High-impact-resistant flame-retardant bamboo-wood composite board, and preparation method and application thereof
By hot-pressing core-shell structured bamboo powder masterbatch and microfiber-toughened wood powder and spraying polystyrene-based carbide dispersion onto the surface, a multi-scale synergistic system was constructed, which solved the problem of mechanical property degradation when improving the flame retardancy of bamboo-wood composite materials. This enabled the preparation of bamboo-wood composite boards with high impact resistance, high flame retardancy, and environmental friendliness.
Patent Information
- Application Number
- CN202610598688.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-04-30
- Publication Date
- 2026-11-20
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to a composite board, its preparation method, and its application, specifically to a high-impact flame-retardant bamboo-wood composite board, its preparation method, and its application. Background Technology
[0002] Bamboo-wood composite materials, with their core advantages of being renewable, low-pollution, and having balanced mechanical properties, have become a core material replacing solid wood and traditional engineered wood products in fields such as building decoration, furniture manufacturing, and packaging logistics, and are entering a stage of rapid development. However, as application scenarios expand towards high-end and stringent requirements, most need to meet flame retardant requirements, and existing technologies generally face a core contradiction: while improving flame retardant performance, mechanical properties, especially impact resistance, often deteriorate.
[0003] The common approach to improving flame retardant performance using existing technologies involves compounding flame retardant components and impregnation modification. For example, CN108995012A discloses a method for preparing flame-retardant and smoke-suppressing bamboo-wood composite engineered wood, which involves water immersion and microwave treatment of bamboo bundles, followed by compounding with wood bundles, aiming to achieve flame retardant and smoke-suppressing effects. However, these methods often rely on large amounts of inorganic flame retardants or chemical impregnation. While improving flame retardancy, this may damage the inherent toughness of bamboo and wood fibers, leading to increased brittleness and decreased impact resistance. Furthermore, the introduction of large amounts of additives often affects the environmental friendliness of the material.
[0004] To address the mechanical losses caused by relying solely on flame retardancy, existing technologies attempt to develop novel adhesive systems. For example, CN120024089A discloses a long-lasting flame-retardant and deformation-resistant composite board, its preparation method, and its application. This involves constructing a bridging layer using a magnesium-based adhesive containing carbon quantum dots to improve the board's flame retardancy and dimensional stability. CN116572336A discloses a bamboo and wood board modifier, its preparation method, and its application, which simultaneously enhances both flame retardancy and mechanical properties. However, these technologies primarily focus on improving the adhesive itself, offering insufficient targeted solutions to the fundamental problem of improving the physical-chemical interface between bamboo and wood fibers and fillers. Weak interfacial bonding remains a major cause of stress concentration and poor impact energy absorption.
[0005] In summary, while existing technologies have explored various approaches, they all have limitations: flame retardancy and mechanical reinforcement methods are disconnected, lacking a systematic solution for integrated collaborative design across multiple scales from the interface to the matrix to the surface. This makes it difficult for current bamboo-wood composite materials to simultaneously meet the high impact resistance requirements of high-end applications (such as cantilever beam notched impact strength ≥15 kJ / m²) while maintaining eco-friendliness. 2This invention addresses the stringent requirements of high impact resistance and flame retardancy (e.g., limiting oxygen index ≥28%, UL-94 vertical flammability rating V-0). Therefore, this invention aims to overcome existing technological bottlenecks and propose a high-impact, flame-retardant bamboo-wood composite board, its preparation method, and its applications. Summary of the Invention
[0006] The technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art and provide a high-impact and flame-retardant bamboo-wood composite board and its application, which is characterized by high impact resistance, high flame retardancy, green environmental protection, readily available raw materials, and low cost.
[0007] The further technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art and provide a method for preparing high impact-resistant and flame-retardant bamboo-wood composite boards with interconnected process steps, continuous process, simple operation, controllable reaction, simple processing, controllable cost, and easy mass production.
[0008] The technical solution adopted by the present invention to solve its technical problem is as follows: a high impact-resistant and flame-retardant bamboo-wood composite board, mainly composed of a primary composite board formed by hot pressing a mixture of core-shell structure reinforced bamboo powder masterbatch and microfiber toughened wood powder, and then spraying a polystyrene-based carbide dispersion onto the surface to form a ceramic barrier coating.
[0009] The inventive concept of this invention is as follows: abandoning simple physical compounding, through chemical and biological modification and multi-scale structural design, starting from the perspective of interfacial chemical bonding, the microfibers of wood flour exposed and the core-shell reinforcing units are interpenetrated through hot pressing, and a continuous, graphite-rich polystyrene-based carbide dense barrier layer is constructed on the matrix surface. This creates a three-dimensional interpenetrating network gradient synergistic system of "core-shell structure interfacial chemical bonding - bio-enzymatic matrix toughening - continuous ceramic dense barrier on the surface", which fundamentally solves the industry problems of weak interfacial bonding, poor stress transmission, and mutual constraints between flame retardancy and mechanical properties, and achieves a leapfrog improvement in the comprehensive performance of materials.
[0010] Preferably, the mass ratio of the core-shell structured reinforced bamboo powder masterbatch to the microfiber-reinforced wood powder is 20–60:80–40 (more preferably 25–55:75–45). This ratio establishes the "skeleton" and "core" of the composite board. If the core-shell structured reinforced bamboo powder masterbatch is used in insufficient quantities as a reinforcing unit, the dominant "core-shell" reinforcing effect (skeleton) is insufficient, resulting in limited improvement in material strength and flame retardancy. If the amount is excessive, the material becomes too "rigid," with a relatively insufficient tough wood powder (core) network, disrupting the continuous tough phase formed by the wood powder, potentially leading to increased brittleness and decreased impact resistance. Conversely, the microfiber-reinforced wood powder, as a toughening unit, provides a continuous tough matrix at the stated ratio, ensuring basic processability and impact resistance. In practical applications, the ratio can be adjusted within this range according to the target performance (emphasis on strength or toughness).
[0011] Preferably, the spraying amount of the polystyrene-based carbide dispersion is 50–300 g / m². 2 (More preferably 100-200 g / m 2 The amount of coating applied directly determines the thickness and integrity of the barrier layer. If the amount applied is too low, it is difficult to form a continuous, defect-free, dense coating, making it difficult to create an effective fire barrier; if the amount applied is too high, the coating will be too thick, resulting in higher costs, potentially poorer adhesion to the substrate, and easy peeling under stress. In practical applications, the amount of coating applied can be calculated based on the solid content of the carbide dispersion and the target dry film thickness.
[0012] Preferably, the solid content of the polystyrene-based carbide dispersion is 5-15% (more preferably 8-12%). The solid content affects the spraying processability and coating quality. If the solid content is too low, the dispersion is too thin, and the dry film formed by a single spray is too thin, requiring multiple sprays to achieve the target coating amount, resulting in low efficiency and difficulty in controlling coating uniformity. If the solid content is too high, the dispersion has high viscosity, poor spray atomization effect, and is prone to forming uneven thick coatings, sagging, and cracking during drying.
[0013] Preferably, the solvent in the polystyrene-based carbide dispersion includes water and / or alcohol solvents, etc.
[0014] Preferably, the alcohol solution includes ethanol, etc.
[0015] Preferably, when the solvent is an alcohol-water solvent, the volume fraction of water is ≤30%.
[0016] Preferably, the preparation method of the polystyrene-based char is as follows: placing the polystyrene-based material in an inert atmosphere, heating it to a programmed temperature, carbonizing it at a constant temperature, cooling it, and pulverizing it to obtain the final product. The purpose of carbonizing the polystyrene-based material is to obtain a polystyrene-based char with a specific porous structure and surface activity. This char has both a high specific surface area and abundant surface active sites, which can serve as both a physical barrier and a reinforcing skeleton, and is also easy to achieve interface strengthening through chemical grafting. It is an ideal filler for synergistically improving mechanical and flame-retardant properties.
[0017] Preferably, the heating rate of the programmed temperature rise is 3–15 °C / min (more preferably 5–10 °C / min). The heating rate is crucial for controlling the pyrolysis behavior of the precursor. If the heating rate is too low, the pyrolysis will be too slow, resulting in low production efficiency and poor economics, and may also lead to unfavorable rearrangement of intermediate products. If the heating rate is too high, the precursor may be heated unevenly, resulting in inconsistent pyrolysis product structures, affecting batch stability. Furthermore, the volatile small molecules generated by rapid pyrolysis may cause the material's pore structure to collapse or generate numerous cracks, affecting the integrity of the carbonized structure. At the preferred heating rate, uniform heat transfer can be ensured, allowing polystyrene to undergo orderly pyrolysis and carbonization, forming a well-developed and stable hierarchical porous structure.
