Carbon fiber reinforced composite material secondary pultrusion plate forming device and forming process thereof

By decoupling the single pultrusion process into a two-stage pultrusion process and controlling the temperature and impregnation process in stages, the problems of uneven curing and internal stress in thick-walled, large-section carbon fiber reinforced composites were solved, the interlaminar shear strength and fiber content were improved, and production losses and costs were reduced.

CN123129494APending Publication Date: 2026-11-20ZHONGFU CARBON FIBER CORE CABLE TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611607821.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-16
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing single-pass pultrusion processes suffer from problems such as uneven curing, internal stress concentration, surface cracks, low interlaminar shear strength, high porosity, and large fiber loss during operation when used in thick-walled, large-section, and high-fiber-content products. They are difficult to balance high fiber content with sufficient impregnation, resulting in low production efficiency and high costs.

Method used

The carbon fiber reinforced composite material secondary pultrusion plate forming device is divided into two independent stages: the first pultrusion and the second pultrusion. Preheating, impregnation and preliminary curing are carried out in the first pultrusion die, and final curing and homogenization are carried out in the second pultrusion die. The temperature distribution is uniform through an independent temperature control system, which reduces the number of fibers and losses at startup.

Benefits of technology

It achieves uniform curing and internal stress control in thick-walled, large-section products, reduces porosity and surface defects, improves interlaminar shear strength and fiber volume fraction, and reduces production losses and costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123129494A_ABST
    Figure CN123129494A_ABST
Patent Text Reader

Abstract

The application discloses a carbon fiber reinforced composite secondary pultrusion plate forming device and a forming process thereof, and belongs to the technical field of pultrusion girder plates. A roller creel is used for arranging carbon fibers in order, a dipping tank is used for dipping glue on the carbon fibers, the roller creel guides the carbon fibers to the dipping tank, the dipping tank guides the carbon fibers after being dipped with glue to the inlet of a first pultrusion die, a preheating zone, an intermediate transition zone and a curing zone are sequentially arranged in the first pultrusion die along a traction direction, and the preheating zone, the intermediate transition zone and the curing zone are respectively provided with independent temperature control systems. The problems of uneven curing, stress concentration, surface cracks, low interlaminar shear strength, high porosity and large fiber loss during a single pultrusion process of thick-walled, large-section and high-fiber-content products are solved, and the application is mainly used for forming carbon fiber reinforced composite secondary pultrusion plates.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of pultrusion molding technology for fiber-reinforced resin-based composite materials, specifically to a molding apparatus and molding process for secondary pultrusion plates of carbon fiber reinforced composite materials. Background Technology

[0002] Pultrusion is a highly efficient continuous molding process for fiber-reinforced composite materials. It typically involves steps such as uniform tension distribution of fiber rovings, resin impregnation, preforming, in-mold gel curing, traction, and cutting. Continuous fibers include glass fibers, carbon fibers, and aramid fibers. The fibers are impregnated with resin in an open-groove mold or injected under high pressure in a closed mold. A traction device then pulls the resin-impregnated fibers through a heated mold, where the resin rapidly cures, resulting in the continuous production of composite profiles with a constant cross-section.

[0003] In traditional single-pass pultrusion processes, impregnation, gelation, and curing are completed in the same mold and during continuous pultrusion, with the mold temperature regime and traction speed being coupled together. For thick-walled, large-section, or high-fiber-content products, due to the exothermic effect of resin curing, uneven thermal conductivity, and the obstruction of resin flow by fiber bundles, inconsistent curing levels between the core and surface layers are prone to occur. This leads to defects such as uneven curing, internal stress concentration, surface cracks, low interlaminar shear strength, and high porosity.

[0004] Meanwhile, single-pass pultrusion process is difficult to balance high fiber content and sufficient impregnation, and it is difficult to steadily increase fiber volume fraction. For ultra-thick and large-section profiles, the forming resistance is high, the requirements for mold temperature control and traction control are high, the number of continuous fibers required for start-up is large, the trial molding and production losses are large, the production efficiency is low, and the cost is high.

