A variable thickness night navigation lamp skin non-thermal press tank forming method based on partitioned wax sheet paving
By combining a variable-thickness silicone rubber male mold with a rigid female mold through partitioned wax sheet application, the problems of heavy weight, low precision, and high cost in the molding of drone night navigation light skin were solved, achieving high-strength, lightweight, and low-cost night navigation light skin molding.
Patent Information
- Application Number
- CN202610964980.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-30
- Publication Date
- 2026-11-20
AI Technical Summary
Existing drone night navigation light skin molding processes suffer from problems such as heavy weight, low molding precision, poor fatigue resistance, poor electromagnetic compatibility, large investment in autoclave equipment, high energy consumption, high unit manufacturing cost, and easy slippage and fiber twisting of prepreg layers in areas of abrupt thickness changes.
A variable-thickness silicone rubber male mold is prepared by partitioned wax sheet application and combined with a rigid female mold. Different thickness wax sheets are applied to the reinforced area and the normal area of the product, respectively. After the silicone rubber is poured, a variable-thickness male mold with a difference in the depth of the recess is formed. This ensures that the prepreg naturally forms a variable-thickness structure when the mold is closed and cured, which solves the problem that it is difficult to accurately form variable-thickness thin-walled parts on traditional molds.
It enables precise molding of the night navigation light skin, reduces mold costs, lightens product weight, improves fatigue life, meets the high-strength requirements of UAVs, and reduces the manufacturing cost per unit.
Smart Images

Figure CN123129485A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of composite material manufacturing technology for unmanned aerial vehicles (UAVs), specifically to a non-autoclave molding method for variable thickness night navigation light skin based on partitioned wax sheet application. Background Technology
[0002] With the widespread application of drones in nighttime logistics delivery, emergency rescue, and low-altitude inspection, night navigation light systems have become one of the standard configurations for drones. As the outer shell structure of the night navigation light, the night navigation light skin is installed on the wingtip or outer side of the fuselage. As a structural load-bearing component, it bears the aerodynamic load, vibration load, and landing impact load during flight. At present, the night navigation light skin is generally made of carbon fiber composite material to meet the requirements of lightweight, high strength, and complex aerodynamic shape. The existing molding process of drone night navigation light skin and similar thin-walled shell parts has the following significant defects: (1) Stamping and forming with aluminum alloy or stainless steel plates results in large weight, low forming accuracy, poor fatigue resistance, and poor electromagnetic compatibility; (2) Using autoclave molding equipment requires large investment, consumes a lot of energy, and has a high cost per piece; (3) When using vacuum bag curing process to lay on curved streamline shape, the prepreg layer in the thickness change area is prone to slippage and fiber twisting during the curing process. Summary of the Invention
[0003] Based on the problems existing in the above-mentioned background technology, the present invention provides a non-autoclave molding method for the skin of a night navigation light based on partitioned wax sheet laying. The method prepares a variable thickness silicone rubber positive mold by partitioned wax sheet laying, that is, by laying wax sheets of different thicknesses in the reinforced area and the ordinary area of the product respectively, and then pouring silicone rubber to form a variable thickness positive mold with a difference in the depth of the depression. This allows the prepreg after laying to naturally form a variable thickness structure when the mold is closed and cured, thus solving the problem that it is difficult to accurately form variable thickness thin-walled parts on traditional molds.
