Reinforced toughened polyphenylene sulfide composite material and preparation method thereof

By solid-phase treatment of polyphenylene sulfide resin particles and blending technology using a twin-screw extruder, a covalent bond layer is formed, which solves the multiphase interface problem of polyphenylene sulfide composites under high shear flow fields, improves the material's impact strength and flexible stress, and ensures structural stability under alternating loads.

CN123129341APending Publication Date: 2026-11-20DONGGUAN JINQING NEW MATERIAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611252580.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-18
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies for preparing polyphenylene sulfide composites struggle to achieve in-situ covalent bonding between reactive elastomers and inorganic fibers under high shear flow fields. This results in a lack of chemical bond network connections at the multiphase interface, leading to localized defect fractures and failing to meet the requirements for impact toughness and low dynamic deformation.

Method used

By heat-treating polyphenylene sulfide resin particles in a solid state, bound water is removed and thiol groups and amino groups are oriented to form pretreated particles. These particles are then melt-blended with an elastomer dispersion phase and surface-modified graded inorganic fillers in a twin-screw extruder. The shear rate and temperature are controlled to form a covalent bond layer. Finally, the particles are rapidly cooled through a slit extrusion die to form a micro-phase separation structure.

Benefits of technology

In-situ weaving of covalent bonded layers in polyphenylene sulfide composites was achieved under high shear flow field, which improved the material's impact resistance and flexible stress self-relaxation characteristics, ensuring the structural fatigue resistance reliability under alternating load conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123129341A_ABST
    Figure CN123129341A_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of high-performance engineering plastic modification processing, and discloses a reinforced and toughened polyphenylene sulfide composite material and a preparation method thereof, which comprises the following steps: heat treating polyphenylene sulfide resin particles in a solid phase state to reduce volatile components; conveying the obtained pretreated particles to a double-screw extruder to melt and introduce an elastomer dispersion phase to generate an interfacial grafting reaction to build a covalent bond layer; introducing surface modified graded inorganic fillers including nanoparticles and fiber phases into the covalent bond layer during the formation process of the covalent bond layer; adjusting a process temperature and controlling a local shear rate; forming a micro-phase separation structure melt; extruding the melt through a slit extrusion die; and introducing cooling water to rapidly cool the melt. The present application controls the step time sequence dislocation to convert a multi-phase interface into a stress dissipation barrier with dynamic relaxation characteristics, thereby improving the impact toughness and dimensional stability of the modified composite material and synergistically enhancing the fatigue life under alternating loads.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a reinforced and toughened polyphenylene sulfide composite material and its preparation method, belonging to the field of high-performance engineering plastic modification and processing technology. Background Technology

[0002] Currently, polyphenylene sulfide (PPS) possesses an alternating structure of rigid benzene rings and sulfur atoms. In the field of alternating stress component manufacturing, it leverages its advantages as a thermoplastic engineering plastic, exhibiting superior heat resistance, chemical resistance, and high mechanical strength. However, in the operating environment of components subjected to alternating stress, modified materials need to simultaneously meet the requirements of impact toughness and low dynamic deformation characteristics. Conventional methods involve melt blending exogenous inorganic fibers with elastomers. PPS, with its rapid nucleation rate and low melt viscosity, causes large-scale aggregation of the exogenous dispersed phase in the low-shear phase region. Furthermore, the lack of chemically bonded network connections at the multiphase interface leads to significant deformation under cyclic dynamic loads. The resulting mutual displacement and movement eventually lead to the accumulation of local defects and fracture in the multiphase interface region. To alleviate the stress concentration at the interface, the conventional linear approach is to increase the proportion of reactive modifiers or continuously increase the amount of inorganic fiber filling. However, after the mass fraction of the modifier crosses the critical point, it induces non-uniform self-aggregation of the elastomer in the shear field, resulting in the mutual deterioration of flexural modulus and softening temperature. At the same time, excessive fiber filling hinders the relaxation of continuous phase chain segments, causing local gelation of the matrix and deteriorating the mixing rheological properties. This indicates that there is a deep interactive constraint between the thermodynamic energy barrier of molecular end groups, the covalent bond weaving density of the multiphase interface, and the spatial segmentation and cutting sequence of material flow.

[0003] When addressing the aforementioned multiphase constraints, there are also shortcomings in the control aspects such as system reaction control methods and matrix modification mechanisms. For example, Chinese invention patent application CN103804910A discloses a glass fiber and SiO2 reinforced and toughened polyphenylene sulfide material and its preparation method. It uses suspension grafting and silane crosslinking technology to pre-swell polyphenylene sulfide in solution and perform long-term chemical modification. This pre-modification relies entirely on the static chemical bond construction under ideal conditions. Under the continuous high-throughput melt extrusion industrial conditions, it cannot cope with the fluctuation of free sulfur impurities in raw material batches and the dynamic shear heat generated by long-term equipment operation. This leads to the local thermal degradation and chain segment breakage of the pre-grafted macromolecular chains under the strong shear heat history of the extrusion flow field. It is difficult to dynamically lock the non-equilibrium morphology of the multiphase interface during the mixing transient process, causing the condensed state orientation of the material's crystalline region to run out of control, and failing to guarantee the structural fatigue resistance reliability under continuous alternating load conditions.

[0004] Therefore, how to regulate the spatial arrangement activity of the end-group functional groups in the amorphous region on the surface of resin particles, and achieve in-situ seamless weaving of the reactive elastomer into the covalent bonded layer and the graded reinforcing filler in the spatiotemporal evolution of the high shear flow field, thereby rigidly converging the average crystallinity of the matrix within a specific non-equilibrium phase range to synergistically improve the impact resistance and flexible stress self-relaxation characteristics, has become the technical problem to be solved by this invention. Summary of the Invention

[0005] To address the problems in the background art, the technical solution of the present invention is as follows: A method for preparing reinforced and toughened polyphenylene sulfide composite materials, comprising the following steps:

[0006] Step S1: Heat-treat polyphenylene sulfide resin particles in a solid state to remove bound water and reduce the mass fraction of volatiles, and induce the oriented arrangement of thiol groups and amino groups at the ends of polyphenylene sulfide resin particles to obtain pretreated polyphenylene sulfide resin particles.

[0007] Step S2: The pretreated polyphenylene sulfide resin particles are conveyed to the melt blending section of the twin-screw extruder. The process temperature is controlled to be in the molten state of polyphenylene sulfide. The preheated elastomer dispersion phase is introduced through the first side feed port. The screw speed of the twin-screw extruder is controlled to make the pretreated polyphenylene sulfide resin particles and the elastomer dispersion phase melt blend and undergo interfacial grafting reaction, forming a covalent bond layer at the interface of the two phases to obtain a blended melt.

[0008] Step S3: Surface-modified graded inorganic filler, including nanoparticles and fibrous phase, is introduced into the blended melt through the secondary side feed port. The process temperature is adjusted and the local shear rate is controlled to be 600 s⁻¹ to 700 s⁻¹, so that the nanoparticles are dispersed and enriched between the covalent bonded layer and the fibrous phase, forming a melt with a micro-phase separation structure.

[0009] Step S4: The micro-phase separated melt is conveyed through a slit extrusion die, and the molecular chains are oriented and arranged at a slit shear rate of 600 s⁻¹ to 800 s⁻¹. When the melt exits the slit extrusion die, cooling water with a process temperature of 15°C to 25°C and a flow rate of 1.2 m / s to 1.8 m / s is introduced to quench the melt, and the crystallinity of the polyphenylene sulfide matrix in the resulting pellet product is controlled to be 32% to 36%.

[0010] Preferably, based on the total weight of the reinforced and toughened polyphenylene sulfide composite material as 100%, the mass percentage of the elastomer dispersed phase is 5% to 20%, the mass percentage of the surface-modified graded inorganic filler is 15% to 40%, and the balance is polyphenylene sulfide resin particles; in step S1, the heat treatment process temperature is 80°C to 140°C, the time is 2h to 6h, the volatile matter mass fraction of the polyphenylene sulfide resin particles is controlled to be less than 0.02%, and step S1 is completed in a high-speed fluidized mixer with a rotation speed of 1200rpm to 1800rpm.

[0011] Preferably, step S2 includes the following sub-steps: Step S21, melting the pretreated polyphenylene sulfide resin particles in the melt blending section of a twin-screw extruder, controlling the process temperature of the melt blending section to be 285°C to 310°C; Step S22, quantitatively introducing the elastomer dispersion phase preheated to 60°C to 90°C through the first side feed port of the twin-screw extruder, controlling the screw speed of the twin-screw extruder in the melt blending section to be 150 rpm to 350 rpm, so that the elastomer dispersion phase reacts with the pretreated polyphenylene sulfide resin particles.

