Antibacterial bamboo integrated material using halloysite nanotube composite antibacterial agent and preparation method thereof
By using a method to prepare a composite antibacterial agent of halloysite nanotubes and quaternary ammonium salts, the problem of insufficient anti-mildew durability of bamboo was solved, achieving long-lasting antibacterial and anti-mildew properties and coating aging resistance, thus improving the anti-mildew durability and antibacterial performance of bamboo.
Patent Information
- Application Number
- CN202611263748.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-20
AI Technical Summary
Existing bamboo anti-mold technologies suffer from insufficient anti-mold durability, especially in warm and humid environments where mold easily grows. Furthermore, traditional coatings and anti-mold agents are difficult to penetrate evenly and provide long-lasting protection.
The method of using halloysite nanotubes and quaternary ammonium salt composite antibacterial agents involves expanding the cavity of halloysite nanotubes by acid etching and loading quaternary ammonium salt molecules to form a nanoscale reservoir. Combined with thiol quaternary ammonium salt modifier and wood wax oil, an organic-inorganic hybrid coating is formed to achieve slow release of antifungal active ingredients and improve antibacterial performance through chemical bonding.
It achieves long-lasting and efficient antibacterial and anti-mildew effects, improves the weather resistance and anti-mildew durability of the coating, reduces aging weak points, and enhances the resistance to external environmental stress.
Smart Images

Figure CN123129292A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to an antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent and its preparation method, belonging to the field of bamboo laminated timber technology. Background Technology
[0002] Bamboo laminated timber, as an environmentally friendly and high-performance bamboo material, is increasingly widely used. However, bamboo itself is rich in nutrients and is a porous, hydrophilic material, making it highly susceptible to mold growth in warm, humid environments. This leads to material deterioration and discoloration, affecting its service life and commercial value.
[0003] Existing bamboo anti-mold technologies are mainly divided into physical and chemical methods. Physical methods, such as heat treatment, easily lead to a decrease in the mechanical properties of bamboo and have a short anti-mold effect. Chemical methods mainly rely on anti-mold agents, such as:
[0004] 1. Inorganic antifungal agents: such as borates and copper-based preparations. Borates are easily washed away by rainwater; copper-based preparations (such as copper naphthenate) pose a risk of heavy metal environmental pollution.
[0005] 2. Organic polymer coatings: such as water-based acrylic resins and polyurethane (PU), although environmentally friendly and with good adhesion, have limited film strength and most of them do not have anti-mildew function and require the addition of anti-mildew agents.
[0006] 3. Organic small molecule antifungal agents: Quaternary ammonium salt compounds, such as dodecyl dimethyl benzyl ammonium chloride (BAC) and dialcyl dimethyl ammonium chloride (DDAC), have the advantages of broad-spectrum antibacterial properties and low toxicity. However, when applied directly, they have drawbacks such as easy solubility in water, easy loss, and poor heat resistance, resulting in insufficient antifungal durability.
[0007] Furthermore, during the molding process of bamboo laminated timber, such as flat pressing, the vascular bundles and thin-walled cells inside are severely compressed, resulting in a dense structure. This makes it difficult for traditional coatings and anti-mildew agents to penetrate evenly, further affecting the uniformity and durability of the anti-mildew effect.
[0008] Therefore, there is an urgent need to develop an antibacterial bamboo laminated timber that can firmly adhere to bamboo and slowly release anti-mildew active ingredients, thereby achieving long-lasting, efficient, and environmentally friendly anti-mildew properties, as well as its preparation method. Summary of the Invention
[0009] The purpose of this invention is to provide an antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent and its preparation method, so as to solve the problem of poor anti-mildew durability of current antibacterial bamboo laminated timber.
[0010] This invention provides a method for preparing antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agents, comprising the following steps: acid etching halloysite and a quaternary ammonium salt are combined to obtain a quaternary ammonium salt modified halloysite composite; then, the quaternary ammonium salt modified halloysite composite is mixed with wood wax oil to obtain an anti-mildew coating liquid; finally, the anti-mildew coating liquid is coated on the surface of bamboo, and after drying, antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agents is obtained; wherein the quaternary ammonium salt is dodecyl dimethyl benzyl ammonium chloride or a mercapto quaternary ammonium salt modifier, and the chemical structure of the mercapto quaternary ammonium salt modifier is as follows:
[0011] .
[0012] Preferably, the method for combining acid-etched halloysite and quaternary ammonium salt is as follows: acid-etched halloysite, quaternary ammonium salt and solvent are stirred at 50~60℃ for 6~8h, centrifuged, and the separated solid is washed and dried to obtain quaternary ammonium salt modified halloysite composite; the mass ratio of acid-etched halloysite to quaternary ammonium salt is 2:1~1.5.
