A carbon fiber material special-shaped co-curing integrated forming process

By using urchin-shaped mesoporous silica nanospheres to modify the resin and a dynamic pressure control algorithm, a one-time integral co-curing molding of the closed cavity structure inside the irregularly shaped carbon fiber composite component was achieved. This solved the problems of reusability of the inner membrane and high-temperature stability, and improved the dimensional accuracy and surface quality of the product.

CN123129487APending Publication Date: 2026-11-20ANHUI HAOXIANG AVIATION TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611517391.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies make it difficult to achieve one-time integral co-curing molding of closed cavity structures in irregularly shaped carbon fiber composite components, and there are problems such as the inner membrane not being reusable, insufficient high-temperature resistance, and poor product dimensional accuracy and surface quality.

Method used

High-temperature resistant thermoplastic resin modified with sea urchin-shaped mesoporous silica nanospheres is used as the polymer inner membrane. Combined with a dynamic pressure control algorithm, the uniform compaction and high-precision molding of carbon fiber prepreg are achieved through the synergistic effect of positive and negative pressure.

Benefits of technology

It enables one-time integral co-curing molding of carbon fiber irregular components, and the inner membrane can be reused, which improves the dimensional accuracy and surface quality of the product and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123129487A_ABST
    Figure CN123129487A_ABST
Patent Text Reader

Abstract

The application belongs to the field of unmanned aerial vehicle shell manufacturing, and particularly relates to a carbon fiber material special-shaped co-curing integrated process, which adopts sea urchin-shaped mesoporous silica nanospheres to modify high-temperature-resistant thermoplastic resin to prepare a rigid / semi-rigid split high polymer inner film, realizes linear controllable micro-deformation, and simultaneously adopts a dynamic pressure control algorithm of a modified power function basic pressure curve superimposed with positive and negative pressure synchronous pulses in a curing temperature rising process. The polymer inner film provides an accurate deformation response basis for the dynamic pressure control algorithm, and the dynamic pressure control algorithm fully plays the regulation and control advantages of the polymer inner film, and the two are indispensable. The special-shaped component prepared by the process has a key matching surface size deviation of not more than ±0.05 mm, a porosity as low as 0.2%, a smooth inner and outer surface, and the inner film can be repeatedly used, and is suitable for batch production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of UAV shell manufacturing technology, specifically relating to a co-curing integral molding process for irregularly shaped carbon fiber materials; it is particularly suitable for the integral molding and manufacturing of irregularly shaped carbon fiber composite components with an internal closed cavity structure. Background Technology

[0002] Carbon fiber reinforced thermosetting resin matrix composites are widely used in high-end manufacturing fields such as aerospace, drones, high-performance ships, and the automotive industry due to their outstanding advantages, including high specific strength, high specific modulus, excellent fatigue resistance, low coefficient of thermal expansion, and strong designability. With the increasing demands for lightweight, integrated, and complex components in these fields, the demand for irregularly shaped carbon fiber composite components with internally enclosed cavity structures is growing, such as drone fuselages, unmanned vessel hulls, and irregularly shaped multi-port pipe fittings.

[0003] Currently, for irregularly shaped carbon fiber composite components with internally enclosed cavity structures, the existing technologies mainly have the following technical solutions and their defects:

[0004] 1. Traditional secondary bonding molding process: For cavity-type carbon fiber components, the two half-shells of the component are usually prepared separately, and then the two half-shells are combined by adhesive bonding or mechanical connection to form a closed cavity structure. This process has inherent defects such as poor product consistency, low reliability of bonded area strength, insufficient overall component integrity, need for secondary processing and assembly, long production cycle and high cost. The bonded interface is also at risk of aging and debonding during long-term service.

[0005] 2. Nylon Air Bag Assisted Molding Process: A nylon air bag is used as an inner mold, and pressurized air is injected into the bag to make the prepreg adhere to the mold. In this process, the nylon bag is a disposable consumable and cannot be reused; the pressure distribution of the air bag is limited, resulting in poor dimensional accuracy; there is a risk of bag bursting; and the temperature resistance of nylon bags typically does not exceed 200℃, making them unsuitable for high-temperature curing systems.

[0006] 3. Molding process based on flexible silicone inner mold: For example, CN116100711A discloses a carbon fiber molding die and its process based on a silicone inner mold. However, silicone material has insufficient dimensional stability and durability above 200℃, and its coefficient of thermal expansion differs significantly from that of carbon fiber composite materials. Thermal mismatch at high temperatures leads to a decrease in product dimensional accuracy. More importantly, the flexible silicone inner mold cannot provide a stable geometric reference for the inner cavity under curing pressure, making it difficult to guarantee the inner cavity accuracy of complex irregular components.

[0007] 4. Molding process based on degradable or peelable inner mold materials: such as the technologies disclosed in CN117024674A and CN117024919A, the inner mold can be removed or reused through the chemical properties of the material. However, when degradable inner molds are demolded, decomposition products may remain and affect the quality of the inner surface. Peelable inner molds are complicated to operate and it is difficult to guarantee the complete demolding of large and complex components.

[0008] 5. Autoclave vacuum bag forming process: As the mainstream forming process for aerospace composite materials, it requires a large amount of disposable auxiliary materials, and the laying operation is complicated, time-consuming, and has low production efficiency, making it difficult to meet the needs of mass production.

[0009] In summary, the existing technology lacks a molding process for irregularly shaped carbon fiber composite components that can simultaneously meet the following requirements: (1) one-time integral co-curing molding of an internally enclosed cavity structure; (2) reusable inner membrane; (3) high temperature resistance; and (4) high dimensional accuracy and good internal and external surface quality. Therefore, developing a new type of integral co-curing molding process for irregularly shaped carbon fiber materials has significant technical and economic value. Summary of the Invention

[0010] The purpose of this invention is to provide a process for integral molding of irregularly shaped carbon fiber materials through co-curing, in order to solve the above-mentioned problems.

[0011] Firstly, a modified high-temperature resistant thermoplastic resin with sea urchin-shaped mesoporous silica nanospheres as reinforcing fillers was used to prepare a rigid / semi-rigid segmented polymer inner membrane as a composite material. Through the unique morphology and structure of the sea urchin-shaped mesoporous silica nanospheres and the resulting mechanical interlocking mechanism, the polymer inner membrane exhibits linearly controllable micro-deformation (compressive strain 0.2%~1.5%) within a normal pressure range of 0.1~1.0 MPa. It exhibits excellent cyclic stability (the strain drift rate does not exceed 10% after 100 pressure cycles) and suppresses high-temperature creep (the cumulative creep strain increment does not exceed 20% of the initial compressive strain after 3 hours of curing at the curing temperature).

[0012] Secondly, a dynamic pressure control algorithm is adopted during the curing and heating process. The base pressure changes nonlinearly with temperature in the form of a power function. The positive pressure increases slowly in the early stage and accelerates in the later stage to match the needs of the venting window and compaction stage. At the same time, the nonlinear growth compensates for the thermal expansion of the inner membrane. In the later stage of the venting stage before resin gelation, positive pressure pulses and negative pressure pulses are superimposed within the preset temperature window. The two work together to efficiently remove the residual volatiles inside the prepreg.