[0005] In actual molding, when the wall thickness of the product is large, exceeding 15mm, the exothermic reaction of the resin curing reaction is concentrated. The outer surface of the product is in contact with the mold, receiving uniform heating and curing well; the inner surface or centerline area of ​​the product is far from the mold, and due to the thickness of the product, temperature isolation and heat loss occur, resulting in uneven heating, poor curing, and a lower degree of curing inside the product compared to the surface layer, which seriously affects the consistency of the product's mechanical properties. When thick-walled products cool inside the mold, the surface layer cures and shrinks first while the core is not fully cured, which easily generates large residual internal stress, often manifesting as surface microcracks, warping, and even delayed cracking after demolding.

[0006] Large-section carbon fiber products are difficult to pultrude in a single process, especially for 48K carbon fiber with a cross-sectional area of ​​5000 mm². 2The product requires approximately 1800 carbon fibers, significantly increasing raw material start-up losses, pultrusion stability, fiber impregnation effect, tensile force control, and the difficulty of maintenance and line monitoring for operators. To ensure sufficient resin impregnation and bubble removal, traditional processes often require reducing the fiber content, with fiber volume fraction typically between 55% and 65%, thus limiting further improvements in the product's specific strength and specific modulus.

[0007] It is evident that existing single-stage pultrusion processes still have significant limitations in thick-walled, large-section, and high-fiber-content products. The thicker the product and the larger the cross-section, the more difficult it becomes to simultaneously achieve uniform curing, internal stress control, and defect suppression. Furthermore, with an increased number of carbon fibers, start-up losses, traction stability, and wetting effects become more difficult to control. These factors collectively constrain the development of pultruded products towards higher fiber content, larger cross-sections, and lower costs. Summary of the Invention

[0008] This invention provides a carbon fiber reinforced composite secondary pultrusion plate forming device and its forming process to solve the problems of uneven curing, internal stress concentration, surface cracks, low interlaminar shear strength, high porosity, and large fiber loss during a single pultrusion process for thick-walled, large-section, and high-fiber-content products.

[0009] The specific technical solution of this invention is as follows:

[0010] A carbon fiber reinforced composite material secondary pultrusion plate forming device includes a roller yarn frame, an impregnation tank, a first pultrusion die, a second pultrusion die, a traction device, and a cutting device. The roller yarn frame is used to neatly arrange carbon fibers, and the impregnation tank is used to impregnate the carbon fibers. Along the traction direction, the carbon fibers output from the roller yarn frame are guided to the impregnation tank, and the impregnation tank guides the impregnated carbon fibers to the entrance of the first pultrusion die.

[0011] Along the traction direction, the impregnation tank, the first pultrusion die, the second pultrusion die, the traction device, and the cutting device are arranged sequentially after the roller yarn frame;

[0012] The first pultrusion die is equipped with a preheating zone, an intermediate transition zone, and a curing zone sequentially along the traction direction. Each of the preheating zone, intermediate transition zone, and curing zone is equipped with an independent temperature control system.

[0013] The second pultrusion die is set with a high-temperature curing zone and a heat preservation homogenization zone in sequence along the traction direction. The high-temperature curing zone and the heat preservation homogenization zone are equipped with independent temperature control systems. The preform obtained by the first pultrusion die is sent into the second pultrusion die for secondary curing and pultrusion. The resin-impregnated carbon fiber is tightly wrapped around the outer surface of the preform.

[0014] The traction device is used to pull out the profile after it has been cured by the second pultrusion die at a constant speed;

[0015] The cutting device is used to cut products to a set length.

[0016] Preferably, both the first and second pultrusion dies are Cr12MoV dies, and the cone angle at the mold cavity inlet is 2° to 5°.

[0017] Preferably, multiple sets of thermocouples are embedded in the cavities of the first pultrusion die and the second pultrusion die to monitor the temperature distribution of the resin-carbon fiber system in the die cavity in real time.

