Method for additive manufacturing of structured porous materials, porous network components and applications
By combining ice crystal laser 3D printing with cryogenic casting technology, we have achieved the fabrication of porous materials with complex macroscopic structures and controllable micropores, solving the problem of cross-scale control that is difficult to achieve with existing technologies. This technology is suitable for free structure design of various material systems.
Patent Information
- Application Number
- CN202611537122.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-20
AI Technical Summary
Existing additive manufacturing technologies struggle to simultaneously achieve complex macroscopic structures and controllable micropores, and the process is too mild. High-precision laser 3D printing using ice crystals as pore-forming agents has not yet been effectively applied.
Porous materials are prepared by selective laser melting and freezing of solvent-ice crystal composite powder, combined with cryogenic casting technology. The macroscopic and microstructures are controlled by laser scanning path and process parameters, and porous network components are formed after removing solvent ice crystals.
It enables the fabrication of porous materials with multidimensional and cross-scale controllability, and can achieve gradient/heterogeneous distribution of local density, local looseness or pore size within the same material. It is applicable to a variety of material systems and supports the free structural design of novel porous materials.
Smart Images

Figure CN123129444A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of additive manufacturing (3D printing) and porous material preparation technology, specifically relating to an additive manufacturing method for structurally controllable porous materials, porous network components and their applications. Background Technology
[0002] Porous materials, due to their low density, high specific surface area, and unique acoustic, thermal, and electrical properties, have wide applications in biomedicine, adsorption separation, energy storage, and sensing. Existing methods for preparing porous materials mainly include: Freeze casting: This method utilizes solvent solidification and crystallization to displace the solute into pore walls, resulting in a porous material after drying. While this method offers excellent control over micropores, it typically only produces simple block or columnar structures, making it difficult to achieve complex macroscopic three-dimensional shape control. Template method: This method uses a sacrificial template to create pores, but the template removal process is complex, and it's difficult to fabricate thick-walled or closed-pore structures. Conventional 3D printing (FDM / SLA / SLS): While capable of achieving complex macroscopic structures, it's difficult to directly fabricate micron- or nanometer-scale micropores, and SLS typically involves high-temperature sintering, making it unsuitable for many heat-sensitive natural polymers or bioactive materials.
[0003] Current additive manufacturing technologies lack a method that can simultaneously achieve both "arbitrarily complex macroscopic shapes" and "tunable microporous structures" with a mild process. Ice crystals, as a natural, green, and easily removable pore-forming agent, have great potential, but how to perform high-precision laser 3D printing of ice crystal powder like metal powder is a technical challenge that urgently needs to be solved in this field. Summary of the Invention
[0004] The main objective of this invention is to provide an additive manufacturing method for structurally controllable porous materials, porous network components, and their applications, in order to overcome the shortcomings of the prior art.
[0005] To achieve the above-mentioned objectives, the present invention adopts the following technical solution: In a first aspect, the present invention provides an additive manufacturing method for structurally controllable porous materials based on ice crystal laser 3D printing, comprising: A solvent-ice crystal composite powder is provided, wherein a framework material and solvent ice crystals are uniformly distributed inside the solvent-ice crystal composite powder; The solvent-ice crystal composite powder is spread out, and patterned melting scanning and refreezing are performed by selective laser melting in an environment where the temperature is lower than the freezing point of the solvent-ice crystal. After multiple repetitions, a solid ice crystal network template is obtained. Remove the solvent ice crystals from the solid ice crystal network template to obtain a porous network component containing the skeleton material.
[0006] Secondly, the present invention also provides a porous network component prepared by the above-mentioned additive manufacturing method for controllable porous materials.
[0007] Thirdly, the present invention also provides the application of the above-mentioned porous network components in the fabrication of tissue engineering scaffolds, drug sustained-release carriers, flexible sensing aerogels, high-efficiency catalyst carriers, high-efficiency adsorbent materials, electrode materials or sacrificial ice templates.
[0008] Compared with the prior art, the beneficial effects of the present invention include at least the following: This invention enables multi-dimensional, cross-scale controllability of the structure. The macroscopic structure is determined by the laser scanning path (such as a CAD model), allowing the fabrication of complex structures. The micropores are determined by the ice crystal size, solid content, and degree of laser sintering, achieving cross-scale control. By adjusting process parameters, the degree of fusion between particles can be controlled, thereby achieving multi-level control of porous materials without changing the raw materials.
[0009] In particular, this invention endows porous materials with "spatial programmability". By setting different laser parameters for different spatial regions in a single printing, local density, local porosity, or gradient / heterogeneous distribution of random and oriented pores can be achieved at the same internal spatial height of the material.
[0010] The method provided by this invention has strong process technology universality and is applicable to a variety of material systems, which is conducive to the development, research and application of free structure design of novel porous materials.