[0013] Thirdly, this invention uses urchin-like mesoporous silica nanospheres as reinforcing fillers to modify the resin. The resulting modified resin granules exhibit linearly controllable micro-deformation properties, which are the basis for the reliable implementation of the dynamic pressure control algorithm. When the polymer inner membrane exhibits linear stress-strain within the range of 0.1~1.0 MPa (… When the pressure is applied correctly, precise size control and uniform pressure can be achieved. Conversely, if the deformation characteristics of the polymer inner membrane are nonlinear, there is no stable mapping relationship between pressure change and deformation response. The adjustment intention of the dynamic pressure control algorithm cannot be accurately executed, resulting in a significant deterioration in dimensional accuracy and compaction uniformity.

[0014] In this application, compressive strain refers to the macroscopic structural deformation rate of the polymer inner membrane along its thickness direction under normal pressure. It is related to the membrane's geometry (segmented structure, wall thickness, cavity shape), support conditions, and load transfer method, and is not equal to the standard compressive strain measured in a uniaxial compression test. When the stress-strain linearity of the polymer inner membrane material reaches a certain level within a low stress range... At the same time, the macroscopic structural deformation rate of the inner membrane also maintains a linear mapping relationship with the applied pressure, which is the basis for the dynamic pressure control algorithm to be accurately executed on polymer inner membranes.

[0015] The modification mechanism of traditional nanofillers in polymer matrices contains an inherent contradiction: to improve modulus (reinforcement), it is necessary to increase the filler content or increase the specific surface area to enhance interfacial interactions; however, excessively strong interfacial interactions can lead to sudden debonding of the interface or local yielding of the matrix under increased stress, resulting in a nonlinear stress-strain relationship and making it impossible to achieve linearly controllable micro-deformation. Conversely, if the filler content is reduced to maintain deformation compliance, the modulus improvement is insufficient, and the inner membrane cannot provide adequate geometric support. In addition, traditional fillers also have poor deformation characteristics retention under repeated pressure cycles and long-term high-temperature loading.

[0016] The urchin-shaped mesoporous silica nanospheres of this invention effectively solve the problem of the strong-toughness mutual repulsion of resins, and their mechanism is more efficient than that of conventional mesoporous materials. Their core (solid or hollow) provides rigid support to bear stress, while the mesoporous channels (smaller inside, larger outside) expand in a conical shape from the inside out, creating a mechanical barb-like locking effect on the polymer chains deep within the channels under stress, ensuring efficient transmission of interfacial stress to enhance strength. Simultaneously, hundreds of open pores and protrusions on the surface form topological entanglements with the molecular chains, allowing restricted slippage of chain segments under external force to dissipate impact energy. At the microscale, simultaneous reinforcement and toughening are achieved through the synergistic effects of physical anchoring, controllable slippage, and crack modulation. This solves the strong-toughness mutual repulsion problem faced by traditional nanofillers.

[0017] Conventional mesoporous silica typically has straight, uniform-diameter pores with an excessively high specific surface area. When resin molecular chains are subjected to force, they are prone to slipping out of the pores and cannot be effectively locked in place. At the same time, the excessively high specific surface area will cause a large amount of curing agent to be adsorbed, resulting in the formation of an over-crosslinked, hard, and brittle layer around the particles. This not only makes it difficult to toughen the material but also exacerbates the brittle fracture of the material.

[0018] This invention provides a process for integral molding of irregularly shaped carbon fiber materials through co-curing, comprising the following steps:

[0019] Step S1: Provide a polymer inner membrane, which has a segmented structure, including multiple segmented modules. Each segmented module cooperates with each other through a positioning structure, and each segmented module has a cavity inside. The shape of the polymer inner membrane matches the inner cavity shape of the carbon fiber material irregular co-cured component (finished product). The outer mold material can be metal or the same material as the finished product. A permanent coating can be applied to the inner wall of the outer mold, or a consumable release agent can be applied.

[0020] The polymer inner membrane is made of a modified high-temperature resistant thermoplastic resin-based composite material. This composite material uses polyimide resin or polyetheretherketone resin as the matrix resin, and adds urchin-shaped mesoporous silica nanospheres and a coupling agent. This allows the polymer inner membrane to achieve the following properties: compressive strain of 0.2%~1.5% under a normal pressure of 0.6 MPa, and a linear stress-strain relationship within the range of 0.1~1.0 MPa, with a linear correlation coefficient of... Furthermore, after 100 pressure cycles under a positive pressure of 0.6 MPa, the compressive strain drift rate does not exceed 10%; and after being kept at the curing temperature for 3 hours, the cumulative creep strain increment does not exceed 20% of the initial compressive strain.

[0021] Step S2: Lay multiple layers of carbon fiber prepreg on the outer surface of the polymer inner membrane to form a carbon fiber prepreg layup structure.

[0022] Step S3: Place the polymer inner membrane covered with carbon fiber prepreg layer structure into the cavity of the outer mold, and close the mold to form a closed mold system; the mold system is provided with a positive pressure channel and a negative pressure channel, the positive pressure channel is connected to the cavity inside the polymer inner membrane (the cavity inside each segment module), and the negative pressure channel is connected to the gap between the cavity of the outer mold and the carbon fiber prepreg layer structure;

[0023] Step S4: The mold system is fed into an autoclave. Positive pressure (including but not limited to high-pressure gas or high-temperature heat-conducting oil) is applied to the cavity inside the polymer inner membrane through a positive pressure channel, causing the polymer inner membrane to undergo linear and controllable deformation. The polymer inner membrane expands outward and presses the carbon fiber prepreg layup structure against the inner wall of the outer mold. At the same time, a vacuum is drawn through a negative pressure channel to apply negative pressure to the gap between the cavity of the outer mold and the carbon fiber prepreg layup structure, so that the carbon fiber prepreg layup structure is tightly attached to the inner wall of the outer mold. The positive and negative pressures work together to form uniform compaction in the thickness direction of the carbon fiber prepreg layup structure.

[0024] Step S5: The autoclave is equipped with a closed-loop control system and a built-in dynamic pressure control algorithm module;

[0025] The dynamic pressure control algorithm module takes the real-time temperature T as input, calculates the positive and negative pressures in real time according to the basic pressure curve formula, and automatically superimposes pulses within a preset window before the effective gelation temperature; at the same time, it performs closed-loop fine-tuning through pressure sensor feedback to ensure that the actual pressure follows the set value; when the hot-pressing temperature reaches the effective gelation temperature, the pressure remains at a high constant level; the pressure fluctuation does not exceed ±0.02MPa.

[0026] The heating, heat preservation, and cooling processes during the curing process are carried out in accordance with the set curing process;

[0027] The curing process can be as follows: heating to 120-140℃ at a rate of 1-3℃ / min and holding for 1-2 hours, then heating to 160-180℃ and holding for 2-4 hours, followed by natural cooling. For bismaleimide systems, the curing temperature can be increased to 200℃.

[0028] The base pressure curve causes the positive pressure to transition non-linearly from the lower limit of the low-temperature range to the upper limit of the high-temperature range as the temperature increases, while the absolute value of the negative pressure gradually increases non-linearly as the temperature increases. In the later stage of the venting phase before resin gelation, within a preset temperature window, a positive pressure pulse is superimposed on the positive pressure, causing an instantaneous increase of 0.2~0.5 MPa. Simultaneously, a negative pressure pulse is superimposed on the negative pressure, causing an instantaneous increase of 0.02~0.05 MPa in the absolute value of the negative pressure, thus forming pulse extrusion and enhanced venting. After the pulse ends, the pressure returns to the base pressure curve. This dynamic adjustment of positive and negative pressure is maintained until curing is complete.