[0018] A process for forming carbon fiber reinforced composite secondary pultrusion plates, using the aforementioned carbon fiber reinforced composite secondary pultrusion plate forming apparatus, includes the following steps:

[0019] Step 1: Arrange the carbon fibers neatly on the roller yarn frame, maintaining the tension of each fiber bundle at 10-25 N / bundle;

[0020] Step 2: After impregnating the arranged carbon fibers with resin in the impregnation tank, the carbon fibers are sent into the first pultrusion mold. The first pultrusion mold is set with a preheating zone of 60-110°C, an intermediate transition zone of 100-170°C, and a curing zone of 150-210°C from the inlet to the outlet. The traction speed V1 is controlled at 80-300 mm / min to allow the fiber-resin system to be impregnated and cured to form a preform.

[0021] Step 3: The second pultrusion die is set with a high-temperature curing zone of 150-180℃ and a heat preservation and homogenization zone of 180-210℃ along the traction direction. The traction speed V2 is controlled at 80-200mm / min to fully impregnate the preform with carbon fiber and resin and cure and shape it, so as to obtain a carbon fiber reinforced composite profile with a curing degree ≥95%.

[0022] Step four: The cured profile is pulled out by the traction device at a constant traction speed and then cut by the cutting device to the set length.

[0023] Preferably, the carbon fiber in step one is 48K carbon fiber, and the fiber bundle tension is 10-25N / bundle.

[0024] Preferably, in step two, the preheating zone temperature of the first pultrusion die is 60-110℃, the intermediate transition zone temperature is 100-170℃, the curing zone temperature is 150-210℃, and the traction speed V1 is 80-300mm / min.

[0025] Preferably, in step three, the high-temperature curing zone temperature of the second pultrusion die is 150-180℃, the temperature of the heat preservation and homogenization zone is 180-210℃, the traction speed V2 is 80-200mm / min, and the profile curing degree is ≥95%.

[0026] Preferably, in step three, the second pultrusion die is independent of the first pultrusion die and is temperature-controlled in separate zones by an independent temperature control system. The final profile has a fiber volume fraction of 65% to 72%, a porosity of ≤1.2%, and an interlaminar shear strength that is 18% to 30% higher than that of a single pultrusion profile of the same specification.

[0027] Compared with the prior art, the technical effects and advantages of the present invention are:

[0028] This invention decouples the impregnation, gelation, and curing processes in the traditional single-stage pultrusion process into two independent pre-gelation and final curing processes. The first pultrusion forms a small-section preform, and the second pultrusion uses the preform as a filler for coating and final curing, thereby reducing the difficulty of molding large-section products in one step, reducing the amount of fiber required for start-up, and reducing production losses.

[0029] Because the first and second pultrusion dies are independently temperature-controlled, and each is zoned for temperature control along the traction direction, the temperature distribution between the core and surface of thick-walled and large-section products can be more uniform. This reduces internal stress caused by concentrated heat release during resin curing, lowers porosity and surface defects, and improves interlaminar shear strength. Using this method, the fiber volume fraction of carbon fiber reinforced composites can be stably increased to 65%–72%, porosity reduced to below 1.2%, and interlaminar shear strength increased by 18%–30%. Attached Figure Description

[0030] Figure 1 This is a process flow diagram of the present invention. Detailed Implementation

[0031] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0032] Example

[0033] like Figure 1 As shown:

[0034] The present invention provides a carbon fiber reinforced composite material secondary pultrusion plate forming device, comprising a roller yarn frame 1, an impregnation tank 2, a first pultrusion die 3, a second pultrusion die 4, a traction device 5, and a cutting device 6. The roller yarn frame 1 is used to neatly arrange carbon fibers, and the impregnation tank 2 is used to impregnate the carbon fibers with resin. Along the traction direction, the carbon fibers output from the roller yarn frame 1 are guided to the impregnation tank 2, and the impregnation tank 2 guides the impregnated carbon fibers to the inlet of the first pultrusion die 3.

[0035] Along the traction direction, after the roller yarn frame 1, the immersion tank 2, the first pultrusion die 3, the second pultrusion die 4, the traction device 5, and the cutting device 6 are arranged in sequence;

[0036] The first pultrusion die 3 is provided with a preheating zone 31, an intermediate transition zone 32 and a curing zone 33 in sequence along the traction direction. Each of the preheating zone 31, intermediate transition zone 32 and curing zone 33 is equipped with an independent temperature control system.