[0018] Preferably, the carbonization temperature is 400–700°C (more preferably 450–680°C, even more preferably 500–600°C), and the time is 1–5 h (more preferably 2–4 h). Temperature directly determines the chemical structure and graphitization degree of the carbonized material. If the carbonization temperature is too low, the polystyrene pyrolysis is incomplete, leaving a large number of aliphatic chain structures in the product. This results in a low degree of carbonization, difficulty in forming graphite microcrystals, low carbon skeleton strength, poor thermal stability, and insufficient specific surface area and flame-retardant catalytic activity. If the carbonization temperature is too high, the graphite microcrystals overgrow and become ordered, leading to an excessively high degree of graphitization. While this enhances conductivity, it significantly reduces the specific surface area, and the carbonized material tends to form an inert, dense structure with fewer oxygen-containing functional groups on the surface. This is detrimental to subsequent chemical bonding with silane coupling agents and increases energy consumption. At the optimal carbonization temperature, sufficient pyrolysis and ordered carbonization can occur, which is typical for forming a "disordered layer graphite structure" with a moderate degree of graphitization (ID / IG value of approximately 1.0–1.2) and well-developed nanopores. This allows for the formation of high specific surface areas (>400 m²). 2 The optimal balance between abundant surface active sites and sufficient graphite sheet strength is achieved. Carbonization time affects the completeness and uniformity of the carbonization process; if the carbonization time is too short, the core may be incompletely carbonized, resulting in an uneven structure and numerous defects; if the carbonization time is too long, the improvement in structural performance will plateau, significantly reducing the marginal effect of structural enhancement, becoming uneconomical, and potentially leading to the sintering closure of already formed micropores; under the optimal carbonization time, it can ensure that the precursor is fully and uniformly converted into the target carbon compound.
[0019] Preferably, the polystyrene-based material includes one or more of polystyrene, polyethylene terephthalate, or polyethylene methylene.
[0020] Preferably, the pulverized material is passed through a 1500-mesh sieve.
[0021] Preferably, the inert atmosphere includes nitrogen and / or argon, etc. The inert atmosphere used in this invention is a high-purity atmosphere with a purity ≥ 99.999%.
[0022] Preferably, the preparation method of the core-shell structure reinforced bamboo powder masterbatch is as follows: bamboo powder, polystyrene-based carbide, and silane coupling agent are mixed with an alcohol solution, and a solvothermal reaction is carried out in a closed reactor, followed by drying. Through a stirring (in-situ grafting) reaction, a core-shell structure reinforcing unit is prepared in an alcohol solvent, with polystyrene-based carbide having specific porosity and active surfaces as the reinforcing core, silane coupling agent as the molecular bridge, and bamboo powder as the shell. This process allows the carbide to be firmly anchored (bonded and wrapped) to the bamboo powder surface through chemical bonds (such as covalent bonds formed by silane coupling agents), fundamentally solving the interfacial compatibility problem between fillers and fibers, and achieving efficient stress transfer.
[0023] It must be pointed out that the polystyrene-based charcoal used to prepare the core-shell structure reinforced bamboo powder masterbatch and the polystyrene-based charcoal in the dispersion used for spraying are prepared by the same process and have the same physicochemical characteristics. Spraying a polystyrene-based charcoal dispersion with consistent internal and external charcoal structures is key to achieving "synergistic flame retardancy," ensuring that under fire conditions, the surface coating and the internal reinforcing units have similar coefficients of thermal expansion, enabling synchronous and coordinated thermal response and char formation behavior. Together, they construct a continuous and stable expanded char layer from the outside to the inside, forming an integrated, highly efficient charcoal protective layer that maximizes physical insulation and thermocatalytic flame retardant effects. Using charcoal from different sources or with different properties may result in differences in their thermal behavior, weakening the synergistic effect.
[0024] Preferably, the mass ratio of bamboo powder, polystyrene-based charcoal, and silane coupling agent is 50–80:20–40:5–20 (more preferably 50–70:20–40:10–20, and even more preferably 60–70:25–35:10–15). This mass ratio aims to maximize effective coating of the filler and strong interfacial bonding. If the amount of polystyrene-based charcoal is too low, the reinforcing phase will be insufficient, resulting in limited reinforcement and flame retardant enhancement of the matrix; if the amount of polystyrene-based charcoal is too high, the bamboo powder will be difficult to completely coat, easily leading to charcoal agglomeration and stress defects in the matrix. If the amount of coupling agent is too low, it will be insufficient to form a complete chemical bond bridging network between the bamboo powder and a large number of polystyrene-based charcoal particles; if the amount of coupling agent is too high, the excessive coupling agent may self-aggregate to form a brittle layer (weak interfacial layer), which will damage the interfacial performance and increase costs. Under optimal ratios, bamboo powder can form a relatively complete and sufficient coating on carbonaceous materials, while the amount of coupling agent is sufficient to meet the requirements for forming a monolayer chemical bridge, achieving the most efficient interface strengthening and constructing a strong and tough chemical interface.
[0025] Preferably, the amount of the alcohol solution used is 20-50% (more preferably 25-40%) of the bamboo powder mass.
[0026] Preferably, the solvothermal reaction temperature is 50–120°C (more preferably 60–110°C), the rotation speed is 100–300 r / min, and the time is 0.5–4.0 h (more preferably 1–3 h). These solvothermal reaction conditions drive the hydrolysis, condensation, and grafting reaction of the silane coupling agent onto the bamboo powder / carbonite surface, collectively determining its completeness. If the reaction temperature, pressure, or time is too low, the reaction kinetics are insufficient, the reaction is incomplete, and the "bridging" effect of the silane coupling agent cannot be fully utilized, resulting in weak interfacial bonding between the carbonite and bamboo powder, and an unstable "core-shell" structure. If the reaction temperature, pressure, or time is too high, excessive solvent evaporation and increased side reactions may occur, or even thermal degradation of surface groups on the bamboo powder or carbonite may occur, which is also detrimental to the formation of a stable "core-shell" structure. The preferred conditions ensure efficient and complete reaction, forming a strong chemically bonded interface.
[0027] Preferably, the solvothermal reaction mixture accounts for 30-70% (more preferably 40-60%) of the reactor volume. When the reaction temperature is too low and the mixture accounts for too small a volume of the reactor, the pressure is low; when the reaction temperature is too high and the mixture accounts for too large a volume of the reactor, the pressure is high.
[0028] Preferably, the bamboo powder has a particle size that passes through an 80-200 mesh sieve and a moisture content of <5%. The bamboo powder of this invention is derived from bamboo processing residues, such as bamboo shavings and bamboo branches.
[0029] Preferably, the silane coupling agent includes one or more of γ-aminopropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, vinyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, or isocyanate-based silane. The amino group in the silane coupling agent can react with the oxygen-containing groups on the surface of the charcoal, while the ethoxy group can react with the hydroxyl groups on the surface of the bamboo powder, making it a preferred bridge for establishing a chemical bond between "bamboo powder-coupling agent-charcoal".
[0030] Preferably, the alcohol solution comprises an alcohol solvent or an aqueous solution thereof, wherein the volume fraction of water in the aqueous alcohol solvent solution is ≤30%.
[0031] Preferably, the alcohol solvent includes ethanol, etc.
[0032] Preferably, the preparation method of the microfiber-toughened wood flour is as follows: wood flour is dispersed in a buffer solution, amylase is added, enzymatic hydrolysis is performed, the mixture is heated to inactivate the amylase, and then washed and dried. After dispersing the wood flour in the buffer solution and adding amylase, the amylase can specifically act on the starch and hemicellulose components in the wood flour, that is, to bioactivate the wood flour with amylase. Through enzymatic hydrolysis, the amorphous regions on the surface and shallow layer of the wood flour are selectively degraded, effectively breaking down the dense structure on the surface of the wood flour fibers, significantly exposing the hydroxyl (-OH) and carboxyl (-COOH) active groups on the cellulose and lignin molecular chains of the wood flour, increasing its surface reactivity and toughening potential, and constructing toughening network units.
