection of the base adhesive thickness before sand planting and the detection of the abrasive layer thickness after sand planting. Before sand planting, the thickness of the wet film of the base adhesive is detected in real time and the initial voltage of the corresponding electric field group is adjusted forward. After sand planting, the thickness of the abrasive layer is detected in real time and the electric field voltage and feeding rate are adjusted in feedback, forming a double closed-loop adjustment circuit of feedforward plus feedback.
[0034] S2, Fluidized homogenized material: The mixed abrasive is fed into a horizontal insulated fluidized chamber, and clean and dry compressed air is introduced to make the abrasive in a fully fluidized state. A DC electric field is applied to make the fluidized abrasive acquire surface charge, and the electric field strength and fluidized gas velocity are synergistically controlled. The initial fluidizing gas velocity for fluidized pre-charging is 0.85 m / s, the initial DC charging voltage applied in the cavity is 5 kV, and the electric field is applied in a parallel vertical arrangement. The coordinated control is achieved by collecting the average charge-to-mass ratio data of the discharged abrasive in real time at the discharge position, comparing the measured value with the preset target value, and then dynamically adjusting the output voltage of the charging electric field and the fluidizing gas velocity. The charge-to-mass ratio detection adopts the Faraday cup method for online acquisition, and the data acquisition frequency is 1 time / second.
[0035] S3. Grouped sand planting: The substrate coated with base adhesive passes through the sand planting electric field area at a uniform speed. Each feeding point will uniformly transport the charged abrasive to the corresponding electric field interval. Under the action of the Coulomb force of the electric field, the abrasive is vertically implanted into the base adhesive layer along the direction of the electric field line. The output voltage of each group of electric fields and the feeding rate of the corresponding point are adjusted synchronously. The charged abrasive is transported to each feeding point through a sealed, insulated channel with an inner wall covered by polytetrafluoroethylene. The air source for the transport is dry compressed air with a relative humidity of no more than 40%, keeping the abrasive charged throughout the process. The specific method for synchronously adjusting the voltage of each electric field and the feeding rate of the corresponding point is as follows: when the sand density of the corresponding interval is lower than the target value, the output voltage of the electric field and the feeding rate of the corresponding point are increased simultaneously; when the sand density of the corresponding interval is higher than the target value, the output voltage of the electric field and the feeding rate of the corresponding point are decreased simultaneously. The substrate is a polyester film substrate, the base adhesive is water-soluble phenolic resin, and the substrate feeding speed is 15m / min.
[0036] S4. Grid-based drift limiting: A conductive grid applies a repulsive force of like charges to the abrasive, separating the deposition regions corresponding to adjacent electric fields. Among them, the repulsive effect generated by the same charge can constrain the lateral diffusion of abrasive, effectively reduce the deposition overlap area of adjacent electric fields, and improve the uniformity of the overall sand planting density.
[0037] S5. Pre-drying and shaping: The substrate with sand planting completed is sent into a segmented drying tunnel for drying treatment. The drying process employs a two-stage heating tunnel, with the first tunnel temperature at 85℃ and the second tunnel temperature at 110℃, for a total drying time of 6 minutes. The dried substrate then undergoes a series of processes including adhesive coating, main drying, high-temperature curing, flexible humidification, slitting, and winding to obtain the finished product. The adhesive coating uses alcohol-soluble phenolic resin, with a dry film thickness controlled at 12μm. The main drying temperature is 105℃, and the drying time is 8 minutes. The high-temperature curing temperature is 130℃, and the curing time is 12 minutes. The flexible humidification process maintains a relative humidity of 55%.