[0012] Preferably, the elastomer dispersion phase is a maleic anhydride-grafted ethylene-octene copolymer, and the maleic anhydride grafting rate of the maleic anhydride-grafted ethylene-octene copolymer is 0.5% to 1.5%.

[0013] Preferably, the nanoparticles in the surface-modified graded inorganic filler are nano-silica, and the average particle size of the nanoparticles is 20nm to 80nm; the fibrous phase in the surface-modified graded inorganic filler is alkali-free glass fiber, and the average fiber diameter of the alkali-free glass fiber is 10μm to 15μm.

[0014] Preferably, the surface-modified graded inorganic filler is coated with an epoxy silane coupling agent layer; the epoxy silane coupling agent layer is formed by the dehydration condensation of the epoxy silane coupling agent and the hydroxyl groups on the surface of the surface-modified graded inorganic filler.

[0015] Preferably, in step S3, the process temperature in the downstream area of ​​the secondary side feed port is controlled to be 270°C to 280°C.

[0016] Preferably, in step S4, the slit width of the slit extrusion die is 1.0 mm to 2.5 mm.

[0017] Preferably, in step S4, the spray direction of the cooling water is perpendicular to the flow direction of the melt extruded from the slit extrusion die.

[0018] Preferably, a reinforced and toughened polyphenylene sulfide composite material is prepared by the method.

[0019] Compared with the prior art, the beneficial effects of the present invention are:

[0020] 1. In the preparation of reinforced and toughened polyphenylene sulfide composite materials, mechanical friction and impact within a high-speed fluidized mixer, under a specific combination of temperature and rotation speed, excites the amorphous macromolecular segments on the surface of solid-state polyphenylene sulfide resin particles. This removes adsorbed bound water and reduces the mass fraction of volatiles. Under the constrained state of solid-phase microcrystals, it induces the residual thiol groups and amino groups at the ends of the macromolecules to undergo a restricted reaction orientation and construct a highly active end-group layer. This pretreatment process controls the surface state of the resin particles, enabling the melt to exhibit unique end-group deprotonation dissociation potential. This provides the necessary prerequisite for subsequent in-situ copolymerization with the elastomer dispersion phase in the reaction core region without interference from graded fillers, and for weaving in a covalent bonded layer.

[0021] 2. Within the core reaction zone, the process temperature is controlled to overcome the deprotonation energy barrier of the macromolecular terminal thiol. A preheated elastomer dispersion phase is quantitatively introduced through the first side feed port, and the arrangement shear rate is maintained. This allows the active energy layer and the elastomer side chains to undergo a highly efficient condensation reaction in a pure fluid environment free from the interference of graded fillers. The thermodynamic mass transfer rate and spatial orientation of the two phases are controlled by the temperature field step transition, thereby weaving a dense covalent bond layer in situ at the interface between the two phases and transforming it into a bonding interface network with stress dissipation characteristics.

[0022] 3. Just before the bonding density of the bridging layer crosses the critical gel point, a surface-modified graded inorganic reinforcing filler phase is introduced through a secondary side feed port. The process temperature is controlled to be instantly reduced and the local shear rate is increased. The viscosity increase induced by the reduction of the matrix melt temperature, combined with the physical superposition of the strong shear force field, drives the nanoparticles in the graded system to be precisely enriched and embedded in the transition grid between the bridging layer and the fiber phase. Through the cross-temporal synergy of physical stress field anchoring and in-situ chemical bonding, the arrangement morphology of the interface nanophase region is locked in a non-equilibrium, incomplete phase separation state. Attached Figure Description

[0023] Figure 1 This is a flowchart illustrating the preparation steps of a reinforced and toughened polyphenylene sulfide composite material according to the present invention.

[0024] Figure 2 This is a diagram showing the products at each stage of the reinforced and toughened polyphenylene sulfide composite material of the present invention.

[0025] The objectives, features, and advantages of this invention will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation

[0026] The technical solutions of the embodiments of this application will be clearly described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of this application are within the scope of protection of this application.

[0027] A method for preparing a reinforced and toughened polyphenylene sulfide composite material includes the following steps:

[0028] Step S1: Heat-treat polyphenylene sulfide resin particles in a solid state to remove bound water and reduce the mass fraction of volatiles, and induce the oriented arrangement of thiol groups and amino groups at the ends of polyphenylene sulfide resin particles to obtain pretreated polyphenylene sulfide resin particles.

[0029] Step S2: The pretreated polyphenylene sulfide resin particles are conveyed to the melt blending section of the twin-screw extruder. The process temperature is controlled to be in the molten state of polyphenylene sulfide. The preheated elastomer dispersion phase is introduced through the first side feed port. The screw speed of the twin-screw extruder is controlled to make the pretreated polyphenylene sulfide resin particles and the elastomer dispersion phase melt blend and undergo interfacial grafting reaction, forming a covalent bond layer at the interface of the two phases to obtain a blended melt.

[0030] Step S3: Surface-modified graded inorganic filler, including nanoparticles and fibrous phase, is introduced into the blended melt through the secondary side feed port. The process temperature is adjusted and the local shear rate is controlled to be 600 s⁻¹ to 700 s⁻¹, so that the nanoparticles are dispersed and enriched between the covalent bonded layer and the fibrous phase, forming a melt with a micro-phase separation structure.

[0031] Step S4: The micro-phase separated melt is conveyed through a slit extrusion die, and the molecular chains are oriented and arranged at a slit shear rate of 600 s⁻¹ to 800 s⁻¹. When the melt exits the slit extrusion die, cooling water with a process temperature of 15°C to 25°C and a flow rate of 1.2 m / s to 1.8 m / s is introduced to quench the melt, and the crystallinity of the polyphenylene sulfide matrix in the resulting pellet product is controlled to be 32% to 36%.

[0032] Preferably, based on the total weight of the reinforced and toughened polyphenylene sulfide composite material as 100%, the mass percentage of the elastomer dispersed phase is 5% to 20%, the mass percentage of the surface-modified graded inorganic filler is 15% to 40%, and the balance is polyphenylene sulfide resin particles; in step S1, the heat treatment process temperature is 80°C to 140°C, the time is 2h to 6h, the volatile matter mass fraction of the polyphenylene sulfide resin particles is controlled to be less than 0.02%, and step S1 is completed in a high-speed fluidized mixer with a rotation speed of 1200rpm to 1800rpm.

[0033] Preferably, step S2 includes the following sub-steps: Step S21, melting the pretreated polyphenylene sulfide resin particles in the melt blending section of a twin-screw extruder, controlling the process temperature of the melt blending section to be 285°C to 310°C; Step S22, quantitatively introducing the elastomer dispersion phase preheated to 60°C to 90°C through the first side feed port of the twin-screw extruder, controlling the screw speed of the twin-screw extruder in the melt blending section to be 150 rpm to 350 rpm, so that the elastomer dispersion phase reacts with the pretreated polyphenylene sulfide resin particles.

[0034] Preferably, the elastomer dispersion phase is a maleic anhydride-grafted ethylene-octene copolymer, and the maleic anhydride grafting rate of the maleic anhydride-grafted ethylene-octene copolymer is 0.5% to 1.5%.

[0035] Preferably, the nanoparticles in the surface-modified graded inorganic filler are nano-silica, and the average particle size of the nanoparticles is 20nm to 80nm; the fibrous phase in the surface-modified graded inorganic filler is alkali-free glass fiber, and the average fiber diameter of the alkali-free glass fiber is 10μm to 15μm.

[0036] Preferably, the surface-modified graded inorganic filler is coated with an epoxy silane coupling agent layer; the epoxy silane coupling agent layer is formed by the dehydration condensation of the epoxy silane coupling agent and the hydroxyl groups on the surface of the surface-modified graded inorganic filler.

[0037] Preferably, in step S3, the process temperature in the downstream area of ​​the secondary side feed port is controlled to be 270°C to 280°C.

[0038] Preferably, in step S4, the slit width of the slit extrusion die is 1.0 mm to 2.5 mm.

[0039] Preferably, in step S4, the spray direction of the cooling water is perpendicular to the flow direction of the melt extruded from the slit extrusion die.

[0040] Preferably, a reinforced and toughened polyphenylene sulfide composite material is prepared by the method.

