Preparation process of a deep-penetration wood micropore invisible protective coating
By preparing coatings with core-shell functional additives and organic-inorganic hybrid networks, the shortcomings of wood protective coatings in terms of deep penetration, invisibility and transparency, superhydrophobicity and flexibility were solved, and the durability and stability were improved.
Patent Information
- Application Number
- CN202611136619.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-29
- Publication Date
- 2026-11-20
AI Technical Summary
Existing wood protective coatings cannot simultaneously achieve deep penetration, invisibility and transparency, superhydrophobicity and mechanical flexibility, making them prone to cracking or peeling under changes in temperature and humidity.
By combining tetraethyl orthosilicate, methyltriethoxysilane, functional additives, and synergistic reinforcing agents, a deep-penetrating wood microporous invisible protective coating is prepared through ultrasonic dispersion, membrane filtration, and stepwise curing, forming a core-shell type functional additive and an organic-inorganic hybrid network.
It achieves deep penetration and invisible protection of the coating, has superhydrophobic properties and good elasticity, and can adapt to the repeated expansion and contraction stress of wood caused by changes in temperature and humidity, preventing cracking or peeling.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of functional coating materials technology, specifically a process for preparing a deep-penetrating, invisible protective coating for wood micropores. Background Technology
[0002] Wood, as a renewable natural material, is widely used in furniture boards, interior and exterior decoration, and other fields. However, the porous structure of wood makes it prone to moisture absorption and expansion, shrinkage and cracking, and it is also susceptible to decay fungi and ultraviolet radiation. Existing protective technologies mostly use surface coatings of resin paint or wax oil, which can block moisture, but the paint film only adheres to the surface, not only clogging the wood pores and covering the natural texture, but also being prone to wear and peeling during use, resulting in poor durability. Although penetrating silane impregnation treatment can enter the wood cell cavity, the hydrophobicity of the pure inorganic network formed by the traditional tetraethyl orthosilicate / methyltriethoxysilane system is limited. If fluorinated silanes are added directly, poor compatibility can easily lead to agglomeration, causing the coating to turn white and lose its invisible and transparent properties. In addition, inorganic silicon coatings are brittle, and in the furniture use environment with drastic temperature and humidity changes, micro-cracks are easily generated inside the coating, which in turn leads to the failure of the protective function.
[0003] Therefore, the preparation process of the invisible protective coating that can deeply penetrate wood micropores according to the present invention is of great significance in the field of functional coating materials technology. Summary of the Invention
[0004] In order to overcome the above-mentioned technical problems, the purpose of this invention is to provide a process for preparing a deep-penetrating wood microporous invisible protective coating, which solves the problem that existing wood protective coatings cannot simultaneously achieve deep penetration, invisibility and transparency, superhydrophobicity and mechanical flexibility.
[0005] The objective of this invention can be achieved through the following technical solutions: This application provides a process for preparing a deep-penetrating, microporous, invisible protective coating for wood, including the following steps: Step 1: Weigh out 50-80 parts of tetraethyl orthosilicate, 20-40 parts of methyltriethoxysilane, 30-50 parts of functional additives, 5-10 parts of synergistic enhancer, 150-250 parts of anhydrous ethanol, and 30-60 parts of deionized water according to the following weight proportions. Step 2: Add anhydrous ethanol, deionized water, and functional additives to the reaction vessel and mix and stir for 30 minutes. Adjust the pH to 2.5-3 with 1 mol / L hydrochloric acid solution. Add tetraethyl orthosilicate and methyltriethoxysilane at 25-30℃ and continue stirring for 30-45 minutes. Add the synergistic reinforcing agent and ultrasonically disperse at 200W for 10-15 minutes. Filter through a filter membrane with a pore size of 0.2-0.25 μm to obtain the impregnation solution. Immerse the wood to be treated in the solution. In the above impregnation solution, vacuum to -0.09MPa and maintain for 30-60 minutes, pressurize to 1-1.5MPa and maintain pressure for 2-6 hours. After depressurization, remove and wipe off excess liquid from the surface. Curing is carried out using a step-by-step procedure: constant temperature at 40℃ for 12 hours, temperature increased to 60℃ and constant temperature for 4 hours, temperature continued to increase to 80℃ and constant temperature for 4 hours, and finally temperature increased to 103℃ and constant temperature for 2 hours. Humidification is carried out at 25℃ and 65% relative humidity for 7 days to obtain a deep-penetrating invisible protective coating for wood micropores.
[0006] In a preferred embodiment of the present invention, the functional additive is prepared by the following steps: Tetraethyl orthosilicate and methyltriethoxysilane were added to a three-necked flask equipped with a stirrer and thermometer. The mixture was magnetically stirred for 30 min under nitrogen protection and at 30 °C. An acidic alcohol aqueous solution was added, and stirring was continued for 30-45 min to obtain a hyperbranched prepolymer sol. 1H,1H,2H,2H-perfluorodecyltriethoxysilane was injected into the hyperbranched prepolymer sol at a rate of 0.5 mL / min, and the mixture was ultrasonically dispersed for 30 min. Deionized water was added, and the mixture was heated to 50 °C and stirred at a constant temperature for 3-4 h. After natural cooling to 25 °C, hexane was added for extraction. The aqueous phase was rotary evaporated under reduced pressure at 35 °C for 3-4 h. The mixture was then dialyzed in distilled water for 24 h using a dialysis bag with a molecular weight cutoff of 1000 to obtain the functional additive.
[0007] In a preferred embodiment of the present invention, the ratio of tetraethyl orthosilicate, methyltriethoxysilane, acidic alcohol aqueous solution, 1H,1H,2H,2H-perfluorodecyltriethoxysilane, deionized water, and n-hexane is 220-230 mL: 90-100 mL: 400 mL: 50-70 mL: 10-20 mL: 500 mL; the acidic alcohol aqueous solution is prepared by mixing anhydrous ethanol and 1 mol / L hydrochloric acid solution at a volume ratio of 8:1.
