A method for preparing a three-dimensional interwoven nanoreinforced ultrahigh strength building membrane

By employing a three-dimensional interwoven nano-reinforcement method, the problem of interlayer delamination in existing architectural membrane materials under alternating wind loads has been solved, achieving a balance between edge tear resistance and central flexibility and light transmission, thereby enhancing the overall strength and flexibility of the membrane material.

CN123129481APending Publication Date: 2026-11-20PEIS FILM IND (BEIJING) CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611582810.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-20

Smart Images

  • Figure CN123129481A_ABST
    Figure CN123129481A_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of building membrane preparation, and particularly relates to a three-dimensional interwoven nano-reinforced ultra-high-strength building membrane preparation method. The method comprises the following steps: spraying a polymer solution into a nanofiber membrane, and mixing a nano-reinforced material with a base fiber to form a yarn; the yarn is interwoven in three directions in space, and a through yarn is reserved in the thickness direction to form a three-dimensional interwoven body with an initial interwoven density and a yarn proportion in the thickness direction; an edge anchoring area and a center light-transmitting area are divided, a target interwoven density ratio is determined, the number of interwoven nodes and the interwoven angle are determined according to the target interwoven density ratio, and the interwoven density and the interwoven angle are gradiently decreased from the edge to the center; a thickness direction yarn proportion compensation amount is determined according to the initial interwoven density and the target interwoven density ratio, a nanofiber membrane is introduced according to the thickness direction yarn proportion compensation amount, and the nanofiber membrane is anchored by the thickness direction yarn; and a membrane is prepared through dip coating treatment. The present application realizes edge tear resistance, center flexible light transmission, interlayer anti-peeling and overall ultra-high strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of architectural membrane material preparation technology, and in particular to a method for preparing a three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material. Background Technology

[0002] Architectural membrane materials are widely used in large-span tensile membrane structures such as stadiums, airport terminals, and convention centers. During their service, they must simultaneously withstand outward shear stress caused by wind vibration, snow loads, and inward bidirectional tension caused by pretension. Existing architectural membrane materials typically use two-dimensional plain-weave fabric as the base material, impregnated with polytetrafluoroethylene (PTFE) or polyvinylidene fluoride (PVDF). The warp and weft yarns only intersect in two directions within the plane, with no yarn connection in the thickness direction. Interlayer bonding relies entirely on resin adhesion, making them prone to delamination under alternating wind loads. Furthermore, the uniform mechanical properties of the base fabric across the entire membrane surface make it difficult to simultaneously meet the dual requirements of tear resistance in the edge anchoring area and flexible tension in the central light-transmitting area. To improve strength, existing technologies attempt to introduce nano-reinforcing materials, but nanofiber membranes are mostly laid out in layers, still relying on resin interface adhesion, and still face the risk of delamination under alternating shear loads. In addition, the weaving density and weaving angle in existing membrane material preparation are usually uniform values ​​across the entire membrane surface, not tied to the actual stress requirements of different areas of the membrane structure, resulting in low material utilization efficiency.

[0003] Chinese Patent Publication No. CN105128350A discloses a method for preparing polytetrafluoroethylene (PTFE) architectural membrane, comprising the following steps: (1) providing an ultrafine glass fiber base fabric and a PTFE dispersion; (2) heat-treating the ultrafine glass fiber base fabric; (3) immersing the heat-treated and cooled base fabric into the PTFE dispersion; (4) sequentially drying, baking, and sintering the impregnated base fabric; (5) repeating the impregnation in step (3) and step (4) to obtain a PTFE architectural membrane. The advantage of this invention is that it uses a multiple impregnation coating method to prepare PTFE architectural membrane materials, resulting in PTFE architectural membranes with high strength, light weight, good flexibility, and ease of transportation and installation.

[0004] Therefore, the existing technology has the following problems:

[0005] The base fabric is a two-dimensional plain weave structure with no yarn connection in the thickness direction. The layers are only bonded by resin. Moreover, the weaving density and weaving angle are uniform across the entire film surface, which cannot meet the differentiated requirements of edge tear resistance and center flexibility and light transmission. Under wind-induced alternating loads, interlayer peeling is prone to occur. Summary of the Invention

[0006] To address this, the present invention provides a method for preparing a three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material, which overcomes the problem that in the prior art, the base fabric is a two-dimensional plain weave structure with no yarn connection in the thickness direction, and the layers are only bonded by resin. Furthermore, the interweaving density and interweaving angle are uniform across the entire membrane surface, which cannot meet the differentiated requirements of edge tear resistance and center flexibility and light transmission, and is prone to interlayer delamination under wind vibration alternating loads.

[0007] To achieve the above objectives, the present invention provides a method for preparing a three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material, comprising:

[0008] Step S1: The polymer solution is sprayed onto the receiving substrate to form a nanofiber membrane, and the nano-reinforcing material is blended with the matrix fiber to obtain a nano-reinforcing yarn.

[0009] Step S2: The nano-reinforced yarns are interwoven in three spatial directions, and through nano-reinforced yarns are retained in the thickness direction. The through nano-reinforced yarns constitute nano-reinforced yarns in the thickness direction, forming a three-dimensional interwoven body with an initial interweaving density and an initial thickness direction yarn ratio.

[0010] Step S3: Divide the three-dimensional interwoven body into an edge anchoring area and a central light-transmitting area, and determine the target interweaving density ratio between the edge anchoring area and the central light-transmitting area;

[0011] Step S4: Determine the number of interlacing nodes according to the target interlacing density ratio, so that the three-dimensional interlacing body has a gradient-changing interlacing density along the direction from the edge anchoring area to the center light-transmitting area;

[0012] Step S5: Determine the interlacing angle according to the target interlacing density ratio, so that the interlacing angle of the edge anchoring area is greater than the interlacing angle of the center light-transmitting area; and determine the compensation amount of the initial thickness direction yarn ratio according to the ratio of the initial interlacing density to the target interlacing density, and control the number of thickness direction nano-reinforcing yarns according to the compensation amount to obtain the compensated thickness direction yarn ratio.

[0013] Step S6: Based on the compensated thickness direction yarn ratio, determine the introduction position and introduction interval of the nanofiber membrane between layers, introduce the nanofiber membrane into the interlayer according to the introduction position and introduction interval, and anchor the nanofiber membrane through the thickness direction nanoreinforcing yarn.

[0014] Step S7: The obtained three-dimensional interwoven body is subjected to several impregnation coating treatments to obtain a three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material.

[0015] Further, in step S2, the three-dimensional interwoven body having an initial interweaving density and an initial thickness direction yarn ratio includes:

[0016] The nano-reinforced yarns are arranged along a first direction to form a first yarn group;

[0017] The nano-reinforced yarns are arranged along the second direction and interwoven with the first yarn group to form a second yarn group;

[0018] The nano-reinforced yarns are arranged along a third direction and interwoven with the first yarn group and the second yarn group, while the through nano-reinforced yarns are retained in the thickness direction. The through nano-reinforced yarns constitute the nano-reinforced yarns in the thickness direction, forming the three-dimensional interwoven body.

[0019] Wherein, the first direction, the second direction, and the third direction are not coplanar; the interlacing node is the intersection point of the thickness-direction nano-reinforced yarn with the first yarn group or the second yarn group; the initial interlacing density is the ratio of the number of interlacing nodes in the three-dimensional interlacing body to the area of ​​the three-dimensional interlacing body; the initial thickness-direction yarn ratio is the proportion of the number of thickness-direction nano-reinforced yarns to the total number of nano-reinforced yarns.

[0020] Further, in step S3, the three-dimensional interwoven body is divided into an edge anchoring area and a central light-transmitting area, including:

[0021] Based on the design load of the target application scenario of the architectural membrane material, the in-plane stress distribution characteristics of the three-dimensional interwoven body are determined;

[0022] Based on the tensioning conditions of the target application scenario of the architectural membrane material, the in-plane strain distribution of the three-dimensional interwoven body during the tensioning process is determined;

[0023] The width of the transition area between the edge anchoring area and the central light-transmitting area is determined based on the in-plane strain distribution.

[0024] According to the in-plane stress distribution characteristics, the region in the three-dimensional interwoven body where the in-plane stress is greater than the preset stress value is divided into the edge anchoring zone;

[0025] The area in the three-dimensional interwoven body where the in-plane stress is less than or equal to the preset stress value and the distance between it and the edge anchoring area is greater than the width of the transition area is defined as the central light-transmitting area.

[0026] Further, in step S3, determining the target interlacing density ratio between the edge anchoring area and the central light-transmitting area includes:

[0027] The reference interlacing density of the edge anchoring zone is determined based on the in-plane stress peak value of the edge anchoring zone. The reference interlacing density of the edge anchoring zone is the number of interlacing nodes per unit area within the edge anchoring zone.

[0028] The reference interlacing density of the central light-transmitting area is determined based on the average in-plane stress of the central light-transmitting area. The reference interlacing density of the central light-transmitting area is the number of interlacing nodes per unit area within the central light-transmitting area.

[0029] Further, in step S4, determining the number of interlacing nodes according to the target interlacing density ratio includes:

[0030] The number of interlacing nodes in the edge anchorage zone is determined based on the reference interlacing density and the area of ​​the edge anchorage zone.

[0031] The number of interlacing nodes in the central light-transmitting area is determined based on the reference interlacing density of the central light-transmitting area and the area of ​​the central light-transmitting area.

[0032] Based on the target interlacing density ratio, the number of interlacing nodes in the transition area is determined to decrease from the number of interlacing nodes in the edge anchoring area to the number of interlacing nodes in the center light-transmitting area along the direction from the edge anchoring area to the center light-transmitting area.

[0033] The rate of decrease in the number of interlaced nodes within the transition region is negatively correlated with the width of the transition region.

