A solid-state silicone rubber die foaming forming method with independent temperature gradient control

By using an independent temperature gradient control method and taking advantage of the temperature difference between azo foaming agents and double 25 vulcanizing agents, the problem of premature cross-linking of mold wall rubber was solved, thereby improving the appearance quality of the products and increasing production efficiency.

CN123129377APending Publication Date: 2026-11-20ZHEJIANG WEIRE TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611596562.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-15
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In the existing solid silicone molding foaming process, the adhesive material at the mold wall is cross-linked and cured in advance, resulting in many product appearance defects, poor cell uniformity, and low yield.

Method used

An independent temperature gradient control method is adopted. By controlling the temperature difference between the mold core and the mold wall, and utilizing the activation temperature difference between the azo foaming agent and the double 25 vulcanizing agent, the temperature is controlled in zones. Foaming occurs first on the mold core side and then crosslinking occurs on the mold wall side, forming a temperature gradient that is high inside and low outside, ensuring that the surface rubber maintains its plasticity and ductility during the foaming stage.

Benefits of technology

It reduces surface scratches, cell collapse, and internal delamination defects, stabilizes the foaming ratio, improves product appearance yield, and enhances process repeatability and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123129377A_ABST
    Figure CN123129377A_ABST
Patent Text Reader

Abstract

This application discloses a method for molding solid silicone with independent temperature gradient control. The method uses methyl vinyl silicone rubber raw material as the matrix, combined with a nitrogen-based foaming agent and a 25% vulcanizing agent. Utilizing the activation temperature difference between the two, the temporal and spatial decoupling of foaming and vulcanization is achieved. During the foaming stage, the core temperature is controlled at 130-140℃ and the mold wall temperature at 55-65℃, creating an internal high and external low temperature gradient. Gas is preferentially generated inside the rubber compound, while the surface layer maintains plasticity. During the vulcanization stage, the temperature is raised to 165-175℃ to complete cross-linking. After demolding, a second vulcanization is performed to obtain the finished product. For thick-walled products, the core and upper and lower molds are heated synchronously, while for thin-walled products, the mold wall temperature is maintained low, relying on heat conduction from the rubber compound for cross-linking. The core is equipped with a ceramic heating rod, and PLC PID closed-loop temperature control allows for pre-stored and recall of process parameters for products with different wall thicknesses. This invention can reduce scratches, cell collapse, and delamination defects caused by premature vulcanization of the silicone surface, improve cell uniformity, product yield, and process repeatability, and is suitable for the industrial production of thick-walled, irregularly shaped solid foamed silicone products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of silicone rubber compression molding technology, specifically relating to a solid silicone compression molding method with independent temperature gradient control. Background Technology

[0002] Solid compound silicone rubber compression molding foaming is the mainstream industrial production process for foamed silicone products. It is suitable for molding irregular, thick-walled, and large-sized products in the fields of new energy, rail transportation, and electronics. The product dimensions are highly controllable and have the characteristics of high and low temperature resistance, aging resistance, good compression resilience, and low VOC. The existing process uses a vulcanizing machine with a flat platen to heat the upper and lower surfaces of the mold. Heat is conducted from the mold wall to the interior of the cavity, which is an "outside-in" heat transfer mode. The rubber compound is pre-mixed with the foaming agent and vulcanizing agent, cut into sheets, and placed into a sealed cavity. After the mold is closed and pressurized, foaming, gas generation, and cross-linking vulcanization are completed simultaneously in the confined space. In this mode, the rubber compound near the mold wall reaches the reaction temperature first, and the surface foaming agent and vulcanizing agent are activated simultaneously. After cross-linking and curing, the plasticity and ductility are lost. Even with a segmented overall heating process, the entire cavity is still in the same temperature field, and the surface layer will still cross-link prematurely. When the internal rubber compound continues to expand due to gas generation, the cured surface layer cannot deform synchronously, which easily leads to defects such as surface scratches, cell collapse, dense surface layer, and large internal cells with delamination. The foaming ratio fluctuates greatly, resulting in low product yield. To improve the uniformity of mold temperature, existing technologies have a solution of independently controlling the temperature by having a heating rod built into the mold core. However, its core objective is to eliminate the temperature difference between different areas of the mold and avoid the upper and lower molds driving the mold core to slowly heat up, so as to shorten the vulcanization time and improve production efficiency. It does not actively create a spatial temperature difference and cannot solve the problem of premature vulcanization and shaping of the surface. Summary of the Invention

