A process for producing a regionally differentiated carbon fiber reinforced nylon material component

By employing a dual-layer design consisting of a core reinforcement layer and a surface impregnation layer, combined with 3D printing and impregnation processes, the problems of fiber gaps and interlayer delamination in complex automotive parts have been solved, enabling efficient and low-cost production that meets the strength requirements of different components.

CN123129459APending Publication Date: 2026-11-20HEZE BAIGANG NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611386694.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-01-12
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies suffer from fiber gaps and interlayer delamination defects when printing complex automotive parts. The printing speed is insufficient to meet the needs of large-scale production, and the strength of the finished product cannot be adjusted, increasing the research and development cycle and costs.

Method used

The design employs a dual-layer synergistic approach, consisting of a core reinforcement layer and a surface impregnation layer. Through a combination of 3D printing and impregnation processes, the core reinforcement layer is printed by mixing a nylon matrix with carbon fiber, while the surface impregnation layer is formed by impregnating carbon fiber into a nylon matrix. The overlapping layers are interwoven, and parameters are adjusted according to sections during the printing process. The impregnation is followed by curing.

Benefits of technology

It improves interlayer bonding, avoids stress concentration, enhances tensile strength, flexural strength and interlayer peel strength, simplifies the process, adapts to the differentiated needs of different components, improves production efficiency and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123129459A_ABST
    Figure CN123129459A_ABST
Patent Text Reader

Abstract

The present application belongs to the field of fiber reinforced nylon material additive-impregnation composite manufacturing technology, and particularly relates to a production process of a regionally differentiated carbon fiber reinforced nylon material part, which adopts a double-layer collaborative design of a core reinforcing layer and a surface impregnation layer in structure, so that the tensile strength, bending strength and interlayer peeling strength are improved; in the production process, 3D printing is combined with impregnation, and only nylon material is printed in the surface transition zone, so that the carbon fiber is impregnated into the nylon matrix, the process flow is simplified, the parameter control difficulty is reduced, the multi-layer material switching and complex path planning are omitted, and the thickness of each layer can be adjusted according to the requirements of the part, so as to adapt to the differentiated requirements of different parts of the automobile.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent application filed on January 12, 2026, with application number 202610032902.6 and invention title "A Production Process for Carbon Fiber Reinforced Nylon Material". Technical Field

[0002] This invention belongs to the field of additive-impregnation composite manufacturing technology of fiber-reinforced nylon materials, specifically relating to a production process for regionally differentiated carbon fiber reinforced nylon material components. Background Technology

[0003] With the rapid development of the automotive industry towards lightweighting and high performance, carbon fiber-nylon composite materials, due to their advantages of both high strength and low weight, have become the preferred material for core components such as automotive body structures, frames, and seat frames. 3D printing technology, with its customized molding capabilities, has made efficient manufacturing of carbon fiber-nylon composite automotive parts possible. Specifically, the "nylon layer, nylon-carbon fiber composite layer, carbon fiber layer" stacked structure and its accompanying multi-layer printing algorithm proposed in CN118493846A achieves continuous carbon fiber composite molding through simultaneous multi-material layer printing, demonstrating significant application value in the mass production of standardized parts.

[0004] However, when the above-mentioned technologies are applied to actual production in the automotive field, there are still many shortcomings: First, automotive parts often contain complex structures such as irregular curved surfaces and hollow cavities. When printing such parts using the CN118493846A method, the program settings are complicated, and defects such as fiber gaps and interlayer delamination are easily caused by errors in material switching between layers. At the same time, in order to avoid carbon fiber breakage, the printing speed must be strictly controlled in the low-speed range, which is difficult to meet the efficiency requirements of large-scale production of automotive parts.