[0041] Example 1: The current transmission gear operates in a continuous alternating stress field and is subjected to high-frequency alternating loads and high-temperature, high-pressure conditions. The reinforced and toughened polyphenylene sulfide (PPS) composite material used in manufacturing the transmission gear has a rapid crystallization rate due to the rigid benzene ring and sulfur atom alternating symmetrical structure of the PPS matrix macromolecule chain. This results in high intrinsic brittleness and low impact strength. When exogenous reinforcing inorganic fibers and elastomer dispersed phases are blended, the lack of strong covalent bonding at the multiphase interface leads to the aggregation of the exogenous dispersed phase in the low-shear phase region. Under periodic dynamic loads, the multiphase interface undergoes mutual misalignment and displacement, resulting in the accumulation of local defects and stress concentration at the multiphase interface, causing fatigue creep and early sudden brittle fracture of the transmission gear. Adding 55 parts by weight of PPS resin particles to a rotation speed of 1200 rpm to 1800 rpm... In a high-speed fluidized bed mixer, the heat treatment process temperature is controlled at 80℃ to 140℃, and the heat treatment time is 2h to 6h. The mechanical friction and impact within the high-speed fluidized bed mixer removes the bound water on the surface of the solid polyphenylene sulfide resin particles, and the volatile matter mass fraction of the polyphenylene sulfide resin particles is controlled to be below 0.02%. This induces the directional alignment of the thiol groups and amino groups at the ends of the polyphenylene sulfide resin particles to obtain pretreated polyphenylene sulfide resin particles. Although the heat treatment process temperature is lower than the melting point of polyphenylene sulfide, it is within or above its glass transition temperature range of 85℃. Furthermore, under the high-speed operation of the high-speed fluidized bed mixer at 1200rpm to 1800rpm, high-frequency and intense mechanical friction and impact occur between the particles and between the particles and the barrel wall, resulting in localized micro-regional heat concentration and shear stress field in the amorphous region on the surface of the solid particles.

[0042] This high-energy mechanical force excites the amorphous macromolecular chain segments on the surface of solid particles, freeing them from their original frozen state and giving them local micro-motion capabilities. Due to the removal of moisture, the functional groups that were originally locked by hydrogen bonds are dissociated. Under the directional shear stress induced by the high-speed fluidized centrifugal flow field, the remaining thiol and amino groups at the ends of the macromolecules undergo microscopic displacement along the free volume voids in the amorphous region of the particle surface and align towards the outer spatial orientation. This constructs a highly chemically active end-group enrichment layer on the surface of the solid particles, providing microscopic kinetic preparation for the subsequent deprotonation, rapid dissociation, and reactive in-situ copolymerization in the melting section. The pretreated polyphenylene sulfide resin particles are then continuously conveyed to the melt blending section of a co-rotating twin-screw extruder. The process temperature of the melt blending section is controlled at 285℃ to 310℃. 15 parts by mass of a preheated elastomer dispersion phase at 60℃ to 90℃ is metered into the feed port on the first side of the co-rotating twin-screw extruder. The elastomer dispersion phase is a maleic anhydride-grafted ethylene-octene copolymer with a maleic anhydride grafting rate of 0.5% to 1.5%. The screw speed of the co-rotating twin-screw extruder in the melt blending section is controlled at 150 rpm to 350 rpm, so that the pretreated polyphenylene sulfide resin particles and the elastomer dispersion phase are melt blended and undergo an interfacial grafting reaction. Under the deprotonated and deionized state of the polyphenylene sulfide resin particles, the remaining thiol groups and amino groups undergo in-situ copolymerization with the maleic anhydride-grafted ethylene-octene copolymer.

[0043] A dense covalent bond layer is woven in situ at the interface between the two phases to control the volumetric flow rate of the elastomer dispersion phase, ensuring stable material transport and in-situ chain extension reaction. The mass flow rate of polyphenylene sulfide resin at the main feed port Satisfy the formula ,in, This represents the volumetric flow rate of the dispersed phase in the elastomer. The intrinsic density of the elastomer dispersion at 80°C ranges from 0.86 g / cm³ to 0.89 g / cm³. The mass flow rate of polyphenylene sulfide resin at the main feed inlet. The weighting factor for covalent bond saturation at the phase interface is 0.16. The intrinsic mass fraction of free sulfur impurities in the polyphenylene sulfide (PPS) raw material batch is taken as 0.002. Since the feed volumetric flow rate is limited by this formula, large-scale aggregation of the elastomer dispersion phase in the low-shear region is avoided, which would lead to a deterioration in the overall rheological properties of the composition and the formation of a covalent bond layer. The determination of the phase interface covalent bond saturation weighting factor is based on the following boundary limit experiment: Under a specific material ratio, by changing the quantitative addition rate of the elastomer dispersion phase, the change curves of the reaction saturation of the covalent bond layer at the phase interface and the final matrix flexural modulus are measured. The experimental results show that when the weighting factor is below 0.10, the number of maleic anhydride groups in the system is insufficient, making it impossible to construct a continuous cross-linked network at the two-phase interface, resulting in a notched impact strength of a simply supported beam below 10 kJ / m². When the weighting factor is gradually increased to the range of 0.14 to 0.18, the interfacial condensation reaction reaches complete thermodynamic equilibrium, the chemical bonding density at the phase interface reaches the saturation limit point of macromolecular chain entanglement, and the impact strength and dimensional stability of the composite material simultaneously reach the optimal equilibrium state. However, when the weighting factor further exceeds the protection limit of 0.22, the excessively introduced elastomer dispersion phase will induce self-aggregation in a strong shear field, causing the flexural modulus of the composition to drop sharply by more than 35%, and the Vicat softening temperature to undergo irreversible performance degradation. Therefore, this invention optimizes the extreme engineering boundary of the range of physical property evolution by performing optimization calculations, and finally precisely fixes the benchmark core value of the weighting factor to 0.16 to ensure that the interfacial strength is maximized while eliminating self-aggregation defects.

[0044] 30 parts by mass of surface-modified graded inorganic filler are continuously and quantitatively fed into the secondary-side feed port of a co-rotating twin-screw extruder at a longitudinal length-to-diameter ratio of 28 to 32. The surface-modified graded inorganic filler is composed of nano-silica with an average particle size of 20 nm to 80 nm and alkali-free glass fiber with an average fiber diameter of 10 μm to 15 μm in a mass ratio of 1:6. The nano-silica and alkali-free glass fiber surfaces are coated with an epoxy silane coupling agent layer, which is formed by the dehydration condensation of the epoxy silane coupling agent and the hydroxyl groups on the surface of the surface-modified graded inorganic filler. The process temperature in the downstream region of the secondary-side feed port is controlled to be reduced to 270°C to 280°C. This temperature reduction initiates the formation of polyphenylene sulfide groups. As the intrinsic viscosity of the bulk melt increases, the shear flow channel of the twin-screw kneading assembly is controlled to maintain the local shear rate of the multiphase blend in the secondary mixing zone at 600 s⁻¹ to 700 s⁻¹. Due to the narrowing of the continuous phase flow channel and the mass transfer resistance caused by the increase in the viscosity of the matrix melt, the high aspect ratio alkali-free glass fibers form a directional and oriented support skeleton in the flow, which enriches and blocks the subsequently inserted nano-silica into the transition grid between the covalent bond layer and the alkali-free glass fibers. In the secondary mixing zone of the twin-screw extruder, a high-shear mixing long section is formed by setting up multiple left-handed kneading discs and right-handed conveying components with a staggered angle of 45°, creating a local high-pressure barrier in the flow channel and a strong three-dimensional chaotic flow field.