[0013] Preferably, the preparation method of the acid-etched halloysite is as follows: halloysite nanotubes are dispersed in hydrochloric acid, stirred at 75~80℃ for 6~8h, centrifuged, and the solid obtained by centrifugation is washed, dried and ground to obtain acid-etched halloysite.
[0014] Preferably, the halloysite nanotube has an inner diameter of 10-15 nm, an outer diameter of 30-50 nm, and a length of 0.5-1 μm.
[0015] Preferably, the volume of hydrochloric acid corresponding to each 10g halloysite nanotube is 200~250mL; the concentration of hydrochloric acid is 1~1.5mol / L.
[0016] Preferably, the mass ratio of the quaternary ammonium salt modified halloysite complex to wood wax oil is 1:10~12.
[0017] Preferably, the method for mixing the quaternary ammonium salt modified halloysite complex and wood wax oil is as follows: the quaternary ammonium salt modified halloysite complex and wood wax oil are subjected to mechanical stirring and ultrasonic treatment in sequence.
[0018] Preferably, the mechanical stirring speed is 500~600 r / min, the time is 30~45 min, and the power density of the ultrasonic treatment is 0.5~0.6 W / cm³. 2 The time is 20-30 minutes.
[0019] Preferably, the preparation method of the mercapto quaternary ammonium salt modifier is as follows: pentaerythritol tetramercaptoacetate and 1-vinyl-3-butylimidazolium bromide are mixed and reacted in a solvent under the action of a photoinitiator and ultraviolet light, and then mixed and reacted with propenyltriethylammonium bromide under the action of a photoinitiator and ultraviolet light to obtain the mercapto quaternary ammonium salt modifier; the molar ratio of pentaerythritol tetramercaptoacetate, 1-vinyl-3-butylimidazolium bromide and propenyltriethylammonium bromide is 1:1:1.
[0020] An antibacterial bamboo laminated timber prepared by the method described above using halloysite nanotube composite antibacterial agent.
[0021] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0022] (1) In this invention, halloysite nanotubes are acid-etched. Acid etching can expand the cavity and surface active sites of halloysite nanotubes, thereby efficiently loading quaternary ammonium salt molecules through physical adsorption and electrostatic interaction. After being composited in a wood wax oil coating, the halloysite nanotubes, as nanoscale reservoirs, can effectively block the direct contact between quaternary ammonium salts and external moisture, and achieve slow and controllable release by relying on concentration difference, thus overcoming the problem of rapid loss caused by direct addition and achieving long-lasting antibacterial effect. In addition, halloysite nanotubes uniformly dispersed in wood wax oil can reflect and scatter some ultraviolet light and block the penetration of aging factors such as oxygen and moisture into the interior of the coating, thereby improving the overall weather resistance of the coating; moreover, the resulting coating is denser, reducing aging weak points caused by phase separation or additive precipitation.
[0023] (2) This invention synthesizes a mercapto quaternary ammonium salt modifier containing mercapto, imidazole bromide, and ammonium bromide, and loads the mercapto quaternary ammonium salt modifier onto acid-etched halloysite through physical adsorption, electrostatic interaction, and chemical bonding, thereby improving the antibacterial properties, anti-mildew durability, and coating aging resistance of bamboo laminated timber. Among them, the "-SH" (mercapto) at the end of the mercapto quaternary ammonium salt modifier can form strong chemical bonds with aluminum hydroxyl groups on the surface of halloysite (such as forming Al-S bonds); the imidazole onion salt and chain quaternary ammonium salt introduced into the molecular structure can produce a synergistic antibacterial effect, broaden the antibacterial spectrum, and improve the bactericidal efficiency; the dendritic structure of the mercapto quaternary ammonium salt modifier with pentaerythritol as the core provides multiple anchoring sites, enabling each modifier molecule to be more firmly grafted onto halloysite and exposing more quaternary ammonium salt active sites, thereby improving the antibacterial properties and long-lasting anti-mildew performance of bamboo laminated timber. Furthermore, the chemically bonded mercapto quaternary ammonium salt-haloite complex exhibits better compatibility with the wood wax oil matrix, enabling the formation of a more uniform and stable organic-inorganic hybrid coating network with stronger resistance to external environmental stresses (light, heat, and humidity). Attached Figure Description
[0024] Figure 1This is a scanning electron microscope (SEM) image of the quaternary ammonium salt modified halloysite complex prepared in Example 1 of the present invention;
[0025] Figure 2 This is the 1H NMR spectrum of the thiol quaternary ammonium salt modifier prepared in Example 4 of the present invention. Detailed Implementation
[0026] The following examples are intended to further illustrate the content of the present invention, rather than to limit the scope of protection of the present invention.
