A flow guide device for ceramic substrate stack decontamination and a decontamination method thereof

By embedding ultrathin boron nitride flow guide plates between ceramic substrate stacks to construct a micro-flow guide network, the problems of low glue removal efficiency and high defect rate of multilayer ceramic substrates are solved, realizing the production of ceramic substrates with high efficiency glue removal and high yield.

CN123129305APending Publication Date: 2026-11-20YANGZHOU XIAOTIAN PHOTOSKOT TECHNOLOGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611310837.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing ceramic substrate stacking and descaling processes are inefficient, have long gas diffusion paths, and high defect rates when stacking multiple layers. Furthermore, existing improvement methods are difficult to effectively improve descaling efficiency without increasing stacking thickness and stress risk.

Method used

An ultra-thin boron nitride guide plate is used, with micro-protrusions distributed on the surface of the guide plate to form a guide channel, which is embedded between the ceramic green ceramic sheet layers to construct a micro-guide network and quickly discharge the decomposition gas of organic binder.

Benefits of technology

It significantly shortens the descaling time, improves descaling efficiency, breaks through the limitation of stacked layers, reduces the defect rate, and maintains the performance of the ceramic substrate.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The application discloses a flow guide device for ceramic substrate stack layer degassing and a degassing method thereof, and belongs to the technical field of electronic ceramic material manufacturing. The flow guide device comprises at least one boron nitride flow guide plate, the thickness of the flow guide plate is 0.05mm-0.3mm, and a plurality of micro protrusions are distributed on at least one main surface of the flow guide plate, the height of the micro protrusions is 10um-150um, and the distribution density is 300 / cm 2 ~1000 / cm 2 . The degassing method comprises the following steps: preparing 20 or more ceramic green ceramic chips and stacking, embedding 1-3 flow guide plates between layers, degassing heat treatment, and rapidly discharging gas through the flow guide channel formed by the micro protrusions. According to the application, the micro protrusion structure is arranged on the ultra-thin boron nitride plate, a flow guide network is constructed between layers, the degassing efficiency is greatly improved, the degassing time is shortened to 6h-15h, 20-30 layers of stacking are supported, the yield can reach more than 99%, and the boron nitride is chemically inert and does not pollute the ceramic matrix.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electronic ceramic material manufacturing technology, and in particular relates to a flow guiding fixture and its adhesive removal method for ceramic substrate stacking and removal. Background Technology

[0002] In the manufacturing process of ceramic substrates (such as aluminum nitride ceramic substrates, silicon nitride ceramic substrates, alumina ceramic substrates, etc.), it is necessary to stack cast ceramic sheets containing a large amount of organic binder, and then perform debinding treatment before high-temperature sintering to remove the organic binder from the green body. However, with the increasing requirements for heat dissipation performance and mechanical strength of electronic ceramic devices, the number of stacked layers of ceramic substrates continues to increase. When the number of stacked layers reaches 10 or more, the traditional debinding process faces severe challenges: First, the debinding efficiency is extremely low. In multi-layer stacking, the internal air passages between layers are easily blocked, the gas diffusion path increases, and the debinding time needs to be significantly increased, usually as long as 48 to 96 hours, resulting in huge energy consumption. Second, the product defect rate is high. Gas retention at the interlayer interface leads to defects such as bubbling and delamination, and uneven debinding leads to uneven overall shrinkage and warping. The scrap rate increases exponentially with the number of layers. Third, there are limited improvement methods. Existing methods for optimizing adhesive removal curves or reducing the number of adhesive removal layers will significantly reduce production efficiency and even reduce the mechanical and thermal properties of ceramic substrates.

[0003] To address the aforementioned technical problems, those skilled in the art have proposed various solutions. For example, patent CN120841967A discloses a method for debinding silicon nitride ceramic green bodies in stacks. The core of this method lies in using a porous boron nitride ceramic plate as an isolation material between silicon nitride green bodies in the stack, thereby improving debinding efficiency. Furthermore, existing technologies also disclose methods such as applying boron nitride powder as an isolation layer to the surface of the ceramic green body, creating crisscrossing grooves and holes on the substrate surface to form gas channels, and pressing and placing perforated boron nitride ceramic blocks onto the stacked green bodies. However, these solutions still have shortcomings: porous ceramic plates rely on the material's own pores for permeability, resulting in limited exhaust channels and difficulty in meeting the debinding requirements of ultra-multi-layer stacks; the groove / hole scheme involves macroscopic trench structures, occupying a large space and increasing stack thickness and stress risk; and the powder application process is complex and easily contaminates the green body.