[0005] Furthermore, the enhanced strength of CN118493846A material depends on the material layer ratio and slicing parameters preset before printing. Once the slicing is determined, the strength of the finished product cannot be adjusted. Different automotive parts (such as body anti-collision beams and interior brackets) have significantly different strength requirements, so slicing programs need to be developed separately for different parts, which increases the R&D cycle and cost. Summary of the Invention

[0006] In view of the problems in the background art, the present invention provides a production process for regionally differentiated carbon fiber reinforced nylon material components.

[0007] The technical solution of the present invention is as follows: The present invention provides a carbon fiber reinforced nylon material, comprising an internal core reinforcement layer and a surface impregnation layer encapsulating the core reinforcement layer; The core reinforcement layer is printed from a mixture of nylon matrix and carbon fiber. The surface impregnation layer is formed by impregnating carbon fibers into a nylon matrix; The surface impregnation layer and the core reinforcement layer have overlapping layers at the interface.

[0008] Furthermore, the carbon fiber length in the core reinforcement layer is 0.5-2mm, the carbon fiber mass fraction is 15%-40%, and the filling density is 70%-80%.

[0009] The thickness ratio of the overlapping layer of the surface impregnation layer and the core reinforcement layer to that of the surface impregnation layer is 0.18-0.25:1.

[0010] The carbon fiber in the surface impregnation layer has a length of 0.5-2 mm and a carbon fiber mass fraction of 15%-40%.

[0011] The present invention also provides a production process for the carbon fiber reinforced nylon material, comprising the following steps: (1) Load the nylon printing filament into the main feed channel of the 3D printing equipment and the carbon fiber into the hopper of the side feed device of the 3D printing equipment; The 3D model to be printed is imported into the slicing software, the core reinforcement zone and the surface transition zone are divided, and the printing parameters are set. The core reinforcement zone uses a dual feeding mode of nylon and carbon fiber, while the surface transition zone uses only a single feeding mode of nylon. The carbon fiber feeding device is turned off. Printing is then performed to obtain the blank. (2) Mix carbon fiber and nylon hot melt adhesive in a certain proportion and stir to make a uniform carbon fiber slurry; The dried blank is completely immersed in carbon fiber slurry, and the impregnated blank is heated and cured, and then cooled to obtain the final product.

[0012] Regarding the printing parameters, the printing speed of the core reinforcement area in step (1) is 25-35 mm / s, and the printing speed of the surface transition area is 50-60 mm / s.

[0013] Based on the above production process, the nozzle temperature is 250-270℃.

[0014] Furthermore, in step (2), the carbon fiber slurry has a carbon fiber length of 1-2 mm and a carbon fiber mass fraction of 25%-40%.

[0015] During step (2) impregnation, the vacuum is drawn to -0.08~-0.1MPa, and the impregnation time is 30-60 minutes.

[0016] Step (2) The heating and curing temperature is 100-120℃ and the time is 2-4 hours.

[0017] Beneficial effects The carbon fiber reinforced nylon material provided by this invention adopts a two-layer synergistic design of "core reinforcement layer and surface impregnation layer". The core reinforcement layer is made by printing a mixture of nylon matrix and carbon fiber to form a stable load-bearing skeleton. The surface impregnation layer completely wraps the core reinforcement layer, in which carbon fiber is impregnated to fill the gaps in the nylon matrix, forming a secondary reinforcement. This not only strengthens the interlayer bonding force and avoids the stress concentration problem that is prone to occur in a single printing layer, but also works synergistically with the core reinforcement layer to improve tensile strength, flexural strength and interlayer peel strength.

[0018] The production process provided by this invention combines 3D printing with impregnation. Only nylon material is printed in the surface transition area, and carbon fiber is immersed into the nylon matrix through impregnation. The process is simplified, the difficulty of parameter control is reduced, and the need for multi-layer material switching and complex path planning is eliminated. Moreover, the thickness of each layer can be adjusted according to the needs of the component, adapting to the differentiated needs of different parts of the automobile (load-bearing components, lightweight components). Attached Figure Description

[0019] Figure 1 This is a structural schematic diagram of a carbon fiber reinforced nylon material provided by the present invention.