[0037] The second pultrusion die 4 is arranged with a high-temperature curing zone 41 and a heat preservation and homogenization zone 42 in sequence along the traction direction. The high-temperature curing zone 41 and the heat preservation and homogenization zone 42 are equipped with independent temperature control systems. The preform obtained by the first pultrusion die 3 is sent into the second pultrusion die 4 for secondary curing and pultrusion. The impregnated carbon fiber is tightly wrapped around the outer surface of the preform.

[0038] The traction device 5 is used to pull out the profile that has been cured by the second pultrusion die 4 at a constant speed;

[0039] Cutting device 6 is used to cut products to a set length.

[0040] The roller yarn frame 1 is used to place carbon fiber spindles and arrange the carbon fibers neatly. At the same time, the roller yarn frame 1 keeps each fiber bundle under stable tension before entering the immersion tank 2.

[0041] Carbon fibers are impregnated with resin in the impregnation tank 2. The outlet of the impregnation tank 2 is connected to the inlet of the first pultrusion mold 3, so that the impregnated carbon fibers continuously enter the first pultrusion mold 3.

[0042] The first pultrusion die 3 is provided with a preheating zone 31, an intermediate transition zone 32 and a curing zone 33 in sequence along the traction direction. The preheating zone 31 is used to gradually heat up the impregnated carbon fiber, reduce the resin viscosity and promote the resin to further impregnate the fiber.

[0043] The intermediate transition zone 32 is used to allow the resin to enter the gelation stage and to gradually shape the fiber bundles within the mold cavity. The curing zone 33 is used to complete the curing of the resin, forming the first pultruded preform. The preheating zone 31, intermediate transition zone 32, and curing zone 33 are each equipped with an independent temperature control system, and the heating power and temperature of each zone can be adjusted separately.

[0044] Multiple thermocouples are embedded in the cavity of the first pultrusion die 3 to monitor the temperature distribution of the resin-carbon fiber system within the die cavity in real time. The first pultrusion die 3 uses a Cr12MoV die with a cone angle of 2° to 5° at the die cavity inlet to facilitate the gradual bundle formation of the fiber bundles and reduce inlet resistance.

[0045] The second pultrusion die 4 is set after the first pultrusion die 3. The second pultrusion die 4 has a high-temperature curing zone 41 and a heat preservation and homogenization zone 42 arranged sequentially along the traction direction inside. The high-temperature curing zone 41 is used to cross-link and cure the outer coating resin and the preform interface resin. The heat preservation and homogenization zone 42 is used to make the core and surface temperatures of the profile more consistent, complete the final curing and reduce internal stress.

[0046] The high-temperature curing zone 41 and the heat preservation and homogenization zone 42 are each equipped with an independent temperature control system and thermocouples to monitor the temperature. The second pultrusion die 4 adopts a Cr12MoV die with a cone angle of 2° to 5° at the die cavity entrance. The second pultrusion die 4 is independent of the first pultrusion die 3 and they do not share a temperature control system. The traction speed can also be controlled separately.

[0047] The traction device 5 is located after the second pultrusion die 4 and is used to pull out the cured profile at a constant traction speed. The cutting device 6 is located after the traction device 5 and uses a follow-up cutting method to cut the product to a set length.

[0048] In use, carbon fibers are drawn out from the roller yarn holder 1 and arranged neatly on the roller yarn holder 1, with the tension of each fiber bundle controlled at 10-25 N / bundle. The carbon fibers enter the impregnation tank 2 to complete the impregnation, and then enter the first pultrusion die 3. The temperature of the preheating zone 31 of the first pultrusion die 3 is controlled at 60-110℃, the temperature of the intermediate transition zone 32 is controlled at 100-170℃, the temperature of the curing zone 33 is controlled at 150-210℃, and the traction speed V1 is controlled at 80-300 mm / min.