[0027] Example 1
[0028] The preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in this embodiment includes the following steps:
[0029] (1) 10g of natural halloysite nanotubes (with an inner diameter of 10~15nm, an outer diameter of 30~50nm, and a length of 0.5~1μm) were dispersed in 200mL of 1mol / L hydrochloric acid and mechanically stirred at 80℃ (stirring speed of 450r / min) for 6h. The mixture was then centrifuged (centrifugation speed of 8000r / min for 15min). The solid obtained by centrifugation was washed with deionized water until the washing liquid was neutral. The washed solid was then dried at 80℃ to obtain acid-etched halloysite.
[0030] (2) 2g of acid-etched halloysite was dispersed in 50mL of n-propanol, and 1g of dodecyl dimethyl benzyl ammonium chloride was added. The mixture was mechanically stirred in a water bath at 60℃ (stirring speed of 600r / min) for 6h, and then centrifuged (centrifugation speed of 8000r / min for 10min). The solid obtained by centrifugation was washed with ethanol (washed 3 times, with 30mL of ethanol used each time). The washed solid was then placed in a vacuum drying oven at 60℃ (absolute pressure maintained at 1kPa) and dried for 12h to obtain the quaternary ammonium salt modified halloysite complex. The scanning electron microscope (SEM) image of the quaternary ammonium salt modified halloysite complex is shown below. Figure 1 As shown. From Figure 1 As can be seen, the surface of the modified halloysite nanotubes becomes rough, indicating that the quaternary ammonium salt was successfully loaded onto its surface.
[0031] (3) 1g of quaternary ammonium salt modified halloysite complex and 10g of wood wax oil (wood wax oil is prepared by mixing linseed oil, carnauba wax and soybean oil in a mass ratio of 6:3:1 at 85℃ and then cooling to room temperature) were mechanically stirred (mechanical stirring speed of 500r / min, time of 30min) and ultrasonically treated (power density of ultrasonic treatment of 0.5W / cm³) in sequence. 2(At a frequency of 25kHz and a duration of 20min), an anti-mildew coating liquid was obtained.
[0032] (4) Sand the surface of the bamboo engineered wood (the specifications of the bamboo engineered wood are 1000mm×200mm×20mm, and the moisture content is 7%) (the sandpaper used for sanding is 240 grit) and clean it (the cleaning is done by wiping with ethanol). Then, apply the anti-mildew coating liquid evenly to the surface of the bamboo with a brush. Apply two coats in total (let it stand at room temperature for 12 hours after the first coat to dry before applying the second coat). The amount of coating each time is 45g / m². 2 Then, it is dried in an oven at 60℃ for 8 hours to obtain antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent.
[0033] Example 2
[0034] The difference between the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in this embodiment and the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in Example 1 is that the temperature used for stirring for 6 hours in step (2) of the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in this embodiment is adjusted from 60℃ to 40℃.
[0035] Example 3
[0036] The difference between the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in this embodiment and the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in Example 1 is that the temperature used for stirring for 6 hours in step (2) of the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in this embodiment is adjusted from 60℃ to 80℃.
[0037] Example 4
[0038] The preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in this embodiment includes the following steps:
[0039] (1) Add 0.1 mol of pentaerythritol tetramercaptoacetate and 400 mL of anhydrous tetrahydrofuran to the reaction flask, stir well, and then purge with nitrogen gas. Then add 0.005 mol of photoinitiator benzoin dimethyl ether and 0.1 mol of 1-vinyl-3-butylimidazolium bromide to the reaction flask, stir until the solid is fully dissolved, and then stir and react for 20 min under 365 nm ultraviolet light irradiation (ultraviolet light intensity is 30 mW / cm). 2With the light source 10 cm above the liquid surface and the stirring speed at 500 r / min, after turning off the UV light, 0.005 mol of photoinitiator benzoin dimethyl ether and 0.1 mol of propenyltriethylammonium bromide were added to the reaction flask. After stirring until the solids were fully dissolved, the reaction was continued under 365 nm UV light irradiation for 35 min with stirring (UV light source intensity 30 mW / cm²). 2 The light source was positioned 10 cm above the liquid surface, and the stirring speed was 500 r / min. Then, the UV light was turned off, and the reaction solution in the reaction flask was subjected to vacuum distillation to remove the solvent tetrahydrofuran, yielding a crude product. 300 mL of anhydrous diethyl ether was added to the crude product, and after stirring evenly, it was allowed to stand for 4 hours. The mixture was then filtered, and the filter cake was washed three times with anhydrous diethyl ether (50 mL each time). Finally, the washed solid was dried in a vacuum drying oven at 40 °C for 12 hours to obtain the thiol quaternary ammonium salt modifier. The 1H NMR spectrum of the thiol quaternary ammonium salt modifier is shown below. Figure 2 As shown, the chemical structure is as follows:
[0040] .
