Energy-saving system and method for low-temperature modification and granulation of waste plastics

By using a variable-pitch screw structure and online detection technology, the problems of uneven melt viscosity and difficulty in removing air bubbles caused by the mixing of waste plastic components have been solved, realizing efficient low-temperature modification and granulation of waste plastics, and improving the quality and production stability of recycled granules.

CN123129342APending Publication Date: 2026-11-20GUANGDONG SHANGNAN FUPAN LOGISTICS EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611287537.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-24
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Waste plastics are mixed with other components. Low-temperature modification technology leads to uneven melt viscosity and poor fluidity, making it difficult for air bubbles to escape and forming hollow particles, which affects the appearance and performance of recycled particles.

Method used

The plasticizing extrusion equipment adopts a variable pitch screw structure, combined with NIR online component detection and rheometer. By controlling the temperature and screw speed, it achieves efficient degassing and uniform mixing, reduces processing temperature, and is equipped with an online rheological detection unit and extreme component reference parameter library to adaptively adjust process parameters.

Benefits of technology

It effectively reduces processing temperature, avoids thermal oxidative degradation of polymer chains, improves the bulk density and performance of recycled particles, reduces emissions of harmful volatiles, and achieves energy-saving production and stable processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123129342A_ABST
    Figure CN123129342A_ABST
Patent Text Reader

Abstract

The application provides a waste plastic low-temperature modification-granulation integrated energy-saving system, which comprises a stock bin, a plasticizing extrusion device, a cooling tank, a granulator and a control system; the plasticizing extrusion device comprises a feeding section, a melting section, an exhaust section, a post-mixing section and a low-temperature modification extrusion section in sequence along the material flow direction, and each section is provided with an independent temperature control system; the plasticizing extrusion device is provided with a screw rod, a driving device is connected with the screw rod to drive the screw rod to rotate; a method is also provided, which comprises the following steps: material component detection; setting initial reference parameters; measuring and obtaining melt viscosity; viscosity deviation adjustment; exhaust; post-mixing homogenization; low-temperature modification extrusion, cooling and granulation. The application prevents the problem of melt homogenization plugging the exhaust port, reduces the hollow probability, improves the mechanical properties, reduces the processing temperature to realize energy-saving production, avoids environmental pollution, has high production stability, and is suitable for mixed waste plastics with complex sources and large component fluctuations.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of plastics plasticization technology, specifically to an integrated energy-saving system and method for low-temperature modification and granulation of waste plastics. Background Technology

[0002] The thermoplasticity of waste plastics allows them to be recycled through hot melt regeneration. However, waste plastics come from a wide range of sources and are of mixed composition, with significant differences in melting point, melting temperature, and thermal decomposition temperature among different types of plastics. Traditional granulation processes often raise the processing temperature to around 400°C to promote the simultaneous melting of mixed plastics. While this achieves overall plasticization, low-melting-point components are prone to overheating and degradation, leading to deterioration of the recycled material's performance and the generation of large amounts of harmful waste gases.

[0003] In recent years, low-temperature modification technology has replaced some heat input by enhancing mechanical shearing, achieving plasticization at lower temperatures to avoid thermal oxidative degradation of polymer chains. However, the mixed composition of waste plastics leads to the following problems with the use of low-temperature modification technology: Taking a mixture of PP (melting point approximately 165℃) and PE (melting point approximately 110℃) as an example, when the processing temperature is controlled at a low range to protect PP, although PE can melt fully, PP is not sufficiently plasticized, resulting in uneven melt viscosity and poor flowability. This heterogeneous melt makes it difficult to effectively expel the trapped moisture and volatile gases, hindering bubble migration and significantly reducing venting efficiency. The trapped bubbles cannot escape during pelleting and cooling, eventually forming cavities inside the pellets, i.e., the "hollow pellet" phenomenon, which seriously affects the appearance, bulk density, and mechanical properties of the recycled pellets. Summary of the Invention

[0004] The purpose of this invention is to address the shortcomings of existing technologies by proposing an integrated energy-saving system and method for low-temperature modification and granulation of waste plastics.

[0005] To achieve the above objectives, the present invention adopts the following technical solution: An integrated energy-saving system for low-temperature modification and granulation of waste plastics includes a silo, plasticizing extrusion equipment, cooling tank, pelletizer, and control system; The hopper is connected to the plasticizing extrusion equipment; The plasticizing extrusion equipment includes, in sequence along the material flow direction, a feeding section, a melting section, a venting section, a post-mixing section, and a low-temperature modified extrusion section, each section being equipped with an independent temperature control system; the plasticizing extrusion equipment is equipped with a screw, and a drive device is connected to the screw to drive the screw to rotate; The extruded strips from the plasticizing extrusion equipment are cooled in a cooling tank and then granulated by a pelletizer to obtain plastic pellets. The drive device, temperature control system, and control system are electrically connected.