[0004] To achieve the above-mentioned objectives, the present invention adopts the following technical solution: A non-autoclave molding method for variable thickness navigation light skin based on partitioned wax sheet application includes the following steps: (1) Mold preparation: The mold is divided into two parts: a rigid female mold and a variable thickness silicone rubber male mold. The variable thickness silicone rubber male mold achieves the variable thickness design of the night navigation light skin by partitioning wax sheets. The preparation of the rigid female mold is as follows: based on the three-dimensional digital model of the night navigation light skin, a rigid female mold is formed by processing Q235B carbon structural steel. The inner surface matches the shape of the outer aerodynamic surface of the night navigation light skin and serves as the forming reference surface for the outer aerodynamic surface of the product. The product is formed on the inner surface of the female mold, and the outer aerodynamic surface is in direct contact with the inner surface of the female mold, so the two shapes are perfectly matched. The preparation of the variable thickness silicone rubber positive mold is as follows: wax sheets are laid on the inner surface of the rigid negative mold according to the variable thickness area of the night navigation light skin. After the wax sheets are laid, the mold is closed and locked. After pouring in silicone rubber and curing at room temperature for ≥24 hours, the mold is demolded to obtain the variable thickness silicone rubber positive mold. (2) Material preparation: High-performance carbon fiber prepreg is selected as raw material. Among them, T700 grade carbon fiber / epoxy resin prepreg is used for the main structural layer, T300 grade carbon fiber / epoxy resin prepreg is used for the inner and outer surface layers, and glass fiber prepreg is used for the outermost auxiliary layer to ensure the lightweight and high strength performance of the product. (3) Material laying and mold assembly: Carbon fiber prepreg is laid on the surface of the silicone rubber male mold in the design layering sequence to form a preform; then it is closed and locked with the rigid female mold to ensure the sealing of the molding cavity; the depth of the silicone rubber male mold is controlled by wax sheet in the variable thickness area, so that the reinforced area can obtain more resin enrichment during mold closing and curing, forming a natural thickness difference. (4) Curing process: The assembled mold and preforms are placed in an oven for heating and curing: The silicone rubber positive mold expands after being heated. No additional external pressure is required during the curing process. The molding pressure is provided entirely by the thermal expansion force of the silicone rubber. After curing, the variable thickness night navigation light skin is obtained by demolding when the temperature is ≤60℃.
[0005] Further, in step (1) of preparing the variable thickness silicone rubber positive mold, the wax sheet laying design is as follows: the wax sheet laying area is divided into a reinforced area and a normal area. The reinforced area corresponds to the load-bearing reinforced area of the night navigation light skin (including the periphery of the installation interface and the high-stress area), and the normal area corresponds to the non-load-bearing or low-load-bearing area of the night navigation light skin. The wax sheet laying thickness of the reinforced area and the normal area should match the thickness of different areas of the night navigation light skin product, and the wax sheet laying thickness of the reinforced area is greater than that of the normal area. When the wax sheets of the reinforced area and the normal area are laid at the junction, a stepped overlap transition is adopted, that is, the wax sheet thickness of the reinforced area is gradually reduced from the wax sheet thickness of the reinforced area along the transition area in a step-decreasing manner according to the number of wax sheet layers to the wax sheet thickness of the normal area, to ensure that the transition area is smooth without abrupt changes. The purpose is to form a smooth thickness transition between the reinforced area and the normal area, and to avoid stress concentration and prepreg slippage caused by abrupt changes in thickness.
[0006] Furthermore, the thickness deviation of the wax sheet in the reinforced area is controlled within ±0.15mm, and the thickness deviation of the wax sheet in the ordinary area is controlled within ±0.1mm.
[0007] Furthermore, the planar dimensions of the wax sheet are determined by the outline of the material sheet, and it is cut to conform to the shape along the product allowance line during application.
[0008] Furthermore, in step (1) the preparation of the variable thickness silicone rubber positive mold, the silicone rubber injection method is as follows: the prepared silicone rubber is slowly injected along the mold wall after the mold is closed to avoid generating a large number of air bubbles. After the mold cavity is completely filled (i.e. the silicone rubber liquid level rises to the height of the contact surface of the top metal mold), the top metal mold is closed.