[0008] In a preferred embodiment of the present invention, the synergistic enhancer is prepared by the following steps: Step b1: Add sodium lignosulfonate and the first portion of deionized water to a three-necked flask equipped with a stirrer and thermometer, mix and stir for 30 min, adjust the pH to 10.5 with sodium hydroxide solution, activate at 70℃ for 1 h, add epichlorohydrin and benzyltriethylammonium chloride, react at 60℃ for 4-5 h, cool naturally to 25℃, adjust the pH to 7 with hydrochloric acid solution, add the second portion of deionized water to precipitate the product, centrifuge, wash the precipitate 2-3 times with distilled water to obtain epoxidized lignin; add epoxidized lignin to tetrahydrofuran, shear at 10000 r / min, add the third portion of deionized water, and rotary evaporate under reduced pressure at 35℃ and -0.09 MPa for 3-4 h to obtain an aqueous dispersion of epoxidized lignin nanoparticles; Step b2: Add bleached hardwood pulp and the first portion of deionized water to a fiber de-fiber machine and de-fiber for 5 minutes to obtain a fiber suspension; add 2,2,6,6-tetramethylpiperidine oxide and sodium bromide to the fiber suspension, mix and stir for 30 minutes, place in a 10°C water bath, add sodium hypochlorite solution, adjust the pH to 10 with sodium hydroxide solution, and determine the carboxyl content by conductivity titration. When the carboxyl content reaches 0.9 mmol / g, add the first portion of anhydrous ethanol and stir for 10 minutes to terminate the oxidation reaction, pour into a funnel and filter, then rinse with distilled water. Wash 2-3 times, add a second portion of deionized water, transfer to a high-pressure microfluidic homogenizer, and treat 6 times at 1000 bar to obtain nanocellulose hydrogel. Replace the dispersion medium with ethanol until the ethanol concentration is >95%. Under nitrogen protection, add isocyanate propyltriethoxysilane and dibutyltin dilaurate, react at 60℃ for 8 hours, centrifuge, wash the precipitate 2-3 times with distilled water, add epoxidized lignin nanoparticle aqueous dispersion, adjust the pH to 8.5 with ammonia, mix and stir for 4 hours, centrifuge, and disperse the precipitate in a second portion of anhydrous ethanol to obtain the synergistic reinforcing agent.
[0009] In a preferred embodiment of the present invention, the ratio of sodium lignosulfonate, total deionized water, epichlorohydrin, benzyltriethylammonium chloride, and tetrahydrofuran in step b1 is 90-100g:6000mL:35-40mL:2g:4000mL; the first part of deionized water accounts for 1 / 5 of the total deionized water; the second part of deionized water accounts for 2 / 15 of the total deionized water; the third part of deionized water accounts for 2 / 3 of the total deionized water; the concentration of the sodium hydroxide solution is 2mol / L; and the concentration of the hydrochloric acid solution is 1mol / L.
[0010] In a preferred embodiment of the present invention, the ratio of the following components in step b2—bleached hardwood pulp, total deionized water, 2,2,6,6-tetramethylpiperidine oxide, sodium bromide, sodium hypochlorite solution, total anhydrous ethanol, propyltriethoxysilane isocyanate, dibutyltin dilaurate, and epoxidized lignin nanoparticle aqueous dispersion—is 25-30 g : 2500-3500 mL : 0.4-0.5 g : 2.5-3.5 g : 34-41 mL : 1500-2000 mL : 1.1- 1.5 mL: 0.04-0.06 g: 80-100 mL; the first part of deionized water accounts for 1 / 2 of the total amount of deionized water; the second part of deionized water accounts for 1 / 2 of the total amount of deionized water; the first part of anhydrous ethanol accounts for 1 / 3 of the total amount of anhydrous ethanol; the second part of anhydrous ethanol accounts for 2 / 3 of the total amount of anhydrous ethanol; the mass fraction of the sodium hypochlorite solution is 12%; the concentration of the sodium hydroxide solution is 0.5 mol / L; the concentration of the ammonia water is 2 mol / L.
[0011] The beneficial effects of this invention are: This invention discloses a process for preparing a deep-penetrating microporous invisible protective coating for wood. The process involves mixing anhydrous ethanol, deionized water, and functional additives, adjusting the pH with hydrochloric acid solution, adding tetraethyl orthosilicate and methyltriethoxysilane, adding a synergistic reinforcing agent, ultrasonically dispersing the mixture, and filtering through a filter membrane to obtain an impregnation solution. The wood to be treated is then immersed in the impregnation solution under vacuum. After depressurization, the wood is removed, excess liquid is wiped off, and the mixture is cured using a step-by-step process and humidified to obtain a deep-penetrating microporous invisible protective coating for wood. This deep-penetrating microporous invisible protective coating allows its protective components to penetrate deeply into the wood. The coating penetrates into the wood and forms a protective layer on the walls of the micropores after in-situ condensation. This transparent coating does not alter the natural color or texture of the wood, achieving invisible protection. The interface of the coating pore walls has strong hydrophobic properties, making it difficult for water and everyday liquid stains to penetrate and give the wood excellent water-repellent and self-cleaning capabilities. The coating network has good elasticity and toughness due to its flexible bio-based reinforcing structure, which can effectively adapt to the repeated expansion and contraction stress caused by changes in temperature and humidity, preventing the protective layer from becoming brittle or peeling off during long-term use, and providing stable dimensional stability and crack resistance.
[0012] In the preparation of a deep-penetrating, microporous, invisible protective coating for wood, functional additives were first prepared. Tetraethyl orthosilicate and methyltriethoxysilane under acidic alcohol-water conditions underwent hydrolysis to generate silanols. These silanols then underwent dehydration or de-alcoholization condensation with each other and with unhydrolyzed alkoxy groups, forming a highly branched Si-O-Si prepolymer network. Then, 1H,1H,2H,2H-perfluorodecyltriethoxysilane was introduced, and its alkoxy groups also underwent hydrolysis condensation. Due to the extremely strong hydrophobic effect of the fluorocarbon chain, the fluorinated segments... During the polycondensation process, it spontaneously curls inward and is covered by a hydrophilic shell composed of methyl and silanol groups, forming a stable core-shell functional additive. This functional additive is completely compatible with the impregnation liquid and can penetrate into the micropores of wood without obstruction. During curing, the core-shell structure disintegrates, and the fluorocarbon chains are oriented towards the surface of the pore wall, creating a micro-nano secondary hydrophobic roughness similar to that of a lotus leaf, giving the coating superhydrophobic properties. At the same time, the functional additive itself is highly transparent, avoiding the whitening problem caused by traditional fluorinated additives and ensuring the invisibility of the coating.