[0003] The technical problem to be solved by this application is that the existing solid silicone molding foaming uses the same temperature heating as the whole, and the rubber material at the mold wall cross-links and cures in advance, which cannot expand with the internal foaming, resulting in many product appearance defects, poor cell uniformity and large fluctuations in yield.

[0004] To address the aforementioned issues, this application provides a method for molding solid silicone rubber using an independently temperature-controlled gradient. The raw materials for the solid compounded silicone rubber include methyl vinyl silicone rubber raw rubber, a 25 vulcanizing agent, and an azo foaming agent. The rapid crosslinking temperature of the 25 vulcanizing agent is ≥170℃, and the rapid decomposition temperature of the azo foaming agent is ≥130℃. The core characteristics of this system are: azo foaming agents can decompose and produce gas in a short time at temperatures above 130°C, while 25 vulcanizing agents can only undergo rapid cross-linking at temperatures above 170°C. By utilizing the activation temperature difference between the two, the foaming and vulcanizing processes can be decoupled in space and time through zoned temperature control.

[0005] The molding method includes a foaming stage and a vulcanization and setting stage performed sequentially. Foaming stage: After the mold is closed and pressurized, the core temperature is independently controlled at 130℃~140℃ and the mold wall temperature is independently controlled at 55℃~65℃. A temperature gradient with higher temperature inside and lower temperature outside is formed along the wall thickness direction of the rubber material in the cavity. The temperature is maintained for 300s~600s. The rubber material near the core reaches the decomposition temperature of the foaming agent first and produces gas. The outer silicone foams and vulcanizes slowly in a lower temperature environment, maintaining surface plasticity. The core temperature is selected at 130℃~140℃, which meets the temperature requirements for rapid decomposition of azo foaming agents without reaching the rapid cross-linking threshold of the 25% vulcanizing agent, ensuring that the core side is dominated by foaming reaction. The mold wall temperature is selected at 55℃~65℃, which does not trigger the decomposition of the surface foaming agent and the cross-linking of the vulcanizing agent, ensuring that the surface rubber has sufficient extensibility, while avoiding the rubber material being too cold and too viscous, which would prevent it from expanding and stretching with the cells. The heat preservation time is adjusted according to the wall thickness of the product; the thicker the wall, the longer the heat preservation time, ensuring that most of the foaming agent on the core side is decomposed, without causing the surface rubber to undergo slow cross-linking due to prolonged heating.

[0006] Vulcanization and setting stage: The mold core is heated to 165℃~175℃ to bring the overall temperature of the rubber compound to the rapid cross-linking temperature of the dual 25 vulcanizing agent. This temperature is maintained until the rubber compound cross-links and sets. Afterwards, it is cooled and demolded. The product undergoes secondary vulcanization to obtain the finished foamed silicone product. During the vulcanization stage, the remaining small amount of undecomposed foaming agent uniformly generates gas during the heating process. This gas generation process is synchronized with the cross-linking process of the rubber compound, allowing the cell walls to set simultaneously and preventing cell rupture and collapse.