[0034] Further, in step S5, determining the interlacing angle according to the target interlacing density ratio includes:

[0035] The interlacing angle of the edge anchoring zone is determined based on the reference interlacing density of the edge anchoring zone;

[0036] The interlacing angle of the central light-transmitting area is determined based on the reference interlacing density of the central light-transmitting area;

[0037] Based on the target interlacing density ratio, the interlacing angle within the transition area is determined to decrease from the interlacing angle of the edge anchoring area to the interlacing angle of the center light-transmitting area along the direction from the edge anchoring area to the center light-transmitting area;

[0038] The deceleration rate of the interlacing angle within the transition region is negatively correlated with the width of the transition region.

[0039] Further, in step S5, the compensated thickness direction yarn percentage is obtained, including:

[0040] Based on the ratio of the initial interlacing density to the target interlacing density, determine the thickness direction yarn quantity compensation value of the edge anchoring zone and the thickness direction yarn quantity compensation value of the central light-transmitting zone;

[0041] The number of nano-reinforcing yarns in the thickness direction of the edge anchoring area is controlled according to the compensation value of the number of yarns in the thickness direction of the edge anchoring area; the number of nano-reinforcing yarns in the thickness direction of the central light-transmitting area is controlled according to the compensation value of the number of yarns in the thickness direction of the central light-transmitting area.

[0042] The ratio of the sum of the number of thickness-direction nano-reinforcing yarns in the edge anchoring area and the number of thickness-direction nano-reinforcing yarns corresponding to the initial thickness-direction yarn ratio to the total number of nano-reinforcing yarns is used as the compensated thickness-direction yarn ratio.

[0043] The thickness direction yarn quantity compensation value of the edge anchoring zone is greater than the thickness direction yarn quantity compensation value of the central light-transmitting zone.

[0044] Further, in step S6, the introduction position and spacing of the nanofiber membrane between layers are determined based on the compensated thickness direction yarn ratio, including:

[0045] The distribution density of nano-reinforcing yarns in the thickness direction in the three-dimensional interwoven body is determined based on the compensated thickness direction yarn ratio.

[0046] The introduction position of the nanofiber membrane between layers is determined based on the distribution density of the nanofiber reinforcing yarn in the thickness direction. The introduction position is located between the interlacing nodes of two adjacent nanofiber reinforcing yarns in the thickness direction.

[0047] The introduction interval of the nanofiber membrane between layers is determined based on the distribution density of the nanofiber reinforcing yarn in the thickness direction, and the introduction interval is negatively correlated with the distribution density of the nanofiber reinforcing yarn in the thickness direction.

[0048] Further, in step S6, the nanofiber membrane is anchored through the thickness-direction nanoreinforcing yarn, including:

[0049] After introducing the nanofiber membrane into the interlayer, the nanofiber reinforcing yarn in the thickness direction is continued to be woven along the thickness direction;

[0050] The thickness-direction nano-reinforcing yarn is passed through the nanofiber membrane, and interlacing nodes are formed on both sides of the nanofiber membrane.

[0051] The interlacing nodes on both sides of the nanofiber membrane are misaligned in the thickness direction.

[0052] Furthermore, the impregnation coating process involves immersing the obtained three-dimensional interwoven body in a polymer dispersion, followed by drying, baking, and sintering, repeated several times.

[0053] Compared with the prior art, the beneficial effects of the present invention are as follows: This embodiment interweaves nano-reinforcing yarns in a non-coplanar manner along the first, second, and third directions, and retains through nano-reinforcing yarns in the thickness direction to form a thickness-direction nano-reinforcing yarn, so that the first yarn group and the second yarn group are connected into an integral structure in the thickness direction. At the same time, the correspondence between the initial interweaving density and the initial thickness-direction yarn ratio is defined. When the density of in-plane intersection points between the first yarn group and the second yarn group is low, the thickness-direction yarn ratio is increased to compensate for the interlayer connection strength. When the density of in-plane intersection points is high, the thickness-direction yarn ratio is reduced to avoid excessive membrane stiffness. Thus, while ensuring the interlayer connection strength, the membrane flexibility is also taken into account, providing a structural basis for subsequent regional differential reinforcement and interlayer nanofiber membrane anchoring.

[0054] Furthermore, this embodiment determines the in-plane stress distribution characteristics based on the design load, the in-plane strain distribution based on the tensioning conditions, the transition region width based on the strain gradient, and divides the edge anchorage area and the central light-transmitting area according to the preset stress value. This allows the regional division of the three-dimensional interwoven body to simultaneously consider the load-bearing requirements during the service phase and the tensioning requirements during the installation phase, while reserving a transition region between the edge anchorage area and the central light-transmitting area. Furthermore, it determines the reference interweaving density of the edge anchorage area and the central light-transmitting area using the peak and average in-plane stress values ​​respectively, and determines the target interweaving density ratio by combining the stress ratio and the transition region width. This allows the target interweaving density ratio to simultaneously reflect the differences in load-bearing requirements between the two areas and the constraints of the tensioning process, providing a parameter basis for determining the number of interweaving nodes and the interweaving angle in the subsequent process.

[0055] Furthermore, in this embodiment, the number of interlacing nodes is determined according to the reference interlacing density of the edge anchoring area and the center light-transmitting area, and the interlacing density is linearly reduced by distance in the transition area, so that the number of interlacing nodes decreases from the number of interlacing nodes in the edge anchoring area to the number of interlacing nodes in the center light-transmitting area, and the rate of reduction is negatively correlated with the width of the transition area, so that the interlacing density gradient is bound to the tensioning process, providing a density distribution basis for the introduction position and introduction interval of the nanofiber membrane.

[0056] Furthermore, in this embodiment, the thickness direction yarn quantity compensation value is determined according to the ratio of the initial interlacing density to the target interlacing density, respectively. The compensation value of the edge anchoring zone is greater than that of the center light-transmitting zone, so that the thickness direction yarn proportion is increased more in the edge anchoring zone to enhance the interlayer shear resistance, and less in the center light-transmitting zone to maintain the flexibility and light transmission performance. This provides a basis for the thickness direction yarn distribution for the introduction position and introduction interval of the nanofiber membrane in step S6.

[0057] Furthermore, in this embodiment, the distribution density of the nanofiber reinforcing yarn in the thickness direction is determined based on the compensated thickness direction yarn ratio. This allows the nanofiber membrane to be introduced between two adjacent interlacing nodes, with the introduction interval negatively correlated with the distribution density and gradually increasing from the edge anchoring area to the center light-transmitting area. This binds the introduction position and interval of the nanofiber membrane to the thickness direction yarn distribution. By allowing the thickness direction nanofiber reinforcing yarn to pass through the nanofiber membrane and form interlacing nodes on both sides, with the interlacing nodes on both sides being staggered in the thickness direction, the nanofiber membrane is subjected to asymmetric constraints in the thickness direction. This increases the contact area and friction between the nanofiber membrane and the thickness direction nanofiber reinforcing yarn, thereby suppressing the reciprocating slippage of the nanofiber membrane along the thickness direction under wind-induced alternating loads. This provides interlayer anti-peeling capability for the finally obtained three-dimensional interlaced nano-reinforced ultra-high strength architectural membrane material. Attached Figure Description

[0058] Figure 1 This is a flowchart of the method for preparing three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material in this embodiment;

[0059] Figure 2 This is a flowchart illustrating the process of forming a three-dimensional interwoven body in the preparation method of the three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material in this embodiment. Detailed Implementation

[0060] To make the objectives and advantages of the present invention clearer, the present invention will be further described below with reference to embodiments; it should be understood that the specific embodiments described herein are merely for explaining the present invention and are not intended to limit the present invention.

[0061] Preferred embodiments of the present invention will now be described with reference to the accompanying drawings. Those skilled in the art should understand that these embodiments are merely illustrative of the technical principles of the present invention and are not intended to limit the scope of protection of the present invention.

[0062] Please see Figures 1-2 As shown, Figure 1 This is a flowchart of the method for preparing three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material in this embodiment; Figure 2 This is a flowchart illustrating the process of forming a three-dimensional interwoven body in the preparation method of the three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material in this embodiment.

[0063] This embodiment provides a method for preparing a three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material, including:

[0064] Step S1: The polymer solution is sprayed onto the receiving substrate to form a nanofiber membrane, and the nano-reinforcing material is blended with the matrix fiber to obtain a nano-reinforcing yarn.

[0065] Step S2: The nano-reinforced yarns are interwoven in three spatial directions, and through nano-reinforced yarns are retained in the thickness direction. The through nano-reinforced yarns constitute nano-reinforced yarns in the thickness direction, forming a three-dimensional interwoven body with an initial interweaving density and an initial thickness direction yarn ratio.

[0066] Step S3: Divide the three-dimensional interwoven body into an edge anchoring area and a central light-transmitting area, and determine the target interweaving density ratio between the edge anchoring area and the central light-transmitting area;

[0067] Step S4: Determine the number of interlacing nodes according to the target interlacing density ratio, so that the three-dimensional interlacing body has a gradient-changing interlacing density along the direction from the edge anchoring area to the center light-transmitting area;

[0068] Step S5: Determine the interlacing angle according to the target interlacing density ratio, so that the interlacing angle of the edge anchoring area is greater than the interlacing angle of the center light-transmitting area; and determine the compensation amount of the initial thickness direction yarn ratio according to the ratio of the initial interlacing density to the target interlacing density, and control the number of thickness direction nano-reinforcing yarns according to the compensation amount to obtain the compensated thickness direction yarn ratio.

[0069] Step S6: Based on the compensated thickness direction yarn ratio, determine the introduction position and introduction interval of the nanofiber membrane between layers, introduce the nanofiber membrane into the interlayer according to the introduction position and introduction interval, and anchor the nanofiber membrane through the thickness direction nanoreinforcing yarn.

[0070] Step S7: The obtained three-dimensional interwoven body is subjected to several impregnation coating treatments to obtain a three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material.