[0029] Step S6: After curing, cool down, release the positive and negative pressures, open the outer mold, and take out each segment of the polymer inner membrane in sequence to obtain an integrally formed carbon fiber material irregular co-cured component.

[0030] Furthermore, the amount of the sea urchin-shaped mesoporous silica nanospheres added is 3% to 15% of the mass of the matrix resin; the coupling agent is at least one of silane coupling agent, titanate coupling agent or amino-functionalized polysiloxane, and the amount of the coupling agent added is 0.5% to 3% of the mass of the matrix resin.

[0031] Furthermore, the polymer inner membrane has a tensile modulus of 3-8 GPa, a compressive strength of not less than 150 MPa, and a coefficient of thermal expansion of [missing value]. The cumulative creep strain increment of the polymer inner membrane under 0.6MPa positive pressure and curing temperature conditions and within 3 hours of heat preservation does not exceed 20% of the initial compressive strain.

[0032] Furthermore, the formula for the basic pressure curve mentioned in step S5 is:

[0033] ;

[0034] ;

[0035] in, It is the base pressure value of the positive pressure during the curing and heating process, in MPa; It is the base pressure value of the negative pressure during the curing and heating process, in MPa; The initial positive pressure ranges from 0.1 to 0.2 MPa. The positive pressure at gelation temperature, with a value ranging from 0.6 to 1.0 MPa; The initial negative pressure ranges from -0.02 to -0.04 MPa. The negative pressure at gelation temperature, with a value range of -0.06 to -0.08 MPa; For reference temperature, room temperature is used. The effective gelation temperature; The first index, with a value range of 1.5 to 3.0; The second index, with a value range of 1.2 to 2.5; T is the real-time temperature within the mold system during the heating process;

[0036] Since the curing process is usually not isothermal, the actual gel point of the resin may change with the heating rate: the faster the heating, the higher the gel point shifts. Therefore, an effective gel temperature T is introduced. gel,eff :

[0037] The effective gel temperature The calculation method is as follows:

[0038] ;

[0039] in, The reference gel temperature is typically set at 2°C / min, which can be determined by DSC isothermal testing at the standard heating rate. The following measurements were taken; The actual heating rate is represented by γ, which is a correction factor obtained by fitting the DSC gel point test at different heating rates, with a value ranging from 3 to 8℃. At that time, take This is a conservative approach, because the actual gel point is usually slightly lower than the baseline value when heating slowly. Using the baseline value allows the pressure acceleration phase to start earlier, which helps to ensure that the compaction stage is entered in time after the venting is completed, thus avoiding insufficient compaction due to pressure lag.

[0040] The above method can effectively prevent pressure acceleration from occurring too early or too late due to changes in the heating rate.

[0041] The pulse window is defined according to the temperature range, and the pulse duration will be changed by the rate of heating.

[0042] The positive and negative pressure pulses are within a preset temperature window. Internal stacking, with the temperature window set at the effective gel temperature. Within the temperature range of 5~20℃, the window width is 5~15℃, and the upper limit of the temperature window does not exceed... To ensure the pulse occurs precisely during the venting stage before resin gelation, the pulse should not be applied to already gelled resin. The positive pressure pulse amplitude is 0.2~0.5 MPa, and the negative pressure pulse amplitude is -0.02~-0.05 MPa. Furthermore, the pulse duration has an upper limit. When the time corresponding to the pulse temperature window during the actual heating process exceeds When the pulse reaches It was terminated early. The value range is 3~10 min; this ensures the short-duration, high-intensity characteristics of the pulse and does not damage the linear micro-deformation characteristics of the intima.

[0043] After the pulse ends, the pressure returns to the baseline pressure curve. When the combined positive pressure pulse exceeds the safe pressure, the output pressure is the safe pressure; when the combined negative pressure pulse exceeds the ultimate vacuum, the output pressure is the ultimate vacuum.

[0044] The reason for using pulsed pressure is that during the later stages of the venting phase, some of the volatiles in the prepreg have been expelled, but residual gas remains trapped between the fiber layers and in the resin micro-regions. At this point, a sudden increase in positive pressure creates a rapid compressive impact on the prepreg, squeezing the trapped gas out of the interlayer. Simultaneously, a sudden increase in the absolute value of negative pressure creates a stronger suction force on the cavity side, quickly removing the extruded gas and preventing backflow. Thus, the synergistic effect of the compression-suction pulse significantly reduces the porosity of the final product, and because the pulse duration is short, it does not damage the linear micro-deformation characteristics of the inner membrane.

[0045] Furthermore, both the positive and negative pressures are equipped with hardware limiting protection, with the upper limit of the positive pressure not exceeding the equipment's safe pressure. The lower limit of negative pressure shall not be lower than the system's ultimate vacuum. When the calculated negative pressure after pulse superposition is lower than the system's ultimate vacuum... At that time, with the system's ultimate vacuum As the actual output value, the negative pressure pulse amplitude is automatically reduced due to the ultimate vacuum constraint; when the pulses are superimposed, the calculated positive pressure value is higher than the equipment's safe pressure. At that time, the equipment safety pressure As the actual output value, the positive pressure pulse amplitude is automatically reduced due to safety pressure constraints. This prevents the controller from outputting pressure commands that exceed the physically achievable or safe range.

[0046] Furthermore, the aforementioned and The prepreg system was determined through isothermal DSC and rheological tests. Calibration was required for different resin systems, prepreg thicknesses, and carbon fiber volume fractions to match the pressure curve with resin viscosity changes and degassing processes.

[0047] Furthermore, the polymer inner membrane has a wall thickness of 3~15mm, and its surface is provided with a release agent layer. The interfacial bonding force between the release agent layer and the cured carbon fiber reinforced thermosetting resin matrix composite material is less than 0.5MPa.

[0048] Furthermore, the joints of each segment module of the polymer inner membrane are provided with a sealing structure, which is a high-temperature resistant sealing strip or a labyrinth-type sealing groove.

[0049] Furthermore, the carbon fiber material irregular co-cured component is a drone fuselage, drone shell, drone wing, unmanned boat hull, or spacecraft structural component with an internal closed cavity structure.

[0050] Furthermore, the carbon fiber prepreg is prepared by impregnating carbon fiber fabric or carbon fiber unidirectional tape with a resin slurry. The resin slurry contains a thermosetting resin (such as epoxy resin E-51), a curing agent (such as dicyandiamide), and an accelerator (such as a urea accelerator). The thermosetting resin is at least one of epoxy resin, bismaleimide resin, or cyanate ester resin. The volume fraction of carbon fiber in the carbon fiber prepreg is 50% to 70%, and the mass fraction of thermosetting resin is 30% to 50%.

[0051] It should be noted that the following points should be observed regarding the dynamic pressure control algorithm built into the dynamic pressure control algorithm module:

[0052] When T≤T ref At this time, it is necessary to force the output of P.正,base =P 正,low P 负,base =P 负,low Do not substitute into the formula for calculation.

[0053] This invention, through extensive research, has discovered that when the inner membrane has linear deformation characteristics, the inner membrane deformation corresponding to any pressure setting value can be accurately predicted through a linear relationship. This enables the low pressure during the exhaust phase to accurately correspond to small deformation, the high pressure after gelation to accurately correspond to large deformation, and the instantaneous pressure change during the pulse to be accurately converted into deformation impact.