[0004] Therefore, there is an urgent need to design a new tooling or glue removal method that can significantly improve glue removal efficiency and the number of glue stacking layers without changing the ceramic formula, so as to achieve the effect of cost reduction and efficiency improvement. Summary of the Invention

[0005] This invention provides a flow guiding fixture and a descaling method for ceramic substrate stacking, aiming to solve the technical problems in existing descaling processes caused by increased stacking layers, such as obstructed airflow, excessively long descaling time, high rates of interlayer bubbling and warping defects, and limited existing improvement methods. In particular, this invention addresses the challenge of balancing efficient airflow channels with minimal stacking (20 layers or more) without significantly increasing stacking thickness and stress risk, thereby achieving a substantial improvement in descaling efficiency and a significant breakthrough in stacking layer count without altering the ceramic formulation.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A flow guiding fixture for adhesive removal in ceramic substrate stacking includes at least one flow guiding plate made of boron nitride (BN) with a single-layer thickness of 0.05 mm to 0.3 mm. At least one main surface of the flow guiding plate has multiple micro-protrusions distributed thereon, the height of which is 10 μm to 150 μm, and the distribution density is 300 protrusions / cm². 2 ~1000 pieces / cm 2 The micro-protrusions form a flow channel between the guide plate and the adjacent green ceramic sheet, allowing the gas generated during the glue removal process to be discharged along the flow channel.

[0007] Furthermore, the number of guide plates is 1 to 3, preferably 2. When there is 1 guide plate, it is disposed in the middle region of the stacked green ceramic sheets along the stacking direction; when there are 2 guide plates, they are disposed at the upper third interface and the lower third interface of the stacked green ceramic sheets along the stacking direction, respectively; when there are 3 guide plates, they are evenly distributed along the stacking direction.

[0008] Furthermore, the micro-protrusions can be distributed on both main surfaces of the guide plate. The shape of the micro-protrusions can be hemispherical, cylindrical, or pyramidal.

[0009] The present invention also provides a method for removing adhesive from a ceramic substrate, comprising the following steps: S1. Prepare more than 20 layers of raw ceramic sheets by stacking the raw ceramic sheets; S2. Embed 1 to 3 of the above-mentioned flow guide plates between the stacked ceramic green ceramic sheets; S3. Perform a heat treatment to remove adhesive from the stacked body after embedding the guide plate; S4. The gas generated during the glue discharge process is quickly discharged through the guide channel formed by the micro-protrusions on the surface of the guide plate.

[0010] Furthermore, the ceramic green ceramic sheet is made of any one of aluminum nitride ceramic, silicon nitride ceramic, or alumina ceramic, and the thickness of a single layer is 0.05mm to 0.2mm.

[0011] Furthermore, the glue removal heat treatment is carried out in an air atmosphere, and the glue removal time is 6h~15h.

[0012] This invention utilizes an ultrathin boron nitride (BN) guide plate with micro-protrusions embedded between stacked green ceramic sheets. These micro-protrusions create microscopic gaps between the guide plate and adjacent green ceramic sheets, which are interconnected to form a dense flow-guiding network. During adhesive removal, gases generated from the decomposition of the organic binder rapidly diffuse and escape horizontally along this flow-guiding network, preventing gas stagnation due to excessively long vertical permeation paths. Simultaneously, the boron nitride material is chemically inert, does not react with the ceramic matrix, and does not introduce contamination. The ultrathin design (0.05~0.3mm) makes the influence of the guide plate on the total stack thickness negligible, without increasing the risk of additional thermal stress.

[0013] Compared with the prior art, the present invention has the following significant advantages: 1. The glue removal rate is doubled, significantly shortening the process cycle. This invention significantly improves the gas diffusion path within a multilayer stack by constructing a microscopic flow-guiding network between layers, drastically reducing the glue removal time from 48-96 hours in traditional processes to 6-15 hours, and increasing glue removal efficiency by more than 50%. Specifically, data from the examples show that the glue removal time is 8 hours when using two 0.25mm BN boards; only 6 hours when using two 0.05mm BN boards; while the comparative example without BN boards under the same conditions has a glue removal time as long as 48 hours.