[0041] (2) 10g of natural halloysite nanotubes (with an inner diameter of 10~15nm, an outer diameter of 30~50nm, and a length of 0.5~1μm) were dispersed in 200mL of 1mol / L hydrochloric acid and mechanically stirred at 80℃ (stirring speed of 450r / min) for 6h. The mixture was then centrifuged (centrifugation speed of 8000r / min for 15min). The solid obtained by centrifugation was washed with deionized water until the washing solution was neutral. The washed solid was then dried at 80℃ to obtain acid-etched halloysite.
[0042] (3) Take 2g of acid-etched halloysite and disperse it in 50mL of n-propanol. Add 1g of mercapto quaternary ammonium salt modifier. Stir mechanically in a water bath at 60℃ (stirring speed is 600r / min) for 6h and then centrifuge (centrifugation speed is 8000r / min, time is 10min). Wash the solid obtained by centrifugation with ethanol (wash 3 times, each time the volume of ethanol is 30mL). Then place the washed solid in a vacuum drying oven at 60℃ (absolute pressure in the vacuum drying oven is maintained at 1kPa) and dry for 12h to obtain quaternary ammonium salt modified halloysite complex.
[0043] (4) 1g of quaternary ammonium salt modified halloysite complex and 10g of wood wax oil (wood wax oil is prepared by mixing linseed oil, carnauba wax and soybean oil in a mass ratio of 6:3:1 at 85℃ and then cooling to room temperature) were mechanically stirred (mechanical stirring speed of 500r / min, time of 30min) and ultrasonically treated (power density of ultrasonic treatment of 0.5W / cm³) in sequence. 2(At a frequency of 25kHz and a duration of 20min), an anti-mildew coating liquid was obtained.
[0044] (5) Sand the surface of the bamboo engineered wood (the specifications of the bamboo engineered wood are 1000mm×200mm×20mm, and the moisture content is 7%) (the sandpaper used for sanding is 240 mesh) and clean it (the cleaning is done by wiping with ethanol). Then, the anti-mildew coating liquid is evenly brushed onto the surface of the bamboo material. The coating is applied twice (the second coating is applied after the first coating is left to stand at room temperature for 12 hours to dry). The coating amount is 45g / m² each time. Then, the material is dried in an oven at 60℃ for 8 hours to obtain antibacterial bamboo engineered wood with halloysite nanotube composite antibacterial agent.
[0045] Comparative Example 1
[0046] The difference between the preparation method of the antibacterial bamboo laminated timber in this comparative example and the preparation method of the antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in Example 1 is that the mass fraction of the quaternary ammonium salt modified halloysite composite in the anti-mildew coating liquid used in step (4) of the preparation method of the antibacterial bamboo laminated timber in this comparative example is 0, that is, only wood wax oil is used to coat the surface of bamboo in this comparative example.
[0047] Comparative Example 2
[0048] The difference between the preparation method of the antibacterial bamboo laminated timber in this comparative example and the preparation method of the antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in Example 1 is that the anti-mildew coating liquid used in step (4) of the preparation method of the antibacterial bamboo laminated timber in this comparative example is that 1g of dodecyl dimethyl benzyl ammonium chloride is dispersed in 10g of wood wax oil (wood wax oil is prepared by stirring and mixing linseed oil, carnauba wax and soybean oil in a mass ratio of 6:3:1 at 85°C and then cooling to room temperature).
[0049] Comparative Example 3
[0050] The difference between the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in this comparative example and the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in Example 1 is that in step (2) of the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in this comparative example, dodecyl dimethyl benzyl ammonium chloride is replaced with dialcyl dimethyl ammonium chloride.
[0051] Comparative Example 4
[0052] The difference between the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in this comparative example and the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in Example 1 is that in step (2) of the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in this comparative example, acid etching halloysite is replaced with natural halloysite nanotubes in step (1).