[0013] In the preparation of a deep-penetrating, microporous, invisible protective coating for wood, a synergistic reinforcing agent was first prepared. Through alkali activation treatment, the phenolic hydroxyl groups in sodium lignin sulfonate molecules were fully ionized, exposing highly reactive phenolic anion sites. The introduced epichlorohydrin, under the action of benzyltriethylammonium chloride, underwent a ring-opening reaction due to nucleophilic attack of the phenolic anions, followed by re-ring closure in an alkaline environment, forming epoxy functional groups chemically bonded to the lignin phenylpropane units, yielding epoxidized lignin. The product was then used to prepare epoxidized lignin nanoparticles via anti-solvent precipitation. The epoxidized lignin nanoparticles can penetrate into the wood interior with the impregnation solution. The epoxy groups on the particle surface provide reaction anchors for subsequent chemical crosslinking with nanocellulose, allowing the organic reinforcing phase to covalently integrate into the inorganic silica network and avoiding separation at the two-phase interface. A 2,2,6,6-tetramethylpiperidine oxide / sodium bromide / sodium hypochlorite catalytic oxidation system is used to selectively oxidize the C6 primary hydroxyl groups on the surface of nanocellulose filaments to sodium carboxylate groups. This carboxylation modification weakens the hydrogen bonding between cellulose filaments and introduces electrostatic repulsion, facilitating subsequent crosslinking with high-molecular-weight cellulose nanoparticles. Single nanofibers were exfoliated at 1000 bar pressure in a microfluidic homogenizer to obtain transparent gel-like nanocellulose. The dispersion medium was replaced with ethanol from water through solvent displacement. A dibutyltin dilaurate catalyzed addition reaction was conducted between the isocyanate groups in propyltriethoxysilane molecule and residual hydroxyl groups on the nanocellulose surface to form carbamate covalent bonds. Hydrolyzable triethoxysilane end groups were then anchored onto the cellulose filaments to obtain silanized nanocellulose. This silanized nanocellulose was then combined with epoxidized lignin nanoparticles under weakly alkaline conditions. Under mixed conditions, epoxy groups and cellulose hydroxyl groups undergo nucleophilic ring-opening crosslinking to obtain a synergistic reinforcing agent. This synergistic reinforcing agent uses a nanocellulose network as a framework to penetrate the interior of the silica coating. Its high aspect ratio filaments improve the fracture toughness of the coating through crack bridging and stress dispersion effects, transforming the rigid inorganic network into an organic-inorganic hybrid system that combines flexibility and strength. This system can withstand the cyclic stress generated by repeated expansion and contraction of wood without brittle cracking. The reinforcing network is chemically bonded to the matrix silica phase through silane anchoring groups, which enhances the coating without affecting its transparency and invisibility. Detailed Implementation
[0014] To enable those skilled in the art to better understand the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0015] Example 1: This embodiment describes a process for preparing a deep-penetrating, microporous, invisible protective coating for wood, including the following steps: Step S1: Add 220 mL of tetraethyl orthosilicate and 90 mL of methyltriethoxysilane to a three-necked flask equipped with a stirrer and thermometer. Stir magnetically for 30 min under nitrogen protection and at 30°C. Add 400 mL of acidic alcohol aqueous solution and continue stirring for 30 min to obtain a hyperbranched prepolymer sol. Inject 50 mL of 1H,1H,2H,2H-perfluorodecyltriethoxysilane into the hyperbranched prepolymer sol at a rate of 0.5 mL / min. Disperse ultrasonically for 30 min. Add 10 mL of deionized water. Heat to 50°C and stir at a constant temperature for 3 h. Allow to cool naturally to 25°C. Add 500 mL of n-hexane for extraction. Evaporate the aqueous phase under reduced pressure at 35°C for 3 h. Dialyze the aqueous phase in distilled water for 24 h using a dialysis bag with a molecular weight cutoff of 1000 to obtain the functional additive. The acidic alcohol aqueous solution is prepared by mixing anhydrous ethanol and 1 mol / L hydrochloric acid solution at a volume ratio of 8:1. Step S2: Add 90g of sodium lignin sulfonate and 1200mL of deionized water to a three-necked flask equipped with a stirrer and thermometer, mix and stir for 30min, adjust the pH to 10.5 with 2mol / L sodium hydroxide solution, stir and activate at 70℃ for 1h, add 35mL of epichlorohydrin and 2g of benzyltriethylammonium chloride, react at 60℃ for 4h, cool naturally to 25℃, adjust the pH to 7 with 1mol / L hydrochloric acid solution, add 800mL of deionized water to precipitate the product, centrifuge, wash the precipitate twice with distilled water to obtain epoxidized lignin; add epoxidized lignin to 4000mL of tetrahydrofuran, shear at 10000r / min and add 4000mL of deionized water, rotary evaporate under reduced pressure at 35℃ and -0.09MPa for 3h to obtain an aqueous dispersion of epoxidized lignin nanoparticles; Step S3: Add 25g of bleached hardwood pulp and 1250mL of deionized water to a fiber de-fiber machine and de-fiberize for 5min to obtain a fiber suspension; add 0.4g of 2,2,6,6-tetramethylpiperidine oxide and 2.5g of sodium bromide to the fiber suspension, mix and stir for 30min, place in a 10℃ water bath, add 34mL of 12% sodium hypochlorite solution, adjust the pH to 10 with 0.5mol / L sodium hydroxide solution, and determine the carboxyl content by conductivity titration. When the carboxyl content reaches 0.9mmol / g, add 500mL of anhydrous ethanol and stir for 10min to terminate the oxidation reaction, pour into a funnel and filter, wash twice with distilled water, add 1250mL of deionized water, and transfer to a high-pressure micro-injector. The nanocellulose hydrogel was obtained by treating the sample six times at 1000 bar in a homogenizer. The dispersion medium was replaced with ethanol until the ethanol concentration was >95%. Under nitrogen protection, 1.1 mL of propyltriethoxysilane isocyanate and 0.04 g of dibutyltin dilaurate were added. The mixture was reacted at 60 °C for 8 h. After centrifugation, the precipitate was washed twice with distilled water. 