[0071] In this embodiment, polyvinylidene fluoride was dissolved in N,N-dimethylacetamide to prepare a polymer solution with a mass fraction of 12%–18%. Electrospinning was performed under conditions of 20–30°C, 40%–60% relative humidity, a spinning voltage of 15–25 kV, and a feed rate of 0.5–1.5 mL / h. The distance between the spinneret and the receiving substrate was 15–25 cm. A nanofiber membrane with an average fiber diameter of 100–600 nm was formed on the receiving substrate. The resulting nanofiber... After the fiber membrane is peeled off from the receiving substrate, it is vacuum dried at 60-80°C for later use; Preparation of nano-reinforced yarn: The nano-reinforcement material and the matrix fiber are blended at a mass ratio of (1-5):(95-99), wherein the nano-reinforcement material is at least one of nano-silica, nano-silicon carbide, carbon nanotubes or nano-cellulose, and the matrix fiber is at least one of glass fiber, polyester fiber or aramid fiber. After blending, the yarn is twisted to obtain a nano-reinforced yarn with a linear density of 50-200 tex.

[0072] In this embodiment, the polymer solution may also be a polyurethane, polyacrylonitrile, or polytetrafluoroethylene dispersion instead of a polyvinylidene fluoride solution; the fiber diameter and areal density of the nanofiber membrane may be adjusted according to the transmittance requirements of the target membrane material.

[0073] Specifically, in step S2, the three-dimensional interwoven body having an initial interweaving density and an initial thickness direction yarn ratio includes:

[0074] Step S21: Arrange the nano-reinforced yarns along a first direction to form a first yarn group;

[0075] Step S22: Arrange the nano-reinforced yarn along the second direction and interweave it with the first yarn group to form a second yarn group;

[0076] Step S23: The nano-reinforced yarn is arranged along a third direction and interwoven with the first yarn group and the second yarn group, while the through nano-reinforced yarn is retained in the thickness direction. The through nano-reinforced yarn constitutes the nano-reinforced yarn in the thickness direction, forming the three-dimensional interwoven body.

[0077] Wherein, the first direction, the second direction, and the third direction are not coplanar; the interlacing node is the intersection point of the thickness-direction nano-reinforced yarn with the first yarn group or the second yarn group; the initial interlacing density is the ratio of the number of interlacing nodes in the three-dimensional interlacing body to the area of ​​the three-dimensional interlacing body, in units of nodes / cm²; the initial thickness-direction yarn ratio is the proportion of the number of thickness-direction nano-reinforced yarns to the total number of nano-reinforced yarns.

[0078] In this embodiment, the first direction, the second direction, and the third direction are not coplanar. Specifically, the first direction is the length direction of the membrane material, the second direction is the width direction of the membrane material, and the third direction is the thickness direction of the membrane material; the angle between the first direction and the second direction is 60° to 90°, preferably 90°; the third direction is perpendicular to both the first direction and the second direction.

[0079] Specifically, the nano-reinforcing yarns in the first yarn group are arranged parallel to each other along the first direction, with a spacing of 0.5–2 mm between adjacent nano-reinforcing yarns, preferably 1 mm; the nano-reinforcing yarns in the second yarn group are arranged parallel to each other along the second direction, with a spacing of 0.5–2 mm between adjacent nano-reinforcing yarns, preferably 1 mm; the second yarn group and the first yarn group are interwoven alternately in a one-up-one-down interlacing pattern to form an in-plane interlacing structure. Alternatively, the second yarn group and the first yarn group can also adopt a two-up-two-down or three-up-three-down interlacing pattern.

[0080] Specifically, the nano-reinforcing yarns arranged in the third direction are the thickness-direction nano-reinforcing yarns. These thickness-direction nano-reinforcing yarns penetrate the first yarn group and the second yarn group along the thickness direction of the three-dimensional interwoven body, connecting them into a single structure in the thickness direction. The proportion of the thickness-direction nano-reinforcing yarns in the three-dimensional interwoven body to the total number of nano-reinforcing yarns is 5% to 30%, preferably 10% to 20%.

[0081] Specifically, the interlacing node is the intersection point of the thickness-direction nano-reinforcing yarn with the first yarn group or the second yarn group; the initial interlacing density is the ratio of the number of interlacing nodes in the three-dimensional interlaced body to the area of ​​the three-dimensional interlaced body, and the initial interlacing density is 2 to 8 nodes / cm², preferably 4 to 6 nodes / cm². The in-plane intersection points between the first yarn group and the second yarn group are not included in the interlacing node count.

[0082] Specifically, the initial interlacing density and the initial thickness direction yarn ratio satisfy the following relationship: the larger the initial interlacing density, the lower the initial thickness direction yarn ratio; the smaller the initial interlacing density, the upper the initial thickness direction yarn ratio. For example, when the initial interlacing density is 2-4 interlacings / cm², the initial thickness direction yarn ratio is 20%-30%; when the initial interlacing density is 4-6 interlacings / cm², the initial thickness direction yarn ratio is 10%-20%; and when the initial interlacing density is 6-8 interlacings / cm², the initial thickness direction yarn ratio is 5%-10%. The reason is that when the initial interlacing density is low, there are fewer interlacing nodes formed by the thickness-direction nano-reinforcing yarn and the first yarn group or the second yarn group, and the constraint effect of the thickness-direction nano-reinforcing yarn on the interlayer is weak. It is necessary to increase the proportion of the initial thickness-direction yarn to compensate for the insufficient interlayer connection strength. When the initial interlacing density is high, the interlacing nodes have provided sufficient interlayer constraint, and the proportion of the initial thickness-direction yarn can be appropriately reduced to avoid excessive thickness-direction yarn leading to excessive membrane stiffness and decreased flexibility.

[0083] In this embodiment, the three-dimensional interwoven body can also be formed by three-dimensional four-way weaving, three-dimensional five-way weaving or three-dimensional six-way weaving, and the arrangement density of the first yarn group, the second yarn group and the thickness direction nano-reinforcing yarn can be adjusted according to the mechanical performance requirements of the target membrane material.

[0084] This embodiment interweaves nano-reinforcing yarns in non-coplanar directions along a first, second, and third direction, while retaining through nano-reinforcing yarns in the thickness direction to form thickness-direction nano-reinforcing yarns. This connects the first yarn group and the second yarn group into a single structure in the thickness direction. Simultaneously, it defines the relationship between the initial interweaving density and the initial thickness-direction yarn ratio. When the density of in-plane intersections between the first and second yarn groups is low, the thickness-direction yarn ratio is increased to compensate for interlayer bonding strength. When the density of in-plane intersections is high, the thickness-direction yarn ratio is decreased to avoid excessive membrane stiffness. This ensures both interlayer bonding strength and membrane flexibility, providing a structural basis for subsequent regional differentiation reinforcement and interlayer nanofiber membrane anchoring.

[0085] Specifically, in step S3, the three-dimensional interwoven body is divided into an edge anchoring area and a central light-transmitting area, including:

[0086] Based on the design load of the target application scenario of the architectural membrane material, the in-plane stress distribution characteristics of the three-dimensional interwoven body are determined;

[0087] Based on the tensioning conditions of the target application scenario of the architectural membrane material, the in-plane strain distribution of the three-dimensional interwoven body during the tensioning process is determined;

[0088] The width of the transition area between the edge anchoring area and the central light-transmitting area is determined based on the in-plane strain distribution.

[0089] According to the in-plane stress distribution characteristics, the region in the three-dimensional interwoven body where the in-plane stress is greater than the preset stress value is divided into the edge anchoring zone;

[0090] The area in the three-dimensional interwoven body where the in-plane stress is less than or equal to the preset stress value and the distance between it and the edge anchoring area is greater than the width of the transition area is defined as the central light-transmitting area.

[0091] In this embodiment, the design load is determined based on the target application scenario of the architectural membrane material. Specifically, when the target application scenario is a stadium canopy, the design load includes standard values ​​for wind load, snow load, and pretension design value; when the target application scenario is an airport terminal roof, the design load includes standard values ​​for wind load and pretension design value. The composition of the design load is differentiated according to the application scenario because stadium canopies are typically large-span enclosed or semi-enclosed structures, where snow load is a significant vertical load; while airport terminal roofs have larger spans and flatter surfaces, resulting in a weaker snow load accumulation effect, making wind load and pretension the controlling factors.

[0092] Specifically, the standard wind load value is determined according to the building structure load code based on the basic wind pressure, terrain roughness category, and structural height of the target membrane structure location; the standard snow load value is determined according to the basic snow pressure and roof snow load distribution coefficient of the target membrane structure location, according to the building structure load code; and the prestressing design value is determined according to the membrane structure technical specifications based on the span and surface shape of the target membrane structure. The in-plane stress distribution characteristics are obtained by calculating the stress state of the target membrane structure under the design load using the finite element analysis method.

[0093] Specifically, the tensioning conditions include at least one of tension stress, boundary constraint method, and target surface shape. The tension stress is the pre-tension applied during membrane installation; the boundary constraint method is the connection method between the membrane edge and the steel cable, slot, or pressure line; and the target surface shape is saddle-shaped, arched, or umbrella-shaped. The in-plane strain distribution is calculated using finite element analysis to determine the deformation state of the three-dimensional interwoven body under the tensioning conditions.

[0094] Specifically, the width of the transition region is determined based on the strain gradient in the in-plane strain distribution, and the width of the transition region is negatively correlated with the strain gradient. The larger the strain gradient, the smaller the width of the transition region; conversely, the smaller the strain gradient, the larger the width of the transition region. This is because in areas with a large strain gradient, the yarn needs to adapt to deformation quickly during tensioning, requiring a narrow transition region to allow the interlacing density to transition rapidly from high to low density, preventing wrinkles from forming in the wide transition area during tensioning. In areas with a small strain gradient, the transition region can be wider, allowing for a gradual change in interlacing density and preventing stress concentration caused by abrupt density changes. The width of the transition region is 5–50 mm, preferably 10–30 mm. The lower limit of 5 mm ensures that the transition region can accommodate at least one complete interlacing node cycle, preventing a step change in interlacing density due to excessive narrowness; the upper limit of 50 mm prevents the transition region from occupying too large a proportion of the membrane surface, affecting the effective area of ​​the edge anchoring area and the central light-transmitting area.