[0011] The above description is merely an overview of the technical solution of the present invention. In order to enable those skilled in the art to better understand the technical means of this application and to implement it in accordance with the contents of the specification, the preferred embodiments of the present invention are described below in conjunction with detailed drawings. Attached Figure Description
[0012] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0013] Figure 1 A schematic diagram of the overall process flow of the additive manufacturing method for structurally controllable porous materials provided in a typical embodiment of the present invention; Figure 2 A schematic diagram of the laser scanning ice crystal melting process provided in a typical embodiment of the present invention; Figure 3A schematic diagram of the melting and bonding process of the solvent-ice crystal composite powder layer and the solidification and crystallization process between particles during the ice crystal laser freezing 3D process, which is a typical embodiment of the present invention; Figure 4 Electron micrograph of the microstructure of ice crystal composite powder raw material after freeze-drying for laser cryogenic 3D printing of ice crystals, provided as a typical embodiment of the present invention; Figure 5 A schematic diagram illustrating the process of removing solvent from an ice crystal laser cryogenic 3D printed product to obtain a directional pore structure, as provided in a typical embodiment of the present invention; Figure 6 Electron micrograph of the microscopic directional hole structure of an ice crystal laser cryogenic 3D printed component, provided as a typical embodiment of the present invention; Figure 7 A schematic diagram illustrating the fabrication process of a random hole structure for an ice crystal laser cryogenic 3D printed component, as provided in a typical embodiment of the present invention; Figure 8 Electron micrograph of the microscopic random pore structure of an ice crystal laser cryogenic 3D printed component, provided as a typical embodiment of the present invention; Figure 9 An electron microscope image of the microscopic loose and random pore structure of an ice crystal laser cryogenic 3D printed component, provided as a typical embodiment of the present invention; Figure 10 Electron micrographs of the microscopic orientation and random pore heterogeneous distribution of ice crystal laser cryogenic 3D printed components provided as a typical embodiment of the present invention; Figure 11 Electron micrograph of the differential distribution of random pores in the microstructure of an ice crystal laser cryogenic 3D printed component, provided as a typical embodiment of the present invention; Figure 12 This is a macroscopic image of an ice crystal laser cryogenic 3D printed component, provided as a typical embodiment of the present invention. Detailed Implementation
[0014] In view of the shortcomings of the prior art, the inventors of this invention, through long-term research and extensive practice, have proposed the technical solution of this invention. The following will further explain and illustrate this technical solution, its implementation process, and its principles.
[0015] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and therefore the scope of protection of the invention is not limited to the specific embodiments disclosed below.
[0016] The purpose of this invention is to provide an additive manufacturing method for structurally controllable porous materials based on ice crystal laser 3D printing. This method combines the microporous construction capability of cryogenic casting technology with the freeform capability of laser 3D printing. Using solvent ice crystal composite powder as raw material, the material is formed at low temperature through a laser-induced "melting-resolidification" mechanism, and finally, a porous solid is obtained through freeze-drying.
[0017] For the purposes described above, see Figures 1-3 As shown, this embodiment of the invention first provides a method for additive manufacturing of controllable porous materials based on ice crystal laser 3D printing, which includes the following steps: A solvent-ice crystal composite powder is provided, wherein a framework material and solvent ice crystals are uniformly distributed inside the solvent-ice crystal composite powder; The solvent-ice crystal composite powder is spread out, and patterned melting scanning and refreezing are performed by selective laser melting in an environment where the temperature is lower than the freezing point of the solvent-ice crystal. After multiple repetitions, a solid ice crystal network template is obtained. Remove the solvent ice crystals from the solid ice crystal network template to obtain a porous network component containing the skeleton material.
[0018] In some embodiments, the method for preparing the solvent-ice crystal composite powder includes: Prepare a solution or dispersion containing a solvent, the laser absorber, and the framework material; The solution or dispersion is sprayed onto a cryogenic medium with a temperature below its freezing point to form the solvent-ice crystal composite powder.
[0019] In some embodiments, the particle size of the solvent ice crystal composite powder is 10-300 μm. The atomizing device used can be a sprayer, a high-pressure airflow dual-fluid nozzle, or an ultrasonic atomizing nozzle to ensure that the prepared solvent ice crystal composite powder has high sphericity and narrow particle size distribution, thereby improving powder flowability. The cryogenic medium can be liquid nitrogen, liquid argon, or a mixture of dry ice and organic solvent. By adjusting the nozzle orifice diameter (10 μm-300 μm) and jet pressure of the atomizing device, the particle size of the solvent ice crystal composite powder is controlled within the range of 10 μm to 300 μm to match the layer thickness requirements of laser printing.
[0020] Based on the above embodiments, the core technical solution proposed in the typical embodiments of the present invention is a method for additive manufacturing of structurally controllable porous materials based on ice crystal laser 3D printing, including: 1) Raw material preparation (microsphere formation): Unlike traditional cryogenic casting methods, this invention first sprays a solution containing a framework material (solute) into the vicinity of a cryogenic medium (liquid or solid medium) or directly into a cryogenic medium (gaseous cryogenic medium, such as a supercooled atmosphere). During flight, the droplets contract into spheres due to surface tension and are instantly "frozen" and shaped by the cryogenic medium, forming micron-sized spherical solvent-ice crystal composite powders. These powders contain uniformly distributed solute molecules and solvent crystals.