[0049] The fiber-resin system undergoes impregnation, gelation, and curing within the first pultrusion die 3, forming a preform with a small cross-section. This preform, acting as a filler, is coated with resin-impregnated carbon fibers and enters the second pultrusion die 4. The temperature of the high-temperature curing zone 41 in the second pultrusion die 4 is controlled at 150–180°C, the temperature of the heat-preserving homogenization zone 42 is controlled at 180–210°C, and the traction speed V2 is controlled at 80–200 mm / min.

[0050] The preform, along with the coated carbon fiber and resin, is fully impregnated and completely cured in the second pultrusion mold 4 to obtain a carbon fiber reinforced composite profile with a curing degree ≥95%. The cured profile is pulled out at a constant speed by the traction device 5 and cut to a set length by the cutting device 6.

[0051] Comparative Example

[0052] To verify the effect of the technical means and temperature settings used in this invention on the necessary technical effects, this embodiment sets up a comparative example to compare the secondary pultrusion scheme of this invention with the existing single pultrusion scheme.

[0053] The comparative example and the embodiment of the present invention used the same batch of 48K carbon fiber, the same epoxy resin system, and the same product specifications. The product cross-sectional dimensions were 120mm × 15mm, with a cross-sectional area of ​​5000mm². 2 The wall thickness is 15mm; except for the process parameters listed in the table below, the other molding conditions remain the same.

[0054] Table 1 Comparison of key process parameters between comparative examples and embodiments

[0055]

[0056] The main process parameters of each comparative example and embodiment are compared in Table 1 below. The defects of the existing single-pass pultrusion process, their causes, and the technical means and corresponding effects adopted in this invention are compared in Table 2 below.

[0057] Table 2 Comparison of Existing Techniques and the Technical Means and Effects of the Invention

[0058]

[0059] Table 3 Comparison of performance test results between comparative examples and embodiments

[0060]

[0061] Products were molded according to the process parameters in Table 1. Samples were taken from each group of products for testing. Five samples were taken from each group and the arithmetic mean was calculated. The test items included degree of curing, porosity, fiber volume fraction, interlaminar shear strength, surface cracks, and uncured core areas. The results are shown in the table below.

[0062] The comparative data above show that Comparative Example 1, using the existing single-stage pultrusion process, couples impregnation, gelation, and curing within the same mold. The curing zone (150–210°C) must simultaneously handle the exothermic reactions of gelation and curing. The core is far from the mold wall, resulting in a long heat conduction path. The curing degree difference between the core and surface reaches 9.6%, the porosity is 2.4%, and the fiber volume fraction is only 58.7%. Microcracks appear after demolding, and the interlaminar shear strength is 52.6 MPa. Comparative Example 2, under single-stage pultrusion conditions, simply increases the traction speed to 300 mm / min, shortening the resin's residence and heat transfer time within the mold. The curing degree difference between the core and surface further widens to 13.4%, the porosity increases to 3.1%, the fiber volume fraction decreases to 56.2%, and the interlaminar shear strength drops to 47.8 MPa. Multiple through-cracks also appear. This indicates that adjusting the traction speed alone under single-stage pultrusion conditions cannot improve the curing uniformity of thick-walled products; instead, it exacerbates defects.

[0063] Compared with Comparative Examples 1 and 2, Example 1 decouples the impregnation, gelation, and curing processes into two independent pultrusion stages, and divides the temperature settings into a preheating zone of 60-110°C, an intermediate transition zone of 100-170°C, and a curing zone of 150-210°C for the first pultrusion die, and a high-temperature curing zone of 150-180°C and a heat preservation and homogenization zone of 180-210°C for the second pultrusion die, with temperature controlled by two independent temperature control systems in each zone. The results showed that the curing degree of the product increased from 88.5% to 96.8%, the curing degree difference between the core and the surface decreased from 9.6% to 2.1%, the porosity decreased from 2.4% to 0.9%, the fiber volume fraction increased from 58.7% to 69.5%, the interlaminar shear strength increased from 52.6 MPa to 65.4 MPa, which is 22.4% higher than Comparative Example 1 and 36.8% higher than Comparative Example 2. The profile cross-section warpage decreased from 1.8 mm to 0.4 mm, the fiber loss during the trial molding decreased from 42 kg to 18 kg, and there were no cracks on the surface of the product and no uncured areas in the core.