[0038] Example 2: This example provides a method for uniformly applying abrasive to sandpaper, including the following steps: S1. Parameter preset: Select abrasives of different particle sizes and mix them according to a preset mass ratio to obtain mixed abrasives. Preset the fluidization and pre-charge operation parameters. Arrange multiple sets of independent adjustable high-voltage electric fields along the material feeding direction of the substrate. Each set of electric fields is matched with a corresponding quantitative feeding point. A conductive grid is arranged horizontally between two adjacent sets of electric fields and a bias voltage consistent with the polarity of the abrasive charge is passed through the grid. Thickness detection process is set before and after the sand planting process. The system includes three sets of high-voltage electric fields, each corresponding to a specific feeding point. The mixed abrasive is composed of two different particle sizes. The abrasive is pre-treated with a modified component for surface conditioning. For every 100 parts of abrasive mass, 0.2 parts of silane coupling agent and 0.1 parts of nano-fumed silica are added. The silane coupling agent used is γ-glycidyl etheroxypropyltrimethoxysilane. The abrasive is silicon carbide, and the mixed abrasive has a particle size span of two sizes. The surface conditioning process employs a high-speed dry mixing process with a mixing speed of 1200 r / min and a mixing time of 5 min. The mixing temperature is controlled within a controlled range. The temperature is set to 40℃ to ensure that the modified components are uniformly coated on the surface of the abrasive particles. The conductive grid is arranged perpendicular to the material feeding direction of the substrate and is located at the boundary between two adjacent high-voltage electric fields. The bias voltage amplitude is 10% of the corresponding main electric field voltage, and the grid aperture is 3 times the maximum particle size of the mixed abrasive. The thickness detection process includes the detection of the base adhesive thickness before sand planting and the detection of the abrasive layer thickness after sand planting. Before sand planting, the thickness of the wet film of the base adhesive is detected in real time and the initial voltage of the corresponding electric field group is adjusted forward. After sand planting, the thickness of the abrasive layer is detected in real time and the electric field voltage and feeding rate are adjusted in feedback, forming a double closed-loop adjustment circuit of feedforward plus feedback.
[0039] S2, Fluidized homogenized material: The mixed abrasive is fed into a horizontal insulated fluidized chamber, and clean and dry compressed air is introduced to make the abrasive in a fully fluidized state. A DC electric field is applied to make the fluidized abrasive acquire surface charge, and the electric field strength and fluidized gas velocity are synergistically controlled. The initial fluidizing gas velocity for fluidized pre-charging is 0.5 m / s, the initial DC charging voltage applied inside the cavity is 2 kV, and the electric field is applied in a parallel vertical arrangement. The coordinated control is achieved by collecting the average charge-to-mass ratio data of the discharged abrasive at the discharge position in real time, comparing the measured value with the preset target value, and then dynamically adjusting the output voltage of the charging electric field and the fluidizing gas velocity. The charge-to-mass ratio detection adopts the Faraday cup method for online acquisition, and the data acquisition frequency is 1 time / 2 seconds.
[0040] S3. Grouped sand planting: The substrate coated with base adhesive passes through the sand planting electric field area at a uniform speed. Each feeding point will uniformly transport the charged abrasive to the corresponding electric field interval. Under the action of the Coulomb force of the electric field, the abrasive is vertically implanted into the base adhesive layer along the direction of the electric field line. The output voltage of each group of electric fields and the feeding rate of the corresponding point are adjusted synchronously. The charged abrasive is transported to each feeding point through a sealed, insulated channel with an inner wall covered by polytetrafluoroethylene. The air source for the transport is dry compressed air with a relative humidity of no more than 40%, keeping the abrasive charged throughout the process. The specific method for synchronously adjusting the voltage of each electric field and the feeding rate of the corresponding point is as follows: when the sand density of the corresponding interval is lower than the target value, the output voltage of the electric field and the feeding rate of the corresponding point are increased simultaneously; when the sand density of the corresponding interval is higher than the target value, the output voltage of the electric field and the feeding rate of the corresponding point are decreased simultaneously. The substrate is a polyester film substrate, the base adhesive is water-soluble phenolic resin, and the substrate feeding speed is 10m / min.
[0041] S4. Grid-based drift limiting: A conductive grid applies a repulsive force of like charges to the abrasive, separating the deposition regions corresponding to adjacent electric fields. Among them, the repulsive effect generated by the same charge can constrain the lateral diffusion of abrasive, effectively reduce the deposition overlap area of adjacent electric fields, and improve the uniformity of the overall sand planting density.
[0042] S5. Pre-drying and shaping: The substrate with sand planting completed is sent into a segmented drying tunnel for drying treatment. The drying process employs a two-stage heating tunnel, with the first tunnel temperature at 75℃ and the second tunnel temperature at 100℃, for a total drying time of 4 minutes. The dried substrate then undergoes a series of processes including adhesive coating, main drying, high-temperature curing, flexible humidification, slitting, and winding to obtain the finished product. The adhesive coating uses alcohol-soluble phenolic resin, with a dry film thickness controlled at 10μm. The main drying temperature is 95℃, and the drying time is 6 minutes. The high-temperature curing temperature is 120℃, and the curing time is 10 minutes. The flexible humidification process maintains a relative humidity of 50%.