[0054] Conversely, if the deformation characteristics of the inner membrane are nonlinear, even with a finely designed pressure regime, the deformation response of the inner membrane cannot form a stable one-to-one mapping with the pressure setpoint. Within the nonlinear range, small pressure increments may cause disproportionate deformation abrupt changes, leading to local over-compaction or under-compaction. In multiple cycles, the hysteresis effect of nonlinear deformation will accumulate deviations, severely deteriorating the dimensional accuracy and internal quality of the finished product.

[0055] Therefore, the linear deformation characteristics of the intima and the dynamic pressure control algorithm form a synergistic relationship, and neither can be dispensed with.

[0056] To supplement existing technologies: In existing technologies involving rigid or semi-rigid inner molds, for example, high-performance thermoplastics such as polyimide (PI) or polyetheretherketone (PEEK) are used as inner mold materials. However, no optimized design for the deformation behavior of the inner mold material under molding pressure has been found. Under positive pressure of 0.3~1.0MPa, the deformation characteristics of pure PI or pure PEEK materials are difficult to meet the dual requirements of composite co-curing processes for the inner mold to provide sufficient support and achieve uniform bonding with the prepreg: pure PI has a low modulus, excessive and nonlinear deformation, and cannot guarantee the dimensional accuracy of the inner cavity; although pure PEEK has a high modulus, it exhibits significant time-varying creep behavior under high-temperature curing conditions, and the deformation continues to drift with the holding time, which also cannot provide a stable geometric reference for the prepreg.

[0057] Existing nanofillers used for polymer modification, such as nano-silica, nano-alumina, and carbon nanotubes, have been widely applied in reinforcement and toughening, but they have significant shortcomings in controlling the deformation linearity and cyclic stability of polymers under low stress (0.1~1.0 MPa). Traditional spherical nanofillers (such as fumed silica) rely primarily on chemical bonding for interfacial stress transfer; under repeated compressive loads, interfacial slippage and debonding lead to a deviation from linear stress-strain relationships, and poor cyclic stability. Fibrous fillers (such as chopped carbon fibers) exhibit anisotropic deformation behavior of the inner film due to orientation effects during injection molding, making it impossible to achieve uniform pressure on complex, irregular structures. These traditional nanofillers struggle to simultaneously address the triple technical challenges of maintaining sufficient stiffness in polymer matrix reinforcement under low stress, controlling deformation linearity, and ensuring stable cyclic use.

[0058] Existing positive and negative pressure molding processes typically maintain a constant pressure throughout the curing process. For irregularly shaped components with internally enclosed cavities, the constant pressure regime presents two prominent problems: 1) In the initial stage of heating, the volatiles in the prepreg need to be expelled, but constant high pressure will cause the prepreg to be compacted prematurely, closing the exhaust channels and leading to increased porosity; 2) There is a difference in the coefficient of thermal expansion between the rigid / semi-rigid inner membrane and the finished composite material. During the heating process, the thermal expansion of the inner membrane may cause the actual deformation to exceed the design range, and constant pressure cannot compensate for this, affecting the dimensional accuracy of the inner cavity.

[0059] Compared with the prior art, the beneficial effects of this invention are as follows:

[0060] 1. This invention enables the one-time integral co-curing and molding of irregularly shaped components with enclosed internal cavities. No secondary bonding is required, eliminating weak interfaces. The polymer inner membrane is reusable, significantly reducing production costs. It has strong engineering feasibility.

[0061] 2. This invention employs the synergistic effect of positive and negative pressure to ensure high dimensional accuracy and surface quality.

[0062] 3. This invention employs a unique polymer inner membrane, coupled with a dynamic pressure control algorithm module. The initial pressure curve shows a gradual increase, providing a window for venting, while the subsequent pressure rises rapidly to match gel compaction. The non-linear growth compensates for the inner membrane's thermal expansion. Temperature rate correction ensures the pressure acceleration phase is synchronized with the actual gel state. Upper limits on pulse time and temperature windows guarantee short, high-intensity pulses without damaging the gel. Positive and negative pressure amplitude limiting ensures the pulses operate within physically feasible and safe ranges. The instantaneous synergistic effect of positive and negative pulse pressure efficiently removes residual volatiles, further reducing porosity. The dynamic pressure control algorithm module fully leverages the linear stress-strain relationship of the polymer inner membrane, achieving precise low-pressure response to small deformation during venting, precise high-pressure response to large deformation after gelation, and precise conversion of instantaneous pulse pressure into deformation impact. Attached Figure Description

[0063] Figure 1 This is a photograph of the finished product of the present invention assembled into a drone. Detailed Implementation

[0064] The present invention will now be described in further detail with reference to specific embodiments and accompanying drawings.

[0065] Example 1

[0066] 1. Preparation of polymeric inner membrane: Using polyimide resin as the matrix, sea urchin-shaped mesoporous silica nanospheres (purchased from Bailingwei, CAS: 7631-86-9; item number: 2748694, developed by Academician Zhao Dongyuan) were added; the center of the sea urchin-shaped mesoporous silica nanospheres is a solid or hollow core, from which numerous dendritic mesoporous channels extend radially outward, with the pore size gradually increasing from the center outward to form conical channels; the surface is covered with hundreds of open pores, forming a topological structure similar to that of a sea urchin; its diameter: 120-250 nm, specific surface area: 200~450 m² 2 The polyimide resin contains 8% (by weight of the polyimide resin) and 1.5% (by weight of the polyimide resin) silane coupling agent KH-550. The urchin-shaped mesoporous silica nanospheres are pre-dispersed via solution blending-precipitation, then melt-blended with the polyimide resin, granulated by twin-screw extrusion, and finally injection molded to obtain a segmented polymer inner membrane. The polymer inner membrane is composed of six segmented modules, which are connected by tapered positioning pins, and the seams are sealed with high-temperature resistant fluororubber strips. The surface of the polymer inner membrane is coated with a PTFE release agent layer, and the interior of the polymer inner membrane is processed with a porous pressure distribution structure.

[0067] Solution blending-precipitation pre-dispersion and melt blending are both conventional processes. These involve liquid-phase mixing of surface-modified sea urchin-shaped mesoporous silica nanospheres with a resin matrix (polyimide or its precursor) in a solvent, followed by precipitation to coat the sea urchin-shaped mesoporous silica nanospheres with the resin, forming a uniform pre-dispersed composite. The purpose is to uniformly disperse the sea urchin-shaped mesoporous silica nanospheres in the resin before melt blending, preventing nanoparticle agglomeration. The specific operation typically includes the following steps:

[0068] Sea urchin-shaped mesoporous silica nanospheres were dispersed in an ethanol solution containing the silane coupling agent KH-550 and heated to react, causing amino functional groups to be grafted onto the surface of the sea urchin-shaped mesoporous silica nanospheres, improving their compatibility with the resin and interfacial bonding. The modified sea urchin-shaped mesoporous silica nanospheres were dispersed in a suitable organic solvent (such as N-methylpyrrolidone, dimethylformamide, etc.), while polyimide resin (or its precursor polyamic acid) was dissolved in the same solvent, and the mixture was stirred to form a homogeneous suspension / solution. A non-solvent (such as water, ethanol, etc.) was added to the suspension / solution, causing the resin to precipitate from the solution. The sea urchin-shaped mesoporous silica nanospheres were coated by the resin and uniformly dispersed in the precipitate, forming a pre-dispersed masterbatch / composite powder. The precipitate was filtered and dried to obtain a resin pre-dispersion containing sea urchin-shaped mesoporous silica nanospheres. The resin pre-dispersion and the remaining resin are added to a twin-screw extruder for melt blending to obtain a modified high-temperature resistant thermoplastic resin-based composite material. The material is then extruded and granulated to finally obtain uniformly dispersed modified resin granules.