[0021] 2) Low-temperature forming (photothermal micro-fusion): This is carried out in a laser 3D printing equipment. The structure of this laser 3D printing equipment is similar to that of ordinary laser 3D printing equipment, but it is preferable to make some structural modifications to adapt to low temperature. For example, the powder spreading chamber needs to be cooled and temperature controlled, and the powder storage and supply structure also needs to be kept at low temperature to prevent the powder from melting and sticking together, etc. Based on the requirements of low-temperature printing, those skilled in the art are fully capable of making modifications on their own.
[0022] This step utilizes the energy of a laser beam to precisely heat ice crystal powder in specific areas. By controlling the laser energy, the microsphere ice crystal printing material is induced to melt to varying degrees. When the laser spot moves away, the deep cooling of the surrounding environment rapidly dissipates the heat, and the laser-scanned molten area solidifies and crystallizes again. By precisely intervening in this thermodynamic process of "melting-crystallization," a morphology-controllable solid ice crystal network template is constructed in situ while simultaneously shaping the macroscopic form.
[0023] In a low-temperature environment below the solvent melting point (e.g., 20°C to -50°C), solvent-ice crystal composite powder is laid on a forming platform using a powder-laying device. A laser beam is used to selectively scan the powder layer based on the 3D model slice data. The laser energy causes the solvent-ice crystal composite powder in the scanning area to melt in a controlled manner. After the laser is removed, the ambient cooling energy is used to induce the molten pool to re-solidify, or to induce unmelted particles to recrystallize in solid form. This process not only achieves physical bonding between particles, but also constructs a solid ice template with a specific interconnected network morphology in situ by controlling the phase change melting degree of the ice crystal raw material. The "powder-scanning-solidification" process is repeated layer by layer until printing is completed. The unbonded powder is then cleaned to obtain a 3D ice crystal blank.
[0024] 3) Pore Formation and Shaping (Solvent Removal Template): After printing, a solid object is obtained, formed by the accumulation and bonding of ice crystal particles. The solvent ice crystals are removed, and the spaces previously occupied by them become pores, while the solute is retained to form a porous framework.
[0025] In the above preparation process, the control of the hierarchical porous structure is achieved through the following methods: First-level (macrostructure) control: The macro geometry of the material is directly defined by the laser scanning path through the 3D model mesh structure designed by 3D modeling software. The second level (micropore) control: This is achieved by controlling the particle size of the solvent-ice crystal composite powder and the solid content of the precursor solution in step S2, and by combining this with the laser energy density in step S3. The powder particle size and solid content determine the initial characteristics of the micropores, while the laser energy density controls the melting-re-solidification degree and solid recrystallization behavior in the local area of the ice crystals, thereby determining the final size and morphological characteristics of the micropores (such as random or oriented structures). Third-level (connecting porosity) control: By adjusting the energy density of laser scanning, the melting degree of ice crystal particles and the size of the liquid phase neck during the printing process are controlled, thereby regulating the packing density and interconnecting porosity between particles.
[0026] Fourth-level (spatial distribution) control: By setting differentiated laser process parameters (such as power, speed, scanning path or interlayer thickness) in different regions of the three-dimensional model, heterogeneous distribution or gradient change of multi-level pore features at different locations within the same three-dimensional entity can be achieved, including the control of local porosity density and the local switching between directional and random pores.
[0027] In some embodiments, the skeleton material includes any one or more of the following: synthetic polymer materials (such as polyvinyl alcohol PVA, polylactic acid PLA, polycaprolactone PCL, polyurethane TPU, etc.), natural polymer materials (such as chitosan, cellulose, collagen, silk fibroin, etc.), inorganic nanomaterials (such as graphene oxide, carbon nanotubes, nanoclay, etc.), bioceramic powders (such as hydroxyapatite, tricalcium phosphate, etc.), metallic materials (such as stainless steel, titanium alloy, etc.), or drugs and bioactive substances (such as growth factors, botulinum toxin, denitrifying bacteria, etc.).
[0028] In some embodiments, the solvent ice crystal composite powder further includes a laser absorber, which includes any one or more of the following: carbon-based nanomaterials (such as carbon black, carbon nanotubes, graphene, graphene oxide), metal nanoparticles (such as gold, silver, copper, iron nanoparticles), biocompatible dyes (such as indocyanine green, methylene blue), or natural melanin.
[0029] Of course, in this invention, the main function of the laser absorber is to improve the absorption rate of the powder to the laser and promote the printing process. However, this component is not absolutely necessary. If the skeleton material itself has strong laser absorption, it is not necessary to add an additional laser absorber.
[0030] In some implementations, the selective laser melting has a scanning spacing of 20-300 μm, a layup thickness of 20-300 μm, a power of 10-500 W, and a scanning speed of 200-6000 mm / s.