[0006] Furthermore, a discharge pipe is provided at the bottom of the silo, and a feeding device is provided on the discharge pipe; a feeding port is provided in the feeding section, and the outlet of the discharge pipe is connected to the feeding port; an NIR online component detection probe is provided on the discharge pipe; The end of the melting section is connected to a sampling branch, a gear pump is installed on the sampling branch, the end of the sampling branch is connected to a rheometer, and a reflux pipe is provided between the rheometer and the melting section. The exhaust section is provided with an exhaust port, and the screw of the exhaust section is designed with a variable pitch thread structure, including a compression section, a release section and an exhaust corresponding section; The screw of the post-mixing section is equipped with a mixing ring assembly and a mixing disc; An extrusion die is provided at the end of the low-temperature modified extrusion section; The feeding device, NIR online component detection probe, rheometer, gear pump, and control system are electrically connected.

[0007] Furthermore, the screw pitch at the front end of the exhaust section is 40-50mm, the screw pitch of the compression section is set to 20-25mm, and the screw groove depth is reduced to 0.6-0.8 times the screw groove depth at the front end of the exhaust section. The screw pitch of the release section is 50-60mm, and the screw groove depth is the same as the screw groove depth at the front end of the exhaust section. The exhaust port is located directly above the exhaust section, with a pitch of 40-50mm and a groove depth that is 1.5-2 times the groove depth of the screw in the release section.

[0008] Furthermore, the front section of the screw in the rear mixing section is provided with at least two sets of mixing rings. Each mixing ring set includes two parallel and inclined mixing rings. The inclination angle between the mixing rings and the screw axis is 30-45°. The inclination directions of adjacent sets of mixing rings are opposite.

[0009] Furthermore, a mixing disc is provided at the rear end of the screw of the post-mixing section. The mixing disc is a circular disc with toothed protrusions on the circumference of its edge. The toothed protrusions of adjacent mixing discs are staggered.

[0010] Furthermore, a side feeding device is also provided at the front end of the post-mixing section.

[0011] An integrated method for low-temperature modification and granulation of waste plastics includes the following steps: S1: Material composition analysis; Obtain the mass fraction of each component of the material; S2: Set initial baseline parameters; An extreme component baseline parameter library is established, and initial baseline parameters are obtained by linear proportional calculation based on the material composition; the initial baseline parameters include initial temperature and initial screw speed. S3: Measure the viscosity of the melt; The obtained initial temperature and initial rotation speed are sent to the temperature control system and drive device of the melting section to control the material to melt and plasticize under the initial temperature and initial rotation speed conditions. Online sampling is performed at the end of the melting section to extract melt samples for viscosity measurement and obtain the viscosity of the melt. S4: Viscosity deviation adjustment; The built-in material composition-rheological property database, based on the detected material composition, uses a multidimensional linear interpolation method to obtain the target viscosity range of the melt from the material composition-rheological property database; the obtained melt viscosity is then compared with the target melt viscosity range. If the viscosity of the melt is greater than the upper limit of the target viscosity range, increase the heating temperature of the melting section by 2-8°C, while reducing the screw speed by 5-15%. If the viscosity of the melt is lower than the lower limit of the target viscosity range, reduce the temperature of the melting section by 2-5°C and increase the screw speed by 5-10%. If the viscosity of the melt is within the target viscosity range, maintain the current temperature and rotation speed; S5: Exhaust; The homogeneous melt, after viscosity adjustment, enters the exhaust section for exhaust. S6: Post-mixing homogenization; The fully vented melt enters the post-mixing section for mixing and shearing, controlling the melt temperature to 180-220℃; S7: Low-temperature modified extrusion, cooling granulation; After being mixed and homogenized, the melt is extruded into strips through a die at 180-220℃. The strips are then cooled to 40-60℃ in a cooling tank and then granulated by a pelletizer to obtain plastic pellets.