[0069] The tensile modulus of the polymer inner membrane was measured to be 5.6 GPa, the compressive strength to be 182 MPa, and the coefficient of thermal expansion to be 2.6 × 10⁻⁶. -5 / ℃. Under a normal pressure of 0.6MPa, the macroscopic compressive strain is 0.62%, and the stress-strain linear fit R in the range of 0.1~1.0MPa is... 2 =0.987. After 100 pressure cycles (0.1~1.0MPa), the compressive strain at 0.6MPa was 0.63%, and the strain drift rate was only 1.6%. After holding at 180℃ and 0.6MPa continuous pressure for 3 hours, the cumulative creep strain increment was 0.09%, which was only 14.5% of the initial compressive strain.

[0070] 2. Preparation of carbon fiber prepreg: Add 7 kg of epoxy resin E-51 and 1 kg of toughening agent polyethersulfone to acetone and stir to dissolve at 60°C; then add 0.8 kg of dicyandiamide and 0.2 kg of urea accelerator UR500, and stir evenly at 70~80°C to prepare a resin slurry; impregnate T700 grade carbon fiber fabric with the resin slurry, and after drying, obtain carbon fiber prepreg with a volume fraction of 60±2%.

[0071] Among them, carbon fiber prepreg is also commercially available.

[0072] 3. Lamination: Eight layers of carbon fiber prepreg are laid on the outer surface of the polymer inner membrane at a 0° / 90° / ±45° angle.

[0073] 4. Mold Closure: The polymer inner membrane covered with carbon fiber prepreg is placed in the outer mold cavity, and the mold is closed to form a closed mold system. The mold system is equipped with positive pressure channels and negative pressure channels.

[0074] 5. Dynamic Pressure Loading and Curing: The dynamic pressure control algorithm of the dynamic pressure control algorithm module is adopted, with the following parameters:

[0075] =0.15MPa, =0.8MPa, =-0.03MPa, =-0.07MPa, =25℃, =130℃ (DSC measurement at a standard heating rate of 2℃ / min), γ=5℃. =2℃ / min, therefore . =2.0, =1.6 (calibrated by isothermal DSC and rheological tests of this prepreg system). Pulse parameters: Pulse window set to 110~120℃ (10~20℃ before gelation, upper limit). The positive pressure pulse amplitude is 0.3 MPa, and the negative pressure pulse amplitude is -0.03 MPa (the calculated negative pressure after superposition is -0.10 MPa, but constrained by the system's ultimate vacuum of -0.098 MPa, the actual output is -0.098 MPa, meaning the actual effective amplitude of the negative pressure pulse is -0.028 MPa). The pulse time upper limit is also specified. =5min. The pressure limit is set to the equipment's safe pressure. =1.2MPa. Curing process: Heat to 130℃ at 2℃ / min and hold for 1.5h, then heat to 180℃ and hold for 3h, followed by natural cooling. Pressure fluctuation during curing is ±0.015MPa.

[0076] 6. Demolding: Cool to 60℃ and remove the segmented polymer inner membrane one by one.

[0077] Test Results: A coordinate measuring machine (CMM) was used to inspect the key mating surfaces of the finished product. The maximum dimensional deviation at the 10 inspection points did not exceed ±0.05 mm, and the overall dimensional tolerance was ±0.15 mm. The finished product had an interlaminar shear strength of 78 MPa, a porosity of 0.2%, and smooth inner and outer surfaces with no resin-rich areas. After 80 consecutive uses, the polymer inner membrane showed no significant change in deformation characteristics.

[0078] See the image of the assembled drone in this example. Figure 1 .

[0079] Example 2

[0080] The difference from Example 1 is that the resin used in this example of carbon fiber prepreg is a conventional bismaleimide resin, with a curing temperature of 200°C. Dynamic pressure parameters: =0.2MPa, =1.0MPa, =-0.04MPa, =-0.08MPa, =150℃, =3℃ / min, γ=6℃, calculated as follows =152.4℃. =2.5, =2.0. Pulse window 135~145℃, positive pressure pulse 0.4MPa, negative pressure pulse -0.02MPa.

[0081] A coordinate measuring machine (CMM) was used to inspect the key mating surfaces of the finished product. The maximum dimensional deviation at the 10 inspection points did not exceed ±0.07 mm, and the overall dimensional tolerance was ±0.18 mm. The temperature resistance of the finished product was improved to 250℃, and the porosity was 0.3%.

[0082] Example 3

[0083] The difference from Example 1 is that the positive pressure medium inside the polymer inner membrane is high-temperature resistant heat-conducting oil. =1℃ / min (slow heating) Pick =130℃), pulse window 110~120℃, if the temperature window is selected, the pulse will last for 10 minutes, but the setting is not applicable. =8min, the pulse terminates prematurely after 8min. =3.0, =2.5, positive pulse amplitude 0.5MPa (the calculated positive pressure after superposition is 1.3MPa, which exceeds the safe pressure of 1.2MPa. It is protected by positive pressure limiting and the actual output is 1.2MPa), negative pulse amplitude -0.03MPa.

[0084] Using the same outer mold size and cavity as in Example 3, and with the same layup thickness as the carbon fiber prepreg layup scheme (both are 8 layers), but the reinforcing material is replaced with E-glass fiber plain weave fabric (area density 800 g / m²). 2 The matrix was replaced with unsaturated polyester resin, and a fiberglass housing reference part with identical geometric dimensions was prepared in the same outer mold through hand lay-up molding and room temperature curing. After curing at 80℃ for 4 hours, the reference part was polished and trimmed to the same outer contour dimensions as the finished product.

[0085] Carbon fiber co-cured components are about 28% lighter than fiberglass casings, have no leaks, and have a porosity of 0.25%.

[0086] Example 4

[0087] The difference from Example 1 is that the initial temperature is 20°C (lower than 10°C). =25℃), verify the control system at Forced output No errors were found in complex number calculations. =0.1MPa, =0.6MPa, =-0.02MPa, =-0.06MPa, =1.5, =1.2; Pulse window 115~125℃, positive pressure pulse 0.2MPa, negative pressure pulse -0.02MPa.

[0088] The key mating surfaces of the finished product were inspected using a coordinate measuring machine. The maximum dimensional deviation at 10 inspection points did not exceed ±0.06 mm, and the overall dimensional tolerance was ±0.17 mm. The porosity was 0.35%, and the performance of the polymer inner membrane remained stable after 70 reuses.