[0020] The attached figures are labeled as follows: 1-Core reinforcement layer; 2-Surface impregnation layer. Detailed Implementation

[0021] The following examples are intended to illustrate the present invention, and not to further limit the invention.

[0022] This invention provides a carbon fiber reinforced nylon material, such as Figure 1 As shown, it includes an internal core reinforcement layer 1 and a surface impregnation layer 2 that wraps around the core reinforcement layer 1; the total thickness is 5.5-10 mm; The core reinforcement layer 1 is printed from a mixture of nylon matrix and carbon fiber. The surface impregnation layer 2 is formed by impregnating carbon fibers into a nylon matrix; The surface impregnation layer and the core reinforcement layer have overlapping layers at the interface.

[0023] Furthermore, the core reinforcement layer 1 has a thickness of 5-8 mm, a carbon fiber length of 0.5-2 mm, preferably 0.5-1 mm, a carbon fiber mass fraction of 15%-40%, preferably 15%-30%, and a filler density of 70%-80%.

[0024] The thickness ratio of the overlapping layer of the surface impregnation layer 2 and the core reinforcement layer 1 to that of the surface impregnation layer 2 is 0.18-0.25:1.

[0025] The carbon fiber in the surface impregnation layer 2 has a length of 0.5-2 mm, preferably 1-2 mm, and a carbon fiber mass fraction of 15%-40%, preferably 25%-40%.

[0026] The carbon fiber reinforced nylon material provided by this invention adopts a two-layer synergistic design of "core reinforcement layer and surface impregnation layer". The core reinforcement layer is made by printing a mixture of nylon matrix and carbon fiber to form a stable load-bearing skeleton. The surface impregnation layer completely wraps the core reinforcement layer, in which carbon fiber is impregnated to fill the gaps in the nylon matrix, forming a secondary reinforcement. This not only strengthens the interlayer bonding force and avoids the stress concentration problem that is prone to occur in a single printing layer, but also works synergistically with the core reinforcement layer to improve tensile strength, flexural strength and interlayer peel strength.

[0027] The present invention also provides a production process for the aforementioned carbon fiber reinforced nylon material, comprising the following steps: (1) Load the nylon printing filament into the main feed channel of the 3D printing equipment and the carbon fiber into the hopper of the side feed device of the 3D printing equipment; The 3D model to be printed is imported into the slicing software, the core reinforcement zone and the surface transition zone are divided, and the printing parameters are set. The core reinforcement zone uses a dual feeding mode of nylon and carbon fiber, while the surface transition zone uses only a single feeding mode of nylon. The carbon fiber feeding device is turned off. Printing is then performed to obtain the blank.

[0028] In terms of 3D printing material selection, nylon printing filaments can be PA6 or PA66 filaments with diameters of 1.75mm / 2.85mm, and they should be dried.

[0029] The carbon fiber is preferably 0.5-1 mm in length and is subjected to drying and impurity removal treatment.

[0030] The 3D printing equipment is equipped with a carbon fiber precision feeder and a screw-reinforced extruder. The feeder speed control accuracy is ±0.1mm / s, and the extruder shear rate is ≥50s. -1 This ensures that the feeding speed matches the extrusion speed, preventing carbon fiber accumulation or uneven dispersion.

[0031] Regarding the printing parameters, the printing speed of the core reinforcement zone is 25-35 mm / s, the carbon fiber mass fraction is set to 15%-30% according to the component requirements, the fill density is 70%-80%, the layer thickness is 0.2 mm, and the interlayer overlap rate is 15%; the printing speed of the surface transition zone is 50-60 mm / s, the fill density is 30%-40%, the layer thickness is 0.2 mm, and the surface roughness is preset to 2.0-3.0 μm.

[0032] The nozzle temperature is 250-270℃, and the heated bed temperature is 80℃.