[0012] Furthermore, step S2 includes: S21: Establish a library of extreme component reference parameters; The optimal process parameters are determined under three extreme conditions; the optimal process parameters include the optimal temperature and the optimal rotational speed. Extreme cases include pure PP, pure PE, and mixtures of PP / PE with a mass ratio of 50:50, with the moisture content controlled below 0.5%; S22: Obtain the mass fraction of PP in the total polymer based on the material composition; If the material composition only includes PP and PE, then the mass fraction W of PP in the total polymer is the mass fraction of PP obtained from the material composition detection. If the material also contains other components, then the other components are equivalent to the mass fraction W of PP. S23: Obtain the initial temperature; If the mass fraction W of PP in the total polymer is ≤50%, then according to the formula: To obtain the initial temperature, where 𝑇 𝑃𝐸 The optimal temperature obtained for pure PE calibration is 𝑇 50 The optimal temperature was obtained by calibration for a PP / PE mixture with a mass ratio of 50:50, where W is the mass fraction of PP in the total polymer; If the mass fraction W of PP in the total polymer is greater than 50%, then according to the formula: Obtain the initial temperature, where The optimal temperature obtained for pure PP calibration. The optimal temperature was obtained by calibration for a PP / PE mixture with a mass ratio of 50:50, where W is the mass fraction of PP in the total polymer; S24: Obtain the initial rotational speed; According to the formula Obtain the initial rotational speed, where The optimal rotational speed was obtained by calibration for a PP / PE mixture with a mass ratio of 50:50, where k is a proportionality coefficient of 1-3 rpm / ℃. The optimal temperature was obtained for calibrating a mixture of PP / PE with a mass ratio of 50:50, where T is the initial temperature obtained.

[0013] Furthermore, the material composition-rheological properties database includes various types of plastics and typical mixing ratios of various plastic types, and records the optimal viscosity window for each combination to achieve efficient exhaust in the exhaust section; the plastic types include PP, PE, PS, and ABS.

[0014] Furthermore, step S21 specifically includes: With the screw speed fixed, the temperature of the melting section is gradually increased from the initial temperature in fixed temperature increments. The discharge state of the die head and the volatilization effect of the vent are observed. If the volatilization effect is good and there are no cavities inside the pellets after pelleting, the optimal temperature of the material is recorded. Next, at the optimal temperature, the rotational speed is gradually increased from the initial speed in fixed increments, and the melt pressure and extrusion stability are observed. If the melt pressure fluctuation range does not exceed ±5% of the set value and the appearance of the extruded strip from the die is uniform, the optimal rotational speed of the material is recorded.

[0015] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) The exhaust section of the present invention adopts a variable pitch screw structure with corresponding compression, release and exhaust sections. The melt is first compressed under high pressure, and then the pressure drops sharply to induce gas precipitation into bubbles. After that, the melt spreads into a thin layer, and the bubbles burst to release gas. Relying on pressure change to drive devolatilization, the problem of melt homogenization blocking the exhaust port is prevented, and the probability of generating a large number of hollow particles after cooling and pelletizing is reduced, effectively improving the bulk density and performance of recycled particles. (2) The extrusion processing temperature of the present invention is controlled at 180-220℃, which greatly reduces the processing temperature, avoids the thermal oxidation degradation of high molecular chains in waste plastics, avoids environmental pollution, retains the mechanical properties of recycled plastics, reduces harmful volatiles generated by high temperature cracking, reduces heating energy consumption, and achieves energy-saving production. (3) The mixing process of this invention is arranged downstream of the exhaust section. The melt has already completed devolatilization. The shearing and mixing operation will not re-enter the air bubbles and will not damage the exhaust effect. The mixing ring group (arranged in an inclined and reverse staggered manner) realizes melt diversion, reversal and folding. The mixing disk with staggered toothed protrusions realizes interlayer shear orientation, which can shear and break up the small amount of unmelted solid particles remaining in the melt and fully disperse them, ensuring the uniformity of the melt and guaranteeing the mechanical properties of the finished product. (4) This invention is equipped with an NIR online component detection probe and an online rheological detection unit. Combined with the extreme component reference parameter library and the material composition-rheological property database, the initial process parameters can be calculated according to the material composition. The temperature and screw speed can be adjusted based on the melt viscosity. It is suitable for mixed waste plastics such as PP, PE, PS and ABS with complex sources and large component fluctuations. It does not require a lot of manual debugging, has strong process adaptability, controllable melt pressure fluctuations during extrusion, uniform material output, and high production stability. Attached Figure Description

[0016] Figure 1 This is a schematic diagram of the process structure of the integrated energy-saving system for low-temperature modification and granulation of waste plastics according to the present invention; Figure 2 This is a schematic diagram of the structure of the hopper and plasticizing extrusion equipment of the present invention; Figure 3 This is an enlarged view of part A of the present invention; Figure 4 This is a flowchart of the steps of the integrated low-temperature modification and granulation method for waste plastics of the present invention. Detailed Implementation

[0017] To provide a further understanding of the purpose, structure, features, and functions of the present invention, detailed descriptions are provided below with reference to specific embodiments.