[0095] Specifically, the preset stress value is 60% to 80% of the allowable stress value of the three-dimensional interwoven body, preferably 70% to 75%. The lower limit of 60% ensures that the edge anchoring zone has sufficient safety margin to avoid tearing due to local stress exceeding the allowable stress during service; the upper limit of 80% avoids the edge anchoring zone being too large, resulting in insufficient area of ​​the central light-transmitting zone, affecting the light transmission and flexible tension of the membrane surface. The allowable stress value is determined based on the tensile strength of the nano-reinforced yarn and the initial interweaving density. When the in-plane stress is greater than the preset stress value, the risk of tearing in this area during service is high, and it is classified as the edge anchoring zone; when the in-plane stress is less than or equal to the preset stress value, the load-bearing requirement in this area is low, and it is classified as the central light-transmitting zone.

[0096] Specifically, the division of the central light-transmitting area also needs to meet the condition that the distance between it and the edge anchoring area is greater than the width of the transition area. That is, there is a gap area between the edge anchoring area and the central light-transmitting area with a width equal to the width of the transition area. This gap area is neither included in the edge anchoring area nor in the central light-transmitting area, and is used to achieve the gradient transition of interlacing density and interlacing angle in subsequent steps S4 and S5.

[0097] In this embodiment, the finite element analysis method can be performed using commercial software such as ANSYS, ABAQUS, or MSC.Marc, and the design load and tensioning conditions can be adjusted according to the specific design requirements of the target membrane structure.

[0098] Specifically, in step S3, determining the target interlacing density ratio between the edge anchoring area and the central light-transmitting area includes:

[0099] The reference interlacing density of the edge anchoring zone is determined based on the in-plane stress peak value of the edge anchoring zone. The reference interlacing density of the edge anchoring zone is the number of interlacing nodes per unit area within the edge anchoring zone.

[0100] The reference interlacing density of the central light-transmitting area is determined based on the average in-plane stress of the central light-transmitting area. The reference interlacing density of the central light-transmitting area is the number of interlacing nodes per unit area within the central light-transmitting area.

[0101] The target interlacing density ratio is determined based on the ratio of the peak in-plane stress in the edge anchoring zone to the average in-plane stress in the central light-transmitting zone, and the width of the transition region.

[0102] In this embodiment, both the peak in-plane stress in the edge anchoring zone and the average in-plane stress in the central light-transmitting zone can be directly extracted from the in-plane stress distribution characteristics obtained in step S3. Specifically, the peak in-plane stress in the edge anchoring zone is the maximum value of the in-plane stress at each node within the edge anchoring zone, and the average in-plane stress in the central light-transmitting zone is the arithmetic mean of the in-plane stress at each node within the central light-transmitting zone. Different statistical measures are used for the two regions because the stress distribution in the edge anchoring zone is uneven, and the peak value is the basis for determining whether the region requires the highest interlacing density; while the stress distribution in the central light-transmitting zone is relatively uniform, and the average value can represent the overall load-bearing capacity.

[0103] Specifically, the reference interlacing density of the edge anchoring zone is determined based on the peak in-plane stress of the edge anchoring zone, and the reference interlacing density of the edge anchoring zone is positively correlated with the peak in-plane stress. The larger the peak in-plane stress, the larger the reference interlacing density of the edge anchoring zone. The reference interlacing density of the edge anchoring zone is 4 to 10 interlacings / cm², preferably 6 to 8 interlacings / cm². The lower limit of 4 interlacings / cm² ensures that the edge anchoring zone has basic tear resistance, while the upper limit of 10 interlacings / cm² avoids excessively high interlacing density, which would lead to excessive stiffness in the area and inability to adapt to boundary deformation during tensioning.

[0104] Specifically, the reference interlacing density of the central light-transmitting area is determined based on the average in-plane stress of the central light-transmitting area, and the reference interlacing density of the central light-transmitting area is positively correlated with the average in-plane stress. The larger the average in-plane stress, the larger the reference interlacing density of the central light-transmitting area. The reference interlacing density of the central light-transmitting area is 1 to 5 strands / cm², preferably 2 to 4 strands / cm². The lower limit of 1 strand / cm² ensures that the central light-transmitting area has basic load-bearing capacity, while the upper limit of 5 strands / cm² avoids excessively high interlacing density from affecting the film's light transmittance and flexible tensile properties.

[0105] Specifically, the target interlacing density ratio is the ratio of the reference interlacing density of the edge anchoring area to the reference interlacing density of the central light-transmitting area. The target interlacing density ratio is positively correlated with the ratio of the peak in-plane stress to the average in-plane stress, and negatively correlated with the width of the transition region. This is because: a larger stress ratio indicates a higher load-bearing requirement for the edge anchoring area relative to the central light-transmitting area, thus requiring a larger interlacing density ratio; a wider transition region results in a smoother transition from high to low interlacing density, allowing for a smaller target interlacing density ratio; a narrower transition region leads to more drastic density changes, requiring a larger density ratio to ensure the reinforcement effect of the edge anchoring area. The target interlacing density ratio is 1.5 to 4, preferably 2 to 3. The lower limit of 1.5 ensures a identifiable density difference between the edge anchoring area and the central light-transmitting area, while the upper limit of 4 avoids an excessively large density ratio that leads to an overly steep density gradient in the transition region, causing stress concentration.

[0106] In this embodiment, the reference interlacing density of the edge anchoring zone and the reference interlacing density of the central light-transmitting zone can also be adjusted according to the specific mechanical performance requirements of the target membrane material.

[0107] This embodiment determines the in-plane stress distribution characteristics based on the design load, the in-plane strain distribution based on the tensioning conditions, the transition region width based on the strain gradient, and divides the edge anchorage zone and the central light-transmitting zone according to the preset stress value. This allows the regional division of the three-dimensional interwoven body to simultaneously consider the load-bearing requirements during service and the tensioning requirements during installation, while reserving a transition region between the edge anchorage zone and the central light-transmitting zone. Furthermore, it determines the reference interweaving density of the edge anchorage zone and the central light-transmitting zone by using the peak and average in-plane stress values ​​respectively, and determines the target interweaving density ratio by combining the stress ratio and the transition region width. This allows the target interweaving density ratio to simultaneously reflect the difference in load-bearing requirements between the two zones and the constraints of the tensioning process, providing a parameter basis for determining the number of interweaving nodes and the interweaving angle in the subsequent process.

[0108] Specifically, in step S4, determining the number of interlacing nodes according to the target interlacing density ratio includes:

[0109] The number of interlacing nodes in the edge anchorage zone is determined based on the reference interlacing density and the area of ​​the edge anchorage zone.

[0110] The number of interlacing nodes in the central light-transmitting area is determined based on the reference interlacing density of the central light-transmitting area and the area of ​​the central light-transmitting area.

[0111] Based on the target interlacing density ratio, the number of interlacing nodes in the transition area is determined to decrease from the number of interlacing nodes in the edge anchoring area to the number of interlacing nodes in the center light-transmitting area along the direction from the edge anchoring area to the center light-transmitting area.

[0112] The rate of decrease in the number of interlaced nodes within the transition region is negatively correlated with the width of the transition region.

[0113] In this embodiment, the number of interlacing nodes in the edge anchoring zone is determined by the product of the reference interlacing density and the area of ​​the edge anchoring zone; the number of interlacing nodes in the central light-transmitting zone is determined by the product of the reference interlacing density and the area of ​​the central light-transmitting zone. The number of interlacing nodes refers to the number of intersections formed by the thickness-direction nano-reinforcing yarn and the first yarn group or the second yarn group. Specifically, the areas of the edge anchoring zone and the central light-transmitting zone are directly obtained from the division results in step S3.

[0114] Specifically, the interlacing density within the transition region decreases proportionally along the direction from the edge anchoring area to the central light-transmitting area, meaning that the interlacing density at any location within the transition region is linearly related to the distance from that location to the edge anchoring area. The interlacing density on the side of the transition region closer to the edge anchoring area is equal to the reference interlacing density of the edge anchoring area, and the interlacing density on the side of the transition region closer to the central light-transmitting area is equal to the reference interlacing density of the central light-transmitting area. The interlacing density at the intermediate location is linearly determined between the reference interlacing density of the edge anchoring area and the reference interlacing density of the central light-transmitting area based on the distance from the edge anchoring area.

[0115] Specifically, the interlacing density within the transition region satisfies the following relationship: Let the reference interlacing density of the edge anchoring zone be ρ1, the reference interlacing density of the central light-transmitting zone be ρ2, the width of the transition region be W, and the interlacing density at a distance x from the edge anchoring zone be ρ(x), then:

[0116] ρ(x) = ρ1 - (ρ1 - ρ2) × x / W

[0117] Where 0 ≤ x ≤ W, and x and W have the same unit.

[0118] Specifically, when x=0, ρ(0)=ρ1, that is, the interlacing density of the transition region on the side closer to the edge anchoring area is equal to the reference interlacing density of the edge anchoring area; when x=W, ρ(W)=ρ2, that is, the interlacing density of the transition region on the side closer to the central light-transmitting area is equal to the reference interlacing density of the central light-transmitting area.

[0119] Specifically, the number of interlacing nodes in the transition area is the integral result of the interlacing density in the transition area over the area of ​​the transition area. Since the interlacing density decreases linearly from the edge anchoring area to the center light-transmitting area, the number of interlacing nodes in the transition area decreases in the same direction from the number of interlacing nodes in the edge anchoring area to the number of interlacing nodes in the center light-transmitting area.