[0014] 2. Breaking through the limitation of stacking layer number, supporting the fabrication of ultra-multilayer materials. This invention effectively increases the number of layers in a ceramic substrate stack from less than 10 layers in traditional processes to 20-30 layers, achieving a significant breakthrough in layer count. In Examples 1-5, both the 20-layer and 25-layer stacks successfully completed adhesive removal, yielding defect-free products.

[0015] 3. Product yield has been significantly improved, and defect rate has been significantly reduced. This invention effectively avoids gas stagnation at interlayer interfaces and eliminates defects such as bubbling and delamination through rapid venting via the flow channel. Simultaneously, the uniform adhesive removal process ensures consistent shrinkage across layers, preventing warping and deformation. Data from the embodiments show that the stacks manufactured using the fixtures and methods of this invention achieve a yield rate of over 99% (99% yield rates for Examples 1, 3, and 4, and no defects in Example 5), while the comparative examples without BN boards have a yield rate of 0%, exhibiting severe bubbling defects.

[0016] 4. Does not contaminate the ceramic matrix and maintains material properties. Boron nitride has excellent chemical inertness. It does not react with ceramic materials such as aluminum nitride, silicon nitride, and alumina at the debinding temperature, does not introduce impurity elements, and does not affect key performance indicators such as dielectric properties, thermal conductivity, and mechanical strength of ceramic substrates.

[0017] In summary, this invention, through simple structural and process improvements, solves the long-standing technical problems of low glue removal efficiency and high defect rate in ultra-multilayer stacking, demonstrating significant technological advancement and industrial application value. Detailed Implementation

[0018] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0019] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be readily apparent to those skilled in the art. This specification and embodiments are merely exemplary.

[0020] The present invention will be further described in detail below with reference to specific embodiments, but the implementation of the present invention is not limited thereto.

[0021] In this invention, the raw ceramic sheets can be prepared using conventional casting methods in the art. Specifically, ceramic powder, organic binder, plasticizer, dispersant, and solvent are mixed in proportion and ball-milled to form a casting slurry, which is then cast, dried, and a raw ceramic sheet of a specified thickness is obtained.

[0022] The preparation method of the deflector is as follows: S1. Boron nitride cast sheets are prepared by casting method. The binder and plasticizer are added to the solvent and stirred evenly. Then, boron nitride powder is added and stirred evenly to form a cast material. After casting, drying at room temperature and demolding, a boron nitride cast sheet of the required thickness is obtained. S2. Micro-protrusion structures are formed on the surface of boron nitride cast sheets by imprinting or molding processes; S3. The formed green body is degreased. The heating rate during degreasing is 2~3℃ / min, the temperature is raised to 600~700℃, and the temperature is held for 0.5~1h to obtain a boron nitride guide plate with micro-protrusions on the surface.

[0023] In the following embodiments, unless otherwise specified, alumina green ceramic sheets with a single layer thickness of 0.1 mm are used, and the debinding atmosphere is air. The debinding heat treatment is performed using a debinding furnace conventional in the art.

[0024] Example 1 This embodiment provides a flow guiding fixture and a flow guiding method for removing adhesive from ceramic substrate stacks. The flow guiding fixture includes two BN plates, and the specific process is as follows: Preparation of S1.BN board: A boron nitride (BN) film with a thickness of 0.25 mm was prepared by casting. Hemispherical micro-protrusions were formed on the two main surfaces of the BN board by imprinting process. The height of the micro-protrusions was 100 μm and the distribution density was 500 protrusions / cm². 2 .

[0025] S2. Debonding method: Prepare 20 layers of alumina green ceramic sheets and stack them; embed one of the above-mentioned BN plates between the 7th and 8th layers and between the 14th and 15th layers of the stack; place the stack with embedded BN plates into a debonding furnace and perform debonding heat treatment in an air atmosphere for 8 hours.

[0026] S3. Exhaust principle: During the adhesive exhaust process, the gas generated by the decomposition of organic adhesive is rapidly discharged along the horizontal direction between the layers through the flow channels formed between the micro-protrusions on the surface of the BN board and the adjacent green ceramic tiles.