80 mL of epoxidized lignin nanoparticle aqueous dispersion was added, and the pH was adjusted to 8.5 with 2 mol / L ammonia. The mixture was stirred for 4 h, centrifuged, and the precipitate was dispersed in 1000 mL of anhydrous ethanol to obtain the synergistic reinforcing agent. Step S4: Weigh out 50 parts of tetraethyl orthosilicate, 20 parts of methyltriethoxysilane, 30 parts of functional additives, 5 parts of synergistic enhancer, 150 parts of anhydrous ethanol and 30 parts of deionized water according to the following weight proportions. Step S5: Add anhydrous ethanol, deionized water, and functional additives to the reaction vessel, mix and stir for 30 min, adjust the pH to 2.5 with 1 mol / L hydrochloric acid solution, add tetraethyl orthosilicate and methyltriethoxysilane at 25℃, continue stirring for 30 min, add synergistic reinforcing agent, ultrasonically disperse at 200W power for 10 min, filter through a 0.2μm pore size filter membrane to obtain impregnation solution; immerse the wood to be treated in the above impregnation solution, vacuum to -0.09MPa and maintain for 30 min, pressurize to 1MPa and hold for 2 h, remove after depressurization, wipe off excess liquid on the surface, and cure using a step-by-step procedure: hold at 40℃ for 12 h, raise the temperature to 60℃ and hold for 4 h, continue to raise the temperature to 80℃ and hold for 4 h, and finally raise the temperature to 103℃ and hold for 2 h, humidify at 25℃ and 65% relative humidity for 7 days to obtain a deep-penetrating wood microporous invisible protective coating.
[0016] Example 2: This embodiment describes a process for preparing a deep-penetrating, microporous, invisible protective coating for wood, including the following steps: Step S1: Add 225 mL of tetraethyl orthosilicate and 95 mL of methyltriethoxysilane to a three-necked flask equipped with a stirrer and thermometer. Under nitrogen protection and at 30°C, stir magnetically for 30 min. Add 400 mL of acidic alcohol aqueous solution and continue stirring for 40 min to obtain a hyperbranched prepolymer sol. Inject 60 mL of 1H,1H,2H,2H-perfluorodecyltriethoxysilane into the hyperbranched prepolymer sol at a rate of 0.5 mL / min. Sonicate and disperse for 30 min. Add 15 mL of deionized water. Heat to 50°C and stir at a constant temperature for 3.5 h. Allow to cool naturally to 25°C. Add 500 mL of n-hexane for extraction. Evaporate the aqueous phase under reduced pressure at 35°C for 3.5 h. Dialyze the aqueous phase in distilled water for 24 h using a dialysis bag with a molecular weight cutoff of 1000 to obtain the functional additive. The acidic alcohol aqueous solution is prepared by mixing anhydrous ethanol and 1 mol / L hydrochloric acid solution at a volume ratio of 8:1. Step S2: Add 95g of sodium lignin sulfonate and 1200mL of deionized water to a three-necked flask equipped with a stirrer and thermometer, mix and stir for 30min, adjust the pH to 10.5 with 2mol / L sodium hydroxide solution, stir and activate at 70℃ for 1h, add 38mL of epichlorohydrin and 2g of benzyltriethylammonium chloride, react at 60℃ for 4.5h, cool naturally to 25℃, adjust the pH to 7 with 1mol / L hydrochloric acid solution, add 800mL of deionized water to precipitate the product, centrifuge, wash the precipitate twice with distilled water to obtain epoxidized lignin; add epoxidized lignin to 4000mL of tetrahydrofuran, shear at 10000r / min and add 4000mL of deionized water, rotary evaporate under reduced pressure at 35℃ and -0.09MPa for 3.5h to obtain an aqueous dispersion of epoxidized lignin nanoparticles; Step S3: Add 28g of bleached hardwood pulp and 1500mL of deionized water to a fiber de-fiber machine and de-fiberize for 5min to obtain a fiber suspension; add 0.45g of 2,2,6,6-tetramethylpiperidine oxide and 3g of sodium bromide to the fiber suspension, mix and stir for 30min, place in a 10℃ water bath, add 37mL of 12% sodium hypochlorite solution, adjust the pH to 10 with 0.5mol / L sodium hydroxide solution, and determine the carboxyl content by conductivity titration. When the carboxyl content reaches 0.9mmol / g, add 585mL of anhydrous ethanol and stir for 10min to terminate the oxidation reaction, pour into a funnel and filter, wash 3 times with distilled water, add 1500mL of deionized water, and transfer to a high-pressure microfluidic jet. The nanocellulose hydrogel was obtained by homogenizing the sample six times at 1000 bar. The dispersion medium was replaced with ethanol until the ethanol concentration was >95%. Under nitrogen protection, 1.3 mL of propyltriethoxysilane isocyanate and 0.05 g of dibutyltin dilaurate were added. The mixture was reacted at 60 °C for 8 h. After centrifugation, the precipitate was washed three times with distilled water. 90 mL of epoxidized lignin nanoparticle aqueous dispersion was added. The pH was adjusted to 8.5 with 2 mol / L ammonia water. The mixture was stirred for 4 h and centrifuged. The precipitate was dispersed in 1165 mL of anhydrous ethanol to obtain the synergistic reinforcing agent. Step S4: Weigh out 65 parts of tetraethyl orthosilicate, 30 parts of methyltriethoxysilane, 40 parts of functional additives, 8 parts of synergistic enhancer, 200 parts of anhydrous ethanol, and 45 parts of deionized water according to the following weight proportions. Step S5: Add anhydrous ethanol, deionized water, and functional additives to the reaction vessel, mix and stir for 30 min, adjust the pH to 2.8 with 1 mol / L hydrochloric acid solution, add tetraethyl orthosilicate and methyltriethoxysilane at 28℃, continue stirring for 38 min, add synergistic reinforcing agent, ultrasonically disperse at 200W power for 13 min, filter through a 0.23μm pore size filter membrane to obtain impregnation solution; immerse the wood to be treated in the above impregnation solution, vacuum to -0.09MPa and maintain for 45 min, pressurize to 1.3MPa and maintain pressure for 4 h, remove after depressurization, wipe off excess liquid on the surface, and cure using a step-by-step procedure: constant temperature at 40℃ for 12 h, raise the temperature to 60℃ and hold for 4 h, continue to raise the temperature to 80℃ and hold for 4 h, finally raise the temperature to 103℃ and hold for 2 h, humidify at 25℃ and 65% relative humidity for 7 days to obtain a deep-penetrating wood microporous invisible protective coating.