[0009] Furthermore, the silicone rubber mentioned in step (1) is a two-component silicone rubber of components A and B, wherein component A is addition-curing silicone rubber 635T and component B is a curing agent. The weight ratio of components A and B is 100:1.5~2, and the components are weighed accurately using an electronic scale. Furthermore, the silicone rubber is prepared by mixing components A and B and stirring for 3~4 minutes to ensure that the bottom of the container and the container wall are fully stirred. Then, it is degassed under a vacuum of -0.1MPa for 3~4 minutes before use.
[0010] Furthermore, the layup design in step (3) is as follows: the first layer uses glass fiber prepreg; the second and last layers use T300 grade carbon fiber prepreg, and the layup direction is designed to be ±45°; the remaining layers use T700 grade carbon fiber prepreg, and the layup direction is alternately laid up at 45°, 0°, -45° and 0°, and the layup is symmetrical.
[0011] Furthermore, in step (3), the average gap between the mold joints is <0.2mm, and the dimensional tolerance of the molding die is controlled within ±0.12mm.
[0012] Further, the curing procedure in step (4) is as follows: first, heat the temperature to 130-140℃ at a rate of 0.5-1.5℃ / min, then keep it at that temperature for 140-160min, and then cool the temperature to 60℃ at a rate of 1-3℃ / min to finish curing.
[0013] Compared with the prior art, the present invention has the following beneficial effects: (1) Controllable thickness: The present invention prepares a silicone rubber positive mold with variable thickness by laying wax sheets in sections. The thickness deviation of the reinforced area is controlled within ±0.15mm, the thickness deviation of the ordinary area is controlled within ±0.1mm, and the transition area of variable thickness is smooth without steps, which meets the differentiated load-bearing requirements of the night navigation light skin.
[0014] (2) Significantly reduced costs: This invention eliminates the need for autoclave equipment investment, reduces mold costs by 60%, and lowers the manufacturing cost of a single product by 45% compared to the autoclave process, which is highly compatible with the cost positioning of night navigation lights as accessories for UAVs.
[0015] (3) Excellent product performance: The T300 / T700 hybrid layup design of this invention ensures the mechanical properties of the structure. The product porosity is ≤0.5%, the interlaminar shear strength is ≥65MPa, the mechanical properties reach the same level as those of autoclave molding, and the fatigue life is more than 5 times that of metal skin, meeting the fatigue life requirement of more than 10,000 hours for UAVs.
[0016] (4) Lightweight: The product of this invention is more than 50% lighter than that of metal skin. Attached Figure Description
[0017] Figure 1 This is a schematic cross-sectional view of the silicone rubber male mold described in this invention.
[0018] Figure 2 This is a schematic diagram of the silicone rubber male mold structure described in this invention.
[0019] Figure 3 This is a schematic diagram showing the disassembly of the rigid female mold structure described in this invention.
[0020] Figure 4 This is a schematic diagram of the cross-section of the rigid female mold described in this invention.
[0021] The following are labeled in the diagram: 1. Cover plate, 2. Left mold template, 3. Right mold template, 4. Locking screw hole, 5. Positioning pin, 6. Demolding groove, 7. Positioning boss. Detailed Implementation
[0022] The present invention will be further described below with reference to specific embodiments and accompanying drawings.
[0023] The mold used in the molding method of the present invention is divided into two parts: a rigid female mold and a variable thickness silicone rubber male mold. The rigid female mold includes 1 cover plate, 2 left mold template, 3 right mold template, 4 locking screw hole, 5 positioning pin, 6 demolding groove, and 7 positioning boss.