[0043] Example 3: This example provides a method for uniformly applying abrasive to sandpaper, including the following steps: S1. Parameter preset: Select abrasives of different particle sizes and mix them according to a preset mass ratio to obtain mixed abrasives. Preset the fluidization and pre-charge operation parameters. Arrange multiple sets of independent adjustable high-voltage electric fields along the material feeding direction of the substrate. Each set of electric fields is matched with a corresponding quantitative feeding point. A conductive grid is arranged horizontally between two adjacent sets of electric fields and a bias voltage consistent with the polarity of the abrasive charge is passed through the grid. Thickness detection process is set before and after the sand planting process. Five high-voltage electric fields are set up, each corresponding to a quantitative feeding point. The mixed abrasive is composed of three different particle sizes. The abrasive is pre-treated with surface conditioning components. Based on 100 parts by weight of abrasive, 0.8 parts of silane coupling agent and 0.3 parts of nano-fumed silica are added. The silane coupling agent used is γ-aminopropyltriethoxysilane. The abrasive is zirconium corundum, and the particle size range of the mixed abrasive is four sizes. The surface conditioning treatment uses a high-speed dry mixing process with a mixing speed of 1500 r / min, a mixing time of 8 min, and a mixing temperature controlled at 50℃, ensuring uniform coating of the modified components on the surface. The abrasive particle surface can reduce the difference in electrostatic properties between abrasive particles of different sizes, and improve the uniformity of subsequent charging. The conductive grid is arranged perpendicular to the material feeding direction of the substrate and is located at the boundary between two adjacent high-voltage electric fields. The bias voltage amplitude is 15% of the corresponding main electric field voltage, and the grid aperture is 5 times the maximum particle size of the mixed abrasive. The thickness detection process includes the detection of the base adhesive thickness before sand planting and the detection of the abrasive layer thickness after sand planting. Before sand planting, the thickness of the wet film of the base adhesive is detected in real time and the initial voltage of the corresponding electric field group is adjusted forward. After sand planting, the thickness of the abrasive layer is detected in real time and the electric field voltage and feeding rate are adjusted in feedback, forming a double closed-loop adjustment circuit of feedforward plus feedback.
[0044] S2, Fluidized homogenized material: The mixed abrasive is fed into a horizontal insulated fluidized chamber, and clean and dry compressed air is introduced to make the abrasive in a fully fluidized state. A DC electric field is applied to make the fluidized abrasive acquire surface charge, and the electric field strength and fluidized gas velocity are synergistically controlled. The initial fluidizing gas velocity for fluidized pre-charging is 1.2 m / s, the initial DC charging voltage applied inside the cavity is 8 kV, and the electric field is applied in a parallel vertical arrangement. The coordinated control is achieved by collecting the average charge-to-mass ratio data of the discharged abrasive at the discharge position in real time, comparing the measured value with the preset target value, and then dynamically adjusting the output voltage of the charging electric field and the fluidizing gas velocity. The charge-to-mass ratio detection adopts the Faraday cup method for online acquisition, and the data acquisition frequency is 2 times / second.
[0045] S3. Grouped sand planting: The substrate coated with base adhesive passes through the sand planting electric field area at a uniform speed. Each feeding point will uniformly transport the charged abrasive to the corresponding electric field interval. Under the action of the Coulomb force of the electric field, the abrasive is vertically implanted into the base adhesive layer along the direction of the electric field line. The output voltage of each group of electric fields and the feeding rate of the corresponding point are adjusted synchronously. The charged abrasive is transported to each feeding point through a sealed, insulated channel with an inner wall covered by polytetrafluoroethylene. The air source for the transport is dry compressed air with a relative humidity of no more than 40%, keeping the abrasive charged throughout the process. The specific method for synchronously adjusting the voltage of each electric field and the feeding rate of the corresponding point is as follows: when the sand density of the corresponding interval is lower than the target value, the output voltage of the electric field and the feeding rate of the corresponding point are increased simultaneously; when the sand density of the corresponding interval is higher than the target value, the output voltage of the electric field and the feeding rate of the corresponding point are decreased simultaneously. The substrate is a polyester film substrate, the base adhesive is water-soluble phenolic resin, and the substrate feeding speed is 20m / min.
[0046] S4. Grid-based drift limiting: A conductive grid applies a repulsive force of like charges to the abrasive, separating the deposition regions corresponding to adjacent electric fields. Among them, the repulsive effect generated by the same charge can constrain the lateral diffusion of abrasive, effectively reduce the deposition overlap area of adjacent electric fields, and improve the uniformity of the overall sand planting density.