[0089] Comparative Example 1: Polymer inner membrane made of pure PI material (unmodified)

[0090] In this example, unmodified pure polyimide resin was used to prepare the polymer inner membrane. Constant pressure was maintained during curing, with a positive pressure of 0.6 MPa and a negative pressure of -0.07 MPa. Other process conditions were the same as in Example 1. The tensile modulus of the pure PI polymer inner membrane was measured to be 2.8 GPa, and the compressive strain at 0.6 MPa reached 2.4%. Furthermore, the stress-strain curve exhibited significant nonlinearity above 0.3 MPa (R0). 2 =0.81). After 10 pressure cycles, the compressive strain at 0.6 MPa increased to 3.1%, with a drift rate of 29%. After holding at 180℃ and 0.6 MPa for 3 hours, the cumulative creep strain increase reached 1.2%, approximately 50% of the initial compressive strain. The internal cavity dimensional deviation of the cured product reached ±0.35 mm, with localized resin enrichment and fiber buckling, and the porosity increased to 2.11%. This was due to the low modulus of pure PI, excessive and nonlinear deformation, and severe creep, which failed to provide a stable geometric reference.

[0091] Comparative Example 2: Pure PI inner membrane (unmodified, same dynamic pressure control algorithm)

[0092] In this example, unmodified pure polyimide resin was used to prepare the polymer inner membrane. The same dynamic pressure control algorithm as in Example 1 was employed, and other process conditions were the same as in Example 1. The tensile modulus of the pure PI polymer inner membrane was measured to be 2.8 GPa, and the compressive strain at 0.6 MPa reached 2.4%. Furthermore, the stress-strain curve exhibited significant nonlinearity above 0.3 MPa (R0). 2=0.81). After 10 pressure cycles, the compressive strain at 0.6 MPa increased to 3.1%, with a drift rate of 29%. After holding at 180℃ and 0.6 MPa for 3 hours, the cumulative creep strain increase reached 1.2%, approximately 50% of the initial compressive strain. However, during the power function acceleration phase and pulse instant of the dynamic pressure control algorithm, the polymer inner membrane's response to pressure changes was severely lagging and disproportionate, leading to alternating periods of localized over-compaction and under-compaction. The maximum dimensional deviation of the key mating surfaces of the cured product reached ±0.50 mm, with a porosity of 2.53%, and localized resin enrichment and fiber buckling. This may be due to the low modulus of pure PI, its excessively large deformation, and its highly nonlinear nature, which prevents it from providing a predictable deformation response under dynamic pressure.

[0093] Comparative Example 3: Pure PEEK inner membrane (unmodified)

[0094] In this example, an unmodified pure PEEK resin was used to prepare a polymeric inner membrane. The same dynamic pressure control algorithm as in Example 1 was employed, and other process conditions were identical to those in Example 1. The tensile modulus of the pure PEEK inner membrane was measured to be 3.8 GPa, and the initial compressive strain at 0.6 MPa was 0.8%. The linear R0 was... 2 =0.88. Under a curing temperature of 200℃ and a dynamic pressure regime, the total strain drifted to 1.4% after 1 hour of holding (creep increment of 0.6%), and reached 1.9% after 3 hours of holding (creep increment of 1.1%, which is 137.5% of the initial compressive strain). Due to the continuous drift of the geometric reference of the inner film during the curing process caused by creep, coupled with the viscoelastic hysteresis of the inner film deformation response during the pulse, the maximum dimensional deviation of the key mating surfaces of the finished product reached ±0.40mm, the porosity was 1.54%, and adhesive wear occurred between the inner film and the inner wall of the finished product during demolding, resulting in scratches on the inner cavity surface. The reason may be that the viscoelastic creep of pure PEEK at high temperature was not effectively suppressed, and its deformation response speed was insufficient to follow the pulse changes in the dynamic pressure regime.

[0095] Comparative Example 4: Flexible Silicone Inner Membrane

[0096] This example uses a silicone inner membrane with a Shore A hardness of 60, and other process conditions are the same as in Example 1. Because the flexible silicone undergoes large deformation during the high-pressure phase of dynamic pressure, it experiences an overshoot response during the pulse instant, failing to provide any stable geometric reference for the inner cavity. After curing, the maximum dimensional deviation of the critical mating surfaces of the finished product reaches ±0.60 mm, with a porosity of 2.07%. Furthermore, the silicone inner membrane exhibits permanent deformation after curing at 180℃, rendering it unusable after only two uses.

[0097] Comparative Example 5: Spherical Nano-Silica Modified PI Inner Membrane

[0098] In this example, spherical nano-silica with the same particle size as in Example 1 was used as the filler, with an addition amount of 8%, and other conditions were the same as in Example 1. The initial tensile modulus of the polymer inner membrane was measured to be 4.1 GPa, the initial compressive strain at 0.6 MPa was 1.3%, and the stress-strain linearity R... 2 =0.91. After 10 compression cycles, the compressive strain at 0.6 MPa increased to 1.8%, the drift rate was 38%, and R 2 The stress-strain ratio dropped to 0.86. Under dynamic pressure, the deformation response of the polymer inner membrane exhibited significant overshoot and hysteresis at the moment of the pulse, and deformation drift accumulated after multiple cycles. The maximum dimensional deviation of the key mating surfaces of the cured product was ±0.30 mm, with a porosity of 1.79%, and localized resin-rich areas were observed. The reason may be that the smooth nanoparticles lack mechanical interlocking ability, and the interfacial slippage causes the stress-strain relationship to deviate from linearity, making it unable to produce a predictable deformation response to pressure changes under dynamic pressure.

[0099] Comparative Example 6: Nanoporous silica-modified PI inner membrane

[0100] This example uses nanoporous silica (average pore size 5 nm, specific surface area 800 m²). 2 / g (with a main particle size of approximately 80nm) was used as a filler, with an addition amount of 8%, and other conditions were the same as in Example 1. The initial tensile modulus of the polymer inner membrane was measured to be 5.5GPa, the first compressive strain at 0.6MPa was 0.72%, and the stress-strain linearity R 2 =0.93. However, under multiple pressure cycles and pulses under a dynamic pressure regime, after 5 cycles, the compressive strain at 0.6 MPa increased to 1.2%, R 2 Reduced to 0.85; strain reached 1.8% after 10 cycles, R 2 The stress-strain ratio dropped to 0.76; simultaneously, numerous whitish areas appeared inside the inner membrane. After curing, the maximum dimensional deviation of the key mating surfaces of the finished product was ±0.30 mm, with a porosity of 1.80%, and localized areas of resin depletion and microcracks were observed. The reason may be that conventional mesopores are straight-through, uniform-diameter channels, lacking the unique conical, large-inner-large-outer-small barbed locking structure characteristic of sea urchin-like structures; during repeated dynamic compression loading-unloading processes, the polyimide molecular chains deep within the channels easily slip out gradually from the straight-through channels under stress; with each cycle, the compressive strain increases (stiffness decreases), and the degree to which the stress-strain relationship deviates from linearity intensifies.

[0101] Comparative Example 7: Fumed silica-modified PI inner membrane

[0102] This example uses fumed silica (specific surface area 200 m²). 2 / g, with a native particle size of approximately 12nm and an aggregate particle size of approximately 200nm) as filler, was added at a rate of 8%. The surface was modified with KH-550 silane, and other conditions were the same as in Example 1. The initial tensile modulus of the polymer inner membrane was measured to be 4.5GPa, the initial compressive strain at 0.6MPa was 0.9%, and the stress-strain linearity R 2 =0.93. Under the pulse action of the dynamic pressure regime, local stress concentration occurs at the aggregates of silica, inducing the initiation of microcracks in the matrix; after 50 cycles, the compressive strain at 0.6 MPa drifts to 1.2%, R 2 When the pH value dropped to 0.85, a network of microcracks appeared on the inner membrane surface. The maximum dimensional deviation of the key mating surfaces of the cured product was ±0.28 mm, and the porosity was 1.55%. This may be because the presence of irregular aggregates caused progressive damage accumulation to the polymer inner membrane under dynamic pressure.