[0033] The nozzle filament output status is monitored in real time during printing to avoid filament breakage and overflow defects. The feeding status is automatically switched according to the zone during printing. In addition, the printing speed gradually increases from 35mm / s to 50mm / s in the bonding layer between the core reinforcement zone and the surface transition zone to avoid poor interlayer bonding caused by sudden speed changes.

[0034] The surface transition zone is printed with only nylon material, and the printing speed is higher than that of the core reinforcement zone. This not only improves printing efficiency but also produces controllable porosity, which is beneficial for subsequent carbon fiber impregnation.

[0035] After printing the blank, the surface burrs are lightly sanded off and then dried.

[0036] (2) Mix carbon fiber and nylon hot melt adhesive in a certain proportion and stir to make a uniform carbon fiber slurry; The dried blank is completely immersed in carbon fiber slurry, and the impregnated blank is heated and cured, and then cooled to obtain the final product.

[0037] Furthermore, in step (2), the carbon fiber slurry has a carbon fiber length of 1-2 mm and a carbon fiber mass fraction of 25%-40%.

[0038] In step (2), the vacuum is drawn to -0.08~-0.1MPa and the impregnation time is 30-60 minutes. The impregnation time directly affects the depth of carbon fiber immersion into the nylon matrix. Therefore, the impregnation time can be adjusted as needed. For example, the impregnation time for load-bearing parts is 60 minutes and the impregnation time for non-load-bearing parts is 30 minutes, so that the carbon fiber slurry can fully penetrate into the blank.

[0039] After impregnation, remove excess slurry from the surface and place in an oven to heat and cure.

[0040] Preferably, the heating and curing temperature in step (2) is 100-120℃ and the time is 2-4 hours.

[0041] After the curing process, the blank is cooled to room temperature, and the surface is finely ground as needed to obtain the finished product.

[0042] After fine grinding, the surface roughness of the finished product is ≤0.8μm, and the finished product is suitable for components such as automotive anti-collision beams, interior brackets, vehicle frames, and seat frames.

[0043] The production process provided by this invention combines 3D printing with impregnation. Only nylon material is printed in the surface transition area, and carbon fiber is immersed into the nylon matrix through impregnation. The process is simplified, the difficulty of parameter control is reduced, and the need for multi-layer material switching and complex path planning is eliminated. Moreover, the thickness of each layer can be adjusted according to the needs of the component, adapting to the differentiated needs of different parts of the automobile (load-bearing components, lightweight components).

[0044] Example 1 This embodiment provides a manufacturing process for carbon fiber reinforced nylon material used in automotive anti-collision beams, including: (1) Raw material preparation PA66 nylon printing filament, 1.75mm in diameter, dried at 80℃ for 2 hours before use; Carbon fiber for printing the core reinforcement area with a length of 0.8 mm is dried and cleaned before use. Impregnated carbon fibers with a length of 1.5 mm are dried and cleaned before use.

[0045] (2) 3D printed blank PA66 printing filament is loaded into the main feed channel, and carbon fiber for printing the core reinforcement area is loaded into the side feeder hopper.

[0046] Import the 3D model of the sample block into the slicing software, and divide it into a core reinforcement zone and a surface transition zone: the core reinforcement zone thickness is 8mm, and the surface transition layer thickness is set to 1.0mm, with the boundary being an inward offset of 1.0mm from the outer surface of the model, and the inner side being the core reinforcement zone; set the printing parameters: the core reinforcement zone uses a dual-feed mode of nylon and carbon fiber, with a carbon fiber mass fraction of 28%, a fill density of 75%, and a printing speed of 30mm / s; the surface transition zone uses a single-feed mode of nylon, with a fill density of 35% and a printing speed of 55mm / s; uniform layer thickness is 0.2mm, and the interlayer overlap rate is 15%. Preheat the nozzle to 260℃ and the heated bed to 80℃, and maintain the temperature for 30 minutes.