[0033] Preferably, the mass-to-volume ratio of the wood flour to the buffer solution is 1:5 to 20 (more preferably 1:8 to 16).
[0034] Preferably, the pH value of the buffer solution is 4.8 to 7.0.
[0035] Preferably, the amount of amylase used is equivalent to 0.3 to 3.0% (more preferably 1 to 2%) of the wood flour mass.
[0036] Preferably, the enzymatic hydrolysis temperature is 38–65°C (more preferably 40–55°C) and the time is 1–8 h (more preferably 1–7 h, and even more preferably 3–5 h).
[0037] If the pH value or temperature exceeds the above range, the enzyme activity will decrease sharply or even become inactive. If the amount of amylase used is too low or the time is too short, the degradation of starch and some hemicellulose in wood flour will be insufficient, and the microfibrillation effect will be weak. If the amount of amylase used is too high or the time is too long, it will not only be uneconomical, but may also excessively erode the fiber, destroy its own strength, and will not help improve performance.
[0038] Preferably, the inactivation temperature is 85–95°C and the time is 10–30 min.
[0039] Preferably, the wood flour has a particle size that passes through an 80-200 mesh sieve and a moisture content of <5%. The wood flour of this invention is derived from fast-growing forest timber, such as poplar and fir.
[0040] Preferably, the buffer solution includes phosphate buffer, citrate-sodium citrate buffer, or acetate-sodium acetate buffer, etc.
[0041] Preferably, the amylase has an enzyme activity of ≥3000 U / g.
[0042] Preferably, the amylase includes α-amylase and / or β-amylase, etc.
[0043] Preferably, when α-amylase and β-amylase are used in combination, the mass ratio of α-amylase to β-amylase is 1–4:1 (more preferably 2–3:1). α-amylase (an endopeptidase) randomly cleaves the α-1,4 glycosidic bonds within starch, while β-amylase (an exopeptidase) sequentially cleaves maltose units from the non-reducing end. The combination of α-amylase and β-amylase produces a synergistic effect, resulting in faster, more efficient, and more thorough degradation of both linear and amylopectin in wood flour, more effectively exposing the internal cellulose microfibril network, thereby maximizing the specific surface area, reactivity, and interpenetration binding capacity with reinforcing units of the wood flour. Within the specified ratio range, the optimal balance between efficiency and effectiveness is achieved, maximizing the exposure of cellulose microfibrils; if the ratio range is exceeded, the synergistic effect weakens.
[0044] The technical solution adopted by the present invention to further solve its technical problem is as follows: A method for preparing a high-impact flame-retardant bamboo-wood composite board, comprising the following steps: (1) Mixing and molding: After uniformly mixing the core-shell structure reinforced bamboo powder masterbatch with microfiber toughened wood powder, place it in a mold and hot press it to obtain a primary composite board; (2) Curing and molding: The polystyrene-based carbide dispersion is sprayed onto the surface of the primary composite board obtained in step (1), dried and cured to obtain a high impact-resistant and flame-retardant bamboo-wood composite board.
[0045] The inventive concept of this invention is as follows: core-shell structure reinforced bamboo powder masterbatch is blended with microfiber toughened wood powder and hot-pressed. During this process, the wood powder microfibers and bamboo powder coated with carbonaceous interpenetrate and entwine with each other. Through hot pressing, the hydrogen bond network of the thermoplastic components of the bamboo and wood fibers interacts to form a stable three-dimensional interpenetrating network matrix. This is a mechanism to improve the strength and toughness of the matrix by optimizing the fiber arrangement. On the surface of the formed matrix, a layer of polystyrene-based carbonaceous dispersion is sprayed to form a dense and continuous surface ceramic barrier layer. This coating is homologous with the internal reinforcing units and can synergistically catalyze carbonization under fire conditions. Together with the internal network, it forms an effective physical and chemical barrier, significantly delaying the transfer of heat and oxygen.
[0046] Preferably, in step (1), the hot pressing temperature is 150–190°C (more preferably 160–185°C), the pressure is 3–9 MPa (more preferably 5–7 MPa), and the time is 5–20 min (more preferably 10–20 min). The hot pressing temperature needs to soften, melt, and flow the thermoplastic components such as lignin and hemicellulose in the bamboo and wood fibers, thus acting as a good natural adhesive. If the hot pressing temperature is too low, the plasticization will be insufficient, the bonding force will be weak, the board will have many internal pores, and the strength will be poor. If the hot pressing temperature is too high, it will easily lead to thermal decomposition of components, darkening of color, and deterioration of mechanical properties. The hot pressing pressure is used to expel gas and promote material flow and close contact. If the hot pressing pressure is too low, the bonding between units will be weak, and the densification will be poor. If the hot pressing pressure is too high, the fiber structure may be over-compressed, resulting in excessive density of the board, decreased toughness, and increased equipment burden.
[0047] Preferably, in step (2), the drying and curing temperature is 60-100℃ (more preferably 70-90℃) and the time is 1-4h (more preferably 2-3h).
[0048] The technical solution adopted by the present invention to further solve its technical problem is as follows: an application of a high impact-resistant and flame-retardant bamboo-wood composite board, which is applied to the technical fields of preparing building decoration materials, transportation vehicle interior materials, furniture manufacturing materials, aerospace interior materials, outdoor facilities and municipal engineering materials, packaging materials or electronic device shell materials.
[0049] The beneficial effects of this invention are as follows: (1) The polystyrene-based carbonized material used in the high impact-resistant and flame-retardant bamboo-wood composite board of the present invention has a porous structure that can form a "mechanical interlock" with the fibers of bamboo and wood materials. At the same time, the surface active groups (such as hydroxyl and carboxyl groups) generated by oxidation during carbonization can undergo hydrogen bonding or chemical cross-linking with the hydroxyl groups of bamboo and wood fibers, thereby improving the mechanical properties of the composite material. (2) The core-shell structure reinforced bamboo powder masterbatch used in the high impact-resistant and flame-retardant bamboo-wood composite board of the present invention solves the defects of pure bamboo powder such as easy moisture absorption, low strength and single function through the synergistic effect of "high temperature physical mixing + crosslinking agent chemical bonding + alcohol solvent dispersion". At the same time, it strengthens the load stability of polystyrene-based carbides and finally gives the masterbatch multiple advantages. Meanwhile, the physicochemical synergistic effect achieves the firm loading of polystyrene-based carbides on the surface of bamboo powder. (3) The microfiber toughened wood powder used in the high impact and flame retardant bamboo and wood composite board of the present invention is activated by amylase catalysis, which can achieve efficient and precise improvement of the surface activity of wood powder. The enzyme catalysis process is mild and avoids the problems of wood powder fiber structure damage and mechanical property decline caused by traditional chemical activation. The flexural strength retention rate of activated wood powder is more than 90%, and there is no chemical reagent residue pollution. In addition, the whole process adopts biological enzyme catalysis, the reaction process is green and environmentally friendly, and there is no toxic and harmful waste discharge, which meets the requirements of green manufacturing and sustainable development, and significantly reduces the environmental protection treatment cost in industrial production. (4) The high impact-resistant and flame-retardant bamboo-wood composite board of the present invention can achieve a synergistic improvement in the flame-retardant performance and comprehensive performance of the board by spraying a layer of polystyrene-based carbide dispersion; the dense flame-retardant protective layer formed after curing has excellent flame-retardant performance: on the one hand, the high temperature resistance and flame-retardant properties of polystyrene-based carbide can directly block the contact between the flame and the substrate of the board, and delay heat conduction; on the other hand, when exposed to fire, the protective layer can quickly form a continuous and dense carbonized barrier layer, effectively suppressing the release of combustible gases generated by the thermal decomposition of the substrate, while reducing the smoke density. (5) The impact strength of the high-impact flame-retardant bamboo-wood composite board of the present invention is ≥18 kJ / m 2 Flexural strength ≥ 50 MPa; Elastic modulus ≥ 4.5 GPa; Limiting oxygen index (LOI) ≥ 30%; UL-94 V-0 rating with no dripping; 24h water absorption thickness swelling rate ≥ 7.9%; Formaldehyde emission ≤ 0.035 mg / m³ 3 Compared to existing high-performance bamboo-wood composite boards, it is green and environmentally friendly, and the raw materials are readily available. (6) The method of the present invention adopts the masterbatch method to pre-construct the reinforcing unit. The process steps are closely linked, the process is continuous, and the operation is simple. It has the characteristics of uniform material mixing, controllable reaction, simple processing, controllable cost, and easy large-scale production. Detailed Implementation
[0050] The present invention will be further described below with reference to the embodiments.