[0018] Please refer to the reference. Figure 1 , Figure 2 and Figure 3This invention provides an integrated energy-saving system for low-temperature modification and granulation of waste plastics, including a silo 100, a plasticizing extrusion equipment 200, a cooling tank 300, a pelletizer 400, and a control system; The bottom of the silo 100 is provided with a discharge pipe 110, and the discharge pipe 110 is provided with a feeding device 120; The plasticizing extrusion equipment 200 includes, in sequence along the material flow direction, a feeding section 210, a melting section 220, a venting section 230, a post-mixing section 240, and a low-temperature modified extrusion section 250, each section being equipped with an independent temperature control system 500; the plasticizing extrusion equipment 200 is equipped with a screw 270, and a drive device 260 is connected to the screw to drive the screw to rotate; The feeding section 210 is provided with a feeding port 211, and the outlet of the discharge pipe 110 is connected to the feeding port 211. The discharge pipe 110 is also provided with an NIR online component detection probe 130, which is connected to the control system via optical fiber to identify the proportion of components such as PP, PE, PS, and ABS in waste plastics.

[0019] The end of the melting section 220 is connected to a sampling branch 221. A gear pump 222 is installed on the sampling branch 221. The end of the sampling branch 221 is connected to a rheometer 223. A return pipe 224 is provided between the rheometer 223 and the melting section. The gear pump 222 takes out the molten melt and enters the rheometer 223 for viscosity measurement. The measured melt is returned to the melting section through the return pipe 224.

[0020] The exhaust section 230 is provided with an exhaust port 231. The screw of the exhaust section 230 is designed with a variable pitch thread structure, including a compression section 232, a release section 233 and an exhaust corresponding section 234. The screw pitch at the front end of the exhaust section 230 is 40-50mm, and the screw pitch of the compression section 232 is set to 20-25mm. The screw groove depth is reduced to 0.6-0.8 times the screw groove depth at the front end of the exhaust section. After the melt enters the compression section 232, the melt is subjected to increased compressive force during the propulsion process, and the pressure rises from about 5MPa to 15-20MPa. This allows the gases dissolved in the melt (water vapor, volatile organic compounds, etc.) to be fully compressed and evenly dispersed in the melt under high pressure, accumulating energy for subsequent release and precipitation.

[0021] The screw pitch of the release section 233 suddenly increases to 50-60 mm from the end of the compression section, and the screw groove depth is the same as the screw groove depth at the front end of the exhaust section 230; the melt pressure in the release section 233 drops suddenly to about 2-5 MPa. This sudden pressure drop induces the dissolved gas in the melt to rapidly supersaturate and precipitate, forming a large number of tiny bubble nuclei that quickly grow into large bubbles; The exhaust port 231 is located directly above the exhaust section 234, with a screw pitch of 40-50 mm and a screw groove depth that is 1.5-2 times the screw groove depth of the release section 233. This allows the melt to spread into a thin layer of 5-15 mm thickness in this area, thinning the bubble walls, causing them to rupture under normal pressure, and allowing the gas to escape through the exhaust port.

[0022] The variable pitch thread utilizes the pressure drop to induce bubble nucleation and growth, and relies on pressure changes to drive gas precipitation, thus avoiding the blockage of the exhaust port after the melt homogenizes, which would prevent the exhaust from being blocked.

[0023] The screw of the post-mixing section 240 is equipped with a mixing ring assembly 241 and a mixing disc 242; The front section of the screw in the post-mixing section 240 is provided with at least two sets of mixing ring groups 241. Each mixing ring group 241 includes two parallel and inclined mixing rings 243. The inclination angle between the mixing rings 243 and the screw axis is 30-45°. The inclination directions of adjacent mixing ring groups 241 are opposite. This applies a diversion, reversal, and folding effect to the melt.

[0024] A mixing disc 242 is installed at the rear end of the screw in the post-mixing section. The mixing disc 242 is a circular disc with toothed protrusions 244 on its circumference. The toothed protrusions 244 of adjacent mixing discs 242 are staggered. This allows the melt to undergo repeated interlayer shearing and reorientation as it flows through, breaking down and evenly dispersing the very small amount of incompletely melted solid particles remaining in the melt under shear force. This location is after the venting section 230, where the melt has already undergone sufficient venting, so the mixing operation does not affect the venting efficiency.

[0025] An extrusion die 251 is provided at the end of the low-temperature modified extrusion section 250.

[0026] The temperature control system 500, feeding device 120, NIR online component detection probe 130, rheometer 223, gear pump 222, screw drive device 260 are electrically connected to the control system.

[0027] Furthermore, the front end of the post-mixing section 240 is also equipped with a side feeding device 600 for adding modifying agents to the melt; the modifying agents include toughening agents, compatibilizers, antioxidants, etc.

[0028] like Figure 4 The integrated method for low-temperature modification and granulation of waste plastics includes the following steps: S1: Material composition analysis; Waste plastic enters the plasticizing extrusion equipment through the hopper. During the feeding process, the NIR online component detection probe performs rapid component detection on the material to obtain the mass fraction of components such as PP, PE, ABS, and PS.