[0007] Furthermore, the solid compounded silicone rubber is prepared through the following steps: Place the raw methyl vinyl silicone rubber in a two-roll mill, control the roll temperature at 18℃~22℃, add 0.5%~5% of the raw rubber mass of double 25 vulcanizing agent, and mix for 5min~10min; then add 0.5%~5% of the raw rubber mass of azo foaming agent, mix for 5min~10min, and extrude the compound rubber. Cut the compounded rubber into sheets of the corresponding size, with a sheet thickness of 1 / 3 to 2 / 3 of the cavity wall thickness. Wrap the sheets around the mold core and then close the mold. Controlling the roller temperature at 30℃ to 40℃ can prevent the additives from reacting prematurely due to heat during the mixing process, ensuring that the additives are evenly dispersed in the raw rubber. Adding the vulcanizing agent first and then adding the foaming agent can prevent the foaming agent from decomposing prematurely due to prolonged shearing. The sheet thickness is designed to allow space for foaming expansion, preventing excessive silicone from limiting the foaming space, affecting the size and uniformity of the cells, and even resulting in a finished product that is not foamed and is close to solid.

[0008] Furthermore, during the foaming stage, the core temperature is controlled at 130℃, the mold wall temperature is controlled at 60℃, the holding time is 300s~600s, and the cavity pressure after mold closing is 10~50kg / cm². 2 . These parameters are the preferred parameters for the foaming stage. The temperature difference is stable at 70℃, which is suitable for most conventional wall thickness products. The cavity pressure is controlled at 5MPa~12MPa, which not only matches the pressure conditions for rapid cross-linking of the double 25 vulcanizing agent, but also inhibits the gas escape during the instantaneous decomposition of the foaming agent, making the cells fine and uniform, and avoiding excessively low pressure leading to excessively high open cell ratio, and excessively high pressure leading to limited cell growth.

[0009] Furthermore, during the vulcanization and setting stage, the mold core is heated to 170°C at a rate of 2°C / min to 4°C / min, and the vulcanization timer is started after the temperature is stabilized for 30 seconds. This heating rate can prevent the rubber compound from heating too quickly, which would cause excessive stress difference between the inside and outside of the cells and lead to cell wall rupture; starting the timer after the temperature stabilizes can ensure uniform temperature in all areas of the mold core and avoid asynchronous local vulcanization.

[0010] Furthermore, during the vulcanization and setting stage, the upper and lower molds are simultaneously heated to 165℃~175℃ at a rate of 1.5℃ / min~3℃ / min and held at that temperature for 10min~20min, so that the rubber material can be heated together with the mold core to complete the cross-linking. The method is suitable for foamed silicone products with a wall thickness of 10mm~50mm. This scheme is the preferred vulcanization method for thick-walled products. The greater the wall thickness, the longer the heat conduction path. Simultaneously raising the temperature of the upper and lower molds can shorten the overall heating time and prevent the bubbles from merging due to prolonged exposure to high temperatures. The heating rate of the upper and lower molds is slightly lower than that of the mold core, which can always maintain a temperature trend of higher inside and lower outside, so that the crosslinking process can proceed smoothly from the inside to the outside.

[0011] Furthermore, during the vulcanization and shaping stage, the mold wall is maintained at 55°C to 65°C, and the mold core is heated to 170°C and kept at that temperature for 15 to 30 minutes. The entire material reaches the cross-linking temperature through its own heat conduction. This method is suitable for foamed silicone products with a wall thickness of ≤10mm. Thin-walled products have low thermal resistance in the adhesive layer. The surface layer can reach the basic temperature required for cross-linking simply by conducting heat through the mold core. Maintaining a low temperature in the mold wall can reduce energy consumption. The degree of cross-linking can be supplemented by secondary vulcanization, while avoiding premature curing of the surface layer due to active heating.