[0051] The raw materials used in the embodiments and comparative examples of this invention are as follows: bamboo powder: processing residue of moso bamboo, passed through an 80-mesh sieve, with a moisture content of <5%; wood powder: fast-growing poplar, passed through an 80-mesh sieve, with a moisture content of <5%; silane coupling agent: γ-aminopropyltriethoxysilane (KH-550), chemically pure; amylase: food-grade α-amylase (enzyme activity ≥4000 U / g) and β-amylase (enzyme activity ≥3000 U / g), commercially available; disodium hydrogen phosphate, sodium dihydrogen phosphate, anhydrous ethanol, etc., are all analytically pure; nitrogen: purity ≥99.999%; unless otherwise specified, the raw materials or chemical reagents used in the embodiments and comparative examples of this invention are obtained through conventional commercial channels.
[0052] Examples 1-16 of this invention (Ex.1-16) employ an L16 (45) orthogonal array design to systematically investigate the effects of five core factors: carbonization temperature (A) for preparing polystyrene-based carbon, ratio of bamboo powder, polystyrene-based carbon, and silane coupling agent in core-shell reinforced bamboo powder masterbatch (B), enzymatic hydrolysis time (C) for preparing microfiber toughened wood powder, mass ratio of core-shell reinforced bamboo powder masterbatch to microfiber toughened wood powder (D), and hot pressing pressure (E) for preparing high-impact flame-retardant bamboo-wood composite board. The feasibility of the scheme is demonstrated while selecting the optimal conditions, as shown in Table 1.
[0053] Table 1. Orthogonal design process parameters for embodiments 1-16 of the present invention.
[0054] Examples 1-16 of a high-impact flame-retardant bamboo-wood composite board The high-impact and flame-retardant bamboo-wood composite board is mainly composed of core-shell structure reinforced bamboo powder masterbatch and microfiber toughened wood powder mixed at a mass ratio D (see parameter D in Table 1) and hot-pressed into a primary composite board surface with a spraying amount of 150 g / m². 2 A ceramicized barrier coating is formed by spraying a polystyrene-based carbide alcohol-water dispersion with a solid content of 10% (water to ethanol volume ratio of 20:80). The preparation method of the polystyrene-based carbon is as follows: polystyrene is placed in a nitrogen atmosphere and heated to A ℃ (see parameter A in Table 1) at a heating rate of 5℃ / min. After being carbonized at a constant temperature for 2 hours, it is cooled, pulverized and passed through a 1500-mesh sieve to obtain the product. The preparation method of the core-shell structure reinforced bamboo powder masterbatch is as follows: bamboo powder, polystyrene-based carbon compound, and γ-aminopropyltriethoxysilane are mixed with ethanol at a mass ratio B (see parameter B in Table 1), with the amount of ethanol being 35% of the mass of bamboo powder. The mixture is carried out in a closed reactor at 100°C and a rotation speed of 200 r / min, with the mixed raw materials occupying 50% of the reactor volume, and subjected to a solvothermal reaction for 2 hours. After drying, the masterbatch is obtained. The preparation method of the polystyrene-based carbon compound is the same as above. The preparation method of the microfiber-toughened wood flour is as follows: wood flour is dispersed in a phosphate buffer solution (containing disodium hydrogen phosphate and sodium dihydrogen phosphate, prepared by conventional method) at a mass-to-volume ratio of 1:10 g / mL. A compound amylase (the mass ratio of α-amylase to β-amylase is 2:1) equivalent to 1.0% of the wood flour mass is added. After enzymatic hydrolysis at 50℃ for C h (see C parameter in Table 1), the mixture is inactivated at 90℃ for 20 min, washed, and dried to obtain the final product.
[0055] A method for preparing a high-impact, flame-retardant bamboo-wood composite board: Examples 1-16 (1) Mixing and molding: The core-shell structure reinforced bamboo powder masterbatch and microfiber toughened wood powder are mixed evenly at a mass ratio D (see parameter D in Table 1), and then placed in a mold. They are hot-pressed for 10 minutes at 175℃ and E MPa (see parameter E in Table 1) to obtain a primary composite board. (2) Curing and molding: A polystyrene-based carbide alcohol-water dispersion with a solid content of 10% (water to ethanol volume ratio of 20:80) is sprayed at a rate of 150 g / m. 2 Spray the coating onto the surface of the primary composite board obtained in step (1), and dry and cure it at 80°C for 2 hours to obtain a high-impact flame-retardant bamboo-wood composite board.
[0056] To evaluate the performance of the high impact-resistant and flame-retardant bamboo-wood composite boards obtained in Examples 1-16 of the present invention, the following tests were conducted: Notched impact strength of cantilever beam: according to ASTM D256 standard, the specimen size is 80mm×10mm×4mm, and the notch depth is 2mm; Bending strength and bending modulus: according to ASTM D790 standard, span 64mm, loading speed 2mm / min; Limiting oxygen index: according to ASTM D2863 standard, sample size 100mm×10mm×4mm; UL-94 vertical flammability rating: according to UL94 standard, sample size 130mm×13mm×3mm; 24h water absorption thickness expansion rate: According to ASTM D1037 standard, the sample was immersed in distilled water at 23±2℃ for 24 hours and then measured. Formaldehyde emission: based on 1m³ in GB / T 17657 3 Climate chamber method for determination; All samples were conditioned for 48 hours under a standard environment of 23±2℃ and 50±5% relative humidity before testing; the test results are shown in Table 2.
[0057] Table 2 Performance test results of the high impact-resistant and flame-retardant bamboo-wood composite boards obtained in Examples 1-16 of this invention
[0058] As shown in Table 2, the LOI value generally exhibits a parabolic trend of first increasing and then decreasing with the increase of the carbonization temperature (factor A) of polystyrene-based charcoals. The LOI of samples carbonized at 525℃ and 600℃ (Ex.5~Ex.12) is higher than 31.5%, and all of them achieve the V-0 UL-94 rating; while the LOI of samples carbonized at 450℃ (Ex.1~Ex.4) and 675℃ (Ex.13~Ex.16) is lower than 31%, and most of them are at the V-1 rating. This is because polystyrene pyrolysis is insufficient in the low-temperature region (450℃), resulting in charcoals with low graphitization, a structure dominated by amorphous carbon, insufficient specific surface area and thermal stability, and low efficiency as a physical barrier and catalytic char formation agent, resulting in mediocre flame retardant performance. The pyrolysis in the optimal temperature range (525–600℃) is thorough and orderly, generating carbides rich in disordered graphite microcrystals and abundant nanopores. This structure features a high specific surface area and a large number of active edge sites. During combustion, it not only forms a robust and dense expanded carbon layer (physical barrier) but also catalyzes the dehydration of bamboo and wood fibers into char (chemical flame retardancy), achieving a synergistic leap in LOI (Liquidity Index). Simultaneously, the carbides prepared at this temperature range have abundant surface active functional groups and the highest bonding efficiency with silane coupling agents, resulting in high levels of flexural strength and flexural modulus in the composite panels (the flexural strength of Ex.6, Ex.10, and Ex.11 all exceed 60 MPa, and the flexural modulus exceeds 6.0 GPa). In addition, the stable interface and dense structure formed in this temperature range also endow the board with excellent water resistance. The 24-hour water absorption thickness expansion rate of Ex.5 to Ex.12 is generally less than 10%, with Ex.6, Ex.10 and Ex.11 being as low as 8.5%, 8.2% and 7.9% respectively, which is significantly better than samples in other temperature ranges. Excessive graphitization in the high-temperature zone (675℃) leads to a denser and more ordered structure of the carbide, a decrease in specific surface area, and a significant reduction in surface oxygen-containing functional groups (such as -COOH and -OH). This weakens the chemical bonding ability between the carbide and the silane coupling agent, reduces its catalytic activity, and lowers its flame retardant performance. At the same time, the decrease in interfacial bonding force also leads to a significant reduction in flexural strength and flexural modulus. For example, the flexural strength of Ex.13 to Ex.16 is lower than 49.6 MPa, and the flexural modulus is lower than 4.9 GPa. Furthermore, due to poor interfacial bonding, water molecules can more easily penetrate along the interface, and its 24-hour water absorption thickness expansion rate increases to 11.0% to 12.0%, and its dimensional stability begins to deteriorate.