[0064] The comparative data above show that: Firstly, decoupling single pultrusion into two-stage pultrusion allows the preform to complete impregnation and pre-curing in the first pultrusion, while only the outer coating layer and interface resin need to be cured in the second pultrusion. The core and surface layer no longer bear all the curing heat at the same time, thus significantly improving the curing uniformity. Secondly, temperature setting is a technical means to achieve the aforementioned necessary technical effects: if only a single high-temperature curing zone is set as in Comparative Example 1, the gel and curing are coupled within the same temperature zone, and the heat release is concentrated in the core; if only the traction speed is increased, the heat transfer time is insufficient, and defects are aggravated; only by setting preheating zones, intermediate transition zones, and curing zones at 60-110℃, 100-170℃, and 150-210℃ in the first pultrusion die, and high-temperature curing zones and heat preservation homogenization zones at 150-180℃ and 180-210℃ in the second pultrusion die, and by having the two temperature control systems be independent of each other, can the temperature distribution of the core and surface layers tend to be consistent, thereby simultaneously achieving the technical effects of curing degree ≥95%, porosity ≤1.2%, fiber volume fraction 65%-72%, and interlaminar shear strength increased by 18%-30%. Therefore, the aforementioned temperature zoning setting and independent temperature control constitute an indispensable technical feature of this invention.

[0065] The working principle of this invention is:

[0066] The traditional single-stage pultrusion process decouples impregnation, gelation, and curing into two independent stages: the first pultrusion and the second pultrusion. In the first pultrusion stage, temperature control in the preheating zone 31, intermediate transition zone 32, and curing zone 33 allows the carbon fiber and resin to gradually impregnate and pre-cur, forming a smaller, more stable preform. This avoids the insufficient core curing that can occur in large-section products during single pultrusion due to the large number of fibers, long impregnation paths, and concentrated heat release during curing. In the second pultrusion stage, the preform acts as a filler, with a new resin-impregnated carbon fiber coating, followed by final curing in the high-temperature curing zone 41 and the heat-insulating homogenization zone 42. The high-temperature curing zone 41 ensures full cross-linking of the outer coating and the interfacial resin, while the heat-insulating homogenization zone 42 ensures a more uniform internal temperature, reducing the difference in curing degree between the core and surface layers, and minimizing residual internal stress, porosity, and surface cracks. Because the first pultrusion die 3 and the second pultrusion die 4 have independent temperature control, and the traction speeds V1 and V2 can be controlled separately, the heating and traction regimes can be set separately for the preform and the outer coating layer, thereby improving the molding stability of thick-walled, large-section and high-fiber-content products.

[0067] Compared with single-stage pultrusion, this invention reduces the difficulty of pultruding large-section composite materials, significantly reduces the number of fibers required for startup, lowers production losses, saves costs, and improves production efficiency. The resulting carbon fiber reinforced composite profiles can stably achieve a fiber volume fraction of 65%–72%, porosity is reduced to below 1.2%, and interlaminar shear strength is increased by 18%–30%, making it suitable for continuous molding of ultra-thick, large-section carbon fiber reinforced composite profiles.