[0045] Since the pre-introduced maleic anhydride-grafted ethylene-octene copolymer has undergone an in-situ interfacial grafting reaction with polyphenylene sulfide and formed a covalent bonded layer with a specific surface tension, and the epoxy silane coupling agent layer on the surface of the alkali-free glass fiber has a surface energy degree of freedom between the covalent bonded layer and the matrix resin; when the local shear rate is controlled at 600s⁻¹ to 700s⁻¹, the two-phase shear stress difference in the high-pressure flow field causes the less rigid elastomer phase to be tangentially stretched along the fiber skeleton, since the wettability coefficient of nano-silica at the two-phase interface is 0. At the critical equilibrium point of 5, under the dual coupling of thermodynamic surface energy and fluid shear thrust, nano-silica particles overcome the viscous resistance of the matrix and migrate laterally. They then undergo layered enrichment and aggregation at the physical interface between the two phases, ultimately constructing a non-equilibrium phase separation transition mesh region with a thickness of 50 nm to 150 nm between the covalently bonded layer and the outer wall of the glass fiber. This physical stress pinning effect, generated by the physical superposition of strong shear force fields and in-situ chemical bonding, hinders the continuous deformation of the phase region, thus stabilizing the arrangement and morphology of the nano-phase region at the interface between the two phases. In the incomplete phase separation state of the non-equilibrium phase, a micro-phase-separated melt with a uniformly distributed multiphase interface is produced. This micro-phase-separated melt is conveyed through a slit extrusion die with a slit width of 1.0 mm to 2.5 mm. The multiphase melt is controlled to orient its macromolecular chains under flow channel constraint at a slit shear rate of 600 s⁻¹ to 800 s⁻¹. Cooling water with a process temperature of 15℃ to 25℃ and a flow velocity of 1.2 m / s to 1.8 m / s is continuously introduced as the melt exits the slit extrusion die. The cooling water is controlled... The spray direction is perpendicular to the melt flow direction extruded from the slit extrusion die to establish forced convection heat transfer. The heat transfer area generated by the forced convection heat transfer rate directly transfers heat to the melt with a micro-phase separation structure, blocking the arrangement of macromolecular chain segments into the crystal lattice. The crystallinity of the polyphenylene sulfide matrix in the obtained pellet product is rigidly converged within a set range of 32% to 36%. The solid condensed state features a flexible chain entanglement network in the amorphous region. When the composite material is subjected to alternating load, the alternating stress self-relaxation is generated by the change in the spatial conformation of the macromolecular chain segments in the amorphous region.

[0046] The final granulated product was injection molded to prepare transmission gears. The notched impact strength of the reinforced and toughened polyphenylene sulfide composite material was measured to be 18.2 kJ / m² to 18.6 kJ / m², the tensile elongation at break was 41.3% to 42.5%, the flexural modulus was 12.1 GPa to 12.4 GPa, and the Vicat softening temperature was 261℃ to 262℃. The material was tested under continuous alternating load conditions of 45 MPa to 50 MPa and 10 Hz frequency. Subsequently, the covalent bond layer formed in situ by the specific reactive melt blend material in the transmission gear continuously maintains the chemical bonding density of the multiphase interface, preventing slippage and defect peeling at the phase boundary between the reinforcing fiber and the matrix resin, inhibiting the in situ initiation and disordered propagation of alternating fatigue microcracks inside the transmission gear, so that the transmission gear maintains its structure without brittle fracture and its dimensional deformation within the preset precision fit tolerance range during operation.

[0047] Example 2: When the manufacturing process of transmission gears involves a combination of high-frequency alternating loads and high-temperature, high-pressure stress, the impact strength variation trend and dimensional stability of reinforced and toughened polyphenylene sulfide composite materials in the industrial loaded phase region are verified on a multiphase reaction melt blending test platform consisting of a continuous metering feeding assembly, a multi-stage temperature-controlled blending extruder, a high-pressure micro-orifice slit die assembly, and a multi-jet convection heat transfer quenching water tank. The material mass flow rate control accuracy of the continuous metering feeding assembly is set to 0.1%, the temperature control resolution of the kneading section of the blending extruder is 0.5℃, the signal response cutoff frequency of the online melt pressure sensor is 50Hz and the absolute measurement accuracy is 0.05MPa, and the adjustable stress frequency range of the alternating fatigue test of the end mechanical stress loading frame is 1Hz to 50Hz and the load resolution is 0.1N. To actively introduce industrial flow field disturbances during the multiphase melting process, the continuous metering feeding assembly... A periodic pulse interference with a material mass flow rate of 5% amplitude is added to the main feeding channel, and an alternating temperature drift interference source with an amplitude of 3℃ is set in the primary melting section to create a non-ideal experimental boundary environment with multiple physical fluctuations. When determining the cooling fluid spray speed at the end of the multiphase reaction melt blending test platform, it is affected by the demolding speed of the matrix melt, the thermal conductivity of polyphenylene sulfide, and the crystallization rate of the crystalline region. The setting of the spray speed is used to balance the degree of non-equilibrium deadlock of macromolecular chains and the internal deformation of the product caused by temperature gradient stress. Its constraint satisfies that when the demolding speed of the matrix melt increases, the interfacial convective heat transfer coefficient increases synchronously to maintain a constant supercooling heat transfer rate, so that the spray speed approaches the upper limit of 1.8m / s. For the typical gear injection molding blending condition with a demolding speed of 0.15m / s and a melt temperature of 295℃, the flow speed of the cooling water is adjusted to 1.5m / s according to this heat transfer constraint.

[0048] In the initial parameter establishment stage of the test materials, the raw polyphenylene sulfide resin particles that had not undergone solid-phase heat treatment contained 0.12% initial bound water and 0.08% initial free volatile matter. The intrinsic mass fraction of free sulfur impurities in the raw material batch was defined as... Based on this, 55 parts by mass of polyphenylene sulfide raw material were quantitatively prepared, and multiple experimental sample groups were set up for phase boundary optimization. The first sample group of this invention, configured corresponding to the lower limit of the preparation process characteristics, used pretreated polyphenylene sulfide resin particles that had been heat-treated in solid state at 80°C for 6 hours, reducing their volatile matter mass fraction to 0.018%. The mass flow rate of polyphenylene sulfide resin at the main feed port was controlled. The flow rate is 0.05 kg / s. 15 parts by mass of ethylene-octene copolymer are metered into the elastomer dispersion phase through the first side feed port. The volumetric flow rate of the elastomer dispersion phase is... According to the formula Implement dynamic follow-up adjustment, among which, This represents the volumetric flow rate of the dispersed phase in the elastomer. The intrinsic density of the elastomer dispersion at 80℃ is taken as 0.86 g / cm³, which is regional data. The mass flow rate of polyphenylene sulfide resin at the main feed inlet. The covalent bond saturation weighting factor at the two-phase interface is 0.16. The intrinsic mass fraction of free sulfur impurities in the raw material batch was taken as 0.002. 30 parts by mass of surface-modified graded inorganic filler were introduced and the local shear rate of the secondary mixing zone was controlled at 600 s⁻¹. After demolding, cooling water at 15°C and a flow rate of 1.2 m / s was sprayed. Under these conditions, although affected by the aforementioned pulse interference, the amplitude of the online melt pressure fluctuation monitored by the online melt pressure sensor decreased from 1.45 MPa before adjustment to 0.12 MPa. The chemical bond density of the covalent bond layer generated in situ at the two-phase boundary was measured to be 2.14 bonds / nm². The specific procedure for determining the chemical bond density is as follows.

[0049] 10g of solid pellets were pulverized to 200 mesh and placed in a Soxhlet extractor. Extraction was performed using chloroform as solvent at 80°C under continuous reflux for 48 hours to remove the free maleic anhydride-grafted ethylene-octene copolymer elastomer phase that had not undergone interfacial grafting. The insoluble material was vacuum dried at 60°C to constant weight, and the absolute mass fraction of the in-situ grafted elastomer was calculated by weighing the mass difference before and after extraction. The dried insoluble material was then placed in a high-pressure reactor, and a 1 mol / L sodium hydroxide aqueous solution was added. Hydrolysis was carried out at 150°C for 24 hours to completely break and release the imide bonds formed by graft condensation at the two-phase interface. The released maleic anhydride in the hydrolysate was determined using a high-performance liquid chromatograph. The total molar amount of small molecules of the anhydride derivative; finally, combined with the total interfacial area of ​​the inorganic filler and the dispersed phase measured by a fully automated specific surface area meter, the total molar amount is converted into the number of molecules, and divided by the total interfacial area, the absolute density of covalent bonds generated in situ on each square nanometer of the phase interface can be accurately calculated. The second sample group of this invention, configured according to the median of the corresponding process characteristics, uses pretreated polyphenylene sulfide resin particles heat-treated at 110℃ for 4 hours. The blending process temperature is set to 298℃, the main screw speed is set to 250 rpm, the local shear rate of the secondary mixing zone is controlled at 650 s⁻¹, the cooling water temperature is set to 20℃ and the flow rate is 1.5 m / s, and the internal melt pressure fluctuation amplitude converges to 0.08 MPa. The average crystallinity of the polyphenylene sulfide matrix was measured to be 34%. The third sample group of this invention, configured to correspond to the upper limit of process characteristics, used pretreated polyphenylene sulfide resin particles heat-treated at 140℃ for 2 hours. The blending process temperature was set to 310℃, the spindle screw speed to 350 rpm, the local shear rate to 700 s⁻¹, and the cooling water temperature to 25℃ with a flow rate of 1.8 m / s. The average crystallinity of the polyphenylene sulfide matrix in the final solid pellet product was limited to the upper limit of 36%. The control group, used as a reference for the lack of multiphase synergistic characteristics, directly selected untreated raw polyphenylene sulfide resin particles and abolished the follow-up control formula for volumetric flow rate. Under pulse interference, its online melt pressure amplitude reached 1. The oscillation at 45 MPa caused the chemical bonding density at the multiphase interface to drop below 0.05 bonds / nm², resulting in the aggregation and coarsening of the dispersed phase. As a control group with a blending process temperature below the lower limit of the reasonable range, the melting process temperature was lowered to 260°C. At this temperature, the polyphenylene sulfide resin hard blocks could not completely melt and flow, causing the torque of the blending extruder screw to surge to 85% of the rated power, forcibly interrupting the feeding. As a control group with a shear rate above the upper limit of the reasonable range, the local shear rate was increased to 900 s⁻¹. The excessive shear stress caused the alkali-free glass fibers in the graded inorganic filler to undergo mechanical fracture and breakage, resulting in topological collapse of the average remaining aspect ratio. The average remaining length was shortened axially from 120 μm to 18 μm.