[0017] Example 3: This embodiment describes a process for preparing a deep-penetrating, microporous, invisible protective coating for wood, including the following steps: Step S1: Add 230 mL of tetraethyl orthosilicate and 100 mL of methyltriethoxysilane to a three-necked flask equipped with a stirrer and thermometer. Under nitrogen protection and at 30°C, stir magnetically for 30 min. Add 400 mL of acidic alcohol aqueous solution and continue stirring for 45 min to obtain a hyperbranched prepolymer sol. Inject 70 mL of 1H,1H,2H,2H-perfluorodecyltriethoxysilane into the hyperbranched prepolymer sol at a rate of 0.5 mL / min. Sonicate and disperse for 30 min. Add 20 mL of deionized water. Heat to 50°C and stir at a constant temperature for 4 h. Allow to cool naturally to 25°C. Add 500 mL of n-hexane for extraction. Evaporate the aqueous phase under reduced pressure at 35°C for 4 h. Dialyze the aqueous phase in distilled water for 24 h using a dialysis bag with a molecular weight cutoff of 1000 to obtain the functional additive. The acidic alcohol aqueous solution is prepared by mixing anhydrous ethanol and 1 mol / L hydrochloric acid solution at a volume ratio of 8:1. Step S2: Add 100g sodium lignin sulfonate and 1200mL deionized water to a three-necked flask equipped with a stirrer and thermometer, mix and stir for 30min, adjust the pH to 10.5 with 2mol / L sodium hydroxide solution, stir and activate at 70℃ for 1h, add 40mL epichlorohydrin and 2g benzyltriethylammonium chloride, react at 60℃ for 5h, cool naturally to 25℃, adjust the pH to 7 with 1mol / L hydrochloric acid solution, add 800mL deionized water to precipitate the product, centrifuge, wash the precipitate 3 times with distilled water to obtain epoxidized lignin; add epoxidized lignin to 4000mL tetrahydrofuran, shear at 10000r / min and add 4000mL deionized water, rotary evaporate under reduced pressure at 35℃ and -0.09MPa for 4h to obtain an aqueous dispersion of epoxidized lignin nanoparticles; Step S3: Add 30g of bleached hardwood pulp and 1750mL of deionized water to a fiber de-fiber machine and de-fiberize for 5min to obtain a fiber suspension; add 0.5g of 2,2,6,6-tetramethylpiperidine oxide and 3.5g of sodium bromide to the fiber suspension, mix and stir for 30min, place in a 10℃ water bath, add 41mL of 12% sodium hypochlorite solution, adjust the pH to 10 with 0.5mol / L sodium hydroxide solution, and determine the carboxyl content by conductivity titration. When the carboxyl content reaches 0.9mmol / g, add 670mL of anhydrous ethanol and stir for 10min to terminate the oxidation reaction, pour into a funnel and filter, wash 3 times with distilled water, add 1750mL of deionized water, and transfer to a high-pressure micro-injector. The nanocellulose hydrogel was obtained by treating the sample six times at 1000 bar in a homogenizer. The dispersion medium was replaced with ethanol until the ethanol concentration was >95%. Under nitrogen protection, 1.5 mL of propyltriethoxysilane isocyanate and 0.06 g of dibutyltin dilaurate were added. The mixture was reacted at 60 °C for 8 h. After centrifugation, the precipitate was washed three times with distilled water. 100 mL of epoxidized lignin nanoparticle aqueous dispersion was added, and the pH was adjusted to 8.5 with 2 mol / L ammonia. The mixture was stirred for 4 h, centrifuged, and the precipitate was dispersed in 1330 mL of anhydrous ethanol to obtain the synergistic reinforcing agent. Step S4: Weigh out 80 parts of tetraethyl orthosilicate, 40 parts of methyltriethoxysilane, 50 parts of functional additives, 10 parts of synergistic enhancer, 250 parts of anhydrous ethanol and 60 parts of deionized water according to the following weight proportions. Step S5: Add anhydrous ethanol, deionized water, and functional additives to the reaction vessel, mix and stir for 30 min, adjust the pH to 3 with 1 mol / L hydrochloric acid solution, add tetraethyl orthosilicate and methyltriethoxysilane at 30℃, continue stirring for 45 min, add synergistic reinforcing agent, ultrasonically disperse at 200W power for 15 min, filter through a 0.25μm pore size filter membrane to obtain impregnation solution; immerse the wood to be treated in the above impregnation solution, vacuum to -0.09MPa and maintain for 60 min, pressurize to 1.5MPa and maintain pressure for 6 h, remove after depressurization, wipe off excess liquid on the surface, and cure using a step-by-step procedure: constant temperature at 40℃ for 12 h, raise the temperature to 60℃ and hold for 4 h, continue to raise the temperature to 80℃ and hold for 4 h, finally raise the temperature to 103℃ and hold for 2 h, and humidify at 25℃ and 65% relative humidity for 7 days to obtain a deep-penetrating wood microporous invisible protective coating.