[0031] In some implementations, the interlayer rotation angle of the selected area laser melting is 10-90°.
[0032] In some implementations, the ambient temperature for the selective laser melting is between 10°C and 40°C below the solidification point.
[0033] Furthermore, the present invention does not impose specific limitations on the composition and concentration of the solution. The concentration range of the skeleton material exemplified in the embodiments can be referenced, for example, 1-10 wt%, and the concentration range of the laser absorber can also be referenced, for example, 0.001-2%, but it is not limited thereto. Different concentrations of skeleton material mainly affect porosity and pore size, etc., and can be adjusted appropriately. Moreover, different laser absorbers have different absorption capacities, so their dosage naturally varies greatly. It should not be limited to specific numerical ranges, but should be designed according to actual printing needs and adjusted based on the printing results.
[0034] In some implementations, the method specifically includes the following steps: By adjusting the power density of the selected area laser melting, the melting mode can be adjusted to include any one or a combination of two or more of the following: shallow micro-melting mode, moderate melting and bonding mode, and complete melting and reconstruction mode. Specifically, the shallow micro-melting mode causes only a phase change on the surface of the solvent-ice crystal composite powder to form a liquid film, which is used to form a loose and disordered porous structure. The complete melting and reconstruction mode completely melts the solvent-ice crystal composite powder, which is used to form an ordered porous structure. The moderate melting and bonding mode is between the shallow micro-melting mode and the complete melting and reconstruction mode, which is used to form a dense and disordered structure.
[0035] Specifically, the different modes mentioned above can be categorized as follows: Shallow micro-fusion mode: Low energy density laser is used to cause phase change only on the surface of ice crystal particles to form a thin liquid film, which is then cooled to form a tiny neck connection. This mode preserves the original packing pores between particles and the internal pore structure of particles to the greatest extent, thereby obtaining a loose random pore structure with high interconnected porosity. Moderate melting and bonding mode: Using a medium energy density laser, ice crystal particles are melted to a greater depth, forming a relatively continuous molten pool; subsequently, non-directional solidification occurs during cooling. In this mode, the internal microscopic features of the original ice crystal particles disappear, forming a random porous structure with continuous pore walls and interconnected pores, without obvious orientation. Complete melting reconstruction mode: High energy density laser is used to completely melt the ice crystal particles in the scanning area into a continuous liquid molten pool, which then undergoes directional solidification under the action of ambient cooling. In this mode, the melt fills the gaps between particles, resulting in a significant reduction in interconnected porosity. At the same time, the internal solidification process promotes the formation of directional pore structures in the micropores. Programmatic composite control mode: During a single printing process, the above three modes are switched or combined in real time according to the preset path strategy, thereby creating a spatial distribution containing oriented holes, random holes or loose random holes within the same entity, achieving differentiated customization between different regions.
[0036] In some implementations, the solvent ice crystals in the solid ice crystal network template are removed by any one or more combinations of freeze drying, supercritical drying, and cryogenic solvent replacement.
[0037] Specifically, the desolventizing process for removing solid solvent crystal templates includes any one or more combinations of the following: When using a freeze-drying process, the drying process includes a one-step continuous drying mode or a staged drying mode consisting of a primary drying stage and a secondary drying stage; in the staged drying mode, the primary drying stage is used to directly sublimate and remove more than 90% of the free solvent crystals, the secondary drying stage is used to remove bound solvents or residual solvents, and the framework collapse is prevented by controlling the heating rate; when using a low-temperature solvent replacement process, a low-temperature non-solvent that is miscible with the solid solvent and does not damage the target framework is used as the replacement liquid, and a single or multi-stage gradient soaking extraction is performed in a low-temperature environment that maintains the original solid solvent from melting, followed by evaporation or supercritical extraction at room temperature or under heating conditions to remove the replacement liquid.
[0038] In some implementations, the method further includes the following steps: The step of heat-treating the porous network component to further bond the skeleton material.