[0050] To evaluate the resilience of multiphase modified compositions to fluctuations in raw material impurities, three gradients of free sulfur impurities were introduced into a multiphase reactive melt blending test platform. The intrinsic mass fraction of free sulfur impurities in each batch of raw materials was adjusted by modifying the purity of the raw materials. The mechanical and physical properties of the injection-molded transmission gear structural components of each test sample group were tested under three conditions: a low free sulfur impurity content of 0.001, a standard physical property defect condition of 0.002, and a high-strength impurity accumulation condition of 0.005. These conditions were then applied to an end-effector mechanical stress loading frame. Under the low free sulfur impurity content condition of 0.001, the structural component of sample group one, cured and molded at the lower limit of the process, exhibited a notched impact strength of 18.6 kJ / m² and a flexural modulus of 12.4 GPa. Under the standard physical property defect condition of 0.002, the structural component of sample group two, cured and molded, showed a notched impact strength of 18.4 kJ / m², a tensile elongation at break of 41.8%, a flexural modulus of 12.2 GPa, and a Vicat softening temperature of 261.5 °C. Furthermore, it operated for 2.4 × 10⁻⁴ hours under a continuous alternating load condition of 48 MPa load and 10 Hz frequency. 6 Subsequently, the deformation of the fit tolerance at the tooth root mating part stabilized at 0.016%, and no internal crack initiation or fracture occurred. Under the condition of high-intensity impurity accumulation of 0.005, the sample group three of this invention configured by the upper limit of the process still maintained a notched impact strength of 18.2 kJ / m² and a flexural modulus of 12.1 GPa, showing a property change trend in which the flexural modulus does not decrease linearly with the increase of impurity concentration. This confirms that the covalent bond layer generated by in-situ condensation polymerization at the two-phase interface has a physical barrier effect of capturing and blocking small molecule free sulfur.

[0051] The underlying cross-scale barrier and capture mechanism lies in the following: the covalently bonded layer generated by the in-situ reaction constructs a high-density grid cross-linked topology, with its local free volume space scale reduced to 0.3 to 0.5 nanometers, far below the grid penetration critical size of free sulfur molecular clusters. This forms a macroscopic grid-like barrier in the microscopic space, greatly increasing the diffusion bending factor of free sulfur molecules. Simultaneously, the bridging layer is rich in unreacted residual maleic anhydride active groups. These highly polar groups possess extremely high local physical affinity and microscopic chemical capture activity for polysulfides and elemental sulfur molecules. When free sulfur molecules come into contact with this phase interface during the high-temperature melting and diffusion process, they are trapped by the bridging layer. The polar centers are firmly adsorbed and anchored in situ, reducing the free diffusion coefficient by more than 85%. Through the cross-temporal synergy of this microscopic high-density chemical trapping sites and mesoscopic tight geometric interception network, macroscopically, the discrete phase interface is transformed into a continuous mass transfer damping layer. This effectively blocks the aggregation of small molecule impurities to lattice defects inside the polyphenylene sulfide matrix, protecting the dimensional stability and modulus characteristics of the overall rigid framework. In contrast, the control group under standard physical property defect conditions, lacking the dissipative structure of the interfacial covalent bond layer, has its simply supported beam notched impact strength reduced to 4.2 kJ / m², flexural modulus reduced to 8.5 GPa, and under the same fatigue stress conditions, it only reaches 1.2 × 10⁻⁶. 4 At this time, local delamination and fracture occurred in the tooth root junction area; at the same time, the control group two, which contained unmelted resin hard block defects, had a notched impact strength of only 5.1 kJ / m² at room temperature, while the control group three, which had skeleton fracture in the fiber bearing phase region, had a flexural modulus that dropped sharply to 6.8 GPa and the overall structural tolerance deformation of the product increased to 0.45%. This quantitative gradient trend confirms that controlling the overall average crystallinity of the polyphenylene sulfide matrix within the set range of 32% to 36% can balance the chain segment entanglement density of the amorphous region of the macromolecule, so that the final material properties are completely free from the dependence on the intrinsic limitation of high purity of raw materials.

[0052] Example 3: This example combines Figures 1 to 2 This document describes a reinforced and toughened polyphenylene sulfide composite material and its preparation method, as follows: Figure 1As shown, in step S1, the polyphenylene sulfide resin particles are heat-treated in a solid state to remove bound water and reduce the volatile matter content, inducing the directional alignment of thiol groups and amino groups at the ends of the polyphenylene sulfide resin particles, resulting in pretreated polyphenylene sulfide resin particles. In step S2, the pretreated polyphenylene sulfide resin particles are conveyed to the melt blending section of a twin-screw extruder. The process temperature is controlled to be in the polyphenylene sulfide molten state. A preheated elastomer dispersion phase is introduced through the first side feed port. The screw speed of the twin-screw extruder is controlled to melt-blend the pretreated polyphenylene sulfide resin particles and the elastomer dispersion phase, causing an interfacial grafting reaction. A covalent bond layer is formed at the interface of the two phases, resulting in a blended melt. Then, in step S3, the blended melt is fed into the secondary side feed port. A surface-modified graded inorganic filler, comprising nanoparticles and fibrous phases, is introduced. The process temperature is adjusted and the local shear rate is controlled at 600 s⁻¹ to 700 s⁻¹, causing the nanoparticles to disperse and accumulate between the covalently bonded layer and the fibrous phase, forming a microphase-separated melt. Finally, in step S4, the microphase-separated melt is conveyed through a slit extrusion die, and the molecular chains are oriented at a slit shear rate of 600 s⁻¹ to 800 s⁻¹. When exiting the slit extrusion die, cooling water at a process temperature of 15°C to 25°C and a flow rate of 1.2 m / s to 1.8 m / s is introduced to quench the melt, controlling the crystallinity of the polyphenylene sulfide matrix in the resulting pellet product to be 32% to 36%.

[0053] like Figure 2 As shown, the material state transformation process presents the evolution relationship of material morphology at each stage. The initial polyphenylene sulfide resin particles are transformed into pretreated polyphenylene sulfide resin particles after undergoing heat treatment in the solid state. Then, the pretreated polyphenylene sulfide resin particles are transformed into a blended melt after undergoing the process of introducing a preheated elastomer dispersion phase through the first side feed port. The blended melt is further evolved into a micro-phase separation structure melt after undergoing the process of introducing surface-modified graded inorganic fillers through the secondary side feed port. Finally, the micro-phase separation structure melt is shaped into pellet products after undergoing the operation of passing through a slit extrusion die and introducing cooling water for rapid cooling.

[0054] Example 4: Under alternating loads and high-temperature, high-pressure stress conditions, the uniformity of physical properties of pretreated polyphenylene sulfide resin granules from different batches fluctuated. The initial bound water mass fraction shifted within the range of 0.10% to 0.18%. Due to the lack of adaptive control during the continuous feeding stage, uneven moisture removal occurred. Subsequently, localized pore defects formed by moisture vaporization occurred inside the melt blending section of the co-rotating twin-screw extruder. This caused uneven interfacial reactions in the elastomer dispersion phase composed of maleic anhydride-grafted ethylene-octene copolymer added from the first side feed port, resulting in a decrease in the chemical bond density at the contact surface between the two phases. Consequently, the stress self-relaxation characteristics of the transmission gear under dynamic loads decreased locally, and fatigue creep and fracture damage occurred on the surface of the structural components due to fatigue stress concentration.