[0103] Comparative Example 8: Short-cut carbon fiber modified PI inner membrane

[0104] In this example, short-cut carbon fibers (average length 3 mm, diameter 7 μm, addition amount 15%) were used as filler, and other conditions were the same as in Example 1. The tensile modulus of the polymer inner membrane was measured to be 5.2 GPa, and the compressive strain at 0.6 MPa was 0.75%, but the stress-strain linearity R... 2 =0.92 (along the fiber orientation direction) and R 2 =0.86 (perpendicular to the fiber orientation direction), exhibiting significant anisotropy. Under dynamic pressure, the deformation response of the inner membrane in different directions is inconsistent, resulting in uneven compaction effects of pulse extrusion in the fiber orientation direction and perpendicular direction. After curing, the maximum dimensional deviation of the key mating surfaces of the finished product is ±0.35mm, with a porosity of 1.83%, and localized poor adhesion occurs in areas of abrupt curvature change. The reason may be that the fiber orientation distribution causes anisotropic deformation of the inner membrane, making it impossible to achieve a uniform deformation response under dynamic pressure.

[0105] Comparative Example 9: Constant Pressure Curing

[0106] This example uses the same polymer inner membrane as in Example 1, but maintains a constant pressure during curing: a positive pressure of 0.6 MPa and a negative pressure of -0.07 MPa. The negative pressure value is consistent with the upper limit of the basic negative pressure in Example 1. The results showed that the maximum dimensional deviation of the key mating surfaces of the finished product was ±0.15 mm, the overall profile tolerance was ±0.25 mm, and the porosity was 0.88%, all inferior to Example 1. This may be because the constant pressure was applied too early in the heating process, prematurely closing the exhaust channels and failing to compensate for the thermal expansion of the inner membrane.

[0107] Comparative Example 10: Step Pressure Effect

[0108] Using the same polymer inner membrane as in Example 1, the pressure application was changed to a stepwise approach: from room temperature to 100°C, the pressure was low (positive pressure 0.15 MPa, negative pressure -0.03 MPa); at 100°C, it instantly stepped to high pressure (positive pressure 0.6 MPa, negative pressure -0.07 MPa), maintaining this pressure until curing was complete. The maximum dimensional deviation of the key mating surfaces of the finished product was ±0.12 mm, and the porosity was 0.75%, which was inferior to Example 1. The reason may be that the instantaneous pressure impact during the stepwise transition caused the gas between the prepreg layers to be trapped before it could escape, and there was no venting reinforcement method after the stepwise transition.

[0109] Comparative Example 11: Linear Base Pressure and Pulse-Free

[0110] Using the same polymer inner membrane as in Example 1, the base pressure curve was changed to a linear change, i.e., the positive pressure linearly increased from 0.15 MPa to 0.8 MPa, and the negative pressure linearly decreased from -0.03 MPa to -0.07 MPa, without any pulsations. The maximum dimensional deviation of the key mating surfaces of the finished product was ±0.10 mm, and the porosity was 0.54%, which was worse than that of Example 1. The reason may be that the linear curve rose too quickly in the early stage, compressing the exhaust window; and the absence of pulsations meant that residual gas could not be effectively expelled in the later stage of the exhaust phase.

[0111] Comparative Example 12: Individual Positive Pressure Pulse

[0112] Using the same polymer inner membrane as in Example 1, only a positive pressure pulse of 0.3 MPa was applied during the pressure treatment; no negative pressure pulse was applied. The rest was the same as in Example 1. The maximum dimensional deviation of the key mating surfaces of the finished product was ±0.09 mm, and the porosity was 0.35%, which was inferior to Example 1. The reason may be that the gas extruded by the single positive pressure pulse lacked synchronous enhanced suction, and some of the extruded gas flowed back into the prepreg layer after the pulse ended.

[0113] Comparative Example 13: Individual Negative Pressure Pulse

[0114] Using the same polymer inner membrane as in Example 1, only a negative pressure pulse of -0.03 MPa was applied during the pressure treatment; no positive pressure pulse was applied. The rest was the same as in Example 1. The maximum dimensional deviation of the key mating surfaces of the finished product was ±0.10 mm, and the porosity was 0.44%, which was inferior to Example 1. This may be because the negative pressure pulse alone only enhances suction and lacks the positive pressure impact extrusion effect, thus having limited effectiveness in removing gas trapped deep within the fiber layers.

[0115] As can be seen from Comparative Examples 1-8, when the R of the polymer inner membrane... 2 As the concentration was gradually increased from 0.81 (pure PI) to 0.987 (Example 1), the critical surface deviation of the finished product decreased from ±0.50 mm to ±0.05 mm, and the porosity decreased from 2.5% to 0.2%. This trend demonstrates that the linear deformation characteristics of the polymer inner membrane are a fundamental condition for the effective execution of dynamic pressure.2 The closer the value is to 1, the higher the accuracy of the pressure action being acted upon by the inner membrane as a deformation response.

[0116] The tensile modulus of Comparative Example 6 reached 5.5 GPa, close to the 5.6 GPa of Example 1, but its R... 2 With a modulus of only 0.93, a finished product deviation of ±0.30 mm, and a porosity of 1.8%, it is far inferior to Example 1. This indicates that the modulus itself is not the decisive factor; linearity is the core indicator.

[0117] The polymer inner membrane of Comparative Example 5 maintained an accuracy of ±0.15 mm under constant pressure, but deteriorated to ±0.30 mm under dynamic pressure. This is because the dynamic pressure regime includes rapid pressure changes (pulse and power function acceleration segments). The nonlinear deformation inner membrane exhibits overshoot, hysteresis, and hysteresis accumulation in response to rapidly changing pressure, amplifying rather than improving the defects.

[0118] Compared with Comparative Examples 5, 6, and 7, under the same matrix, the same amount added, and the same pressure, only the sea urchin-shaped mesoporous silica nanospheres achieved R 2 Linear deformation ≥0.95 indicates the best product quality. This proves that the morphology of silica itself (rather than the chemical composition of silica) is the key structural factor that produces linear deformation characteristics.

[0119] Under the same linear inner membrane conditions, Example 1 showed the best product deviation and porosity. Comparative Example 9 (constant pressure), Comparative Example 10 (step pressure), Comparative Example 11 (linear without pulse), Comparative Example 12 (single positive pressure pulse), and Comparative Example 13 (single negative pressure pulse) were all significantly worse. The dynamic pressure control algorithm described in this invention exhibits the best technical performance.

[0120] The effects of the single positive pressure pulse in Comparative Example 12 and the single negative pressure pulse in Comparative Example 13 were significantly worse than the synchronous pulse in Example 1. This demonstrates that the synchronous synergistic mechanism of extrusion and suction (positive pressure impact squeezes out residual gas, while negative pressure draws gas away and prevents backflow) is key to reducing porosity.