[0059] Table 2 shows that impact strength and LOI are sensitive to changes in the ratio of bamboo powder, polystyrene-based carbides, and silane coupling agent in the core-shell reinforced bamboo powder masterbatch. Ratios of 60:30:10 and 65:25:10 generally perform best. If the proportion of polystyrene-based carbides is too low, the reinforcing phase is insufficient, the "skeleton" strength of the composite board is inadequate, the improvement in impact performance and flame retardancy is limited, and the flexural strength and flexural modulus are also at a low level. Furthermore, due to the incomplete continuous reinforcing network in the matrix, water molecules can more easily penetrate into weak areas, resulting in a higher 24-hour water absorption thickness expansion rate. If the proportion of polystyrene-based carbides is too high, the bamboo powder is insufficient to completely coat the excess polystyrene-based carbides, leading to particle agglomeration. These agglomerates become stress concentration points, easily inducing cracks, which in turn reduces impact strength, flexural strength, and flexural modulus. Simultaneously, interfacial defects between the agglomerates and the matrix provide preferential penetration channels for water molecules, increasing the water absorption thickness expansion rate. Under optimal formulation, bamboo powder can effectively coat polystyrene-based carbon particles, forming a complete "core-shell" structure. The polystyrene-based carbon particles act as rigid reinforcing points, and are evenly dispersed. Through chemical bonding, stress is efficiently transferred to the bamboo and wood fiber network, maximizing the improvement of impact strength, flexural strength, and flexural modulus. At the same time, sufficient and well-dispersed polystyrene-based carbon particles construct a continuous flame-retardant network in the matrix. This uniform and dense structure can effectively block the penetration path of water molecules, giving the board excellent water resistance (e.g., the water absorption thickness swelling rate of Ex.6 and Ex.11 is as low as 8.5% and 7.9%, respectively).
[0060] Table 2 shows that the enzymatic hydrolysis time (factor C) has a relatively mild but clear effect on the microfibrillation toughening of wood flour. Enzymatic hydrolysis aims to selectively remove starch and some hemicellulose from the wood flour, exposing the internal cellulose microfibrils and increasing surface roughness and reactivity. If the hydrolysis time is too short, microfibrillation is insufficient, and the toughening and interfacial interpenetration effects of the wood flour are not fully realized, resulting in limited improvement in impact strength and flexural strength (for example, samples with a hydrolysis time of 1 hour in Ex.1, Ex.6, Ex.11, and Ex.16 show different performances, requiring comprehensive judgment in conjunction with other factors). At the same time, the wood flour surface has a large amount of hydrophilic substances such as starch, which easily absorb water, resulting in a higher water absorption thickness swelling rate. If the time is too long, it may cause excessive erosion of the cellulose backbone, slightly weakening the fiber strength of the wood flour itself and negatively affecting the improvement of toughness. However, the flexural modulus can still be maintained at a high level, and excessive enzymatic hydrolysis may loosen the cell wall structure of the wood flour, which may actually increase the water absorption rate. A suitable enzymatic hydrolysis time (3-5 hours) can fully activate the surface of wood flour, and the resulting microfibers can better entwine and interlock with the "core-shell" reinforcing units, and enhance the bonding through hydrogen bonding and other effects, thereby improving the toughness and comprehensive mechanical properties of the matrix. At the same time, the appropriate removal of hydrophilic starch components is beneficial to reducing the water absorption and swelling rate of the board.
[0061] Table 2 shows that the mass ratio of core-shell reinforced bamboo powder masterbatch to microfiber toughened wood powder (factor D) has a significant impact on performance. This ratio determines whether the composite material is "rigidity-dominated" or "toughness-dominated": increasing the proportion of toughening units (microfiber toughened wood powder) provides a more continuous flexible biomass network, which is beneficial for absorbing impact energy, but may dilute the reinforcing phase, reducing absolute strength, flame retardancy, flexural strength, and flexural modulus. At the same time, since wood powder itself has a certain degree of hydrophilicity, an excessively high proportion of toughening units will lead to an increase in overall water absorption. Increasing the proportion of reinforcing units (core-shell reinforced bamboo powder masterbatch) improves rigidity and flame retardancy, and flexural strength and flexural modulus increase accordingly, but too much will make the material "brittle," and the impact strength tends to decrease. Moreover, the hydrophobic properties of the carbides in the reinforcing units help to reduce water absorption. At the optimal ratio, the rigid reinforcing phase and the tough matrix phase can achieve an optimal co-continuous structure, which allows stress to be effectively dispersed throughout the three-dimensional interpenetrating network, thereby obtaining high impact strength and excellent bending performance. At the same time, the interpenetrating network structure formed at this ratio can effectively limit the diffusion of water molecules at the interface, achieving the best balance of water resistance.
[0062] As shown in Table 2, when the hot-pressing pressure (E factor) of the high-impact flame-retardant bamboo-wood composite board is too low, the board will not be sufficiently densified, resulting in numerous internal pores, low strength, and the pores may become combustion channels. Both flexural strength and flexural modulus will be at a low level. Simultaneously, these residual pores also provide capillary channels for water molecules, leading to a significant increase in the water absorption thickness expansion rate. If the pressure is too high, it may crush the microstructure of the bamboo-wood fibers, even destroying the already constructed "core-shell" units, leading to a decline in performance. While the flexural strength may remain at a high level, the impact toughness will be damaged, and excessive compaction may destroy the elastic structure of the fibers themselves, making the board more prone to irreversible expansion after water absorption. At a moderate pressure (5–7 MPa), the components can be ensured to be in close contact, promoting the flow and adhesion of thermoplastic components such as lignin in the bamboo-wood fibers, forming a strong interface without excessively damaging the fiber structure. At this point, the flexural strength and flexural modulus reach the optimal balance, and the formed dense structure can effectively block the penetration of water molecules, giving the board optimal dimensional stability.
[0063] Furthermore, as shown in Table 2, the formaldehyde release in all embodiments was less than 0.035 mg / m³. 3 It is far superior to the E0 level requirement (≤0.050 mg / m³). 3 (Among them, Ex.6, Ex.10, and Ex.11 have formaldehyde release levels as low as 0.020–0.022 mg / m³.) 3 It is far superior to the highest national environmental protection standard ENF level (≤0.025 mg / m³). 3This is thanks to the green preparation process of "core-shell structure chemical bonding" and "bio-enzymatic activation" adopted in this invention, which completely eliminates the use of traditional formaldehyde-containing adhesives, thus preventing the introduction of formaldehyde at the source and demonstrating the safety and environmental protection advantages of this invention. Meanwhile, the 24-hour water absorption thickness swelling rate and formaldehyde release show a certain trend of co-occurrence, meaning that the samples with the best overall performance (Ex.6, Ex.10, Ex.11) have both the lowest water absorption swelling rate and the lowest formaldehyde release. This indicates that the three-dimensional interpenetrating network structure and surface ceramic barrier layer constructed in this invention not only endow the board with excellent mechanical and flame-retardant properties, but also simultaneously improve its durability and environmental friendliness, achieving synergistic optimization of the material's overall performance.
[0064] Based on the above orthogonal experimental results, the optimal parameter combination was selected to form Example 17.
[0065] Example 17 of a high impact-resistant and flame-retardant bamboo-wood composite board The high-impact and flame-retardant bamboo-wood composite board is mainly composed of a core-shell structure reinforced bamboo powder masterbatch and microfiber toughened wood powder mixed at a mass ratio of 45:55 and hot-pressed into a primary composite board surface with a spray coating amount of 150 g / m². 2 A ceramicized barrier coating is formed by spraying a polystyrene-based carbide alcohol-water dispersion with a solid content of 10% (water to ethanol volume ratio of 20:80). The preparation method of the polystyrene-based carbon is as follows: polystyrene is placed in a nitrogen atmosphere, heated to 525°C at a heating rate of 5°C / min, carbonized at a constant temperature for 2 hours, cooled, and pulverized through a 1500-mesh sieve to obtain the product. The preparation method of the core-shell structure reinforced bamboo powder masterbatch is as follows: bamboo powder, polystyrene-based carbon compound, and γ-aminopropyltriethoxysilane are mixed with ethanol at a mass ratio of 60:30:10, with the amount of ethanol being 35% of the mass of bamboo powder. The mixture is carried out in a closed reactor at 100°C and a rotation speed of 200 r / min, with the mixed raw materials occupying 50% of the reactor volume, and subjected to a solvothermal reaction for 2 hours. After drying, the masterbatch is obtained. The preparation method of the polystyrene-based carbon compound is the same as above. The preparation method of the microfiber-toughened wood flour is as follows: wood flour is dispersed in a phosphate buffer solution (containing disodium hydrogen phosphate and sodium dihydrogen phosphate, prepared by conventional method) at a mass-to-volume ratio of 1:10 g / mL. A compound amylase (the mass ratio of α-amylase to β-amylase is 2:1) equivalent to 1.0% of the wood flour mass is added. After enzymatic hydrolysis at 50℃ for 3 h, the enzyme is inactivated at 90℃ for 20 min. The product is then washed and dried to obtain the final product.