[0012] Furthermore, multiple independent ceramic heating rods are inserted inside the mold core, and each ceramic heating rod is equipped with a thermocouple. The heating power is adjusted by a PLC controller using a PID algorithm. The mold wall temperature is independently controlled by the upper and lower heating plates of the vulcanizing machine. The temperature control parameters corresponding to products with different wall thicknesses are pre-stored in the PLC controller and can be directly called when changing models. Multiple independent heating units can adjust their power according to the heat dissipation differences in different areas of the mold core, avoiding uneven temperature caused by rapid heat dissipation at both ends of the mold core; the heating plate of the vulcanizing machine only undertakes the functions of pressurization and auxiliary heat preservation during the foaming stage, with little interference to the preset gradient and stable process repeatability; parameter pre-storage can reduce the number of debugging times during production changeover and reduce material waste from trial and error.

[0013] Furthermore, the secondary vulcanization process is as follows: the demolded and trimmed product is placed in a hot air environment at 170℃~180℃ for 2h~4h and then cooled in the furnace. These parameters are the general post-vulcanization parameters for double 25 vulcanized solid silicone rubber, which can ensure complete cross-linking of the rubber compound, while removing residual vulcanizing agent decomposition products and undecomposed foaming agent, reducing compression set and improving resilience; furnace cooling can avoid the generation of internal stress due to rapid cooling and prevent deformation of thick-walled products.

[0014] Furthermore, the method is applicable to solid foamed silicone products with a wall thickness of 10mm to 50mm.

[0015] Furthermore, the azo foaming agent is a composite azo foaming agent, with azodicarbonamide as the main foaming agent and a foaming activating agent further compounded therein; the foaming activating agent is N'-((2-methylpyrimidin-5-yl)amino)-N,N-dimethylformamidinium; the bis(25) vulcanizing agent is 2,5-dimethyl-2,5-di-tert-butylperoxyhexane. Azodicarbonamide is the main gas-generating agent, with stable gas production and non-irritating decomposition products; the foaming activating agent does not possess foaming gas-generating capabilities, but is used to activate and adjust the rapid decomposition temperature of azodicarbonamide, making the foaming system compatible with the gradient temperature-controlled foaming process of this application; the bis(25) vulcanizing agent has good scorch safety and an extremely low crosslinking rate at low temperatures, making it compatible with the gradient temperature-controlled process of this application. In this application, the foaming activator N'-((2-methylpyrimidinyl)amino)-N,N-dimethylformamidinium, is named 5-dimethylaminomethyleneamino-2-methylpyrimidinium by the manufacturer, and the manufacturer's CAS number is 84610037. This CAS number cannot be found in the public CAS database. This substance is only used as a foaming activator and does not belong to azo foaming materials.

[0016] The beneficial effects of this application are as follows: By utilizing the activation temperature difference between azo foaming agents and double 25 vulcanizing agents, a directional temperature gradient with a high internal temperature and a low external temperature is actively constructed during the foaming stage. The internal part prioritizes the completion of the main gas generation process, while the surface layer maintains plastic extensibility throughout the foaming stage and can deform synchronously with the expansion of internal cells, reducing surface scratches, insufficient filling, cell collapse, and internal delamination defects, stabilizing the foaming ratio, and improving the product appearance yield. The mold core adopts multi-zone independent ceramic heating rods for closed-loop temperature control. During the foaming stage, the vulcanizing machine heating plate maintains a low temperature and only undertakes the functions of pressurization and auxiliary heat preservation, which has little interference with the preset gradient temperature field. The temperature gradient can be maintained stably for a long time, resulting in good process repeatability between different batches and a low coefficient of variation in cell diameter. The temperature control parameters corresponding to products with different wall thicknesses can be pre-stored in the PLC controller and can be directly called when switching product specifications, reducing changeover debugging time and trial and error losses, and improving the production efficiency of multi-specification products. Attached Figure Description

[0017] Figure 1 This is a schematic diagram illustrating the structural principle of the molding die used in the embodiments of this application; Figure 2 This is a PLC control schematic diagram of the molding die used in the embodiments of this application; Figure 3 This is a schematic diagram illustrating the evolution of the silicone foaming mechanism in this application; Figure 4 This is a process flow diagram of an embodiment of this application.