[0039] As a typical example of the above technical solution, in actual process applications, the specific execution steps may include: The overall process flow is as follows Figure 1 As shown, it includes the following steps: Step S1: Determining the internal structure of the porous material. Based on application requirements, determine the technical requirements that the porous material needs to meet, design the macroscopic structure and internal pore structure of the porous material, and draw a three-dimensional solid model that can be used for additive manufacturing; Step S2: Based on the technical requirements that the porous material needs to achieve, select the type of porous material, determine the state of the material and its corresponding characteristics according to the preparation process, and prepare a solvent ice crystal composite raw material that can be used for cryo-laser printing. Furthermore, the solvent-ice crystal composite powder raw material mentioned in step S2 is prepared by atomization jet freezing technology, and presents a micron-sized spherical shape. The ice crystal composite powder has high sphericity and is composed of a uniform distribution of solid solvent crystals and framework materials inside. The raw material for this porous material can be in the form of powder or slurry, and its properties can be one or more of the following: polymer materials, inorganic nanomaterials, ceramic materials, metallic materials, or drugs and bioactive substances. To improve the photothermal conversion efficiency of pure water ice crystals and framework materials in subsequent laser printing, a trace amount of laser absorber (such as carbon black, carbon nanotubes, graphene, nano-metal particles, or biocompatible dyes) needs to be uniformly dispersed in the precursor solution to impart efficient light absorption properties to the ice crystal composite powder. The solvent can be water or an organic solvent (such as dimethyl sulfoxide, tert-butanol, camphene, cyclohexane, cyclooctane, dimethyl carbonate, dioxane, etc.). Step S3: The three-dimensional solid model obtained in step S1 is converted into a large number of two-dimensional slices, and the obtained two-dimensional slices are converted into preparation path information and imported into the additive manufacturing equipment. Furthermore, step S3 generates preparation path information including the interlayer rotation angle, scanning interval, and interlayer thickness of two adjacent two-dimensional slices. Specifically, the preparation paths of adjacent two-dimensional slices can be at a certain angle. The interlayer rotation angle is determined according to the required structural design. The optimal interlayer rotation angle used in the preparation of the porous material of this invention is 10-90° to effectively reduce residual thermal stress between layers during the molding process and improve the stability of interlayer bonding. The change in scanning interval can affect the efficiency and quality of additive manufacturing. The optimal scanning interval used in the preparation of the porous material of this invention is 20-300 micrometers. The choice of interlayer thickness affects the pore shape and pore size, and also greatly affects the additive manufacturing speed and quality. When the interlayer thickness is too large, the additive manufacturing speed is fast, but the quality is poor. When the interlayer thickness is too small, the additive manufacturing speed is slow, but the quality is high. The optimal interlayer thickness for the porous material preparation of this invention is 20-300 micrometers.
[0040] Step S4: Set the additive manufacturing parameters, load the solvent ice crystal composite powder raw material obtained in step S2 into the additive manufacturing equipment, select the loading amount as needed, then close the chamber of the additive manufacturing equipment, fill the printing chamber with dry gas, and then start automatic printing. Utilize the laser-induced "fusion-re-solidification" process to construct a solid ice crystal network of a specific shape in situ, and finally obtain a three-dimensional ice crystal blank with a solid solvent template inside.
[0041] Furthermore, the additive manufacturing parameters in step S4 include laser power, scanning speed, etc.; when using the self-developed ice crystal laser 3D printing equipment, the additive manufacturing power in step S4 is 10-500W and the scanning speed is 200-6000mm / s. The laser beam scans the ice crystal composite powder layer according to a preset path. The local heat input generated causes the powder in the scanning area to undergo an instantaneous phase change, forming a tiny molten pool. After the laser is removed, the molten area quickly solidifies using the ambient cold, creating a crystallization neck connection between adjacent ice crystal particles, thereby achieving tight bonding and layer-by-layer solidification between powder particles. Furthermore, in step S4, different types of microporous structures can be obtained by adjusting the laser energy density: when the complete melting and reconstruction mode is used, a directional pore structure is formed; when the surface micro-melting and bonding mode is used, a conventional random pore structure is formed; when the energy density is further reduced, a loose random pore structure is formed. According to the structural design requirements, the three-dimensional model can be divided into different parameter regions, and different laser power, scanning speed and scanning strategy can be assigned to different regions to achieve heterogeneity or gradient distribution of the internal pore features of the printed entity.
[0042] Step S5: Solvent template removal and pore creation. The three-dimensional ice crystal preform obtained in step S4 is subjected to a template removal process while maintaining a low temperature or structural stability to remove solid solvent crystals from the preform. The template removal process includes, but is not limited to, freeze-drying (direct sublimation of solid solvent under vacuum), low-temperature solvent displacement extraction (using non-solvent displacement without damaging the framework or melting the ice crystals), or supercritical drying. As the solid solvent template is removed, the space it originally occupied is precisely converted into micropores, ultimately resulting in a porous material with a multi-level controllable micropore structure determined by the laser printing process.
[0043] This invention also provides porous network components prepared by the above-described additive manufacturing method for controllable porous materials.
[0044] The embodiments of the present invention also provide the application of the above-mentioned porous network components in the fabrication of tissue engineering scaffolds, drug sustained-release carriers, flexible sensing aerogels, high-efficiency catalyst carriers, high-efficiency adsorbent materials, electrode materials or sacrificial ice templates.
[0045] The technical solution of the present invention will be further described in detail below through several embodiments and in conjunction with the accompanying drawings. However, the selected embodiments are only for illustrating the present invention and do not limit the scope of the present invention.
[0046] Example 1 This embodiment illustrates a fabrication process for preparing microscopic directional porous structures using a complete melting and reconstruction mode, as detailed below: (1) Raw materials: Sodium alginate powder and conductive carbon black nanomaterial dispersion are mixed and mechanically stirred evenly to prepare a precursor composite solution with sodium alginate mass fraction of 2% and conductive filler mass fraction of 0.01% (solvent is water).