[0027] S4. Inspection Results: After the glue removal process, the resulting products underwent visual inspection and cross-sectional microscopic observation. The results showed that the products were free of defects such as bubbling, delamination, and warping, with a yield rate of 99%.

[0028] Example 2 This embodiment provides a flow guiding fixture and a flow guiding method for removing adhesive from ceramic substrate stacks. The flow guiding fixture includes a BN plate, and the specific process is as follows: Preparation of S1.BN board: A 0.3 mm thick boron nitride cast sheet was prepared using a casting method. Cylindrical micro-protrusions were then formed on the two main surfaces of the BN board using an imprinting process. The micro-protrusions had a height of 150 μm and a distribution density of 400 protrusions / cm². 2 .

[0029] S2. Debonding method: Prepare 20 layers of alumina green ceramic sheets and stack them; embed one of the above-mentioned BN plates between the 10th and 11th layers of the stack (at the middle interface); place the stack with the embedded BN plate into a debonding furnace and perform debonding heat treatment in an air atmosphere for 12 hours.

[0030] S3. Exhaust principle: During the adhesive exhaust process, the gas is discharged horizontally along the interlayer through the flow channel formed between the micro-protrusions on the surface of the BN board and the adjacent green ceramic tiles.

[0031] S4. Inspection Results: After the glue removal process, the resulting product underwent an appearance inspection. The results showed that the product as a whole had no defects such as bubbling or delamination, but there were slight defects caused by uneven shrinkage in the edge areas.

[0032] Example 3 This embodiment provides a flow guiding fixture and a flow guiding method for removing adhesive from ceramic substrate stacks. The flow guiding fixture includes three BN plates, and the specific process is as follows: Preparation of S1.BN board: A 0.2 mm thick boron nitride cast sheet was prepared by casting. Pyramidal micro-protrusions were then formed on the two main surfaces of the BN board using an imprinting process. The height of the micro-protrusions was 80 μm, and the distribution density was 800 protrusions / cm². 2 .

[0033] S2. Debonding method: Prepare 25 layers of alumina green ceramic sheets and stack them; embed one of the above-mentioned BN plates between the 8th and 9th layers, between the 16th and 17th layers and between the 24th and 25th layers of the stack; place the stack with embedded BN plates into a debonding furnace and perform debonding heat treatment in an air atmosphere for 10 hours.

[0034] S3. Exhaust principle: During the adhesive exhaust process, the gas is discharged horizontally along the interlayer through the flow channel formed between the micro-protrusions on the surface of the BN board and the adjacent green ceramic tiles.

[0035] S4. Inspection Results: After the glue removal process, the resulting products underwent visual inspection and cross-sectional microscopic observation. The results showed that the products were free of defects such as bubbling, delamination, and warping, with a yield rate of 99%.

[0036] Example 4 This embodiment provides a flow guiding fixture and a flow guiding method for removing adhesive from ceramic substrate stacks. The flow guiding fixture includes two BN plates, and the specific process is as follows: Preparation of S1.BN board: A 0.1 mm thick boron nitride cast sheet was prepared by casting. Hemispherical micro-protrusions were formed on the two main surfaces of the BN board by imprinting process. The height of the micro-protrusions was 50 μm and the distribution density was 600 protrusions / cm². 2 .

[0037] S2. Debonding method: Prepare 20 layers of alumina green ceramic sheets and stack them; embed one of the above-mentioned BN plates between the 10th and 11th layers and between the 20th and 21st layers of the stack; place the stack with embedded BN plates into a debonding furnace and perform debonding heat treatment in an air atmosphere for 15 hours.

[0038] S3. Exhaust principle: During the adhesive exhaust process, the gas is discharged horizontally along the interlayer through the flow channel formed between the micro-protrusions on the surface of the BN board and the adjacent green ceramic tiles.

[0039] S4. Inspection Results: After the glue removal process, the resulting products underwent visual inspection and cross-sectional microscopic observation. The results showed that the products were free of defects such as bubbling, delamination, and warping, with a yield rate of 99%.