[0018] The markings in the diagram are: upper mold 1, lower mold 2, mold core 3, ceramic heating rod 4, upper heating plate 5, lower heating plate 6, PLC controller 7, upper mold thermocouple 8, mold core thermocouple 9, cavity 10, and adhesive material 100. Detailed Implementation

[0019] The present application will be further described below with reference to the accompanying drawings and embodiments.

[0020] like Figure 1 , 2 As shown, the molding die used in this application includes an upper die 1, a lower die 2, and a die core 3 disposed in the cavity 10. The top surface of the upper die 1 is in contact with the upper heating plate 5 of the vulcanizing machine, and the bottom surface of the lower die 2 is in contact with the lower heating plate 6 of the vulcanizing machine. The upper heating plate 5 and the lower heating plate 6 are independently temperature controlled by the vulcanizing machine system. An upper die thermocouple 8 is embedded inside the upper die 1 for collecting the actual temperature of the die wall.

[0021] The mold core 3 has multiple parallel and spaced mounting holes. The ceramic heating rod 4 is pre-inserted and fixed in the mounting hole before the mold core is assembled into the mold. The hole opening is insulated and sealed. The heating rod wire is led out along the wiring groove at the end of the mold core. A mold core thermocouple 9 is set next to each ceramic heating rod 4.

[0022] The mold has a sealed quick-connect connector on its side. After the mold is closed, the heating rod, thermocouple, and external PLC controller 7 can be connected via the quick-connect connector without opening the mold. The ceramic heating rod 4, the mold core thermocouple 9, and the upper mold thermocouple 8 are all connected to the PLC controller 7, and the heating power of each area can be independently adjusted through a PID algorithm. The adhesive material is filled into the cavity 10 between the outer wall of the mold core 3 and the inner walls of the upper mold 1 and lower mold 2. The radial thickness of the adhesive layer corresponds to the wall thickness of the final product. The PLC controller 7 has a complete set of temperature control parameters pre-stored for products with different wall thicknesses and specifications, which can be directly called up when changing models.

[0023] Example 1: As Figure 4 As shown. In this embodiment, a solid foamed silicone gasket with a wall thickness of 20 mm is prepared using a simultaneous temperature-increasing vulcanization process, the steps of which are as follows: S1. Preparation of compound: Take 100 parts of methyl vinyl silicone rubber raw rubber (vinyl content 0.13%, average molar mass 500,000) and place it in a two-roll mill, controlling the mill roll temperature at 20℃; add 2 parts of bis25 vulcanizing agent (effective content 50%, chemical name 2,5-dimethyl-2,5-di-tert-butylperoxyhexane), and mix lightly for 8 minutes; then add 3 parts of composite azo foaming agent, the foaming main body of which is azodicarbonamide (the nominal rapid decomposition temperature of azodicarbonamide is 135℃), and compounded with foaming activator N'-((2-methylpyrimidinyl)amino)-N,N-dimethylformamide, continue mixing for 8 minutes, then roll out into sheets to obtain solid compound, and let stand for later use.

[0024] S2. Temperature control parameter preset: The parameter set corresponding to the 20mm wall thickness is called through PLC controller 7: target temperature of mold core during foaming stage 130℃, target temperature of upper and lower heating plates 60℃, foaming and heat preservation time 450s, cavity pressure set to 20kg / cm³. 2 The target temperature of the mold core during the vulcanization stage is 170℃, the heating rate is 3℃ / min, the target temperature of the upper and lower heating plates is 170℃, the heating rate is 2℃ / min, and the vulcanization holding time is 15min.

[0025] S3. Pre-forming and Mold Closure: Cut the compounded rubber into 10mm thick sheets and evenly wrap them around the outside of the mold core 3, which has a pre-placed ceramic heating rod 4, ensuring that there are no gaps between the rubber sheet and the mold core wall; position the mold core wrapped with the rubber sheet in the cavity of the lower mold 2, and after mold closing, apply pressure until the cavity pressure stabilizes at 25kg / cm². 2 The control circuit of ceramic heating rod 4 and mold core thermocouple 9 is connected through quick-connect connector on the side of the mold.