[0120] Specifically, the deceleration rate of the interlacing density within the transition region is negatively correlated with the width of the transition region. The wider the transition region, the smaller the deceleration rate; conversely, the narrower the transition region, the larger the deceleration rate. This is because a wider transition region allows the interlacing density to transition from high to low over a longer spatial distance, resulting in a smaller deceleration rate and a smoother density change. Conversely, a narrower transition region requires the interlacing density to complete the same transition over a shorter spatial distance, resulting in a larger deceleration rate and a more drastic density change. The deceleration rate is the ratio of the difference between the reference interlacing density of the edge anchoring area and the reference interlacing density of the central light-transmitting area to the width of the transition region, i.e., (ρ1-ρ2) / W.

[0121] In this embodiment, the decreasing pattern can also be expressed as an exponential decrease or a segmented decrease, and the interlacing density in the transition region can be adjusted according to the specific mechanical performance requirements of the target membrane material.

[0122] This embodiment determines the number of interlacing nodes in the edge anchoring zone and the center light-transmitting zone based on their respective reference interlacing densities. In the transition zone, the interlacing density is linearly reduced by distance, so that the number of interlacing nodes decreases from the number of interlacing nodes in the edge anchoring zone to the number of interlacing nodes in the center light-transmitting zone. The rate of decrease is negatively correlated with the width of the transition zone, thus binding the interlacing density gradient to the tensioning process and providing a density distribution basis for the introduction location and interval of the nanofiber membrane.

[0123] Specifically, in step S5, determining the interlacing angle according to the target interlacing density ratio includes:

[0124] The interlacing angle of the edge anchoring zone is determined based on the reference interlacing density of the edge anchoring zone;

[0125] The interlacing angle of the central light-transmitting area is determined based on the reference interlacing density of the central light-transmitting area;

[0126] Based on the target interlacing density ratio, the interlacing angle within the transition area is determined to decrease from the interlacing angle of the edge anchoring area to the interlacing angle of the center light-transmitting area along the direction from the edge anchoring area to the center light-transmitting area;

[0127] The deceleration rate of the interlacing angle within the transition region is negatively correlated with the width of the transition region.

[0128] In this embodiment, the interlacing angle is the angle between the nano-reinforcing yarn and the in-plane direction of the three-dimensional interlaced body. The interlacing angle of the edge anchoring zone is determined based on the reference interlacing density of the edge anchoring zone, and the interlacing angle of the edge anchoring zone is positively correlated with the reference interlacing density of the edge anchoring zone. The larger the reference interlacing density of the edge anchoring zone, the larger the interlacing angle of the edge anchoring zone. The interlacing angle of the edge anchoring zone is 30° to 60°, preferably 40° to 50°. The lower limit of 30° ensures that the nano-reinforcing yarn has sufficient thickness direction component in the edge anchoring zone to provide the necessary interlayer shear resistance; the upper limit of 60° avoids excessively large interlacing angles that cause the yarn to tilt excessively in the thickness direction, reducing the in-plane tensile strength.

[0129] The interlacing angle of the central light-transmitting zone is determined based on the reference interlacing density of the central light-transmitting zone, and the interlacing angle of the central light-transmitting zone is positively correlated with the reference interlacing density of the central light-transmitting zone. The larger the reference interlacing density of the central light-transmitting zone, the larger the interlacing angle of the central light-transmitting zone. The interlacing angle of the central light-transmitting zone is 10° to 35°, preferably 15° to 25°. The lower limit of 10° ensures that the yarns in the central light-transmitting zone have a certain thickness direction interlacing, avoiding degradation into a pure two-dimensional in-plane structure; the upper limit of 35° avoids that an excessively large interlacing angle will affect the light transmittance and flexible tensile properties of the film surface.

[0130] The interlacing angle within the transition area decreases proportionally along the direction from the edge anchoring area to the central light-transmitting area, meaning that the interlacing angle at any position within the transition area is linearly related to the distance from that position to the edge anchoring area. The interlacing angle on the side of the transition area closer to the edge anchoring area is equal to the interlacing angle of the edge anchoring area, and the interlacing angle on the side of the transition area closer to the central light-transmitting area is equal to the interlacing angle of the central light-transmitting area. The interlacing angle at intermediate positions takes a linear value between the interlacing angles of the edge anchoring area and the central light-transmitting area, depending on the distance from the edge anchoring area.

[0131] Specifically, the interlacing angles within the transition area satisfy the following relationship: Let the interlacing angle of the edge anchoring area be θ1, the interlacing angle of the central light-transmitting area be θ2, the width of the transition area be W, and the interlacing angle at a distance x from the edge anchoring area be θ(x), then:

[0132] θ(x) = θ1 - (θ1 - θ2) × x / W

[0133] Where 0 ≤ x ≤ W, and x and W have the same unit.

[0134] Specifically, when x=0, θ(0)=θ1, that is, the interlacing angle of the transition region on the side closer to the edge anchoring area is equal to the interlacing angle of the edge anchoring area; when x=W, θ(W)=θ2, that is, the interlacing angle of the transition region on the side closer to the central light-transmitting area is equal to the interlacing angle of the central light-transmitting area.

[0135] Specifically, the deceleration rate of the interlacing angle within the transition region is negatively correlated with the width of the transition region. The wider the transition region, the smaller the deceleration rate; conversely, the narrower the transition region, the larger the deceleration rate. This is because when the transition region is wide, the interlacing angle transitions from large to small over a longer spatial distance, resulting in a smaller deceleration rate and a smoother angle change. Conversely, when the transition region is narrow, the interlacing angle needs to complete the same transition over a shorter spatial distance, resulting in a larger deceleration rate and a more drastic angle change. The deceleration rate is the ratio of the difference between the interlacing angle of the edge anchoring area and the interlacing angle of the central light-transmitting area to the width of the transition region, i.e., (θ1-θ2) / W.

[0136] In this embodiment, the decreasing pattern can also be expressed as an exponential decrease or a segmented decrease, and the interlacing angle in the transition region can be adjusted according to the specific mechanical performance requirements of the target membrane material.

[0137] Specifically, in step S5, the compensated thickness direction yarn percentage is obtained, including:

[0138] Based on the ratio of the initial interlacing density to the target interlacing density, determine the thickness direction yarn quantity compensation value of the edge anchoring zone and the thickness direction yarn quantity compensation value of the central light-transmitting zone;

[0139] The number of nano-reinforcing yarns in the thickness direction of the edge anchoring area is controlled according to the compensation value of the number of yarns in the thickness direction of the edge anchoring area; the number of nano-reinforcing yarns in the thickness direction of the central light-transmitting area is controlled according to the compensation value of the number of yarns in the thickness direction of the central light-transmitting area.

[0140] The ratio of the sum of the number of thickness-direction nano-reinforcing yarns in the edge anchoring area and the number of thickness-direction nano-reinforcing yarns corresponding to the initial thickness-direction yarn ratio to the total number of nano-reinforcing yarns is used as the compensated thickness-direction yarn ratio.

[0141] The thickness direction yarn quantity compensation value of the edge anchoring zone is greater than the thickness direction yarn quantity compensation value of the central light-transmitting zone.

[0142] In this embodiment, the thickness direction yarn quantity compensation value of the edge anchoring zone is determined based on the target interlacing density ratio. The larger the target interlacing density ratio, the larger the thickness direction yarn quantity compensation value of the edge anchoring zone. The thickness direction yarn quantity compensation value of the edge anchoring zone is 10% to 50% of the thickness direction nano-reinforcing yarn quantity corresponding to the initial thickness direction yarn ratio, preferably 20% to 40%. The lower limit of 10% ensures a identifiable improvement in the interlayer shear resistance of the edge anchoring zone compared to the initial state; the upper limit of 50% avoids excessive thickness direction yarn quantity compensation value leading to excessively high stiffness in the edge anchoring zone, making it unable to adapt to boundary deformation during tensioning.

[0143] The thickness direction yarn quantity compensation value of the central light-transmitting zone is determined based on the target interlacing density ratio. The larger the target interlacing density ratio, the larger the thickness direction yarn quantity compensation value of the central light-transmitting zone. The thickness direction yarn quantity compensation value of the central light-transmitting zone is 5% to 30% of the thickness direction nano-reinforcing yarn quantity corresponding to the initial thickness direction yarn ratio, preferably 10% to 20%. The lower limit of 5% ensures that the interlayer bonding strength of the central light-transmitting zone is improved relative to the initial state; the upper limit of 30% avoids that an excessively large thickness direction yarn quantity compensation value will affect the flexibility, tensile strength, and light transmittance of the central light-transmitting zone.

[0144] The thickness direction yarn quantity compensation value of the edge anchoring zone is greater than that of the central light-transmitting zone. This is because the edge anchoring zone experiences higher in-plane stress and out-of-plane shear during service compared to the central light-transmitting zone, requiring a larger thickness direction yarn quantity compensation value to enhance interlayer bonding. The central light-transmitting zone, with its primary functional requirements of light transmission and flexible tension, should have a appropriately lower thickness direction yarn quantity compensation value to avoid excessive stiffness.

[0145] Specifically, let N0 be the number of nano-reinforcing yarns in the thickness direction corresponding to the initial thickness direction yarn ratio, N be the total number of nano-reinforcing yarns, ΔN1 be the compensation value for the number of thickness direction yarns in the edge anchoring area, and ΔN2 be the compensation value for the number of thickness direction yarns in the central light-transmitting area. Then, the compensated thickness direction yarn ratio is (N0 + ΔN1 + ΔN2) / N; where ΔN1 is greater than ΔN2, ΔN1 is 10% to 50% of N0, and ΔN2 is 5% to 30% of N0.

[0146] In this embodiment, the thickness direction yarn quantity compensation value of the edge anchoring area and the thickness direction yarn quantity compensation value of the central light-transmitting area can also be adjusted according to the specific mechanical performance requirements of the target membrane material.