[0047] S5. Pre-drying and shaping: The substrate with sand planting completed is sent into a segmented drying tunnel for drying treatment. The drying process employs a two-stage heating tunnel, with the first tunnel temperature at 95℃ and the second tunnel temperature at 120℃, for a total drying time of 8 minutes. The dried substrate then undergoes a series of processes including adhesive coating, main drying, high-temperature curing, flexible humidification, slitting, and winding to obtain the finished product. The adhesive coating uses alcohol-soluble phenolic resin, with a dry film thickness controlled at 15μm. The main drying temperature is 115℃, and the drying time is 10 minutes. The high-temperature curing temperature is 140℃, and the curing time is 15 minutes. The flexible humidification process maintains a relative humidity of 60%.
[0048] Comparative Example 1: The only difference between this comparative example and Example 1 is that the mixed abrasive does not undergo surface conditioning treatment with modified components, and the original state of corundum abrasive is used directly for subsequent processes. The selection of other raw materials, process steps and parameters are completely consistent with Example 1.
[0049] Comparative Example 2: The only difference between this comparative example and Example 1 is that the conductive grid between two adjacent electric fields is removed and no bias voltage is applied. The number of other electric field groups, feeding points, process parameters and raw materials are completely the same as in Example 1.
[0050] Comparative Example 3: The only difference between this comparative example and Example 1 is that the partitioned control settings of the four independent electric fields and corresponding feeding points are cancelled. The four high-voltage electric fields output the same voltage and cannot be adjusted individually. They are equipped with one total quantitative feeding point for unified material supply. The total feeding rate is the same as the total feeding rate of the four groups in Example 1. The remaining process steps, parameters and raw materials are completely the same as in Example 1.
[0051] Comparative Example 4: The only difference between this comparative example and Example 1 is that the horizontal fluidized chamber fluidization pre-charging and charge-to-mass ratio coordinated control process is cancelled, and replaced with the conventional falling corona charging method. The abrasive is charged through the corona field via the material drop channel. The initial charging voltage is the same as the initial DC charging voltage of Example 1. All other steps, parameters and raw materials are completely the same as those of Example 1.
[0052] Comparative Example 5: The only difference between this comparative example and Example 1 is that the thickness detection and feedforward adjustment of the base adhesive before sand planting is cancelled, and only the thickness detection and feedback adjustment loop of the abrasive layer after sand planting is retained. The other process steps, parameters and raw materials are completely consistent with Example 1.
[0053] Comparative Example 6: This comparative example adopts the industry's conventional electrostatic sand-planting method, using unmodified ordinary corundum abrasive, equipped with a single set of full-width high-voltage electric field and a single feeding point, without conductive grid setting, adopts conventional falling charging, and relies solely on manual sampling and adjustment of parameters after sand planting, without online closed-loop control. The selection of other substrates, primers and post-processing procedures are consistent with Example 1.
[0054] I. Sanding layer thickness uniformity test: The test was conducted in accordance with GB / T37884-2019 "Determination of Coated Abrasive Thickness". Three sheets of finished sandpaper prepared in Examples 1 to 3 and Comparative Examples 1 to 6 were used as test samples. Before the test, all samples were placed in an environment with a temperature of 23°C and a relative humidity of 50% for 24 hours to adjust their condition. The thickness was measured using a digital thickness gauge with an accuracy of 0.001 mm under a specified pressure of 0.01 MPa. Ten test points were selected at equal intervals along the width of the substrate for each sample. A test line was selected every 200 mm along the material feeding direction, with 10 test points set for each test line. The thickness values were recorded point by point. The average thickness, thickness range, and relative thickness deviation of each group of samples were calculated. The thickness deviation level directly reflects the uniformity of sanding density of each group of samples. The smaller the deviation, the better the stability and consistency of the sanding process.
[0055] II. Abrasive Adhesion Test: The test was conducted according to GB / T39938-2021 "Determination of Abrasive Adhesion of Coated Abrasives - Steel Brush Method". Five 100mm × 50mm samples were cut from the finished sandpaper prepared in Examples 1 to 3 and Comparative Examples 1 to 6 for each group. Before testing, all samples were placed in an environment of 23℃ and 50% relative humidity for 24 hours for conditioning. A standard rotating steel brush device with a diameter of 100mm and a bristle diameter of 0.3mm was used to brush the abrasive surface of the samples under a constant pressure of 0.5MPa and a constant rotation speed of 60r / min. The brushing time was set to 30s. Before and after brushing, the mass of the samples was weighed using an analytical balance with an accuracy of 0.1mg. The percentage of abrasive grain detachment mass to the initial total mass of the abrasive grains was calculated. The abrasive grain detachment rate was used to characterize the abrasive grain bonding strength of each group of samples. The lower the detachment rate, the stronger the interfacial bonding anchoring force between the abrasive grains and the base coat.