[0024] Example 1 The non-autoclave molding method for variable thickness night navigation light skin based on partitioned wax sheet application described in this embodiment includes the following steps: (1) Mold preparation: The mold is divided into two parts: a rigid female mold and a variable thickness silicone rubber male mold. The variable thickness silicone rubber male mold achieves the variable thickness design of the night navigation light skin by partitioning wax sheets. The preparation of the rigid female mold is as follows: based on the three-dimensional digital model of the night navigation light skin, a rigid female mold is formed by processing Q235B carbon structural steel. The inner surface matches the shape of the outer aerodynamic surface of the night navigation light skin and serves as the forming reference surface for the outer aerodynamic surface of the product. The product is formed on the inner surface of the female mold, and the outer aerodynamic surface is in direct contact with the inner surface of the female mold, so the two shapes are perfectly matched. The preparation of the variable thickness silicone rubber positive mold is as follows: Wax sheets are laid on the inner surface of the rigid negative mold according to the variable thickness area of the night navigation light skin. After the wax sheets are laid, the mold is closed and locked. The prepared silicone rubber is slowly injected along the mold wall after the mold is closed to avoid generating a large number of air bubbles. After the mold cavity is completely filled (i.e. the silicone rubber liquid level rises to the height of the contact surface of the top metal mold), the top metal mold is closed. After curing at room temperature for ≥24 hours, the mold is demolded to obtain the variable thickness silicone rubber positive mold. The wax sheet application design is as follows: A 12.5mm wide area extending 25mm upwards from the bottom net dimension line of the product is designated as the reinforcement zone, with a design thickness of 2.94mm and a silicone rubber wax sheet thickness of 3.0mm. The remaining areas are designated as the standard thickness zone, with a thickness of 1.69mm and a silicone rubber wax sheet thickness of 2.0mm. The reinforcement zone corresponds to the load-bearing reinforcement areas of the navigation light skin (such as around installation interfaces and high-stress areas), while the standard zone corresponds to non-load-bearing or low-load-bearing areas. The wax sheet application thickness ratio between the reinforcement and standard zones is 3:2. At the junction of the reinforcement and standard zones, a stepped overlap transition is used, meaning the wax sheet thickness decreases gradually from the reinforcement zone along the transition zone, down to the standard zone thickness, ensuring a smooth transition without abrupt changes. The purpose is to create a smooth thickness transition between the reinforcement and standard zones, avoiding stress concentration and prepreg slippage caused by abrupt thickness changes. The thickness deviation of the reinforced area is controlled within ±0.15mm, and the thickness deviation of the ordinary area is controlled within ±0.1mm; the planar dimensions of the wax sheet are determined by the outline of the material sheet, and it is cut along the product allowance line during installation.
[0025] The silicone rubber is a two-component silicone rubber, A and B. Component A is addition-curing silicone rubber 635T, and component B is a curing agent. The weight ratio of components A to B is 100:1.75, and the components are weighed precisely using an electronic scale. Furthermore, the silicone rubber is prepared by mixing components A and B and stirring for 3 to 4 minutes to ensure that the bottom and walls of the container are fully stirred. Then, it is degassed under a vacuum of -0.1 MPa for 3 to 4 minutes before use. (2) Material preparation: High-performance carbon fiber prepreg is selected as raw material. Among them, T700 grade carbon fiber / epoxy resin prepreg is used for the main structural layer, T300 grade carbon fiber / epoxy resin prepreg is used for the inner and outer surface layers, and glass fiber prepreg is used for the outermost auxiliary layer to ensure the lightweight and high strength performance of the product. (3) Material laying and mold assembly: Carbon fiber prepreg is laid on the surface of the silicone rubber male mold in the designed layering sequence to form a preform; the depth of the silicone rubber male mold in the variable thickness area is controlled by wax sheets, so that the reinforced area can obtain more resin enrichment during mold closing and curing, forming a natural thickness difference. Then it is closed and locked with the rigid female mold to ensure the sealing of the molding cavity; This embodiment features a 23-layer layup design. The first layer is glass fiber prepreg (DSBBP-100 / DS1202.1), the second and 23rd layers are T300 grade carbon fiber prepreg ±45° (BE121 / 40% / 3KSM200T / W12), and the remaining layers are T700 grade carbon fiber prepreg (BE121 / 33% / UD133 / SM87). A total of 20 sheets / pack of T700 prepreg and 20 sheets / pack of T300 prepreg are used. The details are shown in Table 1 below: Table 1. Layer design for Example 1 The average gap between the mold joints is <0.2mm, and the dimensional tolerance of the molding die is controlled within ±0.12mm; (4) Curing process: The assembled mold and preforms are placed in an oven for heating and curing: The silicone rubber positive mold expands after being heated. No additional external pressure is required during the curing process. The molding pressure is provided entirely by the thermal expansion force of the silicone rubber. After curing, the variable thickness night navigation light skin is obtained by demolding when the temperature is ≤60℃. Step (4) Curing procedure: First, heat to 135℃ at a rate of 1℃ / min, then keep warm for 150min, and then cool down to 60℃ at a rate of 2℃ / min to finish curing.