[0026] S4. Gradient Temperature Controlled Foaming: The temperature control program is activated, raising the mold core from room temperature to 130°C, and the upper and lower heating plates to 60°C. After stabilization, foaming timing begins. A continuous internal high and external low temperature gradient of approximately 3.5°C / mm is formed along the 20mm thick rubber wall, and this temperature is maintained for 450 seconds. At the end of this stage, the temperature of the rubber near the mold core reaches 130°C, and the azodicarbonamide decomposition rate exceeds 95%, completing the main gas generation process. The temperature of the rubber near the mold wall is approximately 60°C, the azodicarbonamide decomposition rate is less than 5%, the crosslinking rate of the bis25 vulcanizing agent is less than 2%, and the rubber maintains high ductility, allowing it to stretch synchronously with the expansion of the internal cells.

[0027] S5. Synchronous heating and vulcanization: After the foaming time is reached, the mold core is heated at a rate of 3℃ / min, and the upper and lower heating plates are heated at a rate of 2℃ / min. After the mold core reaches 170℃, it is maintained for 30 seconds. After the upper and lower mold temperatures reach 170℃ and the overall temperature is uniform, the vulcanization timer is started and the temperature is maintained for 15 minutes. During this stage, the rubber compound enters the rapid cross-linking zone of the double 25 vulcanizing agent. A small amount of undecomposed azodicarbonamide uniformly generates gas, and cell growth occurs simultaneously with the cross-linking of the rubber compound, gradually solidifying the cell walls. After reaching the set holding time, the PLC cuts off the power to all heating units. The silicone foaming mechanism evolves as follows... Figure 3 As shown.

[0028] S6. Cooling and post-processing: Pass room temperature cooling water into the cooling channel built into the mold. After the overall temperature of the mold drops below 50℃, open the mold, take out the product and remove the burrs from the mold seam. Place the product into an oven with forced hot air circulation, set the temperature to 180℃ and keep it at that temperature for 3 hours for secondary vulcanization. After the heat preservation is completed, turn off the heating and let it cool to room temperature with the oven to obtain the finished product.

[0029] Example 2: As Figure 4 As shown. This embodiment prepares a 50mm thick foamed silicone shock absorber block using a simultaneous heating and vulcanization process. The difference from Example 1 is the parameter adjustment: S1. In the mixing stage, the amount of double 25 vulcanizing agent added is 4 parts, and the amount of composite azo foaming agent added is 4.5 parts. The foaming main body of the composite azo foaming agent is azodicarbonamide, and it is compounded with the foaming activator N'-((2-methylpyrimidinyl)amino)-N,N-dimethylformamide. S2. Temperature control parameters: Target core temperature during foaming stage: 135℃; target temperature for upper and lower heating plates: 55℃; foaming and heat preservation time: 600s; cavity pressure set at 40kg / cm³. 2 During the vulcanization stage, the target temperature of the mold core is 175℃, the heating rate is 2℃ / min, the target temperature of the upper and lower heating plates is 175℃, the heating rate is 1.5℃ / min, and the vulcanization holding time is 20min. S4. During the foaming stage, a temperature gradient of about 1.6°C / mm is formed along the 50mm wall thickness; S5. After the mold core is heated up to 175°C and stably maintained for 30s, the vulcanization timing is started; S6. The post-vulcanization is set to hold at 170°C for 4 hours, followed by furnace cooling. The remaining operation steps are completely consistent with those in Example 1.