[0055] To determine the control parameters under varying moisture conditions during the heat treatment process, polyphenylene sulfide (PPS) resin granules with an initial bound water mass fraction of 0.15% and an average particle size of 2.5 mm were input via a continuous quantitative feeding assembly. Five temperature test intervals ranging from 80°C to 140°C with a step gradient of 15°C were set in a high-speed fluidized mixer at 1500 rpm. Within each temperature test interval, the residual moisture on the surface of the solid particles was measured at 0.5-hour sampling intervals to construct a dehydration rate rheological curve. When the heat treatment process temperature was controlled at 110°C and the time was controlled at 4 hours, the volatile matter mass fraction of the pretreated PPS resin granules decreased to 0.018%. This material was continuously fed to the melt blending section of a co-rotating twin-screw extruder, with the melt blending section temperature controlled at 295°C. The mass flow rate of the pretreated PPS resin granules at the main feed inlet was also controlled. The feed rate is 0.05 kg / s, and the intrinsic density of the fluid at 80°C is quantitatively added from the first side feed port. The elastomer dispersion phase is a maleic anhydride-grafted ethylene-octene copolymer with a flow rate of 0.86 g / cm³. The volumetric flow rate of the elastomer dispersion phase is... Following the expression of the fluid stoichiometric equation: ,in, This represents the volumetric flow rate of the dispersed phase in the elastomer. The intrinsic density of the elastomer dispersion at 80°C ranges from 0.86 g / cm³ to 0.89 g / cm³. The mass flow rate of the pretreated polyphenylene sulfide resin particles at the main feed inlet. The chemical bonding saturation factor at the two-phase interface is 0.16. The mass fraction of free sulfur impurities in the raw material batch is 0.002. To compensate for the deviation in flow channel backflow loss caused by the 0.05mm physical gap at the kneading disc surface of the main screw in the co-rotating twin-screw extruder, a fluid backflow attenuation operator calibrated by the kneading disc shear resistance pressure drop formula is introduced. The fluid reflux attenuation operator The value is 0.94 under the current high pressure condition. In the aforementioned calibration procedure, the underlying physical logic of the kneading disc shear resistance pressure drop formula is expressed as follows: the fluid backflow leakage in the gap between the kneading discs of the twin-screw extruder is directly proportional to the steady-state total fluid pressure drop between the front and rear ends of the kneading discs, and is directly proportional to the cube of the side gap of the geometric axial overlap area at the top of the two kneading disc assemblies. At the same time, it is inversely proportional to the apparent shear viscosity of the melt under this shear stress flow field.

[0056] Under standard operating conditions, the initial standard pressure drop before and after the main gap of the kneading disc, measured by the pressure sensor, was 4.2 MPa, and the apparent viscosity of the melt was 120 Pascals per second. Substituting the twin-screw spindle speed and the rated volumetric feed rate into the model, it was calculated that the material flow rate lost due to backflow through the 0.05 mm physical gap accounted for 6% of the main feed rate. Therefore, the percentage of effective fluid throughput to nominal conveying capacity was 94%. Based on this, the baseline value of the fluid backflow attenuation operator was calibrated to be 0.94, thus providing accurate data closed-loop support for the subsequent dynamic increase compensation of the pump stroke. By increasing the increment of the feed pump stroke, the actual output value of the volumetric flow rate was increased to the original set control value. This allows for adaptive dynamic compensation of flow rate within a flow field where mechanical leakage losses exist. When controlling the local shear rate in the secondary mixing zone, a co-rotating twin-screw extruder with a length-to-diameter ratio of 40:1 and independent temperature control zones is used. A high-shear mixing section is set up downstream of the secondary side feed inlet, where the longitudinal length-to-diameter ratio is 28 to 32. This section consists of five left-handed kneading discs and right-handed conveying components arranged alternately at a 45° staggered angle. The screw outer diameter of the co-rotating twin-screw extruder is 30 mm. The top of the kneading discs and the inner wall of the extruder barrel... The physical gap between the feeders is 0.05 mm. The spindle screw speed is controlled within the range of 200 rpm to 235 rpm, maintaining the material conveying rate at the main feed port at 50 kg / h. The shear rate of the material passing through the physical gap is limited to the range of 600 s⁻¹ to 700 s⁻¹. Online melt pressure sensors located before and after the high-shear mixing section are used to monitor the fluid pressure drop. When the pressure drop stabilizes within the range of 3.8 MPa to 4.2 MPa, it is determined that the flow field inside the secondary mixing zone has reached the local shear rate range, and the control is then activated. When constructing a non-equilibrium phase separation transition network with a thickness of 50 nm to 150 nm between a covalently bonded layer and alkali-free glass fibers to produce nano-silica, a morphology locking pressure line is established using an online melt pressure sensor located in the secondary mixing zone of a co-rotating twin-screw extruder. When the local shear rate is between 600 s⁻¹ and 700 s⁻¹ and the process temperature downstream of the secondary side feed inlet is controlled at 270 °C to 280 °C, the reference reading of the online melt pressure sensor shows 4.5 MPa to 5.2 MPa. If the purity of the raw material batch fluctuates, causing the concentration of free sulfur impurities to increase and the pressure reading to drop below 4.1 MPa, the fluid phase shear stress is insufficient to drive the lateral migration of nano-silica. The heating temperature in the downstream area of ​​the secondary side feed port is gradually reduced by 2°C per step to increase the intrinsic viscosity of the melt. When the pressure reading returns to the steady-state high-pressure range above 4.5 MPa, the nano-silica particles are constrained at the phase interface by the fluid shear thrust and the thermodynamic mass transfer resistance between the two phases to stably produce a melt with a micro-phase separation structure.

[0057] 30 parts by mass of a surface-modified graded inorganic filler, composed of nano-silica and alkali-free glass fiber, modified with an epoxy silane coupling agent layer and compounded in a mass ratio of 1:6, is continuously added to the secondary side feed port at a longitudinal length-to-diameter ratio of 30 in a co-rotating twin-screw extruder. The local process temperature is reduced to 275℃, and the kneading channel is controlled to maintain the local shear rate of the multiphase blend in the secondary mixing zone at 650 s⁻¹. Even if the main feed channel experiences a continuous 5% flow rate noise due to external fluctuations, the viscosity of each section of the extruded material flow channel remains stable. The multiphase blend melt passes through a slit extrusion die with a slit width of 1.5 mm and completes the chain segment orientation under flow channel constraints at a slit shear rate of 750 s⁻¹. As the melt flows out of the slit extrusion die, cooling water with a process temperature of 20℃ and a flow rate of 1.5 m / s is continuously sprayed, with the spray direction of the cooling water controlled to be perpendicular to the flow direction of the melt extruded from the slit extrusion die. To establish convective heat transfer, the multiphase blend melt was rapidly cooled via convective heat transfer, blocking the rate of macromolecular chain segment arrangement into the crystal lattice. This controlled the overall average crystallinity of the polyphenylene sulfide matrix in the final pelleted solid product to converge within a set range of 32% to 36%. This solid-state condensed-state characteristic maximizes the retention of the flexible chain entanglement network in the amorphous region. Under alternating loads, the spatial conformational change of the macromolecular chain segments in the amorphous region generates alternating stress self-relaxation characteristics. This pelletized product was then molded into transmission gears using an injection molding die. The measured notched impact strength of the simply supported beam of the resulting material was 18.4 kJ / m² to 18.5 kJ / m², the tensile elongation at break was 41.8% to 42.2%, the flexural modulus was 12.2 GPa to 12.3 GPa, and the Vicat softening temperature was 261℃ to 262℃. The gears operated for 2.4 × 10⁻⁶ hours under continuous alternating load conditions of 48 MPa load and 10 Hz frequency. 6Subsequently, the covalent bond layer generated in situ by the aforementioned reactive melt blending process in the transmission gear continuously maintains the chemical bonding density of the multiphase interface, hindering slippage and peeling defects at the phase boundary between the alkali-free glass fiber and the matrix resin, suppressing the initiation and propagation rate of alternating fatigue microcracks inside the transmission gear, ensuring that the transmission gear maintains its structure without brittle fracture during operation, and that the deformation of the tooth profile is maintained within the tolerance limit of 0.015% to 0.016%. When the melt is quenched by introducing cooling water through a slit extrusion die, the quenching heat transfer intensity is controlled according to the slit width selected by the slit extrusion die. When the slit width is selected as 1.0 mm, the melt ratio is... With a large surface area and short heat conduction path, the cooling water process temperature is controlled at 25℃ and the flow velocity is set at 1.2m / s. When the slit width is selected as 2.5mm, the thermal resistance from the center of the melt to the surface increases. The cooling water process temperature is controlled at 15℃ and the flow velocity is set at 1.8m / s. By adjusting the frequency of the water pump inverter in the heat exchange tank, the water flow velocity is kept in the range of 1.2m / s to 1.8m / s. The refrigeration unit is started simultaneously to control the water temperature in the range of 15℃ to 25℃. This balances the deviation in the internal cooling rate of the melt caused by the change in the slit width, so that the crystallinity of the polyphenylene sulfide matrix is ​​maintained in the range of 32% to 36% as measured by differential scanning calorimetry.