[0066] Example 17: A method for preparing a high-impact, flame-retardant bamboo-wood composite board (1) Mixing and molding: The core-shell structure reinforced bamboo powder masterbatch and microfiber toughened wood powder are mixed evenly at a mass ratio of 45:55, placed in a mold, and hot-pressed at 175℃ and 5 MPa for 10 minutes to obtain a primary composite board. (2) Curing and molding: A polystyrene-based carbide alcohol-water dispersion with a solid content of 10% (water to ethanol volume ratio of 20:80) is sprayed at a rate of 150 g / m. 2 Spray the coating onto the surface of the primary composite board obtained in step (1), and dry and cure it at 80°C for 2 hours to obtain a high-impact flame-retardant bamboo-wood composite board.
[0067] To evaluate the performance of the high-impact and flame-retardant bamboo-wood composite board obtained in Example 17 of this invention, tests were conducted according to the test methods of Examples 1 to 16 of this invention. The test results are as follows: Mechanical properties: The notched impact strength of the cantilever beam is 27.1 kJ / m. 2 The bending strength is 63.1 MPa; the bending modulus is 6.2 GPa. Flame retardant performance: Limiting oxygen index is 35.5%; UL-94 vertical flammability rating is V-0 (no dripping).
[0068] Durability and environmental performance: 24-hour water absorption thickness swelling rate is 7.9%; formaldehyde emission is 0.02 mg / m³. 3 .
[0069] In summary, the test results in Table 2 clearly reveal the effects of five key process parameters, particularly the carbonization temperature (A) for preparing polystyrene-based charcoal and the ratio of bamboo powder, polystyrene-based charcoal, and silane coupling agent in the preparation of core-shell structure reinforced bamboo powder masterbatch (B), on the impact resistance (cantilever beam notched impact strength) and flame retardant properties (limiting oxygen index LOI and UL-94 rating) of the composite board. For example, when the carbonization temperature rises to 675℃ (Ex. 13~16), regardless of the combination of other parameters, the impact strength is always below 18 kJ / m. 2 Furthermore, the LOI failed to exceed 30.8%, and the UL-94 rating reverted to V-1. This strongly demonstrates the necessity of setting the upper limit of the carbonization temperature below 700℃; otherwise, the mechanical properties of the material would deteriorate significantly due to interface degradation. Similarly, at 525℃, the impact strength when the amount of polystyrene-based carbon compound was 35% (Ex.5) was lower than that when the amount of polystyrene-based carbon compound was 30% (Ex.6). This means that the proportion of polystyrene-based carbon compound is not necessarily better the higher it is. This verifies that the structural evolution introduced by the "functional carbon compound" and the interface science highlighted by the "strong interface core-shell structure" are the two cornerstones for the performance breakthrough of this invention.
[0070] Comparative Example 1 (C1, without polystyrene-based carbides) Bamboo powder masterbatch and microfiber-toughened wood powder are uniformly mixed at a mass ratio of 45:55, placed in a mold, and hot-pressed at 175℃ and 5MPa for 10 minutes to obtain the final product. The bamboo powder masterbatch is prepared by mixing bamboo powder and γ-aminopropyltriethoxysilane with ethanol at a mass ratio of 60:10, where the amount of ethanol is 35% of the mass of bamboo powder. The mixture is then subjected to a solvothermal reaction for 2 hours in a closed reactor at 100℃ and 200 r / min, with the mixed raw materials occupying 50% of the reactor volume. After drying, the final product is obtained. The preparation method of the microfiber-toughened wood powder is the same as in Example 17.
[0071] Comparative Example 2 (C2, preparation of core-shell structured reinforced bamboo powder masterbatch by physical blending method) The only difference between this comparative example and Example 17 of the composite board and its preparation method is that the preparation method of the core-shell structure reinforced bamboo powder masterbatch is as follows: bamboo powder, polystyrene-based carbide, and γ-aminopropyltriethoxysilane are mixed with ethanol at a mass ratio of 60:30:10, with the amount of ethanol being 35% of the mass of bamboo powder. The mixture is then dry-mixed in a high-speed mixer for 5 minutes and dried. The rest is the same as in Example 17 of the composite board and its preparation method.
[0072] Comparative Example 3 (C3, wood flour without enzymatic hydrolysis) The only difference between this comparative example and Example 17 of the composite board and its preparation method is that the wood flour is not enzymatically hydrolyzed, and "microfiber-toughened wood flour" is replaced with "wood flour". Otherwise, it is the same as Example 17 of the composite board and its preparation method.
[0073] Comparative Example 4 (C4, without surface ceramic barrier layer) The only difference between this comparative example and Example 17 of the composite board and its preparation method is that the spraying of the polystyrene-based carbide alcohol-water dispersion is omitted, and a ceramicized barrier coating is not formed. Otherwise, it is the same as Example 17 of the composite board and its preparation method.
[0074] Comparative Example 5 (C5, using commercial carbon black) The only difference between this comparative example and Example 17 of the composite board and its preparation method is that the "polystyrene-based carbon" in both the core-shell structure reinforced bamboo powder masterbatch and the polystyrene-based carbon alcohol aqueous dispersion is replaced with "commercial carbon black". Otherwise, it is the same as Example 17 of the composite board and its preparation method.
[0075] Comparative Example 6 (C6, existing impregnation technology) Referring to CN108995012A, bamboo and wood composite substrates of the same specifications are prepared by the following method: bamboo bundles are soaked in water and pretreated with microwave, and then bamboo bundles and wood bundles are sprayed with water-soluble phenolic resin glue, and then impregnated in water-soluble phenolic resin glue containing natural calcium and magnesium mineral powder, dried, assembled, and hot-pressed.
[0076] To evaluate the performance of the high impact-resistant and flame-retardant bamboo-wood composite boards obtained in Comparative Examples 1-6 (C1-6) of the present invention, tests were conducted according to the test methods of Examples 1-16 of the present invention; the test results are shown in Table 3.
[0077] Table 3 Performance test results of bamboo-wood composite boards obtained in Comparative Examples 1-6 of this invention
[0078] As shown in Table 3, Comparative Example 1 (C1, without polystyrene-based carbides) and Comparative Example 6 (C6, existing impregnation technology) constitute the two extremes of the performance baseline. The performance of C1 completely collapsed, with an impact strength of only 9.5 kJ / m. 2 The LOI is as low as 24.8%, and there is no UL-94 rating, directly proving that without the core functional filler polystyrene-based carbide of this invention, the material will simultaneously lose both the reinforcing phase and the highly efficient flame-retardant phase, completely reverting to the performance range of ordinary bamboo-wood composite boards. C6, on the other hand, represents the systemic limitations of the traditional "post-treatment addition" technical route, with poor mechanical properties (impact strength 11.3 kJ / m). 2 It has a flexural strength of 38.7 MPa and extremely poor water resistance (the thickness swelling rate after 24 hours of water absorption is as high as 22.2%), and the formaldehyde release is as high as 0.038 mg / m². 3 This indicates that simple external flame retardant impregnation can disrupt the hydrogen bond network of bamboo and wood fibers, introducing hygroscopic salts and causing performance conflicts. Therefore, Comparative Examples 1 and 6 together define the severity of the technical problem to be solved by the present invention and the shortcomings of existing solutions.