[0030] Example 3: As shown Figure 4 below. In this example, a thin foamed silicone buffer sheet with a wall thickness of 10mm is prepared, and a vulcanization process with constant temperature of the mold wall and only heating of the mold core is adopted. The differences from Example 1 are as follows: S2. Temperature control parameters: the foaming heat preservation duration is 300s, and the cavity pressure is set to 35kg / cm 2 ; during the vulcanization stage, the upper and lower heating plates maintain a constant temperature of 60°C throughout the whole process, only the basic heat preservation power is retained, and no active heating is performed; the target temperature of the mold core is 165°C, the heating rate is 4°C / min, and the vulcanization heat preservation duration is 20min; S5. After the foaming stage, the mold core is heated up to 165°C at a rate of 4°C / min, stably maintained for 30s and then timing is started, followed by heat preservation for 20min. Through the thermal conduction of the rubber material itself, the temperature of the rubber material close to the mold wall reaches above 155°C to complete the basic cross-linking and shaping, which can ensure no deformation during demolding; S6. The post-vulcanization is set to hold at 180°C for 4 hours, followed by furnace cooling, and the surface cross-linking degree is supplemented through the post-vulcanization. The remaining operation steps are consistent with those in Example 1.

[0031] Comparative Example 1: This comparative example adopts the existing integral uniform-temperature heating compression foaming process. The compounded rubber formula, product specifications and post-treatment processes are all completely consistent with those in Example 1; after mold clamping, the ceramic heating rods and the upper and lower heating plates are synchronously controlled to jointly heat up to 170°C at a rate of 3°C / min, no temperature difference is constructed throughout the whole process, and heat preservation is carried out for 15min; the remaining steps of cooling, trimming and post-vulcanization are consistent with those in Example 1. After mold clamping, the ceramic heating rods and the upper and lower heating plates are synchronously controlled to jointly heat up to 170°C at a rate of 3°C / min, no temperature difference is constructed throughout the whole process, and heat preservation is carried out for 15min; the remaining steps of cooling, trimming and post-vulcanization are consistent with those in Example 1.

[0032] Performance test: 100 molded products are taken from each of Examples 1 to 3 and Comparative Example 1 for testing. The evaluation rule is that a product is judged as qualified if there are no appearance defects such as scratches, insufficient glue, bubbling and delamination; for the cell pore size, the cross section is photographed by a scanning electron microscope, and 100 cells are counted to calculate the average pore size and the pore size variation coefficient; the foaming ratio is the ratio of the density of the solid rubber material to the density of the foamed product; the surface cross-linking degree is determined by the xylene extraction method. The test results are shown in the following table: Group Appearance yield Average pore size Pore ​​size variation coefficient Foaming ratio Surface cross-linking degree Example 1 96% 120μm 7.2% 2.0 92% Example 2 92% 180μm 9.5% 2.3 90% Example 3 89% 100μm 10.1% 1.9 88% Comparative Example 1 68% 210μm 22.7% 1.7 91% The above embodiments are only used to illustrate the technical ideas and implementation methods of this application. The scope of protection of this application is not limited to the above parameters. Adaptive adjustments to the temperature gradient and heat preservation time based on the actual structure and wall thickness of the product are all within the scope of protection of this application.

Claims

1. A method for molding solid silicone with independently controlled temperature gradient, characterized in that, The raw materials for the solid compounded silicone rubber include methyl vinyl silicone rubber raw rubber, 25% vulcanizing agent, and azo foaming agent; the rapid crosslinking temperature of the 25% vulcanizing agent is ≥170℃, and the rapid decomposition temperature of the azo foaming agent is ≥130℃; the molding method includes a foaming stage and a vulcanization and setting stage performed sequentially: Foaming stage: After the mold is closed and pressurized, the core temperature is independently controlled at 130℃~140℃, and the mold wall temperature is independently controlled at 55℃~65℃, along the wall thickness of the rubber compound in the cavity. A temperature gradient is formed with higher temperatures on the inside and lower temperatures on the outside, and the temperature is maintained for 300-600 seconds. The rubber material near the mold core reaches the decomposition temperature of the foaming agent first and produces gas, while the temperature of the rubber material near the mold wall is lower than the rapid decomposition temperature of the foaming agent and has not reached the rapid cross-linking temperature of the vulcanizing agent, thus maintaining plasticity. In the vulcanization and shaping stage, the mold core is heated to 165℃-175℃ so that the overall temperature of the rubber material reaches the rapid cross-linking temperature of the double 25 vulcanizing agent. The temperature is maintained until the rubber material cross-links and shapes, and then the temperature is lowered and the mold is removed. The product is then vulcanized twice to obtain the foamed silicone finished product.