Claims

1. A carbon fiber reinforced composite material secondary pultrusion plate forming device, comprising a roller yarn frame (1), an impregnation tank (2), a first pultrusion die (3), a second pultrusion die (4), a traction device (5), and a cutting device (6). The roller yarn frame (1) is used to neatly arrange carbon fibers, and the impregnation tank (2) is used to impregnate the carbon fibers. Along the traction direction, the carbon fibers output by the roller yarn frame (1) are guided to the impregnation tank (2), and the impregnation tank (2) guides the impregnated carbon fibers to the inlet of the first pultrusion die (3). Its features are: Along the traction direction, after the roller yarn frame (1), the immersion tank (2), the first pultrusion die (3), the second pultrusion die (4), the traction device (5), and the cutting device (6) are arranged in sequence. The first pultrusion die (3) is provided with a preheating zone (31), an intermediate transition zone (32) and a curing zone (33) in sequence along the traction direction. Each of the preheating zone (31), intermediate transition zone (32) and curing zone (33) is equipped with an independent temperature control system. The second pultrusion die (4) is arranged with a high-temperature curing zone (41) and a heat preservation and homogenization zone (42) in sequence along the traction direction. The high-temperature curing zone (41) and the heat preservation and homogenization zone (42) are equipped with independent temperature control systems. The preform obtained by the first pultrusion die (3) is sent into the second pultrusion die (4) for secondary curing and pultrusion. The impregnated carbon fiber is tightly wrapped around the outer surface of the preform. The traction device (5) is used to pull out the profile after it has been cured by the second pultrusion die (4) at a constant speed; The cutting device (6) is used to cut the product to a set length.

2. The carbon fiber reinforced composite secondary pultrusion plate forming device according to claim 1, characterized in that, Both the first pultrusion die (3) and the second pultrusion die (4) are Cr12MoV dies, with a cone angle of 2° to 5° at the entrance of the die cavity.

3. The carbon fiber reinforced composite secondary pultrusion plate forming device according to claim 2, characterized in that, Multiple thermocouples are embedded in the cavities of the first pultrusion die (3) and the second pultrusion die (4) to monitor the temperature distribution of the resin-carbon fiber system in the die cavity in real time.

4. A process for forming carbon fiber reinforced composite secondary pultrusion plates, using the apparatus described in claim 3, characterized in that... Includes the following steps: Step 1: Arrange the carbon fibers neatly on the roller yarn frame (1) and maintain the tension of each fiber bundle at 10-25 N / bundle; Step 2: After impregnating the arranged carbon fibers with resin in the impregnation tank (2), the carbon fibers are sent into the first pultrusion mold (3). The first pultrusion mold (3) is set with a preheating zone (31) of 60-110°C, an intermediate transition zone (32) of 100-170°C and a curing zone (33) of 150-210°C from the inlet to the outlet. The traction speed V1 is controlled at 80-300 mm / min so that the fiber-resin system can be impregnated and cured to form a preform. Step 3: The second pultrusion die (4) is set with a high temperature curing zone (41) of 150-180℃ and a heat preservation and homogenization zone (42) of 180-210℃ along the traction direction. The traction speed V2 is controlled at 80-200mm / min so that the preform is fully impregnated with carbon fiber and resin and cured and shaped to obtain a carbon fiber reinforced composite profile with a curing degree ≥95%. Step four: The cured profile is pulled out by the traction device (5) at a constant rear traction speed and cut by the cutting device (6) to the set length.

5. The carbon fiber reinforced composite secondary pultrusion plate forming process according to claim 4, characterized in that, The carbon fiber in step one is 48K carbon fiber, and the fiber bundle tension is 10-25N / bundle.

6. The carbon fiber reinforced composite secondary pultrusion plate forming process according to claim 4, characterized in that, In step two, the temperature of the preheating zone (31) of the first pultrusion die (3) is 60-110℃, the temperature of the intermediate transition zone (32) is 100-170℃, the temperature of the curing zone (33) is 150-210℃, and the traction speed V1 is 80-300mm / min.

7. The carbon fiber reinforced composite secondary pultrusion plate forming process according to claim 4, characterized in that, In step three, the temperature of the high-temperature curing zone (41) of the second pultrusion die (4) is 150-180℃, the temperature of the heat preservation and homogenization zone (42) is 180-210℃, the traction speed V2 is 80-200mm / min, and the curing degree of the profile is ≥95%.

8. The carbon fiber reinforced composite secondary pultrusion plate forming process according to claim 4, characterized in that, In step three, the second pultrusion die (4) and the first pultrusion die (3) are independent of each other and are temperature controlled by an independent temperature control system. The final profile has a fiber volume fraction of 65% to 72%, a porosity of ≤1.2%, and an interlaminar shear strength that is 18% to 30% higher than that of a single pultrusion profile of the same specification.