[0029] S2: Set initial baseline parameters; An extreme component baseline parameter library is established, and initial baseline parameters are obtained by linear proportional calculation based on the material composition; the initial baseline parameters include initial temperature and initial screw speed. S21: Establish a library of extreme component reference parameters; The optimal process parameters are determined under three extreme conditions; the optimal process parameters include the optimal temperature and the optimal rotation speed.

[0030] Calibration was performed using pure PP, pure PE, and a mixture of PP / PE at a mass ratio of 50:50, with the moisture content controlled below 0.5%. With the screw speed fixed at 300 rpm, the melting zone temperature was gradually increased from 150℃ in 3℃ increments. The discharge status of the die head and the devolatilization effect at the vent were observed. If there was no obvious material overflow from the vent, the devolatilization effect was good, and there were no cavities inside the pellets after pelleting (this can be observed by random sampling and cutting or by density testing), this temperature was recorded as the optimal temperature for the material. Next, at the optimal temperature, the rotational speed was gradually increased from 100 rpm in 5 rpm increments, and the melt pressure and extrusion stability were observed. A pressure sensor was installed at the die head to detect and obtain the melt pressure; when the melt pressure fluctuation range did not exceed ±5% of the set value and the extruded strip from the die head had a uniform appearance, this rotational speed was recorded as the optimal rotational speed for that material. The set value is the optimal pressure target value set for the measuring point of the die head based on the quality requirements of the target product, the material formula used, the characteristics of the mold, and the capabilities of the equipment.

[0031] After calibration, the three sets of optimal process parameters are stored in the database of the control system. S22: Obtain the mass fraction of PP in the total polymer based on the material composition; If the material composition only includes PP and PE, then the mass fraction W of PP in the total polymer is the mass fraction w of PP obtained from the material composition analysis. PP If the material contains other components, according to the formula: The other components are equivalent to the PP mass fraction W, where w PP The mass fraction of PP obtained from material composition analysis. Let be the conversion factor for component i. The mass fraction of component i obtained from material composition analysis; For the preset fixed values, the β of component ABS is 1.2, and the β of component PS is 1.1, etc.

[0032] S23: Obtain the initial temperature; If the mass fraction W of PP in the total polymer is ≤50%, then according to the formula: Obtain the initial temperature, where The optimal temperature obtained for pure PE calibration. The optimal temperature was determined for a PP / PE mixture with a mass ratio of 50:50, where W is the mass fraction of PP in the total polymer.

[0033] If the mass fraction W of PP in the total polymer is greater than 50%, then according to the formula: Obtain the initial temperature, where The optimal temperature obtained for pure PP calibration. The optimal temperature was determined for a PP / PE mixture with a mass ratio of 50:50, where W is the mass fraction of PP in the total polymer.

[0034] S24: Obtain the initial rotational speed; According to the formula Obtain the initial rotational speed, where The optimal rotational speed was obtained by calibration for a PP / PE mixture with a mass ratio of 50:50, where k is a proportionality coefficient of 1-3 rpm / ℃. The optimal temperature was obtained for calibrating a mixture of PP / PE with a mass ratio of 50:50, where T is the initial temperature obtained.

[0035] S3: Measure the viscosity of the melt; The obtained initial temperature and initial rotation speed are sent to the temperature control system and drive device of the melting section to control the material to melt and plasticize under the initial temperature and initial rotation speed conditions. Online sampling is performed at the end of the melting section, and melt samples are extracted for viscosity measurement. The detection frequency is ≥1 time / second, and the average viscosity is calculated to obtain the viscosity of the melt.

[0036] S4: Viscosity deviation adjustment; The built-in material composition-rheological property database covers common waste plastic types (PP, PE, PS, ABS, etc.) and their typical mixing ratios (mass ratio range 0:100 to 100:0, step size 5%), and records the optimal viscosity window for each combination to achieve efficient venting in the venting stage. Under laboratory conditions, using standard material formulations as samples, and employing a small extruder with an online rheometer and venting efficiency testing device, the melt viscosity range corresponding to the maximum devolatilization efficiency of each sample in the venting stage was measured and recorded. The database can be reused after a single measurement. It is applicable to single-component and mixed waste plastics in different proportions; it can also convert other components into equivalent PP mass fractions for parameter calculation, adapting to complex mixed recycled materials.

[0037] Based on the detected material composition, a multidimensional linear interpolation method is used to obtain the target viscosity range of the melt from the material composition-rheological property database; Compare the obtained viscosity of the melt with the target viscosity range of the melt: If the viscosity of the melt is greater than the upper limit of the target viscosity range, it indicates that the refractory components such as PP are not sufficiently plasticized. A temperature compensation command is issued to raise the heating temperature of the melting section by 2-8°C, while reducing the screw speed by 5-15%; and to extend the residence time of the melt in the high-temperature zone to promote the full melting of PP.