[0026] Test results: The product's appearance quality is qualified, the thickness of the reinforced area is 2.94±0.147mm, the porosity is ≤0.5%, and the interlaminar shear strength is ≥65MPa, meeting the design requirements.
[0027] Comparative Example 1 The same product was prepared using an autoclave molding method. Mold preparation: The same rigid female mold as in Example 1 is used, and the silicone rubber male mold does not use partitioned wax sheet laying (i.e., equal thickness male mold).
[0028] Materials: Same as in Example 1.
[0029] Laying: Same layup design as in Example 1.
[0030] Curing: Curing is carried out in an autoclave at a pressure of 0.3~0.6MPa, a temperature of 135±5℃, and a holding time of 150±10min.
[0031] Test results: The product's appearance quality is qualified, the thickness of the reinforced area is not significantly different from that of the ordinary area (variable thickness needs to be achieved through additional lay-up), the porosity is ≤0.5%, and the interlaminar shear strength is ≥65MPa.
[0032] The products obtained from Example 1 and Comparative Example 1 were tested, and their performance is shown in Table 2.
[0033] Table 2 Performance Comparison of Examples and Comparative Examples The results in Table 1 show that: This invention prepares a variable-thickness silicone rubber male mold by laying wax sheets in sections. The thickness deviation of the reinforced area is controlled within ±0.15mm, and the thickness deviation of the ordinary area is controlled within ±0.1mm. The mold cost is reduced by 60%, and the manufacturing cost of a single product is reduced by 45% compared with the autoclave process. The porosity of the product of this invention is ≤0.5%, the interlaminar shear strength is ≥65MPa, and the fatigue life is more than 5 times that of metal skin, meeting the fatigue life requirement of more than 10,000 hours for UAVs.
Claims
1. A non-autoclave molding method for variable thickness night navigation light skin based on partitioned wax sheet application, characterized in that, Includes the following steps: (1) Mold preparation: The mold is divided into two parts: a rigid female mold and a variable thickness silicone rubber male mold. The variable thickness silicone rubber male mold achieves the variable thickness design of the night navigation light skin by partitioning wax sheets. The preparation of the rigid female mold is as follows: based on the three-dimensional digital model of the night navigation light skin, a rigid female mold is formed by processing Q235B carbon structural steel. The inner surface matches the shape of the outer aerodynamic surface of the night navigation light skin and serves as the forming reference surface for the outer aerodynamic surface of the product. The product is formed on the inner surface of the female mold, and the outer aerodynamic surface is in direct contact with the inner surface of the female mold, so the two shapes are perfectly matched. The preparation of the variable thickness silicone rubber positive mold is as follows: wax sheets are laid on the inner surface of the rigid negative mold according to the variable thickness area of the night navigation light skin. After the wax sheets are laid, the mold is closed and locked. After pouring in silicone rubber and curing at room temperature for ≥24 hours, the mold is demolded to obtain the variable thickness silicone rubber positive mold. (2) Material preparation: High-performance carbon fiber prepreg is selected as raw material. Among them, T700 grade carbon fiber / epoxy resin prepreg is used for the main structural layer, T300 grade carbon fiber / epoxy resin prepreg is used for the inner and outer surface layers, and glass fiber prepreg is used for the outermost auxiliary layer. (3) Material laying and mold assembly: Carbon fiber prepreg is laid on the surface of the silicone rubber male mold in the designed layering sequence to form a preform; then it is closed and locked with the rigid female mold to ensure the sealing of the molding cavity; (4) Curing process: The assembled mold and prefabricated parts are placed in an oven for heating and curing. After curing, the mold is demolded when the temperature is ≤60℃ to obtain the variable thickness night navigation light skin.