[0053] Comparative Example 5
[0054] The difference between the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in this comparative example and the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in Example 4 is that the step (1) of the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in this comparative example is as follows: 0.1 mol of pentaerythritol tetramercaptoacetate and 400 mL of anhydrous tetrahydrofuran are added to the reaction flask, stirred evenly, and nitrogen gas is introduced. Then, 0.01 mol of photoinitiator benzoin dimethyl ether and 0.2 mol of 1-vinyl-3-butylimidazolium bromide are added to the reaction flask. After stirring until the solid is fully dissolved, the reaction is carried out under 365 nm ultraviolet light irradiation for 55 min (ultraviolet light source intensity is 30 mW / cm). 2 The light source was positioned 10 cm above the liquid surface, and the stirring speed was 500 r / min. Then, the UV light was turned off, and the reaction solution in the reaction flask was subjected to vacuum distillation to remove the solvent tetrahydrofuran, yielding a crude product. 300 mL of anhydrous diethyl ether was added to the crude product, and after stirring evenly, it was allowed to stand for 4 hours. The mixture was then filtered, and the filter cake was washed three times with anhydrous diethyl ether (50 mL each time). Finally, the washed solid was dried in a vacuum drying oven at 40 °C for 12 hours to obtain a mercapto quaternary ammonium salt modifier. The chemical structure of the mercapto quaternary ammonium salt modifier is as follows:
[0055] .
[0056] Comparative Example 6
[0057] The difference between the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in this comparative example and the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in Example 4 is that the step (1) of the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in this comparative example is as follows: 0.1 mol of pentaerythritol tetramercaptoacetate and 400 mL of anhydrous tetrahydrofuran are added to the reaction flask, stirred evenly, and nitrogen gas is introduced. Then, 0.01 mol of photoinitiator benzoin dimethyl ether and 0.2 mol of propenyl triethylammonium bromide are added to the reaction flask, stirred until the solid is fully dissolved, and then stirred and reacted under 365 nm ultraviolet light irradiation for 55 min (ultraviolet light source intensity is 30 mW / cm). 2The light source was positioned 10 cm above the liquid surface, and the stirring speed was 500 r / min. Then, the UV light was turned off, and the reaction solution in the reaction flask was subjected to vacuum distillation to remove the solvent tetrahydrofuran, yielding a crude product. 300 mL of anhydrous diethyl ether was added to the crude product, and after stirring evenly, it was allowed to stand for 4 hours. The mixture was then filtered, and the filter cake was washed three times with anhydrous diethyl ether (50 mL each time). Finally, the washed solid was dried in a vacuum drying oven at 40 °C for 12 hours to obtain a mercapto quaternary ammonium salt modifier. The chemical structure of the mercapto quaternary ammonium salt modifier is as follows:
[0058] .
[0059] Comparative Example 7
[0060] The difference between the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in this comparative example and the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in Example 4 is only that the step (1) of the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in this comparative example is as follows: 0.1 mol of pentaerythritol tetramercaptoacetate and 400 mL of anhydrous tetrahydrofuran are added to the reaction flask, stirred evenly, and nitrogen gas is introduced. Then, 0.005 mol of photoinitiator benzoin dimethyl ether and 0.1 mol of 1-vinyl-3-butylimidazolium bromide are added to the reaction flask, stirred until the solid is fully dissolved, and stirred under 365 nm ultraviolet light irradiation for 20 min (ultraviolet light source intensity is 30 mW / cm). 2 With the light source 10 cm above the liquid surface and the stirring speed at 500 r / min, after turning off the UV light, 0.01 mol of photoinitiator benzoin dimethyl ether and 0.2 mol of propenyltriethylammonium bromide were added to the reaction flask. After stirring until the solids were fully dissolved, the reaction was continued under 365 nm UV light irradiation for 60 min (UV light source intensity 30 mW / cm²). 2 The light source was positioned 10 cm above the liquid surface, and the stirring speed was 500 r / min. Then, the UV light was turned off, and the reaction solution in the reaction flask was subjected to vacuum distillation to remove the solvent tetrahydrofuran, yielding a crude product. 300 mL of anhydrous diethyl ether was added to the crude product, and after stirring evenly, it was allowed to stand for 4 hours. The mixture was then filtered, and the filter cake was washed three times with anhydrous diethyl ether (50 mL each time). Finally, the washed solid was dried in a vacuum drying oven at 40 °C for 12 hours to obtain a mercapto quaternary ammonium salt modifier. The chemical structure of the mercapto quaternary ammonium salt modifier is as follows:
[0061] .
[0062] Comparative Example 8
[0063] The difference between the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in this comparative example and the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in Example 4 is that the step (1) of the preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent in this comparative example is as follows: 0.1 mol of pentaerythritol tetramercaptoacetate and 400 mL of anhydrous tetrahydrofuran are added to the reaction flask, and after stirring evenly, nitrogen gas is introduced. Then, 0.01 mol of photoinitiator benzoin dimethyl ether and 0.2 mol of 1-vinyl-3-butylimidazolium bromide are added to the reaction flask. After stirring until the solid is fully dissolved, the reaction is carried out under 365 nm ultraviolet light irradiation for 45 min (ultraviolet light source intensity is 30 mW / cm). 2 With the light source 10 cm above the liquid surface and the stirring speed at 500 r / min, after turning off the UV light, 0.005 mol of photoinitiator benzoin dimethyl ether and 0.1 mol of propenyltriethylammonium bromide were added to the reaction flask. After stirring until the solids were fully dissolved, the reaction was continued under 365 nm UV light irradiation for 35 min with stirring (UV light source intensity 30 mW / cm²). 2 The light source was positioned 10 cm above the liquid surface, and the stirring speed was 500 r / min. Then, the UV light was turned off, and the reaction solution in the reaction flask was subjected to vacuum distillation to remove the solvent tetrahydrofuran, yielding a crude product. 300 mL of anhydrous diethyl ether was added to the crude product, and after stirring evenly, it was allowed to stand for 4 hours. The mixture was then filtered, and the filter cake was washed three times with anhydrous diethyl ether (50 mL each time). Finally, the washed solid was dried in a vacuum drying oven at 40 °C for 12 hours to obtain a mercapto quaternary ammonium salt modifier. The chemical structure of the mercapto quaternary ammonium salt modifier is as follows:
[0064] .
[0065] Experimental Example
[0066] This experimental example is used to evaluate the anti-mold and aging resistance properties of the antibacterial bamboo laminated timber prepared in each embodiment and comparative example. The test method for anti-mold performance is as follows: Antibacterial bamboo laminated timber samples were cut into 50mm × 50mm × 20mm pieces and placed statically in an accelerated testing chamber at a constant temperature of 30℃ and relative humidity of RH 90%. The chamber was periodically (every 3 days) sprayed with a mixed mold spore suspension of Aspergillus niger + Aspergillus flavus + Trichoderma (spore concentration 1 × 10⁻⁶). 7 CFU / mL, spraying rate 5mL / m² 2The samples were cultured in the dark throughout the process, and the surface mold was observed daily. The time when the earliest visible mold colonies (with a minimum colony diameter of 0.5 mm) appeared on the surface of the antibacterial bamboo laminated material was recorded as the number of days of antibacterial performance. The test method for aging resistance is as follows: the antibacterial bamboo laminated material was subjected to a 40-hour ultraviolet aging test. The difference in lightness ΔL, the difference in red-green index Δa, and the difference in yellow-blue index Δb before and after the ultraviolet aging test were measured and calculated using a colorimeter. The test results are shown in Table 1.
[0067] Table 1. Anti-mildew and aging resistance properties of antibacterial bamboo laminated lumber
[0068]
[0069] As can be seen from the test data in Table 1, the antibacterial bamboo laminated timber prepared by the present invention has good antibacterial properties, durable mildew resistance and coating aging resistance.
[0070] As shown in Examples 1 and 4, when using the synthesized thiol quaternary ammonium salt modifier containing thiol, imidazole bromide, and ammonium bromide, the prepared antibacterial bamboo laminated timber exhibits better antibacterial properties, longer-lasting mildew resistance, and better coating aging resistance. This is because: the "-SH" (thiol group) at the end of the synthesized thiol quaternary ammonium salt modifier can form strong chemical bonds (such as Al-S bonds) with aluminum hydroxyl groups on the surface of halloysite, and its binding strength is far greater than the physical adsorption / electrostatic interaction in Example 1; both imidazole onium salt and chain quaternary ammonium salt are introduced into the molecular structure, and the two produce a synergistic antibacterial effect, broadening the antibacterial spectrum and improving the bactericidal efficiency; the dendritic structure of the thiol quaternary ammonium salt modifier with pentaerythritol as the core provides multiple anchoring sites, enabling each modifier molecule to be more firmly grafted onto halloysite and exposing more quaternary ammonium salt active sites. Therefore, the antibacterial bamboo laminated timber prepared in Example 4 not only has stronger antibacterial properties, but also, due to chemical bonding, its effective components are effectively immobilized and resisted from leaching on the bamboo surface and in the coating, thus exhibiting long-lasting anti-mildew properties. Furthermore, the chemically bonded thiol quaternary ammonium salt-haloysite composite in Example 4 has better compatibility with the wood wax oil matrix, enabling the formation of a more uniform and stable organic-inorganic hybrid coating network, which has stronger resistance to external environmental stresses (light, heat, and humidity).
[0071] As demonstrated in Example 1 and Comparative Examples 1-2, simple wood wax oil or quaternary ammonium salts without carrier protection can hardly provide effective and durable antibacterial and antifungal effects. Quaternary ammonium salts have poor dispersibility in wood wax oil, making effective contact with bacteria impossible. Furthermore, the inherent defects of quaternary ammonium salts, such as easy loss and poor heat resistance, lead to poor antibacterial performance and durability of antifungal properties in antibacterial bamboo engineered wood. Moreover, antifungal coatings prepared from pure wood wax oil or quaternary ammonium salts without carrier protection exhibit extremely poor UV aging resistance, are prone to degradation and yellowing, and cannot provide protection for the substrate and internal components. In Example 1, halloysite nanotubes were acid-etched. Acid etching can expand the cavity and surface active sites of halloysite nanotubes, thereby efficiently loading quaternary ammonium salt molecules (dodecyl dimethyl benzyl ammonium chloride) through physical adsorption and electrostatic interactions. When incorporated into a wood wax oil coating, halloysite nanotubes act as nanoscale reservoirs, effectively preventing direct contact between quaternary ammonium salts and external moisture. They also achieve slow, controlled release through concentration differences, overcoming the rapid loss problem caused by direct addition and achieving long-lasting antibacterial effects. Furthermore, the halloysite nanotubes uniformly dispersed in the wood wax oil in Example 1 reflect and scatter some ultraviolet light and block the penetration of aging factors such as oxygen and moisture into the coating, thereby improving the overall weather resistance of the coating. Moreover, the resulting coating is denser, reducing aging weaknesses caused by phase separation or additive precipitation.
[0072] As shown in Example 1 and Comparative Example 3, although both dodecyl dimethyl benzyl ammonium chloride (BAC) and dialcyl dimethyl ammonium chloride (DDAC) are quaternary ammonium salts, BAC is a single-chain (C12) quaternary ammonium salt with one benzyl group, while DDAC is a double-chain (two C10) quaternary ammonium salt. There are certain differences in their molecular structure, spatial conformation, and hydrophobicity. After acid etching, halloysite nanotubes exhibit confined spaces and active sites on their cavities and surfaces. The molecular structure of BAC (single-chain + benzyl group) may be more conducive to its entry into the nanopores of halloysite and to stronger adsorption with the tube wall through π-π interactions (benzyl group), thereby achieving higher loading capacity and more stable binding. In contrast, the double-chain structure of DDAC may lead to greater steric hindrance, reducing its loading efficiency and compactness within the halloysite channels. The higher loading capacity and optimized binding mechanism enable the BAC-haloysite composite in Example 1 to release antibacterial BAC molecules more efficiently and continuously upon contact with bacteria, resulting in a larger inhibition zone. In contrast, the DDAC loading in Comparative Example 3 may be more inclined towards surface adsorption, leading to rapid release but insufficient total amount, resulting in a sharp decrease in antibacterial efficacy. Furthermore, the stronger interaction between BAC and halloysite (hydrophobic interactions, π-effects, etc.) allows it to be more firmly anchored to the halloysite carrier in the bamboo coating, resulting in better anti-mold durability. The composite system in Example 1 achieves long-term, low-rate BAC release, maintaining an effective concentration above the anti-mold threshold on the bamboo surface for an extended period. In contrast, the relatively weak binding of DDAC to the carrier in Comparative Example 3 may result in insufficient subsequent supply after the initial rapid release, leading to a significantly shortened anti-mold protection period. Furthermore, the BAC-haloysite composite, due to its superior interfacial compatibility and dispersion stability, can form a more uniform nanocomposite coating with fewer defects in wood wax oil. This more uniform dispersion means that halloysite nanotubes can construct a more effective three-dimensional network physical barrier within the coating, more efficiently scattering ultraviolet light and blocking the penetration of aging media such as oxygen and water, thus better protecting both the coating itself and the bamboo substrate. In contrast, the DDAC composite in Comparative Example 3, due to its slightly poorer dispersibility or weaker interfacial bonding with the matrix, is more likely to become stress defect points within the coating during ultraviolet aging, accelerating photodegradation and discoloration.
[0073] As can be seen from Example 1 and Comparative Example 4, compared with the direct loading of quaternary ammonium salts onto natural halloysite nanotubes in Comparative Example 4, hydrochloric acid treatment can not only remove impurities from halloysite, but also significantly increase its inner diameter and specific surface area, thereby greatly improving its loading capacity and binding strength for quaternary ammonium salt molecules, and thus improving its antibacterial properties and antifungal durability.
[0074] As can be seen from Example 1 and Comparative Examples 5-6, when only a mercapto quaternary ammonium salt modifier containing ammonium bromide or imidazole bromide is used, the antibacterial and antifungal properties of the prepared antibacterial bamboo laminated timber deviate. This proves that ammonium bromide and imidazole bromide can work together from different angles to synergistically improve the antibacterial and antifungal properties of the antibacterial bamboo laminated timber.
[0075] As can be seen from Example 1 and Comparative Examples 7-8, when only a thiol quaternary ammonium salt modifier containing one thiol group is used, the antibacterial and antifungal properties of the prepared antibacterial bamboo laminated timber are also poor. This may be because the thiol quaternary ammonium salt modifier containing only one thiol group used in Comparative Examples 7-8 has too many molecular branches, and some active sites are buried inside the molecule or agglomerated, resulting in a significant decrease in spatial accessibility and severely weakening the apparent antibacterial activity. Moreover, the reduced number of thiol groups in the thiol quaternary ammonium salt modifier may lead to a decrease in the ability of the thiol quaternary ammonium salt modifier to form strong chemical bonds with aluminum hydroxyl groups on the halloysite surface, resulting in a decline in performance.
Claims
1. A method for preparing antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent, characterized in that, The process includes the following steps: acid etching of halloysite and quaternary ammonium salt are combined to obtain a quaternary ammonium salt-modified halloysite composite; then, the quaternary ammonium salt-modified halloysite composite is mixed with wood wax oil to obtain an anti-mildew coating liquid; finally, the anti-mildew coating liquid is applied to the surface of bamboo, and after drying, antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent is obtained; the quaternary ammonium salt is dodecyl dimethyl benzyl ammonium chloride or mercapto quaternary ammonium salt modifier, and the chemical structure of the mercapto quaternary ammonium salt modifier is as follows: 。 2. The preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent as described in claim 1, characterized in that, The method for combining acid-etched halloysite and quaternary ammonium salt is as follows: acid-etched halloysite, quaternary ammonium salt and solvent are stirred at 50~60℃ for 6~8h, centrifuged, and the separated solid is washed and dried to obtain quaternary ammonium salt modified halloysite composite; the mass ratio of acid-etched halloysite to quaternary ammonium salt is 2:1~1.
5.
3. The method for preparing antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent as described in claim 2, characterized in that, The method for preparing acid-etched halloysite is as follows: Halloysite nanotubes are dispersed in hydrochloric acid and stirred at 75~80℃ for 6~8h. After centrifugation, the solid obtained by centrifugation is washed, dried and ground to obtain acid-etched halloysite.
4. The preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent as described in claim 3, characterized in that, The halloysite nanotubes have an inner diameter of 10-15 nm, an outer diameter of 30-50 nm, and a length of 0.5-1 μm.
5. The preparation method of antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent as described in claim 3, characterized in that, The volume of hydrochloric acid corresponding to each 10g halloysite nanotube is 200~250mL; the concentration of hydrochloric acid is 1~1.5mol / L.
6. The method for preparing antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent as described in claim 1, characterized in that, The mass ratio of the quaternary ammonium salt modified halloysite complex to wood wax oil is 1:10~12.
7. The method for preparing antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent as described in claim 6, characterized in that, The method for mixing the quaternary ammonium salt modified halloysite complex and wood wax oil is as follows: the quaternary ammonium salt modified halloysite complex and wood wax oil are mechanically stirred and ultrasonically treated in sequence.
8. The method for preparing antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent as described in claim 7, characterized in that, The mechanical stirring speed is 500~600 r / min, the time is 30~45 min, and the power density of the ultrasonic treatment is 0.5~0.6 W / cm³. 2 The time is 20-30 minutes.
9. The method for preparing antibacterial bamboo laminated timber using halloysite nanotube composite antibacterial agent as described in any one of claims 1-8, characterized in that, The preparation method of the mercapto quaternary ammonium salt modifier is as follows: pentaerythritol tetramercaptoacetate and 1-vinyl-3-butylimidazolium bromide are mixed and reacted in a solvent under the action of a photoinitiator and ultraviolet light, and then mixed and reacted with propenyltriethylammonium bromide under the action of a photoinitiator and ultraviolet light to obtain the mercapto quaternary ammonium salt modifier; the molar ratio of pentaerythritol tetramercaptoacetate, 1-vinyl-3-butylimidazolium bromide and propenyltriethylammonium bromide is 1:1:
1.