[0018] Comparative Example 1: This comparative example illustrates a process for preparing a deep-penetrating, microporous, invisible protective coating for wood, including the following steps: Step S1: Weigh out 65 parts of tetraethyl orthosilicate, 30 parts of methyltriethoxysilane, 200 parts of anhydrous ethanol and 45 parts of deionized water according to the following weight proportions. Step S2: Add anhydrous ethanol and deionized water to the reaction vessel and mix and stir for 30 min. Adjust the pH to 2.8 with 1 mol / L hydrochloric acid solution. Add tetraethyl orthosilicate and methyltriethoxysilane at 28℃ and continue stirring for 38 min. Disperse ultrasonically at 200W power for 13 min. Filter through a 0.23μm pore size filter membrane to obtain the impregnation solution. Immerse the wood to be treated in the above impregnation solution, vacuum to -0.09MPa and maintain for 45 min, pressurize to 1.3MPa and hold for 4 h. After depressurization, remove and wipe off excess liquid from the surface. Curing is carried out using a step-by-step procedure: constant temperature at 40℃ for 12 h, temperature increased to 60℃ and constant temperature for 4 h, temperature increased to 80℃ and constant temperature for 4 h, and finally temperature increased to 103℃ and constant temperature for 2 h. Humidify at 25℃ and 65% relative humidity for 7 days to obtain a deep-penetrating microporous invisible protective coating for wood.
[0019] Comparative Example 2: This comparative example illustrates a process for preparing a deep-penetrating, microporous, invisible protective coating for wood, including the following steps: Step S1: Add 225 mL of tetraethyl orthosilicate and 95 mL of methyltriethoxysilane to a three-necked flask equipped with a stirrer and thermometer. Under nitrogen protection and at 30°C, stir magnetically for 30 min. Add 400 mL of acidic alcohol aqueous solution and continue stirring for 40 min to obtain a hyperbranched prepolymer sol. Inject 60 mL of 1H,1H,2H,2H-perfluorodecyltriethoxysilane into the hyperbranched prepolymer sol at a rate of 0.5 mL / min. Sonicate and disperse for 30 min. Add 15 mL of deionized water. Heat to 50°C and stir at a constant temperature for 3.5 h. Allow to cool naturally to 25°C. Add 500 mL of n-hexane for extraction. Evaporate the aqueous phase under reduced pressure at 35°C for 3.5 h. Dialyze the aqueous phase in distilled water for 24 h using a dialysis bag with a molecular weight cutoff of 1000 to obtain the functional additive. The acidic alcohol aqueous solution is prepared by mixing anhydrous ethanol and 1 mol / L hydrochloric acid solution at a volume ratio of 8:1. Step S2: Weigh out 65 parts of tetraethyl orthosilicate, 30 parts of methyltriethoxysilane, 40 parts of functional additives, 200 parts of anhydrous ethanol, and 45 parts of deionized water according to the following weight proportions. Step S3: Add anhydrous ethanol, deionized water, and functional additives to the reaction vessel, mix and stir for 30 min, adjust the pH to 2.8 with 1 mol / L hydrochloric acid solution, add tetraethyl orthosilicate and methyltriethoxysilane at 28℃, continue stirring for 38 min, ultrasonically disperse at 200W power for 13 min, filter through a 0.23μm pore size filter membrane to obtain the impregnation solution; immerse the wood to be treated in the above impregnation solution, vacuum to -0.09MPa and maintain for 45 min, pressurize to 1.3MPa and maintain pressure for 4 h, remove after depressurization, wipe off excess liquid on the surface, and cure using a step-by-step procedure: keep at 40℃ for 12 h, raise the temperature to 60℃ and keep at 60℃ for 4 h, continue to raise the temperature to 80℃ and keep at 80℃ for 4 h, and finally raise the temperature to 103℃ and keep at 103℃ for 2 h, and humidify at 25℃ and 65% relative humidity for 7 days to obtain a deep-penetrating wood microporous invisible protective coating.
[0020] Comparative Example 3: This comparative example illustrates a process for preparing a deep-penetrating, microporous, invisible protective coating for wood, including the following steps: Step S1: Add 95g of sodium lignin sulfonate and 1200mL of deionized water to a three-necked flask equipped with a stirrer and thermometer, mix and stir for 30min, adjust the pH to 10.5 with 2mol / L sodium hydroxide solution, stir and activate at 70℃ for 1h, add 38mL of epichlorohydrin and 2g of benzyltriethylammonium chloride, react at 60℃ for 4.5h, cool naturally to 25℃, adjust the pH to 7 with 1mol / L hydrochloric acid solution, add 800mL of deionized water to precipitate the product, centrifuge, wash the precipitate twice with distilled water to obtain epoxidized lignin; add epoxidized lignin to 4000mL of tetrahydrofuran, shear at 10000r / min and add 4000mL of deionized water, rotary evaporate under reduced pressure at 35℃ and -0.09MPa for 3.5h to obtain an aqueous dispersion of epoxidized lignin nanoparticles; Step S2: Add 28g of bleached hardwood pulp and 1500mL of deionized water to a fiber de-fiber machine and de-fiberize for 5min to obtain a fiber suspension; add 0.45g of 2,2,6,6-tetramethylpiperidine oxide and 3g of sodium bromide to the fiber suspension, mix and stir for 30min, place in a 10℃ water bath, add 37mL of 12% sodium hypochlorite solution, adjust the pH to 10 with 0.5mol / L sodium hydroxide solution, and determine the carboxyl content by conductivity titration. When the carboxyl content reaches 0.9mmol / g, add 585mL of anhydrous ethanol and stir for 10min to terminate the oxidation reaction, pour into a funnel and filter, wash 3 times with distilled water, add 1500mL of deionized water, and transfer to a high-pressure microfluidic jet. The nanocellulose hydrogel was obtained by homogenizing the sample six times at 1000 bar. The dispersion medium was replaced with ethanol until the ethanol concentration was >95%. Under nitrogen protection, 1.3 mL of propyltriethoxysilane isocyanate and 0.05 g of dibutyltin dilaurate were added. The mixture was reacted at 60 °C for 8 h. After centrifugation, the precipitate was washed three times with distilled water. 