[0038] If the viscosity of the melt is lower than the lower limit of the target viscosity range, it indicates that the melt is too thin, which is not conducive to bubble entrainment and stable extrusion. Reduce the temperature of the melting section by 2-5℃ and increase the screw speed by 5-10% to increase the shear heat while avoiding overheating and degradation of the material.

[0039] If the viscosity of the melt is within the target viscosity range, maintain the current temperature and rotation speed.

[0040] S5: Exhaust; After viscosity control, the homogeneous melt enters the exhaust section. First, it passes through the compression section, where the pitch gradually decreases from the normal value, and the melt pressure gradually increases to 15-20 MPa, where the dissolved gas is fully compressed under high pressure. Then, the melt enters the release section, where the pitch suddenly increases and the pressure drops sharply to 2-5 MPa, causing the dissolved gas to rapidly become supersaturated and precipitate, forming a large number of bubble nuclei that grow into large bubbles. Finally, the melt enters the corresponding exhaust section, where it spreads into a thin layer, the bubble walls become thinner, and the bubbles rapidly rupture under normal pressure, allowing the gas to escape through the exhaust port.

[0041] S6: Post-mixing homogenization; The fully vented melt enters the post-mixing section, where the mixing ring group and toothed mixing disc apply diversion, reversal, shearing and interlayer exchange to the melt, shearing and breaking up the very small amount of unmelted solid particles remaining in the melt, and controlling the melt temperature to 180-220℃.

[0042] Furthermore, modified additives (toughening agents, compatibilizers, antioxidants, etc.) are added via a side-feeding device and forcibly and uniformly mixed with the melt to improve product performance. The side-feeding device achieves uniform mixing of additives and melt, facilitating the on-demand adjustment of recycled material product performance.

[0043] S7: Low-temperature modified extrusion, cooling granulation.

[0044] After being mixed and homogenized, the melt is extruded into strips through a die at a low temperature of 180-220℃. The strips are then cooled to 40-60℃ in a cooling tank and then pelletized by a pelletizer to obtain dense, hollow recycled plastic pellets.

[0045] Example 1

[0046] Raw material: waste PP / PE mixed plastic; S1: Material composition analysis: PP mass fraction was 80%, PE mass fraction was 20%; S2: Set initial reference parameters: Based on pure PP and linear interpolation of the 50:50 reference library, the initial melting zone temperature is 195℃ and the screw speed is 280rpm.

[0047] S3: Measure the melt viscosity; the measured melt viscosity is 291.1 Pa·s.

[0048] S4: Viscosity deviation adjustment; by linear interpolating two sets of reference parameters using pure PP and 50:50 PP / PE mixture, the target melt viscosity range is obtained: 295-312 Pa·s; The melt viscosity is lower than the lower limit of the target melt viscosity range; the temperature of the melting section is adjusted to 190℃ and the screw speed is increased to 294 rpm. After adjustment, the viscosity is retested and found to be 298.2 Pa·s, which is within the target melt viscosity range.

[0049] S5: Exhaust; The melt enters the exhaust section to exhaust gas, and the pressure in the exhaust section is monitored at the same time. The pressure in the compression section is 18 MPa; the pressure in the release section is 3.6 MPa. S6: Post-mixing homogenization; control melt temperature at 180℃; S7: Low-temperature modified extrusion, cooling granulation; The melt is extruded into strips through a die at a low temperature of 180°C. The strips are cooled to 40°C in a cooling tank and then granulated by a pelletizer to obtain plastic pellets.

[0050] Example 2

[0051] Raw material: waste PP / PE mixed plastic; S1: Material composition analysis: PP mass fraction was 50%, and PE mass fraction was 50%. S2: Set initial reference parameters: Based on pure PP and linear interpolation of the 50:50 reference library, the initial melting zone temperature is 182℃ and the screw speed is 260rpm.

[0052] S3: Measure the melt viscosity; the measured melt viscosity is 210.5 Pa·s.

[0053] S4: Viscosity deviation adjustment; obtains the target viscosity range of the melt: 206-218 Pa·s; The melt viscosity remains within the target melt viscosity range, while maintaining the current temperature and rotation speed.

[0054] S5: Exhaust; The melt enters the exhaust section to exhaust gas, and the pressure in the exhaust section is monitored at the same time. The pressure in the compression section is 17 MPa; the pressure in the release section is 3.8 MPa. S6: Post-mixing homogenization; control melt temperature at 200℃; S7: Low-temperature modified extrusion, cooling granulation; The melt is extruded into strips through a die at a low temperature of 200°C. The strips are cooled to 50°C in a cooling tank and then granulated by a pelletizer to obtain plastic pellets.