[0047] When the printing program is started, the nylon filaments melt and are evenly mixed with the carbon fiber by the screw shearing during the printing of the core reinforcement area. The carbon fiber feeding is automatically turned off during the printing of the surface transition area. After printing, the hot bed is kept at a constant temperature for 30 minutes and then naturally cooled to room temperature. The surface burrs are lightly polished and dried at 80°C for 1 hour to obtain the sample blank.

[0048] (3) Vacuum impregnation and curing Mix 35% carbon fiber by mass with nylon hot melt adhesive and stir for 30 minutes at 3000 rpm using a high-speed mixer to prepare a uniform carbon fiber slurry without sediment.

[0049] After drying, fix the blank in the impregnation rack, put it into the vacuum impregnation tank, pour in the slurry to completely immerse the blank, draw a vacuum to -0.09MPa, and maintain the impregnation time for 60 minutes.

[0050] Remove the blank, scrape off the excess slurry on the surface, put it into an oven, heat at 110℃ for 3 hours to complete the curing; after cooling to room temperature, finely grind the surface to a roughness of ≤0.8μm to obtain the finished sample block with a thickness of 9mm.

[0051] Analysis of the experimental slices revealed that the thickness ratio of the overlapping layer of the surface impregnation layer 2 and the core reinforcement layer 1 to that of the surface impregnation layer 2 was approximately 0.23:1.

[0052] Comparative Example 1 Using 3D printing technology, a sample of the three-layer cyclic overprinted structure of "nylon layer, nylon carbon fiber composite layer, and carbon fiber layer" disclosed in patent CN118493846A was prepared. The thickness of a single cycle was 0.9 mm, with the nylon layer being 0.1 mm, the nylon carbon fiber composite layer 0.6 mm, and the carbon fiber layer 0.2 mm. A total of 10 cycles were performed, and the overall carbon fiber content was controlled to be comparable to that in Example 1.

[0053] Example 2 This embodiment provides a manufacturing process for carbon fiber reinforced nylon material used in automotive interior brackets, including: (1) Raw material preparation PA66 nylon printing filament, 1.75mm in diameter, dried at 80℃ for 2 hours before use; Carbon fiber for printing the core reinforcement area with a length of 0.5 mm is dried and cleaned before use. Impregnated carbon fibers with a length of 1 mm are dried and cleaned before use.

[0054] (2) 3D printed blank PA66 printing filament is loaded into the main feed channel, and carbon fiber for printing the core reinforcement area is loaded into the side feeder hopper.

[0055] Import the 3D model of the sample block into the slicing software, and divide it into a core reinforcement zone and a surface transition zone: the core reinforcement zone thickness is 5mm, and the surface transition layer thickness is set to 0.8mm, with the boundary offset inward from the outer surface of the model by 0.8mm, the inner side being the core reinforcement zone; set the printing parameters: the core reinforcement zone uses a dual-feed mode of nylon and carbon fiber, with a carbon fiber mass fraction of 18%, a fill density of 70%, and a printing speed of 25mm / s; the surface transition zone uses a single-feed mode of nylon, with a fill density of 30% and a printing speed of 50mm / s; uniform layer thickness is 0.2mm, and the interlayer overlap rate is 15%. Preheat the nozzle to 260℃ and the heated bed to 80℃, and maintain the temperature for 30 minutes.

[0056] When the printing program is started, the nylon filaments melt and are evenly mixed with the carbon fiber by the screw shearing during the printing of the core reinforcement area. The carbon fiber feeding is automatically turned off during the printing of the surface transition area. After printing, the hot bed is kept at a constant temperature for 30 minutes and then naturally cooled to room temperature. The surface burrs are lightly polished and dried at 80°C for 1 hour to obtain the sample blank.

[0057] (3) Vacuum impregnation and curing Mix 25% of the impregnating carbon fiber with nylon hot melt adhesive and stir for 30 minutes at 3000 rpm using a high-speed mixer to prepare a uniform carbon fiber slurry without sedimentation.