[0079] Table 3 shows that Comparative Example 2 (C2, physical blend) and Comparative Example 5 (C5, using commercial carbon black) jointly demonstrate the extreme importance of constructing a strong and tough chemical interface from both the "process" and "material" dimensions. C2 used the correct materials but the wrong process (dry physical blending instead of solvothermal grafting), resulting in an impact strength of 16.8 kJ / m². 2 The LOI (29.8%) was significantly lower than that of Example 17, mainly due to the lack of covalent bridges constructed by silane coupling agents. This resulted in weak interfacial bonding between the carbide and bamboo powder, which became a source of defects under stress. C5, however, used incorrect materials but attempted to follow the correct process, employing surface-inert, dense commercial carbon black (with a specific surface area of only about 80 m²). 2 / g) to replace the polystyrene-based carbide of the present invention (specific surface area > 400 m²) 2 / g), resulting in an impact strength of 13.5 kJ / m. 2The results showed even worse performance, with a LOI (27.5%) and a UL-94 rating of only V-2 accompanied by dripping. This indicates that commercial carbon black not only fails to form effective interfacial bonds, but its flame retardant efficiency is also far lower than that of the polystyrene-based charcoal of this invention. These two sets of data present a stark contrast, demonstrating that specific functional materials (polystyrene-based charcoal) or merely an interfacial design concept (using coupling agents) are insufficient. The two must be combined through a specific process called "in-situ grafting reaction" to form a stable "core-shell structure," which is the crucial first step in achieving a performance leap.
[0080] Table 3 shows that Comparative Example 3 (C3, unhydrolyzed wood flour) and Comparative Example 4 (C4, without surface barrier layer) reveal the necessity of "matrix toughening" and "gradient protection" design on top of the core reinforcement system. The impact strength of C3 (19.1 kJ / m²) is... 2 Compared to Example 17, the impact strength decreased by approximately 42%, and the flexural strength (55.2 MPa) also decreased significantly. However, the flame retardant properties (LOI 32.8%, V-0 rating) were less affected. This indicates that the main contribution of the amylase bioactivation treatment lies in improving the microfibrillation degree, surface activity, and interpenetration ability of the wood flour with the reinforcing units, thereby significantly optimizing the toughness network of the matrix. Without this step, the impact resistance ceiling of the composite material would be limited. C4 exhibits a different characteristic: impact strength (22.9 kJ / m) 2 The flexural strength (60.2 MPa) was slightly lower than that of Example 17, but the LOI dropped significantly to 28.3%, and the flame retardancy rating failed to reach V-0. This clearly shows that the main function of the surface ceramic barrier layer is to provide an immediate and active first physical and chemical barrier in the event of a fire. It works in conjunction with the internal reinforcement network to form a double protection in time and space. Without this layer, the material can hardly achieve the highest flame retardancy safety level.
[0081] Furthermore, in terms of environmental performance, C6 has a formaldehyde emission level of 0.038 mg / m³. 3 The formaldehyde emission level was significantly higher than in other embodiments and comparative examples. This is attributed to the fact that flame retardants used in conventional impregnation processes may carry free formaldehyde or promote the release of residual formaldehyde from the board. While the formaldehyde emission levels of C1 to C5 were less than 0.025 mg / m³, the formaldehyde emission levels of C1 to C5 were significantly higher. 3 However, the water resistance (water absorption thickness expansion rate of 12.5-18.2%) of C1, C2, and C5 is far worse than that of the embodiments of the present invention, which further proves the unique advantages of the "three-dimensional interpenetrating network" and "surface ceramic coating" of the present invention in improving dimensional stability.
[0082] In summary, all the performance defects of the comparative examples point to the same conclusion: the technical solution of this invention is a precise multi-scale synergistic system: "carbides with specific structures" are the functional foundation; "chemically grafted core-shell interfaces" are the key to stress transfer and network construction; "enzyme-activated wood flour" is a sophisticated means to optimize matrix toughness and interfacial interpenetration; and "homogeneous surface coatings" are the finishing touch to achieve ultimate fire protection. These four links are interconnected. The absence of any core component of this invention (such as polystyrene-based carbides) or key process (such as chemical grafting, enzymatic hydrolysis, or surface spraying) will lead to significant shortcomings in the final product in terms of impact strength, flame retardancy, or durability, making it difficult to simultaneously achieve "high impact resistance (≥23kJ / m²)". 2 The synergistic goal of “high flame retardancy (LOI≥33%, V-0 rating)” fully demonstrates the integrity and synergy of the technical solution of this invention. Its technical effect is far beyond what those skilled in the art can easily foresee or achieve through the selection of conventional materials or the simple superposition of processes.
[0083] Application Example 1 of a High Impact-Resistant and Flame-Retardant Bamboo-Wood Composite Board Examples 6, 10, or 11 of the high-impact flame-retardant bamboo-wood composite board are applied to the field of building decoration materials technology, specifically as fireproof partition wall panels, flame-retardant decorative panels, or ceiling materials for public buildings such as high-end hotels, office buildings, hospitals, and schools.
[0084] Cantilever beam notched impact strength ≥22 kJ / m 2 At that time, it was significantly higher than that of ordinary MDF (usually <10 kJ / m). 2 It and most unreinforced bamboo and wood composite materials have excellent toughness and can meet the impact resistance requirements of most furniture and decorative panels.
[0085] A Limit Index (LOI) of ≥32.5% means that the material is self-extinguishing after being removed from an open flame in the air, reaching the level of a flame-retardant material and meeting the basic requirements of fire prevention regulations for general public places.
[0086] With a UL-94 vertical flammability rating of V-0, the dense surface barrier layer and internal reinforcing network work together to suppress combustion. Meanwhile, the formaldehyde emission of this composite board is ≤0.025 mg / m³. 3 It meets the highest national environmental protection standard, ENF level, and satisfies the urgent need for green and environmentally friendly materials in modern buildings.
[0087] Application Example 2 of a High Impact-Resistant and Flame-Retardant Bamboo-Wood Composite Board Example 11 of the high impact-resistant and flame-retardant bamboo and wood composite board is applied to the field of interior materials technology for transportation vehicles, specifically as interior panels, luggage racks, seat back panels, and carriage partitions for rail transit vehicles such as high-speed trains, bullet trains, and subways, or side panels and roof linings for luxury buses and RVs, as well as interior cabin walls and ceilings for yachts and passenger ships.
[0088] Cantilever beam notched impact strength ≥ 24 kJ / m 2 It has excellent impact resistance and toughness, and can effectively resist damage caused by passenger luggage collisions and accidental impacts during the operation of the vehicle, ensuring the service life of the interior parts and passenger safety.
[0089] With a limiting oxygen index (LOI) of ≥32.5%, it falls into the category of highly flammable materials and has excellent fire safety. It meets the stringent requirements for flame retardant performance of interior materials, such as the rail transit industry standard TB / T 3138 and the shipbuilding industry standard IMO A.653(16).
[0090] With a UL-94 vertical flammability rating of V-0, and no molten dripping during combustion, this composite panel avoids the risk of secondary fires caused by molten material igniting other materials. Furthermore, its lightweight yet high-strength properties help reduce the weight of vehicles and lower energy consumption, offering significant application advantages.
[0091] Application Example 3 of a High Impact-Resistant and Flame-Retardant Bamboo-Wood Composite Board Examples 6, 10, or 11 of the high-impact flame-retardant bamboo-wood composite board are applied to the field of furniture manufacturing materials technology, specifically as panels for high-end custom cabinets, wardrobes, and bookcases, or as tabletops, filing cabinets, and screen partitions for office furniture, as well as seat backs and armrests for public places such as auditoriums and gymnasiums.
[0092] Cantilever beam notched impact strength ≥22 kJ / m 2 It can meet the requirements of furniture to resist daily bumps and knocks during use; bending strength ≥60 MPa, bending modulus ≥6.0 GPa, with good load-bearing capacity, and is suitable for large-span furniture panels.
[0093] Formaldehyde emission ≤ 0.025 mg / m³ 3 It meets the highest national environmental protection standard, ENF level, satisfying consumers' pursuit of a healthy home environment. Furthermore, this composite board can be processed with secondary techniques such as veneer and coating, offering excellent surface decoration properties to meet the design needs of various furniture styles.
[0094] Application Example 4 of a High Impact-Resistant and Flame-Retardant Bamboo-Wood Composite Board Example 11 of the high-impact flame-retardant bamboo-wood composite board is applied to the field of aerospace interior materials technology, specifically as an aircraft cabin interior panel, storage cabinet door, partition and kitchen component.