[0040] Example 5 This embodiment provides a flow guiding fixture and a flow guiding method for removing adhesive from ceramic substrate stacks. The flow guiding fixture includes two BN plates, and the specific process is as follows: Preparation of S1.BN board: A boron nitride (BN) film with a thickness of 0.05 mm was prepared by casting. Cylindrical micro-protrusions were formed on the two main surfaces of the BN board by imprinting. The height of the micro-protrusions was 20 μm, and the distribution density was 1000 protrusions / cm². 2 .

[0041] S2. Debonding method: Prepare 20 layers of alumina green ceramic sheets and stack them; embed one of the above-mentioned BN plates between the 5th and 6th layers and between the 15th and 16th layers of the stack; place the stack with embedded BN plates into a debonding furnace and perform debonding heat treatment in an air atmosphere for 6 hours.

[0042] S3. Exhaust principle: During the adhesive exhaust process, the gas is discharged horizontally along the interlayer through the flow channel formed between the micro-protrusions on the surface of the BN board and the adjacent green ceramic tiles.

[0043] S4. Inspection Results: After the glue removal process, the resulting product underwent visual inspection and cross-sectional microscopic observation. The results showed that the product had no defects such as bubbling, delamination, or warping.

[0044] Comparative Example 1 This comparative example provides a traditional method for removing adhesive from a ceramic substrate, without using the flow guiding fixture of this invention. The specific process is as follows: S1. Debinding method: Prepare 20 layers of alumina green ceramic sheets and stack them without embedding any guide plates in the stack; place the stack directly into the debinding furnace and perform debinding heat treatment in an air atmosphere.

[0045] S2. Inspection Results: After the glue removal process, the resulting product underwent visual inspection and cross-sectional microscopic observation. The results showed that the product exhibited severe bubbling defects, with obvious traces of gas retention at the interlayer interfaces, resulting in a product yield of 0%.

[0046] Comparative Example 2 This comparative example is used to verify the necessity and contribution of the "micro-protrusion" structure to the glue removal effect.

[0047] S1. Preparation of BN plate: A boron nitride casting sheet with a thickness of 0.25 mm was prepared by casting method. The BN plate has a smooth surface and no micro-protrusion structure. The thickness and material of the BN plate are the same as in Example 1.

[0048] S2. Debinding method: Prepare 20 layers of alumina green ceramic sheets and stack them; embed one of the above-mentioned smooth BN plates between the 7th and 8th layers and between the 14th and 15th layers of the stack; place the stack with embedded BN plates into a debinding furnace and perform debinding heat treatment in an air atmosphere.

[0049] S3. Test Results: During the glue removal process, due to the tight adhesion between the smooth BN board and the adjacent green ceramic tiles, there was a lack of effective gas escape channels, and the gas could not be discharged smoothly. The glue removal time needs to be extended to more than 36 hours. Local bubbling defects appeared in the product, and the yield rate was 60%.

[0050] This comparative example directly demonstrates that BN boards without micro-protrusion structures cannot effectively construct flow channels, and their glue removal effect is far inferior to that of this invention.

[0051] Comparative Example 3 This comparative example is used to verify the criticality of the micro-protrusion height parameter in the range of 10μm to 150μm.

[0052] Preparation of S1.BN plate: A boron nitride cast sheet with a thickness of 0.25 mm was prepared by casting. Hemispherical micro-protrusions were formed on the two main surfaces of the BN plate by imprinting process. The height of the micro-protrusions was 200 μm (exceeding the upper limit of 150 μm in this invention), and the distribution density was 500 protrusions / cm². 2 .

[0053] S2. Debonding method: Prepare 20 layers of alumina green ceramic sheets and stack them; embed one of the above-mentioned BN plates between the 7th and 8th layers and between the 14th and 15th layers of the stack; place the stack with embedded BN plates into a debonding furnace and perform debonding heat treatment in an air atmosphere.

[0054] S3. Test Results: The adhesive removal time needs to be extended to 20 hours. Due to the excessive height of the micro-protrusions, localized stress concentration occurred under the stacking pressure of adjacent green ceramic tiles, resulting in green ceramic tile indentations or micro-cracks in some areas, reducing the product yield to 70%.

[0055] This comparative example demonstrates that the height of the micro-protrusion is not necessarily better the larger it is—exceeding the upper limit of this invention can lead to new defects due to stress concentration.