[0056] III. Abrasion resistance test of sandpaper was conducted in accordance with GB / T38886-2020 "Determination of Abrasion Resistance of Coated Abrasives - Grinding Wheel Method". Three standard-sized circular samples were cut from the finished sandpapers prepared in Examples 1 to 3 and Comparative Examples 1 to 6 for each group. The samples were fixed flat on the workpiece stage of the test apparatus. A standard silicon carbide grinding wheel with a grit size of 60 mesh and a hardness of K grade was used as the grinding object. A constant grinding pressure of 20 N, a grinding wheel speed of 1500 r / min, and a sample feed speed of 10 mm / s were set. A dry grinding test was continuously conducted until a large area of the abrasive layer of the sandpaper showed signs of failure. The total grinding time and the cumulative material removal were recorded. The abrasion resistance and actual grinding service life of each group of samples were comprehensively evaluated based on the material removal rate per unit time and the total grinding amount before failure.
[0057] Table 1: Test results of sample performance in each embodiment and comparative example Note: All data in the table are the arithmetic mean of three parallel test results.
[0058] As can be seen from Examples 1-3 and Comparative Example 1 and Table 1, the surface conditioning treatment of abrasives can optimize the electrostatic properties of the particle surface, reduce the charge difference of abrasives with different particle sizes, and at the same time build an interface transition layer between the abrasive and the adhesive layer to improve the anchoring bond. This raw material pretreatment method, together with the subsequent fluidized charging and electric field sand planting process, can simultaneously improve the sand planting uniformity and the wear resistance of the finished product.
[0059] As can be seen from Examples 1-3 and Comparative Example 2, and Table 1, the same polarity biased conductive grid between adjacent electric fields can constrain the lateral diffusion of abrasive by relying on the repulsive effect of like charges, clearly separate the deposition intervals corresponding to each electric field, and avoid deposition interference between abrasives in adjacent electric fields. This is a key structural design to improve the uniformity of the overall sand planting density.
[0060] As can be seen from Examples 1-3 and Comparative Example 3, and Table 1, the zoned collaborative control mode with multiple independent high-voltage electric fields corresponding to quantitative feeding points can independently and accurately adjust the sand planting state in different material feeding zones, effectively correcting local sand planting density deviations. Compared with the unified material supply and pressure regulation mode, it can achieve more refined sand planting density control.
[0061] Combining Examples 1-3 and Comparative Example 4 with Table 1, it can be seen that the fluidized pre-charging combined with real-time coordinated control of charge-to-mass ratio can enable the mixed abrasive to obtain a more uniform and stable surface charge in the suspended state, ensuring that the movement trajectory of the abrasive after entering the sand-planting electric field is more consistent. Compared with conventional falling charging, it is more suitable for the uniform sand-planting requirements of multi-particle-size mixed abrasives.
[0062] As can be seen from Examples 1-3 and Comparative Example 5, and Table 1, the feedforward adjustment of the base adhesive thickness before sand planting can predict the fluctuation of the adhesive layer and correct the electric field parameters in advance. It forms a double closed-loop control loop with the feedback adjustment of the abrasive layer thickness after sand planting, which effectively improves the adjustment response speed and sand planting accuracy. The control effect is better than the single feedback adjustment mode.
[0063] As can be seen from Examples 1-3 and Comparative Example 6, and Table 1, the complete sand-planting process proposed in this application, through the mutual coordination of raw material modification, fluidized uniform loading, zoned collaborative control, grid drift limiting and dual closed-loop control, is significantly superior to conventional electrostatic sand-planting methods in the industry in terms of sand-planting uniformity, abrasive bonding strength and finished product wear resistance. The overall technological progress is evident.
[0064] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.