[0147] In this embodiment, the thickness direction yarn quantity compensation value is determined according to the ratio of the initial interlacing density to the target interlacing density, respectively. The compensation value of the edge anchoring zone is greater than that of the center light-transmitting zone, so that the thickness direction yarn proportion is increased more in the edge anchoring zone to enhance the interlayer shear resistance, and less in the center light-transmitting zone to maintain the flexibility and light transmission performance. This provides a basis for the thickness direction yarn distribution for the introduction position and introduction interval of the nanofiber membrane in step S6.

[0148] Specifically, in step S6, the introduction position and spacing of the nanofiber membrane between layers are determined based on the compensated thickness direction yarn ratio, including:

[0149] The distribution density of nano-reinforcing yarns in the thickness direction in the three-dimensional interwoven body is determined based on the compensated thickness direction yarn ratio.

[0150] The introduction position of the nanofiber membrane between layers is determined based on the distribution density of the nanofiber reinforcing yarn in the thickness direction. The introduction position is located between the interlacing nodes of two adjacent nanofiber reinforcing yarns in the thickness direction.

[0151] The introduction interval of the nanofiber membrane between layers is determined based on the distribution density of the nanofiber reinforcing yarn in the thickness direction, and the introduction interval is negatively correlated with the distribution density of the nanofiber reinforcing yarn in the thickness direction.

[0152] In this embodiment, the distribution density of the thickness-direction nano-reinforcing yarns is the number of thickness-direction nano-reinforcing yarns per unit area in the three-dimensional interwoven body. The distribution density is determined by dividing the product of the compensated thickness-direction yarn proportion and the total number of nano-reinforcing yarns by the area of ​​the three-dimensional interwoven body. The larger the compensated thickness-direction yarn proportion, the greater the distribution density of the thickness-direction nano-reinforcing yarns.

[0153] Specifically, the nanofiber membrane is introduced between layers at the interlacing nodes of two adjacent layers of thickness-direction nanofiber reinforcing yarns. The thickness-direction nanofiber reinforcing yarns are distributed in multiple layers along the thickness direction of the three-dimensional interwoven structure, with the interlacing nodes of adjacent layers spaced apart. The nanofiber membrane is introduced within these intervals. This is because if the nanofiber membrane were directly introduced into the layer containing the interlacing nodes of the thickness-direction nanofiber reinforcing yarns, the yarns would need to simultaneously interlac and penetrate the membrane at the nodes, making weaving difficult and prone to causing localized damage. By placing the introduction point between adjacent interlacing nodes, the nanofiber reinforcing yarns can pass through the membrane at a smaller angle, resulting in lower penetration resistance and more uniform stress on the nanofiber membrane.

[0154] Specifically, the introduction interval of the nanofiber membrane between layers is negatively correlated with the distribution density of the nanofiber reinforcing yarns in the thickness direction. The higher the distribution density of the nanofiber reinforcing yarns in the thickness direction, the smaller the introduction interval; conversely, the lower the distribution density, the larger the introduction interval. This is because: in areas with a high distribution density of nanofiber reinforcing yarns in the thickness direction, the interlayer connection points are dense, and there are more locations where the nanofiber membrane is anchored. The interlayer shear load borne by a single nanofiber membrane layer is relatively small, allowing for a reduction in the introduction interval to increase the number of nanofiber membrane layers and further improve interlayer peel resistance. In areas with a low distribution density of nanofiber reinforcing yarns in the thickness direction, the anchoring points are sparse. If too many layers of nanofiber membrane are introduced, there is a lack of sufficient anchoring between single layers, which can easily lead to weak interfaces. Therefore, appropriately increasing the introduction interval ensures that each nanofiber membrane layer is anchored by a sufficient number of yarns in the thickness direction. The introduction interval is 5–50 mm, preferably 10–30 mm. The lower limit of 5mm is to ensure that there is at least one complete interlacing node cycle between two adjacent nanofiber membranes, and to avoid the introduction of too small an interval, which would cause the nanofiber membrane layers to stack and the coating to be difficult to fully penetrate; the upper limit of 50mm is to avoid the introduction of too large an interval, which would cause the interlayer to lack nanofiber membrane reinforcement in local areas, resulting in interlayer delamination under wind vibration alternating load.

[0155] Specifically, the introduction position and the introduction interval are respectively determined in the edge anchoring area, the transition area and the central light-transmitting area, and the introduction interval gradually increases along the direction from the edge anchoring area to the central light-transmitting area.

[0156] In this embodiment, the introduction position and spacing of the nanofiber membrane between layers can be adjusted according to the specific mechanical performance requirements of the target membrane material.

[0157] Specifically, in step S6, the nanofiber membrane is anchored through the thickness-direction nanoreinforcing yarn, including:

[0158] After introducing the nanofiber membrane into the interlayer, the nanofiber reinforcing yarn in the thickness direction is continued to be woven along the thickness direction;

[0159] The thickness-direction nano-reinforcing yarn is passed through the nanofiber membrane, and interlacing nodes are formed on both sides of the nanofiber membrane.

[0160] The interlacing nodes on both sides of the nanofiber membrane are misaligned in the thickness direction.

[0161] In this embodiment, the thickness-direction nano-reinforced yarn passes through the nanofiber membrane in the following manner: during the weaving process, the thickness-direction nano-reinforced yarn travels along the thickness direction. When it reaches the layer where the nanofiber membrane is located, it passes through the nanofiber membrane by needle punching or weft insertion, and continues to travel along the thickness direction to the next layer, where it interweaves with the first yarn group or the second yarn group of the next layer to form an interlacing node.

[0162] Specifically, the interlacing nodes on both sides of the nanofiber membrane are staggered in the thickness direction. This means that the interlacing nodes on the side of the nanofiber membrane closer to the edge anchoring area and the interlacing nodes on the side of the nanofiber membrane closer to the central light-transmitting area are not located on the same vertical line in the thickness direction, and there is a staggered distance between them in the thickness direction. The staggered distance is 1 to 5 times the thickness of the nanofiber membrane, preferably 2 to 3 times. The lower limit of 1 times is to ensure that the interlacing nodes on both sides have a identifiable stagger in the thickness direction, avoiding degeneration into an aligned arrangement; the upper limit of 5 times is to avoid the staggered distance being too large, which would cause the difference in the tilt angle of the nanofiber reinforcing yarns on both sides of the nanofiber membrane in the thickness direction to be too large, affecting the uniformity of the through anchoring.

[0163] The misalignment distance causes the nanofiber membrane to be asymmetrically constrained in the thickness direction. This is because: if the interlacing nodes on both sides are aligned, the nanofiber membrane is uniformly clamped in the thickness direction, and the contact area between the nanofiber membrane and the nano-reinforcing yarns in the thickness direction is limited. Under alternating wind loads, the nanofiber membrane is prone to sliding back and forth along the thickness direction. If the interlacing nodes on both sides are misaligned, the nanofiber membrane undergoes local bending in the thickness direction, increasing the contact area between the nanofiber membrane and the nano-reinforcing yarns in the thickness direction, increasing friction, and the local bending creates a wavy constraint path in the thickness direction, which can more effectively suppress the back-and-forth sliding of the nanofiber membrane along the thickness direction.

[0164] Specifically, the misalignment direction of the interlacing nodes on both sides of the nanofiber membrane is alternately arranged along the direction from the edge anchoring area to the central light-transmitting area. That is, the misalignment direction of the interlacing nodes of two adjacent thickness-direction nanoreinforcing yarns on both sides of the nanofiber membrane is opposite, so that the nanofiber membrane forms an alternating constraint in the thickness direction.

[0165] In this embodiment, the misalignment distance and the misalignment direction can also be adjusted according to the specific mechanical performance requirements of the target membrane material.

[0166] This embodiment determines the distribution density of the nanofiber reinforcing yarns in the thickness direction based on the compensated thickness direction yarn ratio. This allows for the determination of the nanofiber membrane's introduction location between adjacent interlacing nodes, with the introduction interval negatively correlated with the distribution density and gradually increasing from the edge anchoring area to the center light-transmitting area. This binds the nanofiber membrane's introduction location and interval to the thickness direction yarn distribution. Furthermore, by allowing the thickness direction nanofiber reinforcing yarns to pass through the nanofiber membrane and form interlacing nodes on both sides, with the interlacing nodes on both sides staggered in the thickness direction, the nanofiber membrane is subjected to asymmetrical constraints in the thickness direction. This increases the contact area and friction between the nanofiber membrane and the thickness direction nanofiber reinforcing yarns, thereby suppressing the nanofiber membrane's reciprocating slippage along the thickness direction under alternating wind loads. This provides interlayer anti-peeling capability for the final three-dimensional interlaced nano-reinforced ultra-high strength architectural membrane material.

[0167] Specifically, the impregnation coating process involves immersing the obtained three-dimensional interwoven body in a polymer dispersion, followed by drying, baking, and sintering, repeated several times.

[0168] In this embodiment, the polymer dispersion is at least one of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), or polyurethane, preferably PTFE. The mass fraction of the PTFE dispersion is 40%–70%, preferably 50%–60%. The lower limit of 40% ensures that a sufficiently thick coating can be formed after a single impregnation, reducing the number of impregnations; the upper limit of 70% avoids excessively high dispersion viscosity, which would make it difficult for the dispersion to penetrate into the interfiber gaps of the three-dimensional interwoven structure.

[0169] Specifically, the impregnation time is 1 to 10 minutes, preferably 3 to 5 minutes. The lower limit of 1 minute ensures that the polymer dispersion can fully penetrate into the fiber gaps of the three-dimensional interwoven body; the upper limit of 10 minutes avoids excessive accumulation of the polymer dispersion on the surface of the three-dimensional interwoven body due to excessive impregnation time, which would affect the uniformity of subsequent drying and sintering.

[0170] Specifically, the drying temperature is 80–120°C, preferably 90–110°C, and the drying time is 10–30 min, preferably 15–20 min. The lower limit of 80°C ensures that the solvent can effectively evaporate; the upper limit of 120°C avoids the polymer in the polymer dispersion from melting or decomposing prematurely due to excessively high temperatures.