[0095] Cantilever beam notched impact strength ≥ 24 kJ / m 2 It can withstand vibrations and unexpected impacts during flight; With a limiting oxygen index (LOI) ≥ 32.5%, it meets the stringent requirements of aviation standard FAR 25.853 for the flame retardant performance of cabin interior materials; it has a UL-94 vertical flammability rating of V-0 and no dripping, resulting in low smoke density and no release of toxic gases during combustion, thus buying valuable time for passengers to escape.
[0096] Application Example 5 of a High Impact-Resistant and Flame-Retardant Bamboo-Wood Composite Board Examples 6, 10, or 11 of the high-impact flame-retardant bamboo-wood composite board are applied to the field of outdoor facilities and municipal engineering materials technology, specifically as park benches, boardwalk flooring, landscape pavilions, flower racks, or bus shelters, trash can shells, billboard substrates, as well as interior and exterior wall panels and floor slabs of prefabricated buildings.
[0097] This application scenario requires materials with good weather resistance, dimensional stability, and durability. The composite board of this invention has a 24-hour water absorption thickness expansion rate of ≤8.5%, with the best sample reaching 7.9%, exhibiting excellent dimensional stability and water resistance, and can adapt to harsh outdoor environments such as humidity and rain.
[0098] The notched impact strength of the composite panel is ≥22 kJ / m. 2 It can withstand accidental impacts and human damage during outdoor use.
[0099] Flame retardant properties (LOI≥32.5%, UL-94 V-0 rating) also provide additional safety for outdoor public facilities.
[0100] Application Example 6 of a High Impact-Resistant and Flame-Retardant Bamboo-Wood Composite Board Examples 6, 10, or 11 of the high-impact flame-retardant bamboo-wood composite board are applied to the field of packaging materials technology for precision instruments and electronic equipment, specifically as shockproof and flame-retardant packaging boxes for medical devices, optical instruments, and military equipment, or as the outer shell of control cabinets and distribution boxes.
[0101] Cantilever beam notched impact strength ≥22 kJ / m 2 It has excellent energy absorption capabilities, which can effectively buffer vibrations and impacts during transportation and protect precision instruments from damage.
[0102] With a limiting oxygen index (LOI) ≥ 32.5% and a UL-94 vertical flammability rating of V-0, it meets the flame-retardant safety requirements for electronic device housings.
[0103] In summary, the enhanced impact strength of the cantilever beam originates from the strengthening and toughening of the "core-shell" interface and the three-dimensional interpenetrating network structure. The improved Limit Index (LOI) comes from the synergistic internal and external charcoal flame-retardant system and the possible catalytic char formation effect. This invention achieves optimal material performance through the synergistic effect of three core technologies: "core-shell structure enhancement," "bio-enzyme toughening," and "surface ceramic barrier." The high-impact flame-retardant bamboo-wood composite board of this invention can be widely used in the fields of building decoration, transportation vehicle interiors, furniture manufacturing, aerospace interiors, outdoor facilities, and precision instrument packaging.
Claims
1. A high-impact, flame-retardant bamboo-wood composite board, characterized in that, It is mainly composed of a primary composite board formed by hot pressing a mixture of core-shell structured reinforced bamboo powder masterbatch and microfiber toughened wood powder, and then spraying a polystyrene-based carbide dispersion onto the surface to form a ceramic barrier coating.
2. The high-impact, flame-retardant bamboo-wood composite board according to claim 1, characterized in that: The mass ratio of the core-shell structured reinforced bamboo powder masterbatch to the microfiber-toughened wood powder is 20–60:80–40; the spraying amount of the polystyrene-based carbide dispersion is 50–300 g / m³. 2 The solid content of the polystyrene-based carbon dispersion is 5-15%; the solvent in the polystyrene-based carbon dispersion includes water and / or alcohol solvents; the alcohol solution includes ethanol; when the solvent is an alcohol-water solvent, the volume fraction of water is ≤30%.
3. The high-impact, flame-retardant bamboo-wood composite board according to claim 1 or 2, characterized in that: The preparation method of the polystyrene-based carbonized material is as follows: the polystyrene-based material is placed in an inert atmosphere, heated by a programmed temperature, carbonized at a constant temperature, cooled, and pulverized to obtain the carbonized material; the heating rate of the programmed temperature is 3-15℃ / min; the carbonization temperature is 400-700℃, and the time is 1-5h; the polystyrene-based material includes one or more of polystyrene, poly(p-diethylene), or poly(m-diethylene); the pulverization is passed through a 1500-mesh sieve; the inert atmosphere includes nitrogen and / or argon.
4. The high-impact, flame-retardant bamboo-wood composite board according to any one of claims 1 to 3, characterized in that: The preparation method of the core-shell structure reinforced bamboo powder masterbatch is as follows: bamboo powder, polystyrene-based carbide, and silane coupling agent are mixed with an alcohol solution, and a solvothermal reaction is carried out in a closed reactor, followed by drying. The mass ratio of bamboo powder, polystyrene-based carbide, and silane coupling agent is 50-80:20-40:5-20. The amount of alcohol solution used is 20-50% of the mass of bamboo powder. The temperature of the solvothermal reaction is 50-120℃, the rotation speed is 100-300 r / min, and the time is 0.5-4.0 h. The thermal reaction mixture accounts for 30-70% of the reactor volume; the bamboo powder has a particle size that passes through an 80-200 mesh sieve and a moisture content of <5%; the silane coupling agent includes one or more of γ-aminopropyltriethoxysilane, γ-methacryloyloxypropyltrimethoxysilane, vinyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, or isocyanate silane; the alcohol solution includes an alcohol solvent or an aqueous solution thereof, wherein the volume fraction of water in the aqueous alcohol solvent is ≤30%; the alcohol solvent includes ethanol.
5. The high-impact, flame-retardant bamboo-wood composite board according to any one of claims 1 to 4, characterized in that: The preparation method of the microfiber-toughened wood flour is as follows: wood flour is dispersed in a buffer solution, amylase is added, enzymatic hydrolysis is performed, inactivation is carried out by heating, and the mixture is washed and dried. The mass-to-volume ratio of wood flour to buffer solution is 1:5-20 (g / mL). The pH value of the buffer solution is 4.8-7.
0. The amount of amylase used is equivalent to 0.3-3.0% of the mass of wood flour. The enzymatic hydrolysis temperature is 38-65℃, and the time is 1-8 hours. The inactivation temperature is 85-95℃, and the time is 10-30 minutes. The particle size of the wood flour is such that it passes through an 80-200 mesh sieve, and the moisture content is <5%. The buffer solution includes phosphate buffer, citrate-sodium citrate buffer, or acetate-sodium acetate buffer. The enzyme activity of the amylase is ≥3000 U / g. The amylase includes α-amylase and / or β-amylase. When α-amylase and β-amylase are used in combination, the mass ratio of α-amylase to β-amylase is 1-4:
1.
6. A method for preparing a high-impact, flame-retardant bamboo-wood composite board as described in any one of claims 1 to 5, characterized in that, Includes the following steps: (1) Mixing and molding: After uniformly mixing the core-shell structure reinforced bamboo powder masterbatch with microfiber toughened wood powder, place it in a mold and hot press it to obtain a primary composite board; (2) Curing and molding: The polystyrene-based carbide dispersion is sprayed onto the surface of the primary composite board obtained in step (1), dried and cured to obtain a high impact-resistant and flame-retardant bamboo-wood composite board.
7. The method for preparing the high-impact flame-retardant bamboo-wood composite board according to claim 6, characterized in that: In step (1), the temperature of hot pressing is 150-190℃, the pressure is 3-9 MPa, and the time is 5-20 min.
8. The method for preparing the high-impact flame-retardant bamboo-wood composite board according to claim 6 or 7, characterized in that: In step (2), the drying and curing temperature is 60-100℃ and the time is 1-4h.
9. The application of a high-impact, flame-retardant bamboo-wood composite board as described in any one of claims 1 to 5, characterized in that: The high impact-resistant and flame-retardant bamboo-wood composite board described in any one of claims 1 to 5 is applied to the technical field of preparing building decoration materials, transportation vehicle interior materials, furniture manufacturing materials, aerospace interior materials, outdoor facilities and municipal engineering materials, packaging materials, or electronic device shell materials.
Citation Information
Patent Citations
Preparation method for flame-retardation and smoke-suppression bamboo-wood composite integrated material
CN108995012A
Bamboo board modifier as well as preparation method and application thereof
CN116572336A
Long-acting flame-retardant anti-deformation composite board as well as preparation method and application thereof
CN120024089A