[0047] (2) Powdering: Using an airflow sprayer, the above precursor solution was sprayed into a cryogenic medium (such as dry ice or liquid nitrogen) at a uniform flow rate of 10 mL / min. The droplets spheroidized and instantly froze due to surface tension before contacting the cryogenic medium, yielding spherical ice crystal composite powder with a particle size of approximately 10-100 μm. To demonstrate its structural morphology, a portion of the ice crystal composite powder was freeze-dried to obtain the following... Figure 4 The electron microscope images shown clearly reveal the structure of the porous framework material.
[0048] (3) Printing: The ice crystal composite powder was loaded into the powder supply chamber of the low-temperature laser printer and scanned using laser parameters with a high energy density. The printing chamber temperature was set to -30°C, and nitrogen gas was used for protection. A 500W fiber laser was used, with the laser power set to 400W, the scanning speed to 4000mm / s, and the layer thickness to 0.3mm. Under this high energy density, the ice crystal particles completely melted to form a continuous liquid molten pool, which underwent directional solidification under the unidirectional heat flow in the cryogenic environment.
[0049] (4) After freeze-drying and removing the solvent, a micro-oriented porous structure with high orientation was obtained.
[0050] The specific process of the above preparation steps can be found in [reference needed]. Figure 5 As shown, the corresponding obtained SEM images of the microstructure are as follows: Figure 6 As shown, a distinct ordered pore structure can be observed.
[0051] Example 2 This embodiment illustrates a fabrication process for preparing conventional random pore structures using a moderate melt-bonding mode, as detailed below: (1) Raw materials and powder preparation: Same as in Example 1.
[0052] (2) Printing: The ice crystal composite powder was loaded into the powder supply chamber of the low-temperature laser printer. The laser energy density was lowered, and scanning was performed using medium energy density parameters. The printing chamber temperature was set to -30°C, and nitrogen gas was used for protection. A 500W fiber laser was used, with the laser power set to 300W, the scanning speed to 4000mm / s, and the layer thickness to 0.3mm. Subsequently, non-directional solidification occurred during the cooling process. In this mode, the ice crystal particles underwent deep melting and formed a relatively continuous molten pool. The internal microscopic features of the original printing material ice crystal composite particles disappeared, forming a random pore structure with continuous pore walls and interconnected pores without obvious orientation.
[0053] (3) Freeze-dry and remove solvent.
[0054] The above process diagram is shown below. Figure 7 As shown, the interparticle gaps shrink moderately, forming a relatively dense conventional random porous structure. The corresponding SEM diagram of the microstructure is shown below. Figure 8 As shown.
[0055] Example 3 This embodiment illustrates a preparation process for a loose, random porous structure using a shallow micro-fusion mode, as detailed below: (1) Raw materials and powder preparation: Same as in Example 1.
[0056] (2) Printing: The ice crystal composite powder is loaded into the toner supply compartment of the low-temperature laser printer to further reduce heat input, using extremely low energy density parameters. The printing compartment temperature is set to -30°C, and nitrogen gas is used for protection. A 500W fiber laser is used, with the laser power set to 200W, a scanning speed of 4000mm / s, and a layer thickness of 0.3mm. At this time, the laser only causes a phase change on the very surface of the ice crystal particles to form a thin liquid film, which then solidifies to form a very small neck connection.
[0057] (3) After freeze-drying, such as Figure 9 As shown, the original packing pores between particles are preserved to the greatest extent, resulting in a microscopic loose and random pore structure with extremely high interconnected porosity.
[0058] Example 4 This embodiment illustrates a preparation process for heterogeneous spatial morphology control (coexistence of oriented and random pores) of porous materials, as detailed below: (1) Raw material preparation: Sodium alginate ice crystal composite powder prepared in the same batch (preparation method refers to Example 1 above) was used as the standard printing raw material.
[0059] (2) Parameter partitioning and printing: In the 3D slicing software, the block model to be printed is divided into region A and region B. In a single printing task, a full melting reconstruction mode is used for region A, with high energy density printing parameters set: laser power 350W, scanning speed 3000mm / s, and layer thickness 0.25mm; for region B, a moderate melting and bonding mode is used, with medium energy density printing parameters set: laser power 200W, scanning speed 3000mm / s, and layer thickness 0.25mm.
[0060] (3) Result verification: After printing, the product is freeze-dried. For example... Figure 10 As shown, region A forms highly oriented micropores with internal crystallization, while region B retains the conventional random pores formed by particle stacking. This embodiment demonstrates that this method can achieve a customized heterogeneous distribution of micropore morphology within the same entity without changing raw materials or interrupting printing, relying solely on spatial parameter programming.
[0061] Example 5 This embodiment illustrates a preparation process for controlling the spatial density heterogeneity of porous materials (differential distribution between loose and conventional random pores), as detailed below: (1) Raw material preparation: Same as in Example 4.