[0171] Specifically, the baking temperature is 200–280°C, preferably 230–260°C, and the baking time is 5–15 minutes, preferably 8–12 minutes. The lower limit of 200°C ensures that the polymer particles can initially melt and bond; the upper limit of 280°C avoids polymer decomposition due to excessively high temperatures.

[0172] Specifically, the sintering temperature is 350–400°C, preferably 370–390°C, and the sintering time is 1–5 min, preferably 2–3 min. The lower limit of 350°C ensures that the polytetrafluoroethylene particles can fully melt and form a continuous coating; the upper limit of 400°C avoids the decomposition of polytetrafluoroethylene due to excessively high temperatures.

[0173] Specifically, the number of repetitions is 2 to 8 times, preferably 3 to 6 times. The lower limit of 2 times ensures that the interstices between the fibers of the three-dimensional interwoven structure can be fully filled by the coating; the upper limit of 8 times avoids excessive repetitions that could lead to an overly thick coating, excessive film density, and decreased flexibility. During each repetition, the mass fraction of the polymer dispersion can remain constant or decrease gradually. Preferably, the first impregnation uses a polymer dispersion with a mass fraction of 50% to 60%, and subsequent impregnations use a polymer dispersion with a mass fraction of 40% to 50%. The reason is that during the first impregnation, the interstices between the fibers of the three-dimensional interwoven structure are relatively large, and a high-concentration dispersion can quickly fill them; during subsequent impregnations, the interstices between the fibers gradually decrease, and reducing the dispersion concentration can improve its permeability and prevent accumulation on the surface.

[0174] In this embodiment, the mass fraction of the polymer dispersion, impregnation time, drying temperature and time, baking temperature and time, sintering temperature and time, and number of repetitions can be adjusted according to the specific performance requirements of the target membrane material.

[0175] Example: Step 1, Preparation of nanofiber membrane: Polyvinylidene fluoride was dissolved in N,N-dimethylacetamide to prepare a polymer solution with a mass fraction of 15%. Electrospinning was carried out at a temperature of 25°C and a relative humidity of 50%, with a spinning voltage of 20kV and a feeding speed of 1mL / h. The distance between the spinneret and the receiving substrate was 20cm. A nanofiber membrane with an average fiber diameter of 300nm was formed on the receiving substrate. The obtained nanofiber membrane was peeled off from the receiving substrate and vacuum dried at 70°C for later use.

[0176] Step 2: Preparation of nano-reinforced yarn: Nano-silica and glass fiber are blended at a mass ratio of 3:97, and then twisted to obtain nano-reinforced yarn with a linear density of 100 tex.

[0177] Step 3, Three-dimensional interlacing: The nano-reinforced yarns are arranged parallel to each other along the first direction at 1mm intervals to form a first yarn group. They are then arranged parallel to each other along the second direction at 1mm intervals and interlaced with the first yarn group in a one-up-one-down pattern to form a second yarn group. They are then arranged along a third direction and interlaced with both the first and second yarn groups. Through-through nano-reinforced yarns are retained in the thickness direction to form thickness-direction nano-reinforced yarns, thus forming a three-dimensional interlaced body. The angle between the first and second directions is 90°, and the third direction is perpendicular to both the first and second directions. The initial interlacing density is 5 interlacing points / cm², and the initial thickness-direction yarn ratio is 15%. The initial interlacing density is the ratio of the number of interlacing nodes formed by the thickness-direction nano-reinforced yarns and the first or second yarn group to the area of ​​the three-dimensional interlaced body.

[0178] Step 4: Region Division: Based on the design loads of the stadium canopy (standard values ​​of wind load, standard values ​​of snow load, and design values ​​of pretension), the in-plane stress distribution characteristics of the three-dimensional interwoven body are determined through finite element analysis; based on the tensioning conditions (tensioning stress, boundary constraint method, and target surface shape), the in-plane strain distribution is determined through finite element analysis; the width of the transition region is determined based on the strain gradient in the in-plane strain distribution, and the width of the transition region is negatively correlated with the strain gradient, which is taken as 20mm in this embodiment; the region where the in-plane stress is greater than the preset stress value (70% of the allowable stress value in this embodiment) is divided into the edge anchorage zone, and the region where the in-plane stress is less than or equal to the preset stress value and the distance from the edge anchorage zone is greater than the width of the transition region is divided into the central light-transmitting zone.

[0179] Step 5: Determine the target interlacing density ratio: The peak in-plane stress of the edge anchoring area is 80 MPa, and the average in-plane stress of the central light-transmitting area is 30 MPa. The baseline interlacing density of the edge anchoring area is determined to be 7 interlacings / cm², and the baseline interlacing density of the central light-transmitting area is 3 interlacings / cm². The target interlacing density ratio is 7:3, approximately 2.33.

[0180] Step 6: Determine the number of interlacing nodes and the interlacing angle: The number of interlacing nodes in the edge anchoring zone is 7 / cm² × the area of ​​the edge anchoring zone, and the number of interlacing nodes in the central light-transmitting zone is 3 / cm² × the area of ​​the central light-transmitting zone; the interlacing density in the transition zone decreases linearly according to ρ(x) = 7 - (7 - 3) × x / 20; the interlacing angle in the edge anchoring zone is 45°, the interlacing angle in the central light-transmitting zone is 20°, and the interlacing angle in the transition zone decreases linearly according to θ(x) = 45 - (45 - 20) × x / 20.

[0181] Step 7: Compensation for the proportion of yarns in the thickness direction: The compensation value for the number of yarns in the thickness direction in the edge anchoring area is 30% of the initial number of yarns in the thickness direction, and the compensation value for the number of yarns in the thickness direction in the center light-transmitting area is 15% of the initial number of yarns in the thickness direction. Based on the total number of yarns on the entire membrane surface, the proportion of yarns in the thickness direction after compensation is 15%×(1+30%+15%)=21.75%, of which the proportion of yarns in the thickness direction after compensation in the edge anchoring area is higher than that in the center light-transmitting area.

[0182] Step 8: Introduce and anchor the nanofiber membrane: Determine the distribution density of the nanofiber reinforcing yarn in the thickness direction based on the compensated thickness direction yarn ratio. Determine the introduction position of the nanofiber membrane between the interlacing nodes of two adjacent thickness direction nanofiber reinforcing yarns. The introduction interval is 10mm in the edge anchoring area, 30mm in the center light-transmitting area, and gradually increases from 10mm to 30mm in the transition area along the direction from the edge anchoring area to the center light-transmitting area. Introduce the nanofiber membrane into the interlayer according to the introduction position and introduction interval, and continue to weave the thickness direction nanofiber reinforcing yarn along the thickness direction, so that the thickness direction nanofiber reinforcing yarn passes through the nanofiber membrane and forms interlacing nodes on both sides. The interlacing nodes on both sides are misaligned in the thickness direction, and the misalignment distance is twice the thickness of the nanofiber membrane.

[0183] Step 9, Impregnation Coating: The obtained three-dimensional interwoven body is immersed in a 55% polytetrafluoroethylene dispersion for 4 min, dried at 100℃ for 18 min, baked at 250℃ for 10 min, and sintered at 380℃ for 2.5 min; the above impregnation, drying, baking and sintering steps are repeated 5 times, wherein the first impregnation uses a 55% polytetrafluoroethylene dispersion, and the subsequent impregnation uses a 45% polytetrafluoroethylene dispersion, to obtain a three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material.

[0184] The membrane material prepared according to the above embodiments of the present invention was selected as the experimental group, and the polytetrafluoroethylene building membrane prepared by the prior art was selected as the control group. The areal density of the two membrane materials was basically the same (about 1200g / m²). The interlayer peel strength test, edge tear resistance test, center light transmittance test and wind vibration fatigue test were carried out respectively.

[0185] The preparation process of the control group was as follows: A plain weave fabric of ultrafine glass fiber with an areal density of 1200 g / m² was selected as the base fabric, and a 55% polytetrafluoroethylene (PTFE) dispersion was provided. The base fabric was heat-treated at 380℃ for 2 min, cooled, and then immersed in the 55% PTFE dispersion for 4 min. It was then dried at 100℃ for 18 min, baked at 250℃ for 10 min, and sintered at 380℃ for 2.5 min. This process was repeated five times, with the first immersion using a 55% PTFE dispersion and subsequent immersions using a 45% PTFE dispersion, to obtain the PTFE architectural membrane. The base fabric of the control group had a two-dimensional plain weave structure, with warp and weft yarns crossing only in two directions within the plane. There were no yarn connections in the thickness direction, and the interlayer bonding relied entirely on PTFE resin adhesion. The weaving density and weaving angle of the base fabric were uniform throughout the entire membrane surface.

[0186] The test results are shown in Table 1:

[0187] Table 1

[0188] Test Project experimental group control group Increase Interlayer peel strength (N / cm) 85 42 +102% Edge tear strength (N) 320 180 +78% Center transmittance (%) 18 8 +125% Retention rate of interlaminar peel strength after wind-induced fatigue (%) 92 61 51% Surface density (g / m²) 1200 1200 0

[0189] Test method description:

[0190] The interlayer peel strength was tested according to ASTM D2724 standard, with a sample width of 50 mm and a peeling speed of 100 mm / min. The average value of 5 samples was taken.

[0191] Edge tear strength was tested according to ASTM D5587 standard using the trapezoidal tear method, and the average value of 5 specimens was taken.

[0192] The center transmittance was measured using a spectrophotometer in the visible light band (380–780 nm), and the average value of 5 test points in the center transmittance area was taken.

[0193] The wind-induced fatigue test was conducted on a wind-induced fatigue testing machine. An alternating load amplitude of 30% of the allowable stress of the membrane material was applied at a frequency of 2 Hz, and the number of cycles was 1 million. After the test, the interlayer peel strength was remeasured and the retention rate was calculated.

[0194] The samples in the experimental group and the control group were tested under the same temperature (23±2℃) and relative humidity (50±5%) conditions, using the same testing equipment. Five samples were taken from each group to calculate the average value.