[0055] Example 3

[0056] Raw material: waste PP / PE mixed plastic; S1: Material composition analysis: PP mass fraction was 20%, PE mass fraction was 80%; S2: Set initial reference parameters: Based on pure PP and linear interpolation of the 50:50 reference library, the initial melting zone temperature is 168℃ and the screw speed is 240rpm.

[0057] S3: Measure the melt viscosity; the measured melt viscosity is 147.1 Pa·s.

[0058] S4: Viscosity deviation adjustment; obtains the target melt viscosity range: 150-165 Pa·s; The melt viscosity is lower than the lower limit of the target melt viscosity range; the temperature of the melting section is adjusted to 166℃ and the screw speed is increased to 264 rpm. After adjustment, the viscosity is retested and found to be 154.2 Pa·s, which is within the target melt viscosity range.

[0059] S5: Exhaust; The melt enters the exhaust section to exhaust gas, and the pressure in the exhaust section is monitored at the same time. The pressure in the compression section is 16 MPa; the pressure in the release section is 2.8 MPa. S6: Post-mixing homogenization; control melt temperature at 220℃; S7: Low-temperature modified extrusion, cooling granulation; The melt is extruded into strips through a die at a low temperature of 220°C. The strips are cooled to 60°C in a cooling tank and then granulated by a pelletizer to obtain plastic pellets.

[0060] One hundred particles from each of Examples 1-3 were randomly selected, cut open, and the percentage of hollow particles was statistically analyzed. The results are shown in Table 1:

[0061] The present invention has been described in the above-described embodiments; however, these embodiments are merely examples for implementing the present invention. It must be noted that the disclosed embodiments do not limit the scope of the present invention. Conversely, any modifications and refinements made without departing from the spirit and scope of the present invention are within the scope of patent protection of the present invention.

Claims

1. An integrated energy-saving system for low-temperature modification and granulation of waste plastics, characterized in that: This includes a silo, plasticizing extrusion equipment, cooling tank, pelletizer, and control system; The hopper is connected to the plasticizing extrusion equipment; The plasticizing extrusion equipment includes, in sequence along the material flow direction, a feeding section, a melting section, a venting section, a post-mixing section, and a low-temperature modified extrusion section, each section being equipped with an independent temperature control system; the plasticizing extrusion equipment is equipped with a screw, and a drive device is connected to the screw to drive the screw to rotate; The extruded strips from the plasticizing extrusion equipment are cooled in a cooling tank and then granulated by a pelletizer to obtain plastic pellets. The drive device, temperature control system, and control system are electrically connected.

2. The integrated energy-saving system for low-temperature modification and granulation of waste plastics as described in claim 1, characterized in that: The bottom of the silo is equipped with a discharge pipe, and the discharge pipe is equipped with a feeding device; the feeding section is equipped with a feeding port, and the outlet of the discharge pipe is connected to the feeding port; the discharge pipe is equipped with an NIR online component detection probe; The end of the melting section is connected to a sampling branch, a gear pump is installed on the sampling branch, the end of the sampling branch is connected to a rheometer, and a reflux pipe is provided between the rheometer and the melting section. The exhaust section is provided with an exhaust port, and the screw of the exhaust section is designed with a variable pitch thread structure, including a compression section, a release section and an exhaust corresponding section; The screw of the post-mixing section is equipped with a mixing ring assembly and a mixing disc; An extrusion die is provided at the end of the low-temperature modified extrusion section; The feeding device, NIR online component detection probe, rheometer, gear pump, and control system are electrically connected.

3. The integrated energy-saving system for low-temperature modification and granulation of waste plastics as described in claim 2, characterized in that: The screw pitch at the front end of the exhaust section is 40-50mm, the screw pitch of the compression section is set to 20-25mm, and the screw groove depth is reduced to 0.6-0.8 times the screw groove depth at the front end of the exhaust section. The screw pitch of the release section is 50-60mm, and the screw groove depth is the same as the screw groove depth at the front end of the exhaust section. The exhaust port is located directly above the exhaust section, with a pitch of 40-50mm and a groove depth that is 1.5-2 times the groove depth of the screw in the release section.

4. The integrated energy-saving system for low-temperature modification and granulation of waste plastics as described in claim 2, characterized in that: The front section of the screw in the post-mixing section is provided with at least two sets of mixing rings. Each mixing ring set includes two parallel and inclined mixing rings. The inclination angle between the mixing rings and the screw axis is 30-45°. The inclination directions of adjacent sets of mixing rings are opposite.

5. The integrated energy-saving system for low-temperature modification and granulation of waste plastics as described in claim 2, characterized in that: The rear section of the screw in the post-mixing section is provided with a mixing disc, which is a circular disc with toothed protrusions on the circumference of the edge of the mixing disc, and the toothed protrusions of adjacent mixing discs are staggered.

6. The integrated energy-saving system for low-temperature modification and granulation of waste plastics as described in claim 1, characterized in that: The front end of the post-mixing section is also equipped with a side feeding device.