[0058] After drying, fix the blank in the impregnation rack, put it into the vacuum impregnation tank, pour in the slurry to completely immerse the blank, draw a vacuum to -0.08MPa, and maintain the impregnation time for 30 minutes.

[0059] Remove the blank, scrape off the excess slurry on the surface, put it into an oven, heat at 100℃ for 2 hours to complete the curing; after cooling to room temperature, finely grind the surface to a roughness of ≤0.8μm to obtain the finished sample block with a thickness of 5.8mm.

[0060] Analysis of the experimental slices revealed that the thickness ratio of the overlapping layer of the surface impregnation layer 2 and the core reinforcement layer 1 to that of the surface impregnation layer 2 was approximately 0.20:1.

[0061] Comparative Example 2 Using 3D printing technology, a sample of the three-layer cyclically overprinted structure of "nylon layer, nylon carbon fiber composite layer, and carbon fiber layer" disclosed in patent CN118493846A was prepared. The thickness of a single cycle was 0.58 mm, with the nylon layer being 0.08 mm, the nylon carbon fiber composite layer 0.3 mm, and the carbon fiber layer 0.2 mm. A total of 10 cycles were performed, and the overall carbon fiber content was controlled to be comparable to that in Example 2.

[0062] Experimental results The finished products of Examples 1 and 2 and Comparative Examples 1 and 2 were subjected to the following performance tests, and the results are shown in Table 1.

[0063] Tensile strength and flexural strength shall be performed in accordance with GB / T 1040.1-2025, impact strength shall be performed in accordance with GB / T 1843-2008, interlaminar shear strength shall be performed in accordance with GB / T 1450.1-2005, and surface roughness shall be performed in accordance with GB / T 1031-2009.

[0064] Table 1 Comparison of Performance Test Data As shown in Table 1, the mechanical properties of Examples 1 and 2 are superior to their corresponding counterparts, indicating that the material structure provided by this invention fills the internal pores and interlayer gaps, improving structural density and bonding strength. Examples 1 and 2 also exhibit lower surface roughness because the surface transition layer is a pure nylon structure, and fine grinding after impregnation and curing eliminates fiber exposure defects. Furthermore, the production process of this invention combines 3D printing with impregnation, resulting in higher production efficiency and lower costs.

[0065] Application Example 1 This application example is a specific application of the production process of carbon fiber reinforced nylon material proposed in this invention, based on the above specific embodiments. This process is used to manufacture components with regionally differentiated reinforcement to meet the mechanical design requirements of some special mechanical components. Specifically, in this application example, keeping other steps unchanged, the original process is followed to print out an integral blank containing a core reinforcement area and a surface transition area and prepare carbon fiber slurry. The difference is that before immersing the dried blank into the carbon fiber slurry, the areas that need to be reinforced and the areas that need to remain lightweight are designed in advance based on the CAD model and mechanical simulation results of the component. A flexible or rigid material that does not wet or adhere to nylon hot melt adhesive and is resistant to a certain temperature (above 100°C) is selected as the mask material. The mask is tightly wrapped or coated on the non-reinforced areas of the blank. The blank with the mask is immersed in the slurry and selectively vacuum impregnated. The slurry can only penetrate the areas not covered by the mask. After curing, the mask is removed to obtain the target component with clear performance partitioning.

[0066] Alternatively, based on the CAD model and mechanical simulation results of the component, the areas requiring gradient reinforcement can be designed in advance. Following the original process, an integral blank containing the core reinforcement area and the surface transition area can be printed, and carbon fiber slurry can be prepared. The dried blank is first immersed in the slurry and subjected to overall vacuum impregnation for the first time. After being taken out, rinsed, and dried, a flexible or rigid material that does not wet or stick to nylon hot melt adhesive and can withstand a certain temperature (above 100℃) is selected as the mask material. The mask is tightly wrapped or coated on a local area of ​​the blank. The blank with the mask is then immersed in the slurry and subjected to selective vacuum impregnation for the second time. The slurry is impregnated in different areas in a gradient manner. After curing, the mask is removed to obtain the target component with gradient reinforcement zones.