[0056] Comparative Example 4 This comparative example is used to compare and verify the microprotrusion distribution density parameter of 300 protrusions / cm. 2 ~1000 pieces / cm 2 The criticality.

[0057] Preparation of S1.BN board: A boron nitride (BN) film with a thickness of 0.25 mm was prepared by casting. Hemispherical micro-protrusions were formed on the two main surfaces of the BN board by imprinting process. The height of the micro-protrusions was 100 μm and the distribution density was 100 protrusions / cm². 2.

[0058] S2. Debonding method: Prepare 20 layers of alumina green ceramic sheets and stack them; embed one of the above-mentioned BN plates between the 7th and 8th layers and between the 14th and 15th layers of the stack; place the stack with embedded BN plates into a debonding furnace and perform debonding heat treatment in an air atmosphere.

[0059] S3. Test Results: Due to the low density of the protrusions and sparse flow channels, a continuous gas discharge network cannot be formed. The degreasing time needs to be extended to more than 30 hours. Localized bubbling occurred in the product, resulting in a yield rate of 50%.

[0060] This comparative example demonstrates that when the micro-protrusion density is lower than the range of this invention, the guiding network becomes discontinuous, and the glue removal effect is significantly deteriorated.

[0061] The embodiments described above are merely preferred embodiments of the present invention, but the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combining various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A flow guiding fixture for adhesive removal in ceramic substrate stacking, characterized in that, include: At least one flow deflector, wherein the flow deflector is made of boron nitride and the thickness of a single layer is 0.05mm~0.3mm; The guide plate has multiple micro-protrusions distributed on at least one main surface, the height of which is 10μm~150μm and the distribution density is 300 per cm. 2 ~1000 pieces / cm 2 ; The micro-protrusions form a flow channel between the guide plate and the adjacent green ceramic sheet, allowing the gas generated during the adhesive discharge process to be discharged along the flow channel.

2. The flow guiding fixture for ceramic substrate stacking and adhesive removal according to claim 1, characterized in that, The number of the deflector plates is 1 to 3.

3. The flow guiding fixture for ceramic substrate stacking and adhesive removal according to claim 1, characterized in that, The micro-protrusions are distributed on both main surfaces of the guide plate.

4. The flow guiding fixture for ceramic substrate stacking and adhesive removal according to claim 1 or 3, characterized in that, The micro-protrusions are hemispherical, cylindrical, or pyramidal in shape.

5. The flow guiding fixture for ceramic substrate stacking and adhesive removal according to claim 2, characterized in that, When the number of the guide plates is one, the guide plate is disposed in the middle area along the stacking direction of the stacked ceramic green ceramic sheets.

6. The flow guiding fixture for ceramic substrate stacking and adhesive removal according to claim 2, characterized in that, When there are two guide plates, the two guide plates are respectively disposed at the upper third interface and the lower third interface along the stacking direction of the stacked ceramic green ceramic sheets.

7. The flow guiding fixture for ceramic substrate stacking and adhesive removal according to claim 2, characterized in that, When the number of the guide plates is 3, the 3 guide plates are evenly distributed along the stacking direction.

8. A method for removing adhesive from a ceramic substrate, characterized in that, Includes the following steps: S1. Prepare more than 20 layers of raw ceramic sheets by stacking the raw ceramic sheets; S2. Embedding a flow guide plate as described in any one of claims 1 to 7 between the layers of stacked green ceramic sheets; S3. Perform a heat treatment to remove adhesive from the stacked body after embedding the guide plate; S4. The gas generated during the glue discharge process is discharged through the guide channel formed by the micro-protrusions on the surface of the guide plate.

9. The glue removal method according to claim 8, characterized in that, The material of the ceramic green ceramic sheet is selected from any one of aluminum nitride ceramic, silicon nitride ceramic or alumina ceramic, and the single layer thickness of the ceramic green ceramic sheet is 0.05mm~0.2mm.

10. The glue removal method according to claim 8, characterized in that, The heat treatment time for debinding is 6h~15h.

Citation Information

Patent Citations

  • Lamination glue discharging method of silicon nitride ceramic green body, preparation method of pre-sintered body, substrate and preparation method of substrate

    CN120841967A