[0058] Example 5: When the system faces the processing condition of lightweight, low-deformation, wear-resistant structural parts where the physical wear of the screw assembly caused by long-term continuous operation of the extrusion equipment leads to changes in local flow resistance, the pressure drop and temperature rise in the flow channel become coupled and shifted. This causes the extrusion rheological state of the multiphase blend at the slit die to deviate from the preset phase behavior boundary, resulting in the overall average crystallinity of the polyphenylene sulfide matrix after final cooling and pelletizing exceeding the set range of 32% to 36%. Therefore, it is necessary to provide a periodic in-situ calibration method for the flow channel thermal resistance and pressure boundary under on-site operating conditions. In the specific implementation of this calibration method, a pressure sensor and temperature measuring component installed at the 1.5mm slit width flow channel of the extruder head are used to collect the transient pressure of the multiphase melt flowing out in real time. and transient temperature The clearance change rate of the current die head flow channel is calculated based on the fluid rheological resistance equation, and the clearance change rate is converted into the transient die head flow resistance pressure drop difference value during the feeding process. This allows for dynamic adjustment of the spray speed within the cooling water tank. Specifically, it involves decoupling the fluid rheological resistance equation and the pressure drop difference. The discrete mapping procedure is as follows: The control system performs time-domain time series moving average low-pass filtering on the collected transient pressure and transient temperature data. The filtering period is set to 30 minutes to filter out the high-frequency noise of transient rheology at the second level caused by material pulse feeding and local eddies in the flow field, and extract the quasi-steady-state axial pressure drop trend value caused by equipment wear. Under the established quasi-steady-state flow field, according to the standard power-law fluid shear rheological model in the slit channel, the volumetric flow rate of the melt through the die head is directly proportional to the cube of the width of the flow channel gap and is positively correlated with the pressure drop along the slit. At the same time, the intrinsic viscosity of the material is calibrated and corrected in real time according to the Arrhenius formula through the filtered quasi-steady-state temperature.

[0059] The control system compares the theoretical clean pressure drop value after viscosity calibration with the actual extracted quasi-steady-state pressure drop trend value in real time. When the actual pressure drop trend value is lower than the theoretical clean pressure drop value for five consecutive filtering cycles, it indicates that the flow channel cross-sectional area has expanded due to micron-level wear on the metal wall caused by long-term mechanical friction. At this time, the pressure drop deviation value is substituted into the slit flow dynamics back equation to calculate the percentage expansion of the current actual gap width of the flow channel relative to the initial standard gap width. This percentage is defined as the gap change rate, thereby achieving complete decoupling between the structural changes caused by macroscopic mechanical wear and the transient fluctuations of microscopic fluids. The sampling cutoff frequency of the pressure sensor and temperature measuring component is fixed at 50Hz. To correct the deviation caused by heat convection dissipation, the steady-state pressure drop difference corresponding to the gap change rate is directly used. Adjust the flow rate of cooling water. Satisfy the follow-up adjustment control relationship: ,in, This refers to the actual flow velocity of the cooling water. The basic fluid flow velocity is taken as 1.5 m / s. This is the pressure disturbance compensation coefficient. The difference between the actual measured pressure and the initial standard pressure of the process is used to control the heat transfer flux of the cooling flow field through this closed-loop real-time feedback control. The forced cooling intensity at the outlet of the flow channel remains in situ matched with the transient thermal properties of the melt. The pressure disturbance compensation coefficient in the aforementioned follow-up adjustment control relationship is accurately determined to be 0.04 MPa⁻¹ under the current equipment structure and material resistance system. The on-site in-situ calibration procedure for this coefficient is as follows: After the extrusion equipment has been running stably and continuously for 100 hours, the increase in channel flow resistance caused by physical wear of the screw assembly is simulated by gradually closing the die head throttle valve. When the actual measured pressure collected by the online fluid pressure sensor increases by 2.5 MPa compared with the initial standard pressure of the process, the flow channel flow dynamic resistance increases. This causes a synchronous increase in the transient actual shear heat generation rate of the melt upon demolding, and consequently increases the flow orientation energy of the macromolecular chain segments. To prevent the melt crystallinity from jumping out of the preset equilibrium window of 32% to 36%, the control system calculates the required subcooling heat transfer flux based on the heat transfer convection heat transfer matrix model, and adjusts the spray velocity of the cooling flow field from the initial 1.5 m / s to 1.65 m / s. By substituting the actual measured pressure deviation value and velocity increment into the control relationship for inverse limit deduction, the required spray velocity compensation increment per MPa pressure deviation is calibrated, thus locking the discrete absolute value of the pressure disturbance compensation coefficient to 0.04 MPa⁻¹, thereby ensuring the accurate locking of the non-equilibrium state of the polymer chain segments during long-term operation on site.

[0060] In the final pellet product quality verification process, differential scanning calorimetry (DSC) was used to scan the heat flow profile of the product according to a standard procedure. The overall average crystallinity of the polyphenylene sulfide (PPS) matrix was calculated using the ratio of the melt endothermic peak area to the enthalpy of melting of standard fully crystalline PPS. The measured data points were distributed within a narrow window of non-equilibrium phases, ranging from 33.2% to 34.5%, confirming that the cooling intensity after on-site servo calibration could lock the morphology of each phase region of the polymer chain segments. The pellet product was continuously fed into an injection molding machine and processed at a temperature of 290°C to 310°C to obtain wear-resistant transmission gear structural parts. These parts were then tested under a continuous alternating load condition of 48 MPa load and 10 Hz frequency for 2.4 × 10⁻⁶ hours. 6 Subsequently, the maximum deformation of the outer contour of the structural component stabilized within 0.015% of the dimensional accuracy. The covalent bond layer at the multiphase boundary and the oriented filler skeleton seamlessly maintained the stress dissipation barrier characteristics. No local phase peeling, phase separation agglomeration cracks, or fatigue creep fractures occurred on the toothed load-bearing surface.

[0061] Example 6: When the system faces the processing conditions of lightweight, low-deformation, wear-resistant structural parts, the initial mass fraction of functional groups at the end of the molecular chain in different batches of polyphenylene sulfide resin raw materials fluctuates and the local flow resistance changes due to physical wear of the screw assembly caused by long-term continuous operation of the extrusion equipment, the pressure drop and temperature rise inside the flow channel cause a coupling shift, resulting in the deviation of the melting reaction window of the multiphase blend material inside the twin-screw extruder. At this time, a standardized offline calibration and follow-up compensation procedure for process parameters is used to establish an adaptive control matrix of screw speed and heating temperature of each section in order to maintain the stability of the interfacial grafting reaction in the mass transfer process.

[0062] In the offline calibration step of establishing the adaptive control matrix, polyphenylene sulfide resin particles with a melt flow rate of 120 g / 10 min and a purity of 99.6% as measured according to GB / T3682.1-2018 standard at 315℃ and 5.0 kg load were selected as the continuous phase matrix. Maleic anhydride-grafted ethylene-octene copolymer with a maleic anhydride grafting rate of 1.0%, a melt index of 1.5 g / 10 min and a density of 0.88 g / cm³ as measured according to GB / T3682.1-2018 standard at 190℃ and 2.16 kg load was selected as the elastomer dispersion phase. Nano-silica with an average particle size of 50 nm and an average particle size of 10 nm were used as the elastomer dispersion phase. Alkali-free glass fibers with a diameter of 12 μm were compounded at a mass ratio of 1:6 and graded inorganic fillers coated with an epoxy silane coupling agent layer were used as the reinforcing phase. Multiple test sample groups were prepared by mixing polyphenylene sulfide resin particles, elastomer dispersion phase and graded inorganic fillers at a mass ratio of 55:15:30. In a co-rotating twin-screw extruder with an aspect ratio of 40:1 and a zoned temperature control accuracy of ±1℃, the local flow resistance gradient of the flow channel caused by physical wear of the screw assembly was simulated by adjusting the opening of the die head throttle valve. The transient melt pressure drop and melt temperature jump values ​​in the core reaction zone of the twin-screw extruder were measured for each flow resistance gradient to establish the material conveying compensation parameters.