Claims
1. A method for uniformly applying abrasive to sandpaper, characterized in that: Includes the following steps: S1. Parameter preset: Select abrasives of different particle sizes and mix them according to a preset mass ratio to obtain mixed abrasives. Preset the fluidization and pre-charge operation parameters. Arrange multiple sets of independent adjustable high-voltage electric fields along the material feeding direction of the substrate. Each set of electric fields is matched with a corresponding quantitative feeding point. A conductive grid is arranged horizontally between two adjacent sets of electric fields and a bias voltage consistent with the polarity of the abrasive charge is passed through the grid. Thickness detection process is set before and after the sand planting process. S2, Fluidized homogenized material: The mixed abrasive is fed into a horizontal insulated fluidized chamber, and clean and dry compressed air is introduced to make the abrasive in a fully fluidized state. A DC electric field is applied to make the fluidized abrasive acquire surface charge, and the electric field strength and fluidized gas velocity are synergistically controlled. S3. Grouped sand planting: The substrate coated with base adhesive passes through the sand planting electric field area at a uniform speed. Each feeding point will uniformly transport the charged abrasive to the corresponding electric field interval. Under the action of the Coulomb force of the electric field, the abrasive is vertically implanted into the base adhesive layer along the direction of the electric field line. The output voltage of each group of electric fields and the feeding rate of the corresponding point are adjusted synchronously. S4. Grid-based drift limiting: A conductive grid applies a repulsive force of like charges to the abrasive, separating the deposition regions corresponding to adjacent electric fields. S5. Pre-drying and shaping: The substrate with sand-coated material is sent into a segmented drying tunnel for drying.
2. The method for uniformly applying abrasive to sandpaper according to claim 1, characterized in that: In step S1, the high-voltage electric field is set up in 3 to 5 groups, and each group of high-voltage electric field is arranged in a one-to-one correspondence with the quantitative feeding point.
3. The method for uniformly applying abrasive to sandpaper according to claim 1, characterized in that: In step S1, the mixed abrasive is composed of two to three different abrasive particles. The abrasive is pre-treated with a surface-modifying component, which includes a silane coupling agent and nano-fumed silica. The abrasive is one or more of corundum, silicon carbide, zirconium corundum, or ceramic corundum. The particle size range of the mixed abrasive does not exceed four particle size numbers.
4. The method for uniformly applying abrasive to sandpaper according to claim 1, characterized in that: In step S2, the initial fluidizing gas velocity of the fluidizing pre-charge is 0.5 m / s to 1.2 m / s, the initial DC charging voltage applied in the cavity is 2 kV to 8 kV, and the electric field is applied in a parallel vertical arrangement.
5. The method for uniformly applying abrasive to sandpaper according to claim 1, characterized in that: In step S2, the coordinated control is achieved by collecting the average charge-to-mass ratio data of the discharged abrasive at the discharge position in real time, comparing the measured value with the preset target value, and then dynamically adjusting the output voltage of the charged electric field and the fluidizing gas velocity.
6. The method for uniformly applying abrasive to sandpaper according to claim 1, characterized in that: In step S3, the charged abrasive is transported to each unloading point through a sealed, insulated channel with an inner wall covered by polytetrafluoroethylene. The air source for the transport is dry compressed air with a relative humidity of no more than 40%, and the abrasive is kept charged throughout the process.
7. The method for uniformly applying abrasive to sandpaper according to claim 1, characterized in that: In step S1, the bias voltage amplitude of the conductive grid is 10% to 15% of the corresponding main electric field voltage, and the grid aperture is 3 to 5 times the maximum particle size of the mixed abrasive.
8. The method for uniformly applying abrasive to sandpaper according to claim 1, characterized in that: In step S1, the thickness detection process includes detecting the thickness of the base adhesive before sand planting and detecting the thickness of the abrasive layer after sand planting; before sand planting, the thickness of the wet film of the base adhesive is detected in real time and the initial voltage of the corresponding electric field group is adjusted forward; after sand planting, the thickness of the abrasive layer is detected in real time and the electric field voltage and feeding rate are adjusted in feedback, forming a double closed-loop adjustment circuit of feedforward and feedback.
9. The method for uniformly applying abrasive to sandpaper according to claim 1, characterized in that: In step S3, the specific method for synchronously adjusting the voltage of each group of electric fields and the feeding rate of the corresponding point is as follows: when the sand density of the corresponding interval is lower than the target value, the output voltage of the electric field group and the feeding rate of the corresponding point are increased synchronously; when the sand density of the corresponding interval is higher than the target value, the output voltage of the electric field group and the feeding rate of the corresponding point are decreased synchronously.
10. The method for uniformly applying abrasive to sandpaper according to claim 1, characterized in that: In step S5, the dried substrate undergoes a series of processes including adhesive coating, main drying, high-temperature curing, flexible humidification, slitting, and winding to obtain the finished product.