[0062] (2) Parameter partitioning and printing: The block model is divided into region C and region D. While maintaining the random hole generation mechanism, a shallow micro-melting mode is adopted for region C, and the printing parameters are set to extremely low energy density: laser power 150W, scanning speed 6000mm / s, and layer thickness 0.25mm. For region D, a moderate melting and bonding mode is adopted, with laser power set to 250W, scanning speed 5000mm / s, and layer thickness 0.25mm.
[0063] (3) Result verification: After printing, the product is freeze-dried. For example... Figure 11 As shown, region C, due to its extremely low local laser energy density, generates a small liquid phase neck, resulting in loose, random pores with high interconnectivity; while region D, with its moderate energy input, forms relatively dense, conventional random pores. This embodiment demonstrates that by fine-tuning the local heat input, it is possible to achieve a continuous or abrupt distribution of density characteristics within the same macroscopic material.
[0064] Example 6 This embodiment illustrates the preparation process of a sodium alginate conductive adsorption sponge for marine microbial attachment, as detailed below: (1) Solution preparation: Sodium alginate powder and conductive carbon black nanomaterial dispersion are mixed and mechanically stirred to prepare a precursor composite solution with sodium alginate mass fraction of 5% and conductive filler mass fraction of 0.02%.
[0065] (2) Powdering: Using an ultrasonic sprayer, the above precursor solution was sprayed into the cryogenic medium liquid nitrogen at a uniform flow rate of 8 mL / min. The droplets were sphericalized and instantly frozen by surface tension before contacting the cryogenic medium, and spherical ice crystal composite powder with a particle size of about 10-200 μm was collected.
[0066] (3) Printing: The ice crystal composite powder was loaded into the powder supply chamber of the low-temperature laser printer at -30°C. The printing chamber temperature was set to -30°C and filled with nitrogen for protection. A 500W fiber laser was used, with the laser power set to 300W, the scanning speed to 5000mm / s, and the layer thickness to 0.3mm. The scanning was performed according to the preset three-dimensional mesh model. The laser scanning caused the surface of the ice crystal particles to melt slightly and solidify rapidly, stacking them layer by layer to obtain a three-dimensional ice crystal blank.
[0067] (4) Freeze-drying: The printed three-dimensional ice crystal preform is transferred to a freeze dryer and freeze-dried at -50°C and 10Pa vacuum for 48 hours, allowing the solid solvent ice crystals to sublimate directly, yielding a sodium alginate conductive aerogel framework. The porous material prepared using this invention has a preset geometric shape, such as... Figure 12 As shown, its macroscopic shape is defined by a three-dimensional model, and it has the characteristics of structural integrity and surface continuity.
[0068] (5) Crosslinking: In order to prevent the aerogel from collapsing in the aqueous phase, the dried aerogel was immersed in an anhydrous ethanol solution containing anhydrous calcium chloride for 12 hours to crosslink and solidify the sodium alginate molecular chains. Then it was taken out and washed with ethanol and evaporated to dryness.
[0069] (6) Surface modification: The cross-linked aerogel was immersed in a Tris-HCl buffer solution (pH = 8.5) containing dopamine (concentration of 2 mg / mL). The reaction was carried out at room temperature with shaking in the dark for 12-24 hours. Dopamine underwent self-polymerization in a weakly alkaline and aerobic environment, forming a polydopamine (PDA) coating on the inner and outer pore walls of the aerogel. After removal, residual reagents were washed with deionized water and then freeze-dried again.
[0070] (7) Results: The following results were obtained. Figure 12 The image shows a dark-colored conductive adsorbent sponge with a hierarchical, interconnected pore structure. This sponge not only possesses excellent compression resilience and a good conductive network, but its uniformly coated surface with polydopamine provides abundant catechol groups and amino groups, greatly enhancing its hydrophilicity and interfacial adhesion in marine environments. This significantly promotes the rapid attachment and biofilm formation of marine microorganisms, making it an ideal material for marine bioelectrochemical systems (such as anodes in marine microbial fuel cells) and for pollutant adsorption.
[0071] Example 7 This embodiment illustrates the preparation process of a graphene oxide conductive aerogel, as detailed below: (1) Raw materials: 5 mg / mL of graphene oxide (GO) aqueous dispersion was used.
[0072] (2) Powdering: GO ice crystal powder was prepared by high-pressure airflow spraying method, and the particle size was controlled at 100-200μm.
[0073] (3) Printing: The low-temperature printing parameters were adjusted to a laser power of 350W, a scanning speed of 4000mm / s, and a layer thickness of 0.28mm. The higher energy density made the ice crystal particles fuse more tightly, increasing the connectivity of the skeleton.
[0074] (4) Post-treatment: After freeze-drying, high-temperature thermal reduction treatment is carried out.
[0075] (5) Results: Graphene aerogel with a complex lattice structure was obtained, which has ultra-light weight, high conductivity and excellent compression resilience. This is a complex geometric structure that cannot be achieved by traditional mold cryogenic casting.
[0076] Example 8 This embodiment illustrates the preparation process of a controllable structure ice template (for investment casting), as detailed below: (1) Raw materials: pure water, and 0.1wt% of trace carbon black nanopowder as laser absorber, which is ultrasonically dispersed evenly.