[0063] Based on the reproducible data from the calibration test, when the change in the opening of the die head throttle valve caused an increase in local flow resistance within the first range of 5% to 12%, the screw speed in the melt blending section of the co-rotating twin-screw extruder was increased from 200 rpm to 235 rpm via the servo control system to enhance the shear mass transfer rate. Simultaneously, the set heating temperature in the reaction core area and the downstream area of ​​the secondary side feed port was reduced by 2°C to 3°C to offset shear heat generation. The measured online melt pressure fluctuation amplitude at the screw end was maintained between 0.08 MPa and 0.10 MPa, and the chemical bond density of the covalent bond layer formed in situ at the two-phase boundary was measured to be between 2.18 bonds / nm² and 2.2. At 4 nm², the average crystallinity of the polyphenylene sulfide matrix in the final solid pellet product rigidly converged to 33.2% to 34.5%. When the increase in local flow resistance was in the second range of 12% to 25%, the screw speed was further increased from 235 rpm to 280 rpm, and the set heating temperature of the reaction core area and the downstream area of ​​the secondary side feed port was reduced by 4°C to 6°C. At this time, the measured online melt pressure fluctuation amplitude was limited to 0.09 MPa to 0.11 MPa, the chemical bond density at the phase interface was maintained at 2.12 nm² to 2.16 nm², and the average crystallinity of the polyphenylene sulfide matrix was stable at 34.6% to 35%. 8%; For the control group without follow-up control matrix compensation, the increased local flow resistance in the flow channel led to uncontrolled shear heat accumulation and prolonged material residence time, resulting in local degradation and denaturation of the polyphenylene sulfide macromolecular chain. The online melt pressure fluctuation amplitude increased to 1.35 MPa, and the phase boundary chemical bond density dropped below 0.04 bonds / nm², causing large-scale agglomeration defects in the elastomer dispersed phase. Solid pellets prepared according to the follow-up control matrix calibration parameters were molded into transmission gear structural parts using injection molding. The measured notched impact strength of the simply supported beam of the material was between 18.3 kJ / m² and 18.7 kJ / m², and the tensile fracture elongation was... With an elongation of 41.5% to 42.4%, a flexural modulus of 12.2 GPa to 12.4 GPa, and a Vicat softening temperature of 261℃ to 262℃, after 2,400,000 cycles of continuous alternating load conditions with 48 MPa load and 10 Hz frequency, the covalent bond layer maintains a multiphase interface chemical bonding state, preventing slippage or peeling at the phase boundary between the alkali-free glass fiber and the matrix resin, inhibiting the initiation and propagation of alternating fatigue cracks inside the transmission gear, and ensuring that the transmission gear structure does not experience brittle fracture during operation, while the deformation of the tooth profile remains within the tolerance limit of 0.015% to 0.016%.

[0064] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the present invention.

[0065] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention.

Claims

1. A method for preparing a reinforced and toughened polyphenylene sulfide composite material, characterized in that, Includes the following steps: Step S1: Heat-treat polyphenylene sulfide resin particles in a solid state to remove bound water and reduce the mass fraction of volatiles, and induce the oriented arrangement of thiol groups and amino groups at the ends of polyphenylene sulfide resin particles to obtain pretreated polyphenylene sulfide resin particles. Step S2: The pretreated polyphenylene sulfide resin particles are conveyed to the melt blending section of the twin-screw extruder. The process temperature is controlled to be in the molten state of polyphenylene sulfide. The preheated elastomer dispersion phase is introduced through the first side feed port. The screw speed of the twin-screw extruder is controlled to make the pretreated polyphenylene sulfide resin particles and the elastomer dispersion phase melt blend and undergo interfacial grafting reaction, forming a covalent bond layer at the interface of the two phases to obtain a blended melt. Step S3: Surface-modified graded inorganic filler, including nanoparticles and fibrous phase, is introduced into the blended melt through the secondary side feed port. The process temperature is adjusted and the local shear rate is controlled to be 600 s⁻¹ to 700 s⁻¹, so that the nanoparticles are dispersed and enriched between the covalent bonded layer and the fibrous phase, forming a melt with a micro-phase separation structure. Step S4: The micro-phase separated melt is conveyed through a slit extrusion die, and the molecular chains are oriented and arranged at a slit shear rate of 600 s⁻¹ to 800 s⁻¹. When the melt exits the slit extrusion die, cooling water with a process temperature of 15°C to 25°C and a flow rate of 1.2 m / s to 1.8 m / s is introduced to quench the melt, and the crystallinity of the polyphenylene sulfide matrix in the resulting pellet product is controlled to be 32% to 36%.

2. The method for preparing a reinforced and toughened polyphenylene sulfide composite material according to claim 1, characterized in that, Based on the total weight of the reinforced and toughened polyphenylene sulfide composite material as 100%, the mass percentage of the elastomer dispersed phase is 5% to 20%, the mass percentage of the surface-modified graded inorganic filler is 15% to 40%, and the balance is polyphenylene sulfide resin particles; in step S1, the heat treatment process temperature is 80℃ to 140℃, the time is 2h to 6h, the volatile matter mass fraction of the polyphenylene sulfide resin particles is controlled to be less than 0.02%, and step S1 is completed in a high-speed fluidized mixer with a rotation speed of 1200rpm to 1800rpm.

3. The method for preparing a reinforced and toughened polyphenylene sulfide composite material according to claim 1, characterized in that, Step S2 includes the following sub-steps: Step S21, the pretreated polyphenylene sulfide resin particles are melted in the melt blending section of a twin-screw extruder, and the process temperature of the melt blending section is controlled at 285°C to 310°C; Step S22, the elastomer dispersion phase preheated to 60°C to 90°C is quantitatively introduced through the first side feed port of the twin-screw extruder, and the screw speed of the twin-screw extruder in the melt blending section is controlled at 150 rpm to 350 rpm, so that the elastomer dispersion phase reacts with the pretreated polyphenylene sulfide resin particles.

4. The method for preparing a reinforced and toughened polyphenylene sulfide composite material according to claim 1, characterized in that, The elastomer dispersion phase is a maleic anhydride-grafted ethylene-octene copolymer, and the maleic anhydride grafting rate of the maleic anhydride-grafted ethylene-octene copolymer is 0.5% to 1.5%.

5. The method for preparing a reinforced and toughened polyphenylene sulfide composite material according to claim 1, characterized in that, The nanoparticles in the surface-modified graded inorganic filler are nano-silica, and the average particle size of the nanoparticles is 20nm to 80nm; the fibrous phase in the surface-modified graded inorganic filler is alkali-free glass fiber, and the average fiber diameter of the alkali-free glass fiber is 10μm to 15μm.

6. The method for preparing a reinforced and toughened polyphenylene sulfide composite material according to claim 1, characterized in that, The surface-modified graded inorganic filler is coated with an epoxy silane coupling agent layer; the epoxy silane coupling agent layer is formed by the dehydration condensation of the epoxy silane coupling agent and the hydroxyl groups on the surface of the surface-modified graded inorganic filler.

7. The method for preparing a reinforced and toughened polyphenylene sulfide composite material according to claim 1, characterized in that, In step S3, the process temperature in the downstream area of ​​the secondary side feed port is controlled to be 270°C to 280°C.

8. The method for preparing a reinforced and toughened polyphenylene sulfide composite material according to claim 1, characterized in that, In step S4, the slit width of the slit extrusion die is 1.0 mm to 2.5 mm.

9. The method for preparing a reinforced and toughened polyphenylene sulfide composite material according to claim 1, characterized in that, In step S4, the spray direction of the cooling water is perpendicular to the flow direction of the melt extruded from the slit extrusion die.

10. A reinforced and toughened polyphenylene sulfide composite material, characterized in that, The reinforced and toughened polyphenylene sulfide composite material is prepared by the method described in claim 1.

Citation Information

Patent Citations

  • Glass fiber, SiO2 enhanced toughened polyphenylene sulfide material and preparation method thereof

    CN103804910A