In-situ repair method for net size of inner cavity of composite material launch tube

By preparing a skin inside the composite material launch tube and then vacuum-infusing resin, the problems of dimensional accuracy and structural reliability in repairing defects in the inner cavity of the composite material launch tube were solved, enabling efficient field repair and after-sales maintenance of large tubes.

CN123129498APending Publication Date: 2026-11-20TIANJIN ISTAR ADVANCED MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611320028.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing methods for repairing defects in the inner cavity of composite material launch tubes are difficult to guarantee dimensional accuracy, and the repair equipment is bulky, energy-intensive, and difficult to implement in the field, affecting the structural strength and reliability of the repaired area.

Method used

By preparing a single-sided mold with the same curvature as the inner wall of the launch tube, laying prepreg and hot-pressing to form a skin, drilling holes and laying dry fiber cloth on the skin, using an inner cavity limiting tooling for support, vacuum-injecting resin and curing to form a composite material repair layer, and setting resin nails to enhance the bonding strength.

Benefits of technology

It achieves net dimensional restoration of the launch tube cavity, with high surface smoothness, no need for secondary grinding, high inner diameter accuracy, suitable for field operations, reduces equipment requirements and transportation costs, and improves the structural reliability and number of uses of the repaired area.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123129498A_ABST
    Figure CN123129498A_ABST
Patent Text Reader

Abstract

The present application relates to a kind of composite material launch tube inner cavity net size in situ repair method;Step is prepared single-sided mould, pre-impregnated material is laid on single-sided mould, hot-pressing is cured, skin is obtained, hole is punched on skin, perforation is formed, and prefabricated skin is obtained;Dry fiber cloth is laid on the inner wall of launch tube;Prefabricated skin is laid on dry fiber cloth, and prefabricated skin is supported using inner cavity limiting tooling, release cloth, porous release film and flow guide net are laid, glue injection port and air extraction port are respectively arranged at the both ends of flow guide net, vacuum bag film is sealed, vacuum is extracted, resin is poured, and curing is carried out;Vacuum bag film sealing, flow guide net, porous release film, release cloth and inner cavity limiting tooling are removed, and composite material repair layer is formed;Through the proposal of the composite material launch tube inner cavity net size in situ repair method, the technical problems that the existing repair is mostly repaired by hand or repaired by using hot press tank, equipment volume is large, energy consumption is high, precision is poor, and it is difficult to implement in the field are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of composite material launch tube inner wall repair technology, and in particular to an in-situ repair method for the net dimensions of the inner cavity of a composite material launch tube. Background Technology

[0002] Fiber-reinforced resin-based composite materials (such as carbon fiber reinforced epoxy resin, glass fiber reinforced epoxy resin, or phenolic resin) are widely used in aerospace, defense, and pressure vessel industries due to their advantages such as high specific strength, high specific modulus, ablation resistance, and strong design flexibility. However, in composite material launch tubes (such as launch tubes, pressure-resistant launch tubes, and ammunition launch tubes), defects often develop on the inner surface during manufacturing, transportation, or use due to ablation, erosion, impact, scratches, etc., affecting the product's performance.

[0003] Currently, the main problems with repair techniques for defects in the inner cavity of composite material launch tubes are as follows: 1) Existing repair methods mostly use hand lay-up or partial bonding, making it difficult to precisely control the thickness of the repair layer. This results in the inner diameter dimension being out of tolerance after repair, making it difficult to meet the strict requirements of the launch tube for net dimensions. 2) The surface roughness of the hand-applied repair layer is large, requiring secondary grinding to meet the usage requirements, which increases the complexity of the process and processing costs. Moreover, it is difficult to guarantee the high dimensional accuracy requirements for large launch tubes. 3) Insufficient adhesion between the repair layer and the launch tube body can easily lead to secondary repair defects such as delamination and detachment, affecting the structural strength and reliability of the repaired area; 4) Existing repair processes mostly rely on large heating and pressurizing equipment such as autoclaves. These equipment are bulky, energy-intensive, and difficult to implement in the field. They need to be transported back to the factory, making after-sales maintenance of large launch tubes extremely inconvenient and with long maintenance cycles. 5) Existing pipeline repair technologies such as CIPP (Cured In-Situ Liner) cannot achieve precise control over the size of the repair area.

[0004] Therefore, in order to address the above problems, the present invention urgently needs to provide a method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube. Summary of the Invention

[0005] The purpose of this invention is to provide an in-situ repair method for the net dimensions of the inner cavity of a composite material launch tube. This method addresses the technical problems in the prior art where manual repair of defects in the inner cavity of a composite material launch tube is difficult to guarantee dimensional accuracy, or where autoclave repair is used, which involves bulky equipment, high energy consumption, and is difficult to implement in the field.

[0006] This invention provides a method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube, characterized by the following steps: Prepare a single-sided mold with the same curvature as the inner wall of the launