A bamboo softening agent with insect prevention, corrosion prevention and mildew prevention functions, and a preparation method and application thereof

By preparing a bamboo softener that combines insect-proof, anti-corrosion, and anti-mildew functions, the problem of separating bamboo softening and protection was solved, achieving stable plasticization and integrated protection of bamboo, reducing resilience and energy consumption, and improving environmental friendliness.

CN123129294APending Publication Date: 2026-11-20GUANGDONG ZHIYUAN CHUANGNENG TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611382239.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-07
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing bamboo softening and insect-proofing, anti-corrosion and anti-mildew treatments are separate processes. The chemicals are easily rendered in alkaline environments, the protective components are easily lost, the treatment conditions are harsh, the softening effect is uneven, the bamboo is prone to rebound, and some chemicals have poor environmental performance.

Method used

The bamboo softener, which combines insect-proof, anti-corrosion, and anti-mildew functions, includes a basic carrier component, a core modified composite additive, and a functional regulator. It is prepared by shearing and curing and mixing and standing, followed by impregnation, shaping, and drying treatments to achieve integrated bamboo softening and protection.

Benefits of technology

It achieves stable plasticization of bamboo under mild conditions, reduces resilience, enhances the adhesion of protective components, has good insect-proof, anti-corrosion and anti-mildew properties, is environmentally friendly and non-toxic, simplifies the production process, and reduces energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The application provides a bamboo softening agent with insect prevention, corrosion prevention and mildew prevention functions, and a preparation method and application thereof, and belongs to the technical field of bamboo processing and modification. The softening agent comprises the following components in mass fractions: 40-70 parts of a basic carrier component, 15-40 parts of a core modified composite additive, and 8-20 parts of a function regulator; wherein the core modified composite additive comprises a weak alkaline buffer regulator, a lignin directional cracking additive, a cellulose crystallinity regulator, and a bio-based polyol plasticizer; and the function regulator comprises a chelated metal ion passivator, a plant flavone natural crosslinking stabilizer, a micro-molecule penetration synergist, and a bioactive composite agent. The temperature of the softening agent in the process of treating bamboo is not higher than 65 DEG C, and the softening agent does not need to be treated in cooperation with high-temperature steam, does not need high-temperature and high-pressure equipment, and has a significantly lower energy consumption than the existing DES-high-temperature steam cooperation technology, has a small equipment investment, is high in safety, and is more suitable for the industrialization popularization of existing bamboo processing enterprises.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of bamboo processing and modification technology, and in particular to a bamboo softener with insect-proof, anti-corrosion and anti-mildew functions, its preparation method and application. Background Technology

[0002] Bamboo, as a renewable and environmentally friendly resource, is widely used in building materials, furniture, and composite materials due to its short growth cycle, excellent mechanical properties, and strong carbon sequestration ability. However, the high cellulose crystallinity (60-70%) in bamboo cell walls and the dense, three-dimensionally cross-linked lignin structure result in poor natural plasticity. Direct processing easily leads to brittleness, deformation, and springback, severely restricting the high-value utilization of bamboo. Furthermore, bamboo is rich in nutrients such as starch, sugars, and proteins, making it highly susceptible to mold and decay fungi and insect infestation by pests like bamboo borers under suitable temperature and humidity conditions. Untreated bamboo products have a short lifespan. Therefore, softening treatment is necessary to improve bamboo processing performance while simultaneously providing integrated protection against insects, decay, and mold.

[0003] Currently, the commonly used bamboo softening methods in the industry mainly include the following categories: (1) Strong alkali cooking method: Bamboo is cooked at high temperature using strong alkali solutions such as NaOH and KOH to soften it by breaking the ester bonds of lignin and hemicellulose. This method softens bamboo quickly, but it has problems such as strong alkali corrosion, low bamboo yield, difficulty in wastewater treatment, and easy rebound after softening. In addition, high-temperature cooking consumes a lot of energy, has almost no protective function, and requires separate insect and rot prevention treatment afterward, making the process lengthy.

[0004] (2) Ammonia-urea combined treatment method: softening is carried out by soaking in ammonia water combined with boiling in urea solution. Although this method improves the softening effect to a certain extent, the treatment cycle is long, ammonia volatilization causes environmental pollution and health risks, and the softening uniformity is poor, with no long-term insect and mold prevention effect.

[0005] (3) Eutectic Solvent (DES) Treatment: In recent years, DES technology has emerged, which uses hydrogen bond acceptors and donors to form an eutectic system for pretreatment of lignocellulosic biomass. Examples include the method of using metal ion-based eutectic solvents and high-temperature steam to soften bamboo, and the method of using lactic acid / zinc chloride-based DES in conjunction with high-temperature steam treatment. Although this type of method has a good softening effect, it usually requires high-temperature (above 100~130℃) steam treatment, which results in high energy consumption, demanding equipment requirements, and the acidic DES system may cause a certain degree of degradation damage to bamboo, resulting in a lack of protective performance.

[0006] (4) Supramolecular solvent softening method: The hydrophobic barrier on the surface of bamboo fibers is destroyed by supramolecular solvents. This method is mainly used for the extraction of bamboo raw fibers, and its application scenarios are relatively limited. In addition, it involves biological enzyme catalysis steps, and the process is complex and time-consuming.

[0007] (5) Traditional composite softening agent method: Softeners with glycerol, surfactants, aldehydes and other main components can improve the flexibility of bamboo to a certain extent, but they often contain harmful substances such as formaldehyde, which are not environmentally friendly and the softening effect is not stable enough. Most of the existing bamboo insect and mildew prevention agents are independent impregnation processes, which are separate from the softening process. The agents have weak bonding with the bamboo cell walls, are easy to be lost, and have poor weather resistance. Some of the protective agents containing heavy metals pose environmental safety hazards.

[0008] Existing technologies have significant drawbacks: bamboo softening and insect-proofing, anti-corrosion, and anti-mildew protection are handled in two separate processes, resulting in low production efficiency; the protective agents have poor compatibility with the softening system, and some antibacterial and insect-proofing agents decompose and become ineffective in alkaline environments; the protective components only adhere to the surface of the bamboo, exhibiting poor resistance to leaching; they often rely on strong acids and alkalis or high-temperature and high-pressure conditions, leading to high energy consumption and demanding equipment requirements; the softening effect is uneven, with the surface layer easily becoming too soft while the core layer remains unsoftened; the softened bamboo is prone to springing back, resulting in a short period of plasticity retention; and some technologies use toxic and harmful chemicals, leading to poor environmental performance.

[0009] Therefore, the research and development of a bamboo softener that does not require high temperature and high pressure, has mild processing conditions, integrates bamboo softening, insect prevention, anti-corrosion and anti-mildew, has good compatibility of the agent system, good fixation effect of protective components, and is suitable for a variety of bamboo varieties, as well as its preparation method and application, have important engineering application value. Summary of the Invention

[0010] The purpose of this invention is to provide a bamboo softener with insect-proof, anti-corrosion, and anti-mildew functions, as well as its preparation method and application, thereby solving the technical problems in existing bamboo technology, such as separation of softening and protection processes, easy failure of agents in alkaline environments, easy loss of protective components, harsh treatment conditions, poor softening uniformity, easy rebound after treatment, and poor environmental friendliness of some chemicals.

[0011] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides a bamboo softener that combines insect-repellent, anti-corrosion, and anti-mildew functions. The softener comprises the following components in parts by weight: 40-70 parts of basic carrier components, 15-40 parts of core modified composite additives, and 8-20 parts of functional regulators; Among them, the core modified composite additives include weakly alkaline buffer regulators, lignin-directed pyrolysis aids, cellulose crystallinity regulators, and bio-based polyol plasticizers; The functional regulators include chelated metal ion passivators, natural cross-linking stabilizers of plant flavonoids, micro-molecular penetration enhancers, and bioactive complexes.

[0012] Preferably, the base carrier component is a polar solvent and / or water; The polar solvent is propylene glycol methyl ether or ethanol.

[0013] Preferably, in the core modified composite additive, the weakly basic buffer regulator is one or more of sodium carbonate, sodium bicarbonate, and organic amine buffers; The lignin-directed cleavage aid is a lignin enzymatic hydrolysis aid and / or a phenolic derivative modification aid; Cellulose crystallinity regulators are inorganic acid salts and / or low molecular weight alcohol ether compounds; Bio-based polyol plasticizers are plant-based glycerol and / or polyethylene glycol modified derivatives; The mass ratio of the weak alkaline buffer regulator, lignin-directed pyrolysis aid, cellulose crystallinity regulator and bio-based polyol plasticizer is 15~35:10~30:10~25:20~45.

[0014] Preferably, the functional regulator includes chelating metal ion passivators, natural cross-linking stabilizers of plant flavonoids, micro-molecular penetration enhancers, and bioactive complexes; Among them, the chelating metal ion passivating agent is ethylenediaminetetraacetic acid salt and / or hydroxycarboxylic acid chelating agent; The natural cross-linking stabilizers of plant flavonoids are one or more of ginkgo flavonoids, rutin, and quercetin; Micro-molecular penetration enhancers are nonionic surfactants and / or low-carbon alcohol penetration enhancers; The bioactive compound is two or more of the following: matrine, azadirachtin, tea saponin, borate ester, bamboo vinegar, and chitosan quaternary ammonium salt; The mass ratio of chelated metal ion passivating agent, plant flavonoid natural cross-linking stabilizer, micro-molecule penetration enhancer and bioactive compound is 10~25:10~20:25~40:15~30.

[0015] This invention also provides a method for preparing a bamboo softener that has insect-proof, anti-corrosion, and anti-mildew functions. The preparation method includes the following steps: shearing and maturing the basic carrier component and the core modified composite additive to obtain a mixture, and then mixing the mixture with a functional regulator and allowing it to stand to obtain the bamboo softener.

[0016] Preferably, in the shearing curing process, the temperature is 45~65℃, the time is 15~40min, the pressure is 0.5~1.2MPa, and the shearing rate is 6000~12000rpm; During the mixing process, the temperature is 30~45℃, the time is 10~25min, and the mixing rate is 200~400rpm. During the settling process, the temperature is 20~35℃ and the time is 0.5~2h.

[0017] This invention also provides an application of a bamboo softener with insect-repellent, anti-corrosion, and anti-mildew functions in bamboo treatment, the application comprising the following steps: The pretreated bamboo is immersed in a bamboo softening agent solution, and then shaped and dried sequentially after being removed. The bamboo softener is the bamboo softener according to any one of claims 1 to 4.

[0018] Preferably, the density of the bamboo is 0.7~1.2 g / cm³. 3 The moisture content of the pretreated bamboo is 10-18%. The mass concentration of bamboo softener in the bamboo softener solution is 15-40%.

[0019] Preferably, the impregnation is performed sequentially by vacuum pressure impregnation and room temperature and atmospheric pressure impregnation; In vacuum pressure impregnation, the vacuum degree is -0.09 to -0.05 MPa, and the holding time is 2 to 60 minutes; During immersion at normal temperature and pressure, the immersion temperature is 25~45℃ and the immersion time is 60~150min.

[0020] Preferably, the setting process is carried out in a constant temperature and humidity environment, with a temperature of 35~55℃, a humidity of 55~85%, and a setting time of 12~48h. The moisture content of dried bamboo is 8-12%.

[0021] Compared with the prior art, the present invention has the following beneficial effects: The entire process of this invention is carried out at a temperature not exceeding 65°C, without the need for high-temperature steam above 100°C or high-temperature and high-pressure equipment. It has low energy consumption and low equipment investment, and can be directly modified for production in existing bamboo processing plants. The softening, insect prevention, anti-corrosion, and mildew prevention of bamboo are integrated into the same impregnation process, eliminating the need for a separate protective impregnation process and shortening the production process.

[0022] Excellent softening properties: Through the synergistic regulation of the bamboo cell wall by the core modified composite additives, the elastic modulus of bamboo is reduced by 57-63% after treatment, the bending deflection ratio is 3.1-3.6, and the rebound rate after 30 days is ≤5%, achieving stable permanent plasticization and making it less prone to brittleness and rebound during processing.

[0023] Excellent integrated protective performance: The ternary bioactive compound of matrine-boronic acid ester-chitosan quaternary ammonium salt works synergistically and maintains stable performance in this weakly alkaline system; the protective components enter the core layer of bamboo with the help of penetration enhancers and are fixed to the cell wall through hydrogen bonding, resulting in good anti-leakage performance; it also has good inhibitory / toxic and repellent effects on common bamboo molds (Aspergillus niger, Penicillium), decay fungi (Agromycetes velutina), and bamboo beetle pests.

[0024] Green and environmentally friendly: It eliminates formaldehyde and heavy metal salt protective agents; the core components use plant-derived and bio-based raw materials, the treatment process has no highly corrosive waste liquid, and the bamboo material after treatment has no highly toxic chemical residues, which meets the requirements for the manufacture of green artificial boards and home furnishing products.

[0025] Good process synergy: The entire process of shearing-impregnation-shaping-drying takes into account the protection of the activity of bioactive components; the natural cross-linking stabilizer of plant flavonoids not only improves the plasticizing rebound problem, but also helps to fix bioactive agents; the chelating passivating agent eliminates the catalytic degradation of the agent system by metal ions and improves the storage stability of the softener. Detailed Implementation

[0026] This invention provides a bamboo softener that combines insect-repellent, anti-corrosion, and anti-mildew functions. The softener comprises the following components in parts by weight: 40-70 parts of basic carrier components, 15-40 parts of core modified composite additives, and 8-20 parts of functional regulators; Among them, the core modified composite additives include weakly alkaline buffer regulators, lignin-directed pyrolysis aids, cellulose crystallinity regulators, and bio-based polyol plasticizers; The functional regulators include chelated metal ion passivators, natural cross-linking stabilizers of plant flavonoids, micro-molecular penetration enhancers, and bioactive complexes.

[0027] In this invention, the mass fraction of the basic carrier component is preferably 45-65 parts, more preferably 50-60 parts, and even more preferably 55-58 parts. The basic carrier component serves as a solvent and dispersion medium to ensure uniform mixing of all components. The preferred mass fraction of the core modified composite additive is 18-36 parts, more preferably 20-32 parts, and even more preferably 24-28 parts; The functional regulator is preferably 10-18 parts by mass, more preferably 12-16 parts, and even more preferably 14-15 parts by mass.

[0028] In this invention, the basic carrier component is preferably a polar solvent and / or water; The polar solvent is preferably propylene glycol methyl ether or ethanol.

[0029] In this invention, the weakly alkaline buffer regulator is preferably one or more of sodium carbonate, sodium bicarbonate, and organic amine buffers in the core modified composite additive. The preferred lignin-directed cleavage aid is a lignin enzymatic hydrolysis aid and / or a phenolic derivative modification aid; Cellulose crystallinity regulators are preferably inorganic acid salts and / or low molecular weight alcohol ether compounds; The preferred bio-based polyol plasticizers are plant-based glycerol and / or polyethylene glycol modified derivatives; The preferred mass ratio of the weakly alkaline buffer regulator, lignin-directed pyrolysis aid, cellulose crystallinity regulator, and bio-based polyol plasticizer is 15~35:10~30:10~25:20~45, more preferably 20~30:15~25:15~20:25~40, and even more preferably 25~28:18~20:16~18:30~35.

[0030] In this invention, the lignin-directed pyrolysis aid is preferably polyvinylpyrrolidone or sulfonated lignin, and the phenolic derivative modification aid is preferably lignin catechol, lignin resorcinol or cashew nut shell phenol.

[0031] In this invention, the inorganic acid salt in the cellulose crystallinity regulator is preferably sodium bisulfate or sodium dihydrogen phosphate, and the low molecular weight alcohol ether compound is preferably ethylene glycol methyl ether or diethylene glycol dimethyl ether.

[0032] In this invention, the plant-based glycerin in the bio-based polyol plasticizer is preferably palm oil, soybean oil, coconut oil, rapeseed oil, flaxseed oil or olive oil, and the polyethylene glycol modified derivative is preferably polyethylene glycol 200 or polyethylene glycol 400, etc.

[0033] In this invention, the core modified composite additive is the key to achieving the softening effect. It works synergistically to break the hydrogen bonds and ether bonds in the bamboo cell wall, reducing crystallinity; a weak alkaline buffer regulator maintains the pH stability of the system, preventing strong acids and alkalis from corroding the bamboo; a lignin-directed cleavage aid promotes the loosening of the lignin structure, increasing the porosity of the bamboo; a cellulose crystallinity degradation regulator reduces the crystallinity of cellulose, enhancing plasticity; and a bio-based polyol plasticizer introduces flexible functional groups to achieve permanent plasticization and reduce rebound.

[0034] In this invention, the proportions of each component in the core modified composite additive are preferably dynamically adjusted within the aforementioned proportion range based on parameters such as the age, density, and moisture content of the bamboo to be treated. For bamboo with high age (≥5 years) and high density (≥1.0 g / cm³), within the above-mentioned proportion range of each component, a higher proportion of lignin-directed pyrolysis aid and cellulose crystallinity regulator should be selected to enhance the destruction of the dense structure. For bamboo with low age (≤3 years) and low density (≤0.8g / cm³), a higher proportion of bio-based polyol plasticizer should be selected to enhance the plasticizing effect; For bamboo with high moisture content, a higher proportion of micro-molecular penetration enhancer should be selected to improve the efficiency of solution replacement.

[0035] In this invention, the functional regulator preferably includes chelating metal ion passivators, natural cross-linking stabilizers of plant flavonoids, micro-molecular penetration enhancers, and bioactive complexes; Among them, the preferred chelating metal ion passivating agent is ethylenediaminetetraacetic acid salt and / or hydroxycarboxylic acid chelating agent; The preferred natural cross-linking stabilizer of plant flavonoids is one or more of ginkgo flavonoids, rutin, and quercetin; The preferred micro-molecular penetration enhancer is a nonionic surfactant and / or a low-carbon alcohol-based penetration enhancer; The bioactive compound is two or more of the following: matrine, azadirachtin, tea saponin, borate ester, bamboo vinegar, and chitosan quaternary ammonium salt; The preferred mass ratio of the chelating metal ion passivator, the plant flavonoid natural cross-linking stabilizer, the micro-molecular penetration enhancer, and the bioactive compound is 10~25:10~20:25~40:15~30, more preferably 15~20:12~18:28~36:20~28, and even more preferably 16~18:14~16:30~32:22~26.

[0036] In this invention, the chelating metal ion passivating agent preferably contains ethylenediaminetetraacetic acid salt disodium EDTA and hydroxycarboxylic acid chelating agent preferably sodium citrate or sodium gluconate. In the micro-molecular penetration enhancer, the nonionic surfactant is preferably an alkyl glycoside or a fatty alcohol polyoxyethylene ether, and the low-carbon alcohol penetration enhancer is preferably isopropanol or n-butanol.

[0037] In this invention, the functional regulator further optimizes the performance of the softener: the chelating metal ion passivator prevents metal ions in bamboo from affecting the softening effect and improves stability; the plant flavonoid natural cross-linking stabilizer can cross-link with cell wall components on the one hand, reducing rebound after plasticization, and on the other hand, it can help fix the bioactive composite agent and reduce drug dissolution and loss; the micro-molecule penetration enhancer reduces the surface tension of the drug solution and promotes the bioactive composite agent and softening aid to penetrate into the core layer of bamboo together, so as to achieve simultaneous softening and protection of the inner and outer layers.

[0038] In this invention, when the bioactive compound agent is selected from chitosan quaternary ammonium salt, borate ester, and matrine, its mechanism of action is as follows: Chitosan quaternary ammonium salt has a large number of cationic groups, which can form hydrogen bonds with the hydroxyl groups of cellulose and hemicellulose in bamboo cell walls, making the agent fixed and resistant to loss; it can destroy the permeability of cell membranes of mold and decay fungi, inhibit the growth of spores and hyphae, and has a contact killing and repellent effect on bamboo beetles. It is suitable for the weakly alkaline environment of the system and is not easily hydrolyzed and ineffective. Boric acid esters can inhibit fungal enzyme activity, broadly inhibit decay fungi and molds, and also interfere with insect metabolism to play a role in stomach poisoning and insect repellency. Compared with boric acid, they have better water solubility and good compatibility with the system. With the assistance of penetration enhancers, they can penetrate deep into the core layer of bamboo. Matrine is a plant-derived alkaloid that acts on the nervous system of pests to repel and kill them, and also has a certain ability to inhibit mold growth. It is a green and low-toxicity alkaloid.

[0039] The combination of the three has a synergistic effect: chitosan quaternary ammonium salt disrupts the cell membrane of bacteria, making it easier for borate ester and matrine to enter the cell and exert their effects; chitosan quaternary ammonium salt mainly targets mold prevention, borate ester mainly targets corrosion prevention, and matrine mainly targets insect prevention, working together to achieve integrated protection against insects, corrosion and mold.

[0040] This invention also provides a method for preparing a bamboo softener that has insect-proof, anti-corrosion, and anti-mildew functions. The preparation method includes the following steps: shearing and maturing the basic carrier component and the core modified composite additive to obtain a mixture, and then mixing the mixture with a functional regulator and allowing it to stand to obtain the bamboo softener.

[0041] In this invention, when the basic carrier components are a polar solvent and water, it is preferable to place them in a closed reaction vessel and stir them before use. The mass ratio of the polar solvent to water is preferably 1:3 to 8, more preferably 1:4 to 7, and even more preferably 1:5 to 6; the stirring temperature is preferably 25 to 45°C, more preferably 30 to 40°C, and even more preferably 32 to 38°C; the stirring time is preferably 10 to 30 min, more preferably 15 to 28 min, and even more preferably 20 to 25 min; the stirring speed is preferably 150 to 300 rpm, more preferably 200 to 250 rpm, and even more preferably 220 to 240 rpm.

[0042] In this invention, when the core modified composite additive is added, the preferred order of addition is to add a weak alkaline buffer regulator, a lignin-directed pyrolysis aid, a cellulose crystallinity regulator, and a bio-based polyol plasticizer in sequence; the preferred addition interval is 5-15 min, more preferably 6-12 min, and even more preferably 8-10 min.

[0043] In this invention, when the functional regulator is added, the preferred order of addition is to add the chelated metal ion passivator, the plant flavonoid natural cross-linking stabilizer, the micro-molecular penetration enhancer, and the bioactive compound in sequence.

[0044] In this invention, an appropriate amount of polar solvent helps to improve the solubility and permeability of each additive, but an excessively high proportion will increase costs and may affect the stability of the softener.

[0045] In this invention, during the shearing and curing process, the temperature is preferably 45-65℃, more preferably 50-60℃, and even more preferably 54-58℃; the time is preferably 15-40 min, more preferably 20-35 min, and even more preferably 25-30 min; the pressure is preferably 0.5-1.2 MPa, more preferably 0.6-1 MPa, and even more preferably 0.8-0.9 MPa; and the shearing rate is preferably 6000-12000 rpm, more preferably 7000-11000 rpm, and even more preferably 8000-10000 rpm. In the mixing process, the temperature is preferably 30~45℃, more preferably 32~40℃, and even more preferably 35~38℃; the time is preferably 10~25min, more preferably 14~22min, and even more preferably 18~20min; and the mixing rate is preferably 200~400rpm, more preferably 250~350rpm, and even more preferably 300~320rpm. During the settling process, the temperature is preferably 20~35℃, more preferably 24~32℃, and even more preferably 26~30℃, and the time is preferably 0.5~2h, and even more preferably 1~1.5h.

[0046] In this invention, the shearing curing is preferably a three-stage shearing curing, comprising a first stage, a second stage, and a third stage; The preferred rotational speed for the first stage is 6000-8000 rpm, more preferably 6500-7500 rpm, and even more preferably 7000-7200 rpm; the preferred shearing time is 5-10 min, more preferably 6-9 min, and even more preferably 7-8 min. The rotational speed in the second stage is preferably 8000~10000rpm, more preferably 8500~9500rpm, and even more preferably 8800~9000rpm. The shearing time is preferably 5~15min, more preferably 7~14min, and even more preferably 10~12min. The rotational speed in the third stage is preferably 10,000 to 12,000 rpm, more preferably 10,500 to 11,500 rpm, and even more preferably 11,000 to 11,200 rpm. The shearing time is preferably 5 to 15 minutes, more preferably 6 to 12 minutes, and even more preferably 8 to 10 minutes.

[0047] In this invention, the heating rate of the shearing curing is preferably 0.5~2℃ / min, more preferably 1~1.5℃ / min, and even more preferably 1.2~1.4℃ / min.

[0048] In the shearing and ripening process described in this invention, a sealed environment is maintained inside the reactor and a condensation reflux device is provided.

[0049] This invention also provides an application of a bamboo softener with insect-repellent, anti-corrosion, and anti-mildew functions in bamboo treatment, the application comprising the following steps: The pretreated bamboo is immersed in a bamboo softening agent solution, and then shaped and dried sequentially after being removed. The bamboo softener is the bamboo softener described above.

[0050] In this invention, the density of the bamboo is preferably 0.7~1.2 g / cm³. 3 Further preferred values ​​are 0.8~1.1 g / cm³. 3 More preferably 0.9~1g / cm 3 The moisture content of the pretreated bamboo is preferably 10-18%, more preferably 12-16%, and even more preferably 14-15%. In the bamboo softener solution, the mass concentration of the bamboo softener is preferably 15-40%, more preferably 20-35%, and even more preferably 25-30%.

[0051] In this invention, the bamboo material is preferably moso bamboo, nan bamboo, etc.

[0052] In this invention, the impregnation is preferably performed sequentially by vacuum pressure impregnation and room temperature and pressure impregnation; In the vacuum pressure impregnation, the vacuum degree is preferably -0.09 to -0.05 MPa, more preferably -0.08 to -0.06 MPa, and even more preferably -0.075 to -0.07 MPa. The pressure holding time is preferably 20 to 60 min, more preferably 30 to 50 min, and even more preferably 35 to 45 min. In the ambient temperature and pressure immersion, the immersion temperature is preferably 25~45℃, more preferably 30~45℃, and even more preferably 35~40℃, and the immersion time is preferably 60~150min, more preferably 80~140min, and even more preferably 100~120min.

[0053] In this invention, the setting process is carried out in a constant temperature and humidity environment. The temperature is preferably 35~55℃, more preferably 40~50℃, and even more preferably 42~48℃. The humidity is preferably 55~85%, more preferably 60~80%, and even more preferably 70~75%. The setting time is preferably 12~48h, more preferably 24~42h, and even more preferably 32~36h. The moisture content of the dried bamboo is preferably 8-12%, more preferably 9-11%, and even more preferably 10-10.5%.

[0054] In this invention, the drying process is preferably natural air drying or low-temperature drying.

[0055] The technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0056] In the embodiments and comparative examples of this invention, the number of parts refers to parts by mass.

[0057] Example 1

[0058] Components and dosage of bamboo softener: The basic carrier component consists of 60 parts: 8 parts anhydrous ethanol and 52 parts water; 25 parts of core modified composite additives: 8 parts of sodium carbonate (weak alkaline buffer regulator), 6 parts of polyvinylpyrrolidone 8000 (lignin directional pyrolysis aid), 4 parts of ethylene glycol methyl ether (cellulose crystallinity regulator), and 7 parts of coconut oil (bio-based polyol plasticizer). Functional regulator 12 parts: EDTA disodium (chelating metal ion passivator) 3 parts, Ginkgo flavonoids (natural cross-linking stabilizer of plant flavonoids) 2 parts, alkyl glycoside C8-10 (micro-molecule penetration enhancer) 4 parts, bioactive compound (matrine, borate ester and chitosan quaternary ammonium salt in a mass ratio of 2:6:9) 3 parts; Preparation of bamboo softening agent: Anhydrous ethanol and water were mixed and placed in a sealed reaction vessel. The temperature was raised to 35°C, the stirring rate was controlled at 220 rpm, and the stirring time was 20 min to obtain the basic carrier mixture. Sodium carbonate, polyvinylpyrrolidone 8000, ethylene glycol methyl ether, and coconut oil were added sequentially to the base carrier mixture. The addition intervals for each component were 10 min. The mixture was stirred until completely dissolved, and the temperature was increased to 60°C at a rate of 1°C / min. A homogenizer was then started to perform three-stage shearing and maturation: the first stage was shearing at 7000 rpm for 8 min, the second stage was shearing at 9000 rpm for 10 min, and the third stage was shearing at 11000 rpm for 10 min. The homogenization pressure was 1 MPa. During the shearing process, a closed environment was maintained in the reactor and a reflux condenser was set up to obtain the core modified composite mother liquor. Cool the core modified composite mother liquor to 38℃, add EDTA disodium, ginkgo flavonoids, alkyl glycoside C8-10 and bioactive composite agent in sequence, continue stirring for 18 minutes at a stirring speed of 300 rpm, then cool to 30℃ and let stand for 1.5 hours to obtain bamboo softener. Application of bamboo softener: The target material has a density of 0.86 g / cm³. 3 Four-year-old moso bamboo; The bamboo was cut into boards 2m long, 0.2m wide, and 0.05m thick. The green and yellow parts of the bamboo were removed, and the bamboo was dried to a moisture content of 14% to obtain pre-treated bamboo. The pretreated bamboo was placed in a bamboo softener diluted to a mass concentration of 30%, and treated by vacuum pressure impregnation method. The vacuum degree was -0.07MPa, the pressure holding time was 40min, and after depressurization, it was continued to be impregnated at normal pressure for 110min. The impregnation temperature was controlled at 35℃. The bamboo was then removed to obtain the impregnated bamboo. After soaking, place the bamboo in a constant temperature and humidity environment, with the temperature controlled at 45℃ and the relative humidity at 72%, and let it stand for 32 hours. Then, take out the shaped bamboo and let it air dry naturally until the moisture content is 10%, which completes the softening treatment.

[0059] Example 2

[0060] Components and dosage of bamboo softener: The basic carrier component consists of 62 parts: 6 parts propylene glycol methyl ether and 56 parts water. 26 parts of core modified composite additives: 8 parts of sodium bicarbonate (weak alkaline buffer regulator), 7 parts of cashew nut shell phenol (lignin directional pyrolysis aid), 4 parts of sodium dihydrogen phosphate (cellulose crystallinity regulator), and 7 parts of polyethylene glycol 400 (bio-based polyol plasticizer). Functional regulator 14 parts: sodium citrate (chelating metal ion passivator) 3 parts, rutin (natural cross-linking stabilizer of plant flavonoids) 2.5 parts, isopropanol (micro-molecular penetration enhancer) 5 parts, bioactive compound (matrine, borate ester and chitosan quaternary ammonium salt in a mass ratio of 2:7:10) 3.5 parts; Preparation of bamboo softening agent: Propylene glycol methyl ether was mixed with water and placed in a sealed reaction vessel. The temperature was raised to 32°C, the stirring rate was controlled at 180 rpm, and the stirring time was 18 min to obtain the basic carrier mixture. Sodium bicarbonate, cashew nut shell powder, sodium dihydrogen phosphate, and polyethylene glycol 400 were added sequentially to the base carrier mixture at 9-minute intervals. The mixture was stirred until completely dissolved and heated to 55°C at a rate of 0.8°C / min. A homogenizer was then started for three-stage shearing and ripening: the first stage was shearing at 6500 rpm for 6 minutes, the second stage was shearing at 8500 rpm for 12 minutes, and the third stage was shearing at 10500 rpm for 8 minutes. The homogenization pressure was 0.8 MPa. During the shearing process, a sealed environment was maintained inside the reactor and a reflux condenser was installed to obtain the core modified composite mother liquor. Cool the core modified composite mother liquor to 36℃, add sodium citrate, rutin, isopropanol and bioactive composite agent in sequence, continue stirring for 16 minutes at a stirring rate of 280 rpm, then cool to 25℃ and let stand for 1 hour to obtain bamboo softener.

[0061] Application of bamboo softener: The target material has a density of 1.05 g / cm³. 3 8-year-old moso bamboo: The bamboo was cut into boards 1.5m long, 0.15m wide, and 0.04m thick. Surface impurities were removed, and the boards were dried to a moisture content of 13% to obtain pretreated bamboo. The pretreated bamboo was placed in a bamboo softener diluted to a mass concentration of 25%, and treated by vacuum pressure impregnation method. The vacuum degree was -0.08MPa, the pressure holding time was 45min, and after depressurization, it was continued to be impregnated at normal pressure for 120min. The impregnation temperature was controlled at 30℃. The bamboo was then removed to obtain the impregnated bamboo. After soaking, place the bamboo in a constant temperature and humidity environment, with the temperature controlled at 40℃ and the relative humidity at 65%, and let it stand for 40 hours. Then, take out the shaped bamboo and let it air dry naturally until the moisture content is 9.5%, which completes the softening treatment.

[0062] Example 3

[0063] Components and dosage of bamboo softener: Basic carrier components: 58 parts; water 58 parts; The core modified composite additives consist of 28 parts: triethanolamine (weakly alkaline buffer regulator) 9 parts, sulfonated lignin (lignin directional pyrolysis aid) 7 parts, diethylene glycol dimethyl ether (cellulose crystallinity regulator) 5 parts, and polyethylene glycol 200 (bio-based polyol plasticizer) 7 parts. Functional regulator 16 parts: sodium gluconate (chelating metal ion passivator) 3 parts, quercetin (natural cross-linking stabilizer of plant flavonoids) 3 parts, fatty alcohol polyoxyethylene ether (micro-molecular penetration enhancer) 6 parts, bioactive compound (matrine, borate ester and chitosan quaternary ammonium salt in a mass ratio of 1:5:8) 4 parts.

[0064] Preparation of bamboo softening agent: Triethanolamine, sulfonated lignin, diethylene glycol dimethyl ether, and polyethylene glycol 200 were added to water sequentially, with each component added at 12-minute intervals. The mixture was stirred until completely dissolved, and the temperature was increased to 65°C at a rate of 1.5°C / min. A homogenizer was then started for three-stage shearing and ripening: the first stage was shearing at 7500 rpm for 10 minutes, the second stage was shearing at 9500 rpm for 15 minutes, and the third stage was shearing at 11500 rpm for 12 minutes. The homogenization pressure was 1.1 MPa. During the shearing process, a sealed environment was maintained inside the reactor, and a reflux condenser was installed to obtain the core modified composite mother liquor. Cool the core modified composite mother liquor to 42°C, then add sodium gluconate, quercetin, fatty alcohol polyoxyethylene ether and bioactive composite agent in sequence, continue stirring for 20 minutes at a stirring rate of 350 rpm, then cool to 28°C and let stand for 2 hours to obtain bamboo softener.

[0065] Application of bamboo softener: The application is for bamboo-based composite material substrates (bamboo shavings); Bamboo is crushed into 30-mesh particles, impurities are removed, and dried to a moisture content of 15% to obtain pre-treated bamboo. The pretreated bamboo was placed in a bamboo softener diluted to a mass concentration of 35%, and treated by vacuum pressure impregnation method. The vacuum degree was -0.06MPa, the pressure holding time was 30min, and after depressurization, it was continued to be impregnated at normal pressure for 80min. The impregnation temperature was controlled at 40℃. The bamboo was then removed to obtain the impregnated bamboo. The soaked bamboo granules are placed in a constant temperature and humidity environment, with the temperature controlled at 50℃ and the relative humidity at 80%, and left to stand for 30 hours. After that, the shaped bamboo granules are taken out and dried at low temperature (45℃) until the moisture content is 10.5%, which completes the softening treatment.

[0066] Comparative Example 1

[0067] The addition of "polyvinylpyrrolidone 8000" in Example 1 is omitted, and the other steps are the same as in Example 1.

[0068] Comparative Example 2

[0069] The "impregnated bamboo" in Example 1 was directly air-dried until the moisture content was 10%, and the other steps were the same as in Example 1.

[0070] Comparative Example 3

[0071] Replace "three-stage shearing and curing" in Example 1 with "shearing and curing at 10,000 rpm for 30 minutes", and the other steps are the same as in Example 1.

[0072] Comparative Example 4

[0073] The addition of the "bioactive compound" in Example 1 is omitted, and the other steps are the same as in Example 1.

[0074] Comparative Example 5

[0075] Replace “3 parts of bioactive compound (mass ratio of matrine, borate ester and chitosan quaternary ammonium salt of 2:6:9)” in Example 1 with “3 parts of matrine”, and the other steps are the same as in Example 1.

[0076] The bamboo materials obtained in Examples 1-2 and Comparative Examples 1-5 were subjected to the following performance tests, and the results are shown in Table 1.

[0077] Modulus of elasticity: Referring to the national standard GB / T 15780-1995 "Test Methods for Physical and Mechanical Properties of Bamboo", the reduction rate of modulus of elasticity = (before MOE treatment - after MOE treatment) / before MOE treatment × 100%.

[0078] Plastic deformation ratio: Sample preparation: Untreated bamboo and softened bamboo were processed into test strips with dimensions of 160mm × 10mm × t (t is the natural thickness of the bamboo wall), with no less than 6 samples in each group. Ensure that the sample surface is flat and free of defects visible to the naked eye.

[0079] A universal testing machine (accuracy not less than 1%) was used, equipped with a three-point bending support. The support span was 120 mm, and the loading head and support radius were 5 mm. The test was conducted in an environment with a temperature of 20℃ and a relative humidity of 65%. The specimen was placed symmetrically on the support, and a uniform loading speed of 5 mm / min was applied until the specimen showed obvious yielding or the deflection reached 20% of the span (i.e., 24 mm). The load-deflection curve was recorded, and the maximum load and the corresponding bending deflection, or the deflection value under the specified load, were read.

[0080] Plastic deformation ratio = maximum deflection of softened bamboo / maximum deflection of untreated bamboo.

[0081] Resilience determination: Mark the measurement area on the softened and shaped bamboo strip sample and measure its initial chordal bending radius of curvature R0. Place the sample in a constant temperature and humidity chamber (temperature 25℃, relative humidity 60%) and after 30 days, measure the radius of curvature R1 at the same location again; Rebound rate = (1-R0 / R1)×100%, the test is repeated 5 times and the average value is taken.

[0082] Anti-mold performance: Refer to GB / T 18261-2013 "Test methods for the efficacy of anti-mold agents against wood mold and discoloration fungi", test for Aspergillus niger and Penicillium, and count the anti-mold level (0 is the best and 4 is the worst).

[0083] Corrosion resistance: Refer to GB / T 13942.1-2009 "Durability of wood - Part 1: Laboratory test methods for natural decay resistance", use the *Acer truncatum* decay test to determine the mass loss rate.

[0084] Insect resistance performance: Referencing LY / T 3211-2020 "Insect-resistant treatment and evaluation method for bamboo", a contact feeding test was conducted on bamboo borers, and the corrected mortality rate of the test insects was determined after 7 days.

[0085] Anti-leaking of chemicals: The loss rate of bioactive components was determined according to GB / T 27651-2011 Anti-leaking test of wood preservatives.

[0086] Table 1. Mechanical property test results of bamboo obtained in Examples 1-2 and Comparative Examples 1-5

[0087] As shown in Table 1, in Examples 1 and 2, the reduction rate of elastic modulus reached 58% and 62%, respectively, the bending deflection ratios were 3.2 and 3.5, respectively, and the 30-day rebound rates were only 3.2% and 2.8%. This indicates that under the formulation and process of the present invention, the rigidity of bamboo is significantly reduced, the bending deformation capacity is greatly improved, and the rebound rate is controlled at a low level, thus achieving stable permanent plasticization of bamboo.

[0088] Comparative Example 1 lacked a lignin-directed cleavage aid, resulting in ineffective loosening of the bamboo lignin network, severely insufficient softening, poor plasticity, and significant rebound. Comparative Example 2, while containing a complete softening agent composition, lacked a setting process, preventing the rearrangement and fixation of the bamboo's internal molecular chains, leading to poor plasticization and significant rebound in the later stages. This confirms that constant temperature and humidity setting is a key process for suppressing rebound and achieving permanent plasticization. Comparative Example 3, by replacing the three-stage shearing curing with a single-stage high-speed shearing, showed significantly worse performance compared to the examples, demonstrating that the three-stage gradient shearing curing ensures sufficient dispersion and compounding of the additives. The insufficient mixing uniformity of the single-stage shearing weakened the system's regulatory effect on the bamboo cell walls, reducing the softening effect. Comparative Examples 4 and 5, by deleting or altering the bioactive composite agent, showed similar reduction rates in elastic modulus, bending deflection ratio, and rebound rate as Example 1. This indicates that the bioactive composite agent primarily functions as an insect repellent, anti-corrosion, and anti-mildew agent, with almost no impact on the softening, plasticizing, and mechanical properties of the bamboo.

[0089] Therefore, lignin-directed pyrolysis aids, three-stage shearing and curing processes, and constant temperature and humidity shaping are key to ensuring the excellent softening and plasticizing properties of bamboo.

[0090] Table 2. Results of efficacy and performance tests of bamboo obtained in Examples 1-2 and Comparative Examples 1-5

[0091] As shown in Table 2, Examples 1 and 2, using a ternary bioactive compound of matrine-boron ester-chitosan quaternary ammonium salt, achieved a mildew resistance level of 0, with a corrosion loss rate of only 4.2% and 3.7%, respectively. The 7-day corrected mortality rate of bamboo borers reached 94.2% and 95.7%, respectively, while the loss rate of bioactive components was as low as 7.3% and 6.8%. This indicates that the ternary compound system works synergistically, providing excellent comprehensive protection against mildew, corrosion, and insects in bamboo. Combined with the entire process, the protective agent can be firmly adhered to the interior of the bamboo, exhibiting excellent resistance to loss.

[0092] Comparative Example 1 lacked a lignin-directed cleavage aid, but the protective components remained intact. It achieved a mildew resistance rating of 0 and good anti-corrosion and insect-repellent effects, but the loss rate of bioactive components increased to 18.2%. This was because lignin cleavage was insufficient, the internal pores of the bamboo were underdeveloped, the penetration depth of the agent into the cell wall was limited, and more agent remained on the surface, making it easier to lose under washing conditions.

[0093] Comparative Example 2, by omitting the constant temperature and humidity setting process, resulted in a decrease in the anti-mildew level to Grade 1, a slight reduction in anti-corrosion and anti-insect effects, and a chemical leaching rate of 13.4%. In addition to achieving plasticization and setting, constant temperature and humidity setting also promotes hydrogen bonding between bioactive components and bamboo cell walls; omitting this step weakens the chemical fixation effect and deteriorates the protective effect and anti-leaching performance.

[0094] Comparative Example 3 employed single-stage shear curing, ensuring the integrity of the protective components. It achieved a mildew resistance rating of 0 and satisfactory anti-corrosion and insect-proof properties, but the agent loss rate was 16.2%. Single-stage shearing resulted in uneven dispersion of functional components, with some bioactive compounds failing to form a stable composite system with other adjuvants, leading to decreased penetration and fixation effects and increased loss.

[0095] Comparative Example 4 completely removed the bioactive compound agent, had no protective agent present, and had the worst anti-mold level of 4. The decay quality loss rate was as high as 32.6%, while the bamboo borer mortality rate was only 6.1%, indicating that it did not have the ability to prevent insects, decay, or mold.

[0096] Comparative Example 5, using only matrine as the protective component, resulted in a mold prevention level dropping to Grade 2, a 16.3% loss rate in preservative quality, a corrected mortality rate of only 58.7% for bamboo borers, and a pesticide runoff rate as high as 24.5%. This demonstrates that relying solely on a single plant-derived matrine cannot achieve a comprehensive protection against insects, decay, and mold. The pesticide's fixation ability is also poor, proving that the combination of the three components has a significant synergistic effect and cannot be simply replaced by a single component.

[0097] It is evident that the bioactive composite agent described in this invention is the core of achieving integrated protection; the lignin-directed pyrolysis, three-stage shear curing, and constant temperature and humidity setting process can improve the penetration and fixation effect of the agent, reduce agent loss, and further ensure long-term protective performance.

[0098] The softening effect of the bamboo obtained in Example 3 was evaluated for its mechanical properties. Referring to the method for determining static bending strength (flexural strength) in the national standard GB / T 17657-2022 "Test Methods for Physical and Chemical Properties of Wood-based Panels and Decorative Wood-based Panels", bamboo-based composite materials were prepared by hot pressing softened bamboo shavings and untreated bamboo shavings according to the same process, and their static bending strength was determined on a universal testing machine.

[0099] The flexural strength of the composite material prepared from untreated bamboo shavings was measured to be 32.5 MPa, while that prepared from softened bamboo shavings was 41.6 MPa, representing an increase of 28%. The calculations are as follows: The flexural strength improvement rate = (41.6-32.5) / 32.5 × 100% = 28%. Meanwhile, the board's anti-mildew rating is 0, the decay quality loss is 4.8%, and the corrected mortality rate of bamboo beetles is 92.8%, indicating that the softening treatment of this invention can significantly improve the interfacial bonding performance between bamboo shavings and the resin matrix, and enhance the mechanical properties of the composite material.

[0100] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A bamboo softener with insect-repellent, anti-corrosion, and anti-mildew functions, characterized in that, The softener comprises the following components in parts by weight: 40-70 parts of basic carrier components, 15-40 parts of core modified composite additives, and 8-20 parts of functional regulators; Among them, the core modified composite additives include weakly alkaline buffer regulators, lignin-directed pyrolysis aids, cellulose crystallinity regulators, and bio-based polyol plasticizers; The functional regulators include chelated metal ion passivators, natural cross-linking stabilizers of plant flavonoids, micro-molecular penetration enhancers, and bioactive complexes.

2. The bamboo softener with insect-repellent, anti-corrosion, and anti-mildew functions according to claim 1, characterized in that, The basic carrier components are polar solvents and / or water; The polar solvent is propylene glycol methyl ether or ethanol.

3. The bamboo softener with insect-repellent, anti-corrosion, and anti-mildew functions according to claim 1, characterized in that, In the core modified composite additive, the weakly basic buffer regulator is one or more of sodium carbonate, sodium bicarbonate, and organic amine buffers. The lignin-directed cleavage aid is a lignin enzymatic hydrolysis aid and / or a phenolic derivative modification aid; Cellulose crystallinity regulators are inorganic acid salts and / or low molecular weight alcohol ether compounds; Bio-based polyol plasticizers are plant-based glycerol and / or polyethylene glycol modified derivatives; The mass ratio of the weak alkaline buffer regulator, lignin-directed pyrolysis aid, cellulose crystallinity regulator and bio-based polyol plasticizer is 15~35:10~30:10~25:20~45.

4. The bamboo softener with insect-repellent, anti-corrosion, and anti-mildew functions according to claim 1, characterized in that, The functional regulators include chelated metal ion passivators, natural cross-linking stabilizers of plant flavonoids, micro-molecular penetration enhancers, and bioactive complexes. Among them, the chelating metal ion passivating agent is ethylenediaminetetraacetic acid salt and / or hydroxycarboxylic acid chelating agent; The natural cross-linking stabilizers of plant flavonoids are one or more of ginkgo flavonoids, rutin, and quercetin; Micro-molecular penetration enhancers are nonionic surfactants and / or low-carbon alcohol penetration enhancers; The bioactive compound is two or more of the following: matrine, azadirachtin, tea saponin, borate ester, bamboo vinegar, and chitosan quaternary ammonium salt; The mass ratio of chelated metal ion passivating agent, plant flavonoid natural cross-linking stabilizer, micro-molecule penetration enhancer and bioactive compound is 10~25:10~20:25~40:15~30.

5. A method for preparing a bamboo softener with insect-repellent, anti-corrosion, and anti-mildew functions as described in any one of claims 1 to 4, characterized in that, The preparation method includes the following steps: shearing and maturing the basic carrier component and the core modified composite additive to obtain a mixture, and then mixing the mixture with the functional regulator and letting it stand to obtain the bamboo softener.

6. The method for preparing a bamboo softener with insect-repellent, anti-corrosion, and anti-mildew functions according to claim 5, characterized in that, During the shearing and curing process, the temperature is 45~65℃, the time is 15~40min, the pressure is 0.5~1.2MPa, and the shearing rate is 6000~12000rpm. During the mixing process, the temperature is 30~45℃, the time is 10~25min, and the mixing rate is 200~400rpm. During the settling process, the temperature is 20~35℃ and the time is 0.5~2h.

7. The application of the bamboo softener with insect-repellent, anti-corrosion, and anti-mildew functions as described in any one of claims 1 to 4 in bamboo treatment, characterized in that, The application includes the following steps: The pretreated bamboo is immersed in a bamboo softening agent solution, and then shaped and dried sequentially after being removed. The bamboo softener is the bamboo softener according to any one of claims 1 to 4.

8. The application of the bamboo softener with insect-repellent, anti-corrosion, and anti-mildew functions according to claim 7 in bamboo treatment, characterized in that, The density of the bamboo is 0.7~1.2 g / cm³. 3 The moisture content of the pretreated bamboo is 10-18%. The mass concentration of bamboo softener in the bamboo softener solution is 15-40%.

9. The application of a bamboo softener with insect-repellent, anti-corrosion, and anti-mildew functions as described in claim 7 or 8 in bamboo treatment, characterized in that, The impregnation process involves sequentially performing vacuum pressure impregnation and room temperature and pressure impregnation. In vacuum pressure impregnation, the vacuum degree is -0.09 to -0.05 MPa, and the holding time is 2 to 60 minutes; During immersion at normal temperature and pressure, the immersion temperature is 25~45℃ and the immersion time is 60~150min.

10. The application of the bamboo softener with insect-repellent, anti-corrosion, and anti-mildew functions according to claim 9 in bamboo treatment, characterized in that, The curing process is carried out in a constant temperature and humidity environment, with a temperature of 35~55℃, a humidity of 55~85%, and a curing time of 12~48h. The moisture content of dried bamboo is 8-12%.