90 mL of epoxidized lignin nanoparticle aqueous dispersion was added. The pH was adjusted to 8.5 with 2 mol / L ammonia water. The mixture was stirred for 4 h and centrifuged. The precipitate was dispersed in 1165 mL of anhydrous ethanol to obtain the synergistic reinforcing agent. Step S3: Weigh out 65 parts of tetraethyl orthosilicate, 30 parts of methyltriethoxysilane, 8 parts of synergistic reinforcing agent, 200 parts of anhydrous ethanol and 45 parts of deionized water according to the following weight proportions. Step S4: Add anhydrous ethanol and deionized water to the reaction vessel, mix and stir for 30 min, adjust the pH to 2.8 with 1 mol / L hydrochloric acid solution, add tetraethyl orthosilicate and methyltriethoxysilane at 28℃, continue stirring for 38 min, add synergistic reinforcing agent, ultrasonically disperse at 200W power for 13 min, filter through a 0.23μm pore size filter membrane to obtain impregnation solution; immerse the wood to be treated in the above impregnation solution, vacuum to -0.09MPa and maintain for 45 min, pressurize to 1.3MPa and maintain pressure for 4 h, remove after depressurization, wipe off excess liquid on the surface, and cure using a step-by-step procedure: constant temperature at 40℃ for 12 h, raise the temperature to 60℃ and hold for 4 h, continue to raise the temperature to 80℃ and hold for 4 h, finally raise the temperature to 103℃ and hold for 2 h, humidify at 25℃ and 65% relative humidity for 7 days to obtain a deep-penetrating wood microporous invisible protective coating.
[0021] The deep-penetrating microporous invisible protective coatings for wood prepared in Examples 1-3 and Comparative Examples 1-3 were analyzed using scanning electron microscopy combined with energy dispersive spectroscopy. Linear scanning of silicon elements in the treated wood was performed along the cross-section, and the distance from the surface where the silicon signal intensity abruptly drops to the substrate background level was taken as the penetration depth. The color difference value ΔE was calculated according to standard GB / T 7921-2008 "Uniform Color Space and Color Difference Formula". Simultaneously, the transmittance at a wavelength of 550 nm was measured using a UV-Vis spectrophotometer. The static contact angle between the coating surface and water was measured using a contact angle meter via the static drop method, according to standard GB / T 30693-2014 "Measurement of Contact Angle between Plastic Film and Water". The test method for the physical and mechanical properties of wood from June 1927 to 2021, "Test Methods for Physical and Mechanical Properties of Flawless Small Samples - Part 6: Determination of Drying Shrinkage", involved 10 cycles of moisture absorption and drying (one cycle consisted of soaking in water for 24 hours followed by drying at 60°C for 24 hours). After each cycle, the cross-section of the coating was observed using a 20x stereomicroscope to check for microcracks, and the swelling resistance was measured. The test results are shown in the table below.
[0022] Comparing Examples 1-3 with Comparative Examples 1-3: In Example 1, the amount of functional additives and synergistic reinforcing agents was relatively low, and the coating established a complete protective structure. However, the coverage density of fluorocarbon segments on the pore walls was insufficient, the volume ratio of the reinforcing network was low, and the water repellency and stress buffering capacity were low. In Example 2, the amount of the two core components was increased, the internal structure of the coating was optimized, and the increase of functional additives made the anchoring points of perfluorinated nanoclusters on the pore wall surface more dense, the hydrophobic interface tended to be complete, and the coating's ability to repel liquid water was enhanced. The increased proportion of synergistic reinforcing agents made the nanocellulose-lignin interpenetrating network form a finer through-structure in the siliceous phase, improving the stress buffering capacity of the coating. In Example 3, the amount of functional additives and synergistic reinforcing agents was the highest, the coating structure was complete, and a superhydrophobic monolayer was formed, achieving the best water repellency. The synergistic reinforcing agents constructed a flexible skeleton network, effectively dissipating the cyclic stress caused by wood expansion and contraction. Comparing Example 2 with Comparative Example 1, it can be seen that: Comparative Example 1 only used The pure silane system of tetraethyl orthosilicate and methyltriethoxysilane, after curing, forms a single inorganic silica network. Its hydrophobicity relies solely on the weak repulsive effect of methyl groups, resulting in a low water contact angle and high water absorption. Simultaneously, this pure inorganic network is brittle and prone to brittle cracking under repeated stress generated by the wood's wet-dry cycle. Comparing Example 2 with Comparative Example 2, it is evident that Comparative Example 2, with the addition of functional additives, imparts superhydrophobic properties to the coating and a high water contact angle. However, lacking the flexible cellulose nanoframework and lignin nanoparticles in the synergistic reinforcing agent, the coating remains a rigid system, lacking an effective stress dissipation mechanism. After multiple moisture absorption-drying cycles, interfacial stress accumulation leads to microcracks. Comparing Example 2 with Comparative Example 3, it is evident that Comparative Example 3, with only the addition of a synergistic reinforcing agent, effectively improves the coating's flexibility through a bio-based reinforcing network, preventing cracking during wet-dry cycles. However, the coating's pore wall interface is only hydrophobically modified by methylsilane, lacking the low surface energy effect of fluorocarbon segments, resulting in a low water contact angle and high water absorption.
[0023] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0024] The above description is merely an example and illustration of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described or use similar methods to replace them, as long as they do not deviate from the invention or exceed the scope defined in this application, they should all fall within the protection scope of the present invention.