[0067] Preferably, the mask material can be a PTFE film, a photocurable resin coating, etc.

[0068] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. A manufacturing process for regionally differentiated carbon fiber reinforced nylon material components, characterized in that, Including the following steps: Print out the entire blank containing the core reinforcement area and the surface transition area and prepare carbon fiber slurry. Before immersing the dried blank into the carbon fiber slurry, design the areas that need to be reinforced and the areas that need to be kept lightweight based on the CAD model and mechanical simulation results of the part. Select a flexible or rigid material that does not wet or stick to nylon hot melt adhesive and can withstand temperatures above 100°C as the mask material. Tightly wrap or coat the mask around or coat the non-reinforced area of ​​the blank. Immerse the entire blank with the mask into the slurry and perform selective vacuum impregnation. The slurry can only penetrate the areas not covered by the mask. After curing, remove the mask to obtain the target part with clear performance partitioning.

2. The manufacturing process for regionally differentiated carbon fiber reinforced nylon material components according to claim 1, characterized in that, Printing the integral blank containing the core reinforcement region and the surface transition region and preparing the carbon fiber slurry includes the following steps: (1) Load the nylon printing filament into the main feed channel of the 3D printing equipment and the carbon fiber into the hopper of the side feed device of the 3D printing equipment; The 3D model to be printed is imported into the slicing software, the core reinforcement zone and the surface transition zone are divided, and the printing parameters are set. The core reinforcement zone uses a dual feeding mode of nylon and carbon fiber, while the surface transition zone uses only a single feeding mode of nylon. The carbon fiber feeding device is turned off. Printing is then performed to obtain the blank. (2) Mix carbon fiber and nylon hot melt adhesive in proportion and stir to make a uniform carbon fiber slurry.

3. The manufacturing process for regionally differentiated carbon fiber reinforced nylon material components according to claim 1, characterized in that, The mask material is a PTFE film or a photocurable resin coating.

4. A manufacturing process for regionally differentiated carbon fiber reinforced nylon material components, characterized in that, Including the following steps: Based on the CAD model and mechanical simulation results of the component, the areas requiring gradient reinforcement are designed in advance. The entire blank containing the core reinforcement area and the surface transition area is printed out, and carbon fiber slurry is prepared. The dried blank is first immersed in the slurry and subjected to overall vacuum impregnation for the first time. After being taken out, rinsed and dried, a flexible or rigid material that does not wet or stick to nylon hot melt adhesive and can withstand temperatures above 100°C is selected as the mask material. The mask is tightly wrapped or coated on a local area of ​​the blank. The blank with the mask is then immersed in the slurry and subjected to selective vacuum impregnation for the second time. The slurry is impregnated in different areas in a gradient manner. After curing, the mask is removed to obtain the target component with gradient reinforcement zones.

5. The manufacturing process for regionally differentiated carbon fiber reinforced nylon material components according to claim 4, characterized in that, Printing the integral blank containing the core reinforcement region and the surface transition region and preparing the carbon fiber slurry includes the following steps: (1) Load the nylon printing filament into the main feed channel of the 3D printing equipment and the carbon fiber into the hopper of the side feed device of the 3D printing equipment; The 3D model to be printed is imported into the slicing software, the core reinforcement zone and the surface transition zone are divided, and the printing parameters are set. The core reinforcement zone uses a dual feeding mode of nylon and carbon fiber, while the surface transition zone uses only a single feeding mode of nylon. The carbon fiber feeding device is turned off. Printing is then performed to obtain the blank. (2) Mix carbon fiber and nylon hot melt adhesive in proportion and stir to make a uniform carbon fiber slurry.

6. The manufacturing process for regionally differentiated carbon fiber reinforced nylon material components according to claim 4, characterized in that, The mask material is a PTFE film or a photocurable resin coating.