[0195] The comparative tests above show that, under the premise of comparable areal density and identical impregnation coating processes, the three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material prepared by this invention is significantly superior to polytetrafluoroethylene architectural membranes prepared by existing technologies in terms of interlayer peel strength, edge tear resistance, center light transmittance, and retention rate of interlayer peel strength after wind vibration fatigue. This is because this invention achieves differentiated enhancement of regional characteristics in the edge anchoring area (tear resistance), the center light-transmitting area (flexibility and light transmittance), and the interlayer mechanical anchoring through techniques such as three-dimensional interweaving, interweaving density gradient distribution, differentiated interweaving angle settings, thickness direction yarn ratio compensation, and interlayer nanofiber membrane penetration and anchoring. In contrast, existing technologies rely solely on resin bonding for interlayer bonding and lack uniform mechanical properties across the entire membrane surface, failing to meet these multiple requirements simultaneously.

[0196] The technical solution of the present invention has been described above with reference to the preferred embodiments shown in the accompanying drawings. However, it will be readily understood by those skilled in the art that the scope of protection of the present invention is obviously not limited to these specific embodiments. Without departing from the principles of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will all fall within the scope of protection of the present invention.

Claims

1. A method for preparing a three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material, characterized in that, include: Step S1: The polymer solution is sprayed onto the receiving substrate to form a nanofiber membrane, and the nano-reinforcing material is blended with the matrix fiber to obtain a nano-reinforcing yarn. Step S2: The nano-reinforced yarns are interwoven in three spatial directions, and through nano-reinforced yarns are retained in the thickness direction. The through nano-reinforced yarns constitute nano-reinforced yarns in the thickness direction, forming a three-dimensional interwoven body with an initial interweaving density and an initial thickness direction yarn ratio. Step S3: Divide the three-dimensional interwoven body into an edge anchoring area and a central light-transmitting area, and determine the target interweaving density ratio between the edge anchoring area and the central light-transmitting area; Step S4: Determine the number of interlacing nodes according to the target interlacing density ratio, so that the three-dimensional interlacing body has a gradient-changing interlacing density along the direction from the edge anchoring area to the center light-transmitting area; Step S5: Determine the interlacing angle according to the target interlacing density ratio, so that the interlacing angle of the edge anchoring area is greater than the interlacing angle of the center light-transmitting area; and determine the compensation amount of the initial thickness direction yarn ratio according to the ratio of the initial interlacing density to the target interlacing density, and control the number of thickness direction nano-reinforcing yarns according to the compensation amount to obtain the compensated thickness direction yarn ratio. Step S6: Based on the compensated thickness direction yarn ratio, determine the introduction position and introduction interval of the nanofiber membrane between layers, introduce the nanofiber membrane into the interlayer according to the introduction position and introduction interval, and anchor the nanofiber membrane through the thickness direction nanoreinforcing yarn. Step S7: The obtained three-dimensional interwoven body is subjected to several impregnation coating treatments to obtain a three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material.

2. The method for preparing three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material according to claim 1, characterized in that, In step S2, the three-dimensional interwoven body having an initial interweaving density and an initial thickness direction yarn ratio includes: The nano-reinforced yarns are arranged along a first direction to form a first yarn group; The nano-reinforced yarns are arranged along the second direction and interwoven with the first yarn group to form a second yarn group; The nano-reinforced yarns are arranged along a third direction and interwoven with the first yarn group and the second yarn group, while the through nano-reinforced yarns are retained in the thickness direction. The through nano-reinforced yarns constitute the nano-reinforced yarns in the thickness direction, forming the three-dimensional interwoven body. Wherein, the first direction, the second direction, and the third direction are not coplanar; the interlacing node is the intersection point of the thickness-direction nano-reinforced yarn with the first yarn group or the second yarn group; the initial interlacing density is the ratio of the number of interlacing nodes in the three-dimensional interlacing body to the area of ​​the three-dimensional interlacing body; the initial thickness-direction yarn ratio is the proportion of the number of thickness-direction nano-reinforced yarns to the total number of nano-reinforced yarns.

3. The method for preparing three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material according to claim 1, characterized in that, In step S3, the three-dimensional interwoven body is divided into an edge anchoring zone and a central light-transmitting zone, including: Based on the design load of the target application scenario of the architectural membrane material, the in-plane stress distribution characteristics of the three-dimensional interwoven body are determined; Based on the tensioning conditions of the target application scenario of the architectural membrane material, the in-plane strain distribution of the three-dimensional interwoven body during the tensioning process is determined; The width of the transition area between the edge anchoring area and the central light-transmitting area is determined based on the in-plane strain distribution. According to the in-plane stress distribution characteristics, the region in the three-dimensional interwoven body where the in-plane stress is greater than the preset stress value is divided into the edge anchoring zone; The area in the three-dimensional interwoven body where the in-plane stress is less than or equal to the preset stress value and the distance between it and the edge anchoring area is greater than the width of the transition area is defined as the central light-transmitting area.

4. The method for preparing three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material according to claim 3, characterized in that, In step S3, determining the target interlacing density ratio between the edge anchoring area and the central light-transmitting area includes: The reference interlacing density of the edge anchoring zone is determined based on the in-plane stress peak value of the edge anchoring zone. The reference interlacing density of the edge anchoring zone is the number of interlacing nodes per unit area within the edge anchoring zone. The reference interlacing density of the central light-transmitting area is determined based on the average in-plane stress of the central light-transmitting area. The reference interlacing density of the central light-transmitting area is the number of interlacing nodes per unit area within the central light-transmitting area. The target interlacing density ratio is determined based on the ratio of the peak in-plane stress in the edge anchoring zone to the average in-plane stress in the central light-transmitting zone, and the width of the transition region.

5. The method for preparing three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material according to claim 4, characterized in that, In step S4, determining the number of interlacing nodes according to the target interlacing density ratio includes: The number of interlacing nodes in the edge anchorage zone is determined based on the reference interlacing density and the area of ​​the edge anchorage zone. The number of interlacing nodes in the central light-transmitting area is determined based on the reference interlacing density and the area of ​​the central light-transmitting area. Based on the target interlacing density ratio, the number of interlacing nodes in the transition area is determined to decrease from the number of interlacing nodes in the edge anchoring area to the number of interlacing nodes in the center light-transmitting area along the direction from the edge anchoring area to the center light-transmitting area. The rate of decrease in the number of interlaced nodes within the transition region is negatively correlated with the width of the transition region.

6. The method for preparing three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material according to claim 4, characterized in that, In step S5, determining the interlacing angle according to the target interlacing density ratio includes: The interlacing angle of the edge anchoring zone is determined based on the reference interlacing density of the edge anchoring zone; The interlacing angle of the central light-transmitting area is determined based on the reference interlacing density of the central light-transmitting area; Based on the target interlacing density ratio, the interlacing angle within the transition area is determined to decrease from the interlacing angle of the edge anchoring area to the interlacing angle of the center light-transmitting area along the direction from the edge anchoring area to the center light-transmitting area; The deceleration rate of the interlacing angle within the transition region is negatively correlated with the width of the transition region.

7. The method for preparing three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material according to claim 1, characterized in that, In step S5, the compensated thickness direction yarn percentage is obtained, including: Based on the ratio of the initial interlacing density to the target interlacing density, determine the thickness direction yarn quantity compensation value of the edge anchoring zone and the thickness direction yarn quantity compensation value of the central light-transmitting zone; The number of nano-reinforcing yarns in the thickness direction of the edge anchoring area is controlled according to the compensation value of the number of yarns in the thickness direction of the edge anchoring area; the number of nano-reinforcing yarns in the thickness direction of the central light-transmitting area is controlled according to the compensation value of the number of yarns in the thickness direction of the central light-transmitting area. The ratio of the sum of the number of thickness-direction nano-reinforcing yarns in the edge anchoring area and the number of thickness-direction nano-reinforcing yarns corresponding to the initial thickness-direction yarn ratio to the total number of nano-reinforcing yarns is used as the compensated thickness-direction yarn ratio. The thickness direction yarn quantity compensation value of the edge anchoring zone is greater than the thickness direction yarn quantity compensation value of the central light-transmitting zone.

8. The method for preparing three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material according to claim 7, characterized in that, In step S6, the introduction position and spacing of the nanofiber membrane between layers are determined based on the compensated thickness direction yarn ratio, including: The distribution density of nano-reinforcing yarns in the thickness direction in the three-dimensional interwoven body is determined based on the compensated thickness direction yarn ratio. The introduction position of the nanofiber membrane between layers is determined based on the distribution density of the nanofiber reinforcing yarn in the thickness direction. The introduction position is located between the interlacing nodes of two adjacent nanofiber reinforcing yarns in the thickness direction. The introduction interval of the nanofiber membrane between layers is determined based on the distribution density of the nanofiber reinforcing yarn in the thickness direction, and the introduction interval is negatively correlated with the distribution density of the nanofiber reinforcing yarn in the thickness direction.

9. The method for preparing three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material according to claim 7, characterized in that, In step S6, the nanofiber membrane is anchored through the thickness-direction nanoreinforced yarn, including: After introducing the nanofiber membrane into the interlayer, the nanofiber reinforcing yarn in the thickness direction is continued to be woven along the thickness direction; The thickness-direction nano-reinforcing yarn is passed through the nanofiber membrane, and interlacing nodes are formed on both sides of the nanofiber membrane. The interlacing nodes on both sides of the nanofiber membrane are misaligned in the thickness direction.

10. The method for preparing three-dimensional interwoven nano-reinforced ultra-high strength architectural membrane material according to claim 1, characterized in that, The impregnation coating process involves immersing the obtained three-dimensional interwoven body in a polymer dispersion, followed by drying, baking, and sintering, repeated several times.

Citation Information

Patent Citations

  • Method for preparing polytetrafluoroethylene building membrane

    CN105128350A