2. The method for molding solid silicone with independently controlled temperature gradient according to claim 1, characterized in that, The solid compounded silicone rubber is prepared by the following steps: placing raw methyl vinyl silicone rubber in a two-roll mill, controlling the roll temperature at 18℃~22℃, adding 0.5%~5% of a double 25 vulcanizing agent by weight of the raw rubber, and mixing for 5min~10min; then adding 0.5%~5% of an azo foaming agent by weight of the raw rubber, mixing for 5min~10min, and extruding the compounded rubber into sheets; cutting the compounded rubber into sheets of corresponding sizes, with a sheet thickness of 1 / 3~2 / 3 of the corresponding wall thickness of the cavity, wrapping the mold core, and then closing the mold.

3. The method for molding and foaming solid silicone with independent temperature gradient control according to claim 1, characterized in that, During the foaming stage, the core temperature is controlled at 130℃, the mold wall temperature is controlled at 60℃, the holding time is 300s~600s, and the cavity pressure after mold closing is 10~50kg / cm². 2 .

4. The method for molding and foaming solid silicone with independent temperature gradient control according to claim 1, characterized in that, During the vulcanization and shaping stage, the mold core is heated to 170°C at a rate of 2°C / min to 4°C / min, and the vulcanization timer is started after the temperature is stabilized for 30 seconds.

5. The method for molding and foaming solid silicone with independent temperature gradient control according to claim 4, characterized in that, During the vulcanization and setting stage, the upper and lower molds are heated simultaneously at a rate of 1.5℃ / min to 3℃ / min to 165℃ to 175℃, and held at that temperature for 10min to 20min, so that the rubber material can be heated together with the mold core to complete the cross-linking. The method is suitable for foamed silicone products with a wall thickness of 10mm to 50mm.

6. The method for molding and foaming solid silicone with independent temperature gradient control according to claim 4, characterized in that, During the vulcanization and shaping stage, the mold wall is maintained at 55℃~65℃, and the mold core is heated to 170℃ and kept at that temperature for 15min~30min. The entire material reaches the cross-linking temperature through its own heat conduction. This method is suitable for foamed silicone products with a wall thickness ≤10mm.

7. The method for molding and foaming solid silicone with independent temperature gradient control according to claim 1, characterized in that, Multiple independent ceramic heating rods are inserted inside the mold core, and each ceramic heating rod is equipped with a thermocouple. The heating power is adjusted by a PLC controller using a PID algorithm. The mold wall temperature is independently controlled by the upper and lower heating plates of the vulcanizing machine. The temperature control parameters corresponding to products with different wall thicknesses are pre-stored in the PLC controller and can be directly called when changing models.

8. The method for molding solid silicone with independently controlled temperature gradient according to claim 1, characterized in that, The secondary vulcanization process is as follows: after demolding and trimming, the product is placed in a hot air environment at 170℃~180℃ for 2h~4h and then cooled in the furnace.

9. The method for molding solid silicone with independently controlled temperature gradient according to claim 1, characterized in that, The azo foaming agent is a composite azo foaming agent, with azodicarbonamide as the main foaming agent and a foaming activating agent; the foaming activating agent is N'-((2-methylpyrimidin-5-yl)amino)-N,N-dimethylformamidinium; the bis25 vulcanizing agent is 2,5-dimethyl-2,5-di-tert-butylperoxyhexane.