7. An integrated method for low-temperature modification and granulation of waste plastics, characterized in that: Includes the following steps: S1: Material composition analysis; Obtain the mass fraction of each component of the material; S2: Set initial baseline parameters; An extreme component baseline parameter library is established, and initial baseline parameters are obtained by linear proportional calculation based on the material composition; the initial baseline parameters include initial temperature and initial screw speed. S3: Measure the viscosity of the melt; The obtained initial temperature and initial rotation speed are sent to the temperature control system and drive device of the melting section to control the material to melt and plasticize under the initial temperature and initial rotation speed conditions. Online sampling is performed at the end of the melting section to extract melt samples for viscosity measurement and obtain the viscosity of the melt. S4: Viscosity deviation adjustment; The built-in material composition-rheological property database, based on the detected material composition, uses a multidimensional linear interpolation method to obtain the target viscosity range of the melt from the material composition-rheological property database; the obtained melt viscosity is then compared with the target melt viscosity range. If the viscosity of the melt is greater than the upper limit of the target viscosity range, increase the heating temperature of the melting section by 2-8°C, while reducing the screw speed by 5-15%. If the viscosity of the melt is lower than the lower limit of the target viscosity range, reduce the temperature of the melting section by 2-5°C and increase the screw speed by 5-10%. If the viscosity of the melt is within the target viscosity range, maintain the current temperature and rotation speed; S5: Exhaust; The homogeneous melt, after viscosity adjustment, enters the exhaust section for exhaust. S6: Post-mixing homogenization; The fully vented melt enters the post-mixing section for mixing and shearing, controlling the melt temperature to 180-220℃; S7: Low-temperature modified extrusion, cooling granulation; After being mixed and homogenized, the melt is extruded into strips through a die at 180-220℃. The strips are then cooled to 40-60℃ in a cooling tank and then granulated by a pelletizer to obtain plastic pellets.

8. The integrated method for low-temperature modification and granulation of waste plastics as described in claim 7, characterized in that: Step S2 includes: S21: Establish a library of extreme component reference parameters; The optimal process parameters are determined under three extreme conditions; the optimal process parameters include the optimal temperature and the optimal rotational speed. Extreme cases include pure PP, pure PE, and mixtures of PP / PE with a mass ratio of 50:50, with the moisture content controlled below 0.5%; S22: Obtain the mass fraction of PP in the total polymer based on the material composition; If the material composition only includes PP and PE, then the mass fraction W of PP in the total polymer is the mass fraction of PP obtained from the material composition detection. If the material also contains other components, then the other components are equivalent to the mass fraction W of PP. S23: Obtain the initial temperature; If the mass fraction W of PP in the total polymer is ≤50%, then according to the formula: To obtain the initial temperature, where 𝑇 𝑃𝐸 The optimal temperature obtained for pure PE calibration is 𝑇 50 The optimal temperature was obtained by calibration for a PP / PE mixture with a mass ratio of 50:50, where W is the mass fraction of PP in the total polymer; If the mass fraction W of PP in the total polymer is greater than 50%, then according to the formula: Obtain the initial temperature, where The optimal temperature obtained for pure PP calibration. The optimal temperature was obtained by calibration for a PP / PE mixture with a mass ratio of 50:50, where W is the mass fraction of PP in the total polymer; S24: Obtain the initial rotational speed; According to the formula Obtain the initial rotational speed, where The optimal rotational speed was obtained by calibration for a PP / PE mixture with a mass ratio of 50:50, where k is a proportionality coefficient of 1-3 rpm / ℃. The optimal temperature was obtained for calibrating a mixture of PP / PE with a mass ratio of 50:50, where T is the initial temperature obtained.

9. The integrated method for low-temperature modification and granulation of waste plastics as described in claim 7, characterized in that: The material composition-rheological properties database includes various types of plastics and typical mixing ratios of various plastic types, and records the optimal viscosity window for each combination to achieve efficient exhaust in the exhaust section; the plastic types include PP, PE, PS, and ABS.

10. The integrated method for low-temperature modification and granulation of waste plastics as described in claim 8, characterized in that: Step S21 specifically includes: With the screw speed fixed, the temperature of the melting section is gradually increased from the initial temperature in fixed temperature increments. The discharge state of the die head and the volatilization effect of the vent are observed. If the volatilization effect is good and there are no cavities inside the pellets after pelleting, the optimal temperature of the material is recorded. Next, at the optimal temperature, the rotational speed is gradually increased from the initial speed in fixed increments, and the melt pressure and extrusion stability are observed. If the melt pressure fluctuation range does not exceed ±5% of the set value and the appearance of the extruded strip from the die is uniform, the optimal rotational speed of the material is recorded.