Claims
1. A process for preparing a deep-penetrating, microporous, invisible protective coating for wood, characterized in that, Includes the following steps: Step 1: Weigh out 50-80 parts of tetraethyl orthosilicate, 20-40 parts of methyltriethoxysilane, 30-50 parts of functional additives, 5-10 parts of synergistic enhancer, 150-250 parts of anhydrous ethanol, and 30-60 parts of deionized water according to the following weight proportions. Step 2: Mix anhydrous ethanol, deionized water and functional additives, adjust the pH with 1 mol / L hydrochloric acid solution, add tetraethyl orthosilicate and methyltriethoxysilane and stir, add synergistic enhancer and ultrasonically disperse, filter through a filter membrane to obtain impregnation solution; The wood to be treated is immersed in the above impregnation solution, removed and the excess liquid on the surface is wiped off. The wood is then cured using a step-by-step process and humidified to obtain an invisible protective coating that can deeply penetrate the micropores of the wood.
2. The process for preparing a deep-penetrating, microporous, invisible protective coating for wood according to claim 1, characterized in that, The functional additive is prepared by the following steps: Tetraethyl orthosilicate and methyltriethoxysilane were mixed and stirred, and then an acidic alcohol aqueous solution was added and stirred continuously to obtain a hyperbranched prepolymer sol. 1H,1H,2H,2H-perfluorodecyltriethoxysilane was injected, and the mixture was ultrasonically dispersed. Deionized water was added and stirred, and the mixture was cooled. Hexane was added for extraction, and the aqueous phase was subjected to rotary evaporation under reduced pressure and dialyzed to obtain the functional additive.
3. The process for preparing a deep-penetrating, microporous, invisible protective coating for wood according to claim 2, characterized in that, The ratio of tetraethyl orthosilicate, methyltriethoxysilane, acidic alcohol aqueous solution, 1H,1H,2H,2H-perfluorodecyltriethoxysilane, deionized water, and n-hexane is 220-230 mL: 90-100 mL: 400 mL: 50-70 mL: 10-20 mL: 500 mL; the acidic alcohol aqueous solution is prepared by mixing anhydrous ethanol and 1 mol / L hydrochloric acid solution at a volume ratio of 8:
1.
4. The process for preparing a deep-penetrating, microporous, invisible protective coating for wood according to claim 1, characterized in that, The synergistic enhancer is prepared by the following steps: Step b1: Mix sodium lignosulfonate and the first portion of deionized water, adjust the pH with sodium hydroxide solution, stir to activate, add epichlorohydrin and benzyltriethylammonium chloride to react, cool, adjust the pH with hydrochloric acid solution, add the second portion of deionized water to precipitate the product, centrifuge, wash the precipitate with distilled water to obtain epoxidized lignin; add epoxidized lignin to tetrahydrofuran, add the third portion of deionized water under shear, and evaporate under reduced pressure to obtain an aqueous dispersion of epoxidized lignin nanoparticles; Step b2: Bleached hardwood pulp and the first portion of deionized water were added to a fiber de-fiber machine to de-fiber, resulting in a fiber suspension. 2,2,6,6-Tetramethylpiperidine oxide and sodium bromide were added and mixed. The mixture was placed in a water bath, and sodium hypochlorite solution was added. The pH was adjusted with sodium hydroxide solution. The carboxyl content was determined by conductivity titration. When the carboxyl content reached 0.9 mmol / g, the first portion of anhydrous ethanol was added to terminate the oxidation reaction. The mixture was poured into a funnel and filtered, washed with distilled water, and the second portion of deionized water was added. The mixture was then transferred to a high-pressure microfluidic homogenizer for further processing to obtain nanocellulose hydrogel. The dispersion medium was replaced with ethanol until the ethanol concentration was >95%. Under nitrogen protection, propyltriethoxysilane isocyanate and dibutyltin dilaurate were added to react. The mixture was centrifuged, and the precipitate was washed with distilled water. An aqueous dispersion of epoxidized lignin nanoparticles was added, and the pH was adjusted with ammonia. The mixture was mixed, centrifuged, and the precipitate was dispersed in the second portion of anhydrous ethanol to obtain a synergistic reinforcing agent.
5. The process for preparing a deep-penetrating, microporous, invisible protective coating for wood according to claim 4, characterized in that, The ratio of sodium lignosulfonate, total deionized water, epichlorohydrin, benzyltriethylammonium chloride, and tetrahydrofuran in step b1 is 90-100g: 6000mL: 35-40mL: 2g: 4000mL.
6. The process for preparing a deep-penetrating, microporous, invisible protective coating for wood according to claim 4, characterized in that, In step b1, the first portion of deionized water accounts for 1 / 5 of the total amount of deionized water; the second portion of deionized water accounts for 2 / 15 of the total amount of deionized water; the third portion of deionized water accounts for 2 / 3 of the total amount of deionized water; the concentration of the sodium hydroxide solution is 2 mol / L; and the concentration of the hydrochloric acid solution is 1 mol / L.
7. The process for preparing a deep-penetrating, microporous, invisible protective coating for wood according to claim 4, characterized in that, The ratio of the following components in step b2 is as follows: bleached hardwood pulp, total deionized water, 2,2,6,6-tetramethylpiperidine oxide, sodium bromide, sodium hypochlorite solution, total anhydrous ethanol, propyltriethoxysilane isocyanate, dibutyltin dilaurate, and epoxidized lignin nanoparticle aqueous dispersion: 25-30g: 2500-3500mL: 0.4-0.5g: 2.5-3.5g: 34-41mL: 1500-2000mL: 1.1-1.5mL: 0.04-0.06g: 80-100mL.
8. The process for preparing a deep-penetrating, microporous, invisible protective coating for wood according to claim 4, characterized in that, In step b2, the first portion of deionized water accounts for 1 / 2 of the total amount of deionized water; the second portion of deionized water accounts for 1 / 2 of the total amount of deionized water; the first portion of anhydrous ethanol accounts for 1 / 3 of the total amount of anhydrous ethanol; the second portion of anhydrous ethanol accounts for 2 / 3 of the total amount of anhydrous ethanol; the mass fraction of the sodium hypochlorite solution is 12%; the concentration of the sodium hydroxide solution is 0.5 mol / L; and the concentration of the ammonia solution is 2 mol / L.