[0077] (2) Powder preparation: Carbon-doped ice crystal composite powder is prepared by atomized spray freezing.
[0078] (3) Printing: Using the low-temperature SLM process of the present invention, the ice model of the turbine blade is directly printed. The addition of carbon black enables the ice crystal powder to effectively absorb laser energy and achieve interlayer melting and bonding. By controlling the laser parameters, the surface of the ice mold is made dense and smooth.
[0079] (4) Application: This ice template can be used as a sacrificial template for ceramic slip casting or shell casting processes. The printed ice template, which is in a cryogenic state, is immersed in ceramic slurry pre-cooled to near its freezing point. After the ceramic body solidifies, the internal ice template can be removed by in-situ melting or sublimation to obtain a ceramic shell for metal casting. Compared with traditional lost-wax casting, the ice template method has the advantages of simple demolding process, green and pollution-free, and low cost. In addition, the trace amount of carbon black absorbent added to the printing material will be completely oxidized and volatilized during the subsequent high-temperature sintering of the ceramic shell, without introducing any impurities or defects into the final metal casting.
[0080] It should be understood that the above embodiments are merely illustrative of the technical concept and features of the present invention, and are intended to enable those skilled in the art to understand the content of the present invention and implement it accordingly. They should not be construed as limiting the scope of protection of the present invention. All equivalent changes or modifications made in accordance with the spirit and essence of the present invention should be covered within the scope of protection of the present invention.
Claims
1. A method for additive manufacturing of structurally controllable porous materials based on ice crystal laser 3D printing, characterized in that, include: A solvent-ice crystal composite powder is provided, wherein a framework material and solvent ice crystals are uniformly distributed inside the solvent-ice crystal composite powder; The solvent-ice crystal composite powder is spread out, and patterned melting scanning and refreezing are performed by selective laser melting in an environment where the temperature is lower than the freezing point of the solvent-ice crystal. After multiple repetitions, a solid ice crystal network template is obtained. Remove the solvent ice crystals from the solid ice crystal network template to obtain a porous network component containing the skeleton material.
2. The additive manufacturing method for structurally controllable porous materials according to claim 1, characterized in that, The preparation method of the solvent-ice crystal composite powder includes: Prepare a solution or dispersion containing a solvent, the laser absorber, and the framework material; The solution or dispersion is sprayed onto a cryogenic medium with a temperature below its freezing point to form the solvent-ice crystal composite powder.
3. The additive manufacturing method for structurally controllable porous materials according to claim 1, characterized in that, The particle size of the solvent ice crystal composite powder is 10-300 μm.
4. The additive manufacturing method for structurally controllable porous materials according to claim 1, characterized in that, The skeleton material includes any one or a combination of two or more of the following: synthetic polymer materials, natural polymer materials, inorganic nanomaterials, bioceramic powders, metallic materials, drugs and bioactive substances. And / or, the solvent ice crystal composite powder further includes a laser absorber, which includes any one or a combination of two or more of carbon-based nanomaterials, metal nanoparticles, dyes or natural pigments.
5. The additive manufacturing method for structurally controllable porous materials according to claim 1, characterized in that, The selective laser melting has a scanning interval of 20-300μm, a layer thickness of 20-300μm, a power of 10-500W, and a scanning speed of 200-6000mm / s. And / or, the interlayer rotation angle of the selected area laser melting is 10-90°; And / or, the ambient temperature of the selected area laser melting is between 10°C and 40°C below the solidification point.
6. The additive manufacturing method for structurally controllable porous materials according to claim 1, characterized in that, Specifically, it includes: By adjusting the power density of the selected area laser melting, the melting mode can be adjusted to include any one or a combination of two or more of the following: shallow micro-melting mode, moderate melting and bonding mode, and complete melting and reconstruction mode. Specifically, the shallow micro-melting mode causes only a phase change on the surface of the solvent-ice crystal composite powder to form a liquid film, which is used to form a loose and disordered porous structure. The complete melting and reconstruction mode completely melts the solvent-ice crystal composite powder, which is used to form an ordered porous structure. The moderate melting and bonding mode is between the shallow micro-melting mode and the complete melting and reconstruction mode, which is used to form a dense and disordered structure.
7. The additive manufacturing method for structurally controllable porous materials according to claim 1, characterized in that, The methods for removing solvent ice crystals from the solid ice crystal network template include any one or more combinations of freeze drying, supercritical drying, and low-temperature solvent replacement.
8. The additive manufacturing method for structurally controllable porous materials according to claim 1, characterized in that, Also includes: The step of heat-treating the porous network component to further bond the skeleton material.
9. A porous network component manufactured by the additive manufacturing method of structurally controllable porous materials according to any one of claims 1-8.
10. The application of the porous network component of claim 9 in the fabrication of tissue engineering scaffolds, drug sustained-release carriers, flexible sensing aerogels, high-efficiency catalyst carriers, high-efficiency adsorbent materials, electrode materials, or sacrificial ice templates.