[0121] A comparison between Comparative Example 9 and Example 1 shows that even with superior inner membrane material performance, the deviation of the finished product under constant pressure is still 3 times worse than that under dynamic pressure, and the porosity is 4 times worse. This proves that both the inner membrane material and dynamic pressure are indispensable and work synergistically.

[0122] As can be seen from the above, there is a synergistic relationship between the linear deformation characteristics of the inner membrane and the dynamic pressure action. Only a linear inner membrane can accurately execute the regulatory intent of the dynamic pressure action; and only the dynamic pressure action can fully utilize the regulatory advantages of the linear inner membrane. The combined effect of the two results in a finished product accuracy (critical surface deviation ±0.05mm) and porosity (0.2%) that far exceed those of traditional processes.

[0123] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A process for integrally molding irregularly shaped carbon fiber materials through co-curing, characterized in that, Includes the following steps: Step S1: Provide a polymer inner membrane, which has a segmented structure, including multiple segmented modules. Each segmented module cooperates with each other through a positioning structure, and each segmented module has a cavity inside. The polymer inner membrane is made of a modified high-temperature resistant thermoplastic resin-based composite material, which uses polyimide resin or polyether ether ketone resin as the matrix resin and adds sea urchin-shaped mesoporous silica nanospheres and coupling agents. Step S2: Lay multiple layers of carbon fiber prepreg on the outer surface of the polymer inner membrane to form a carbon fiber prepreg layup structure. Step S3: Place the polymer inner membrane covered with carbon fiber prepreg layer structure into the cavity of the outer mold, and close the mold to form a closed mold system; the mold system is provided with a positive pressure channel and a negative pressure channel, the positive pressure channel is connected to the cavity inside the polymer inner membrane, and the negative pressure channel is connected to the gap between the cavity of the outer mold and the carbon fiber prepreg layer structure. Step S4: The mold system is sent into the autoclave. Positive pressure is applied to the cavity inside the polymer inner membrane through the positive pressure channel, causing the polymer inner membrane to undergo linear and controllable deformation. The polymer inner membrane expands outward and presses the carbon fiber prepreg layup structure against the inner wall of the outer mold. At the same time, negative pressure is applied by evacuating the gap between the cavity of the outer mold and the carbon fiber prepreg layup structure through the negative pressure channel, so that the carbon fiber prepreg layup structure is tightly attached to the inner wall of the outer mold. Step S5: The autoclave is equipped with a closed-loop control system and a built-in dynamic pressure control algorithm module; The dynamic pressure control algorithm module takes the real-time temperature T as input, calculates the positive and negative pressures in real time according to the basic pressure curve formula, and automatically superimposes pulses within a preset window before the effective gelation temperature; when the hot-pressing temperature reaches the effective gelation temperature, the pressure remains high and constant; the pressure fluctuation does not exceed ±0.02MPa. The heating, heat preservation, and cooling processes during the curing process are carried out in accordance with the set curing process; Step S6: After curing, cool down, release the positive and negative pressures, open the outer mold, and take out each segment of the polymer inner membrane in sequence to obtain an integrally formed carbon fiber material irregular co-cured component.

2. The integral molding process for irregularly shaped co-curing carbon fiber materials according to claim 1, characterized in that, The amount of the sea urchin-shaped mesoporous silica nanospheres added is 3% to 15% of the mass of the matrix resin; the coupling agent is at least one of silane coupling agent, titanate coupling agent or amino-functionalized polysiloxane, and the amount of the coupling agent added is 0.5% to 3% of the mass of the matrix resin.

3. The integral molding process for irregularly shaped carbon fiber materials according to claim 1, characterized in that, The polymer inner membrane has a tensile modulus of 3-8 GPa, a compressive strength of not less than 150 MPa, and a coefficient of thermal expansion of [missing value]. The cumulative creep strain increment of the polymer inner membrane under 0.6MPa positive pressure and curing temperature conditions and within 3 hours of heat preservation does not exceed 20% of the initial compressive strain.

4. The integral molding process for irregularly shaped co-curing carbon fiber materials according to claim 1, characterized in that, The formula for the basic pressure curve mentioned in step S5 is: ; ; in, It is the base pressure value of the positive pressure during the curing and heating process, in MPa; It is the base pressure value of the negative pressure during the curing and heating process, in MPa; The initial positive pressure ranges from 0.1 to 0.2 MPa. The positive pressure at gelation temperature, with a value ranging from 0.6 to 1.0 MPa; The initial negative pressure ranges from -0.02 to -0.04 MPa. The negative pressure at gelation temperature, with a value range of -0.06 to -0.08 MPa; For reference temperature, room temperature is used. The effective gelation temperature; The first index, with a value range of 1.5 to 3.0; The second index, with a value range of 1.2 to 2.5; T is the real-time temperature within the mold system during the heating process; The effective gel temperature The calculation method is as follows: ; in, The reference gel temperature was determined by DSC isotherm testing at a standard heating rate. The following measurements were taken; The actual heating rate; γ is a correction factor, ranging from 3 to 8℃; when At that time, take ; The positive and negative pressure pulses are within a preset temperature window. Internal stacking, with the temperature window set at the effective gel temperature. Within the temperature range of 5~20℃, the window width is 5~15℃, and the upper limit of the temperature window does not exceed... The positive pressure pulse amplitude is 0.2~0.5MPa, and the negative pressure pulse amplitude is -0.02~-0.05MPa; and the pulse duration has an upper limit. When the time corresponding to the pulse temperature window during the actual heating process exceeds When the pulse reaches It was terminated early. The value range is 3~10min.

5. The integral molding process for irregularly shaped co-curing carbon fiber materials according to claim 4, characterized in that, Both the positive and negative pressures are equipped with hardware limiting protection, and the upper limit of the positive pressure shall not exceed the equipment's safe pressure. The lower limit of negative pressure shall not be lower than the system's ultimate vacuum. When the calculated negative pressure after pulse superposition is lower than the system's ultimate vacuum... At that time, with the system's ultimate vacuum As the actual output value; When the pulse superposition results in a positive pressure value higher than the equipment's safe pressure... At that time, the equipment safety pressure As the actual output value.

6. The integral molding process for irregularly shaped co-curing carbon fiber materials according to claim 5, characterized in that, The and Determined by isothermal DSC and rheological tests of the prepreg system.

7. The integral molding process for irregularly shaped co-curing carbon fiber materials according to claim 1, characterized in that, The polymer inner membrane has a wall thickness of 3-15 mm and a release agent layer on its surface.

8. The integral molding process for irregularly shaped co-curing carbon fiber materials according to claim 1, characterized in that, The joints of each segment module of the polymer inner membrane are provided with a sealing structure.

9. The integral molding process for irregularly shaped co-curing carbon fiber materials according to claim 1, characterized in that, The carbon fiber material irregular co-cured components are drone fuselages, drone shells, drone wings, unmanned vessel hulls, or spacecraft structural components with an internally enclosed cavity structure.

10. The integral molding process for irregularly shaped co-curing carbon fiber materials according to claim 1, characterized in that, The carbon fiber prepreg is prepared by impregnating carbon fiber fabric or carbon fiber unidirectional tape with resin slurry.

Citation Information

Patent Citations

  • Carbon fiber forming mold based on silica gel inner mold and technology of carbon fiber forming mold

    CN116100711A

  • Reusable internal mold material suitable for carbon fiber special-shaped part

    CN117024674A

  • Degradable internal mold material suitable for carbon fiber special-shaped part

    CN117024919A