2. The non-autoclave molding method for variable thickness navigation light skin according to claim 1, characterized in that, In step (1), the wax sheet laying design for the preparation of the variable thickness silicone rubber positive mold is as follows: The wax sheet application area is divided into a reinforced area and a normal area. The reinforced area corresponds to the load-bearing reinforced area of the navigation light skin, and the normal area corresponds to the non-load-bearing or low load-bearing area of the navigation light skin. The thickness of the wax sheets in the reinforced and ordinary areas is matched with the thickness of different areas of the night navigation light skin product, and the thickness of the wax sheets in the reinforced area is greater than that in the ordinary area. When the wax sheets in the reinforced and ordinary areas are laid at the junction, a stepped overlap transition is adopted, that is, the thickness of the wax sheets in the reinforced area is gradually reduced from the thickness of the wax sheets in the transition area to the thickness of the wax sheets in the ordinary area in a stepped manner, so as to ensure that the transition area is smooth and without abrupt changes.
3. The non-autoclave molding method for variable thickness navigation light skin according to claim 2, characterized in that, The thickness deviation of the wax sheet in the reinforced area is controlled within ±0.15mm, and the thickness deviation of the wax sheet in the ordinary area is controlled within ±0.1mm.
4. The non-autoclave molding method for variable thickness navigation light skin according to claim 2, characterized in that, The planar dimensions of the wax sheet are determined by the outline of the material sheet, and it is cut to fit the shape along the product allowance line during application.
5. The non-autoclave molding method for variable thickness navigation light skin according to claim 1, characterized in that, In step (1) the preparation of the variable thickness silicone rubber positive mold, the silicone rubber injection method is as follows: the prepared silicone rubber is slowly injected along the mold wall after the mold is closed to avoid generating a large number of air bubbles. After the mold cavity is completely filled, the top metal mold is closed.
6. The non-autoclave molding method for variable thickness navigation light skin according to claim 1, characterized in that, The silicone rubber mentioned in step (1) is a two-component silicone rubber of A and B, wherein component A is addition-curing silicone rubber 635T and component B is a curing agent, and the weight ratio of components A to B is 100:1.5~2. The silicone rubber is prepared by mixing components A and B and stirring for 3-4 minutes to ensure that the bottom and wall of the container are fully stirred. Then, it is degassed under a vacuum of -0.1MPa for 3-4 minutes before use.
7. The non-autoclave molding method for variable thickness navigation light skin according to claim 1, characterized in that, In step (3), the layup design is as follows: the first layer uses glass fiber prepreg; the second and last layers use T300 grade carbon fiber prepreg, and the layup direction is designed to be ±45°; the remaining layers use T700 grade carbon fiber prepreg, and the layup direction is alternately laid up at 45°, 0°, -45° and 0°, and the layup is symmetrical.
8. The non-autoclave molding method for variable thickness navigation light skin according to claim 1, characterized in that, Step (3) The average gap between the mold joints is <0.2mm, and the dimensional tolerance of the forming mold is controlled within ±0.12mm.
9. The non-autoclave molding method for variable thickness navigation light skin according to claim 1, characterized in that, Step (4) Curing procedure: First, heat to 130-140℃ at a rate of 0.5-1.5℃ / min, then keep warm for 140-160min, and then cool down to 60℃ at a rate of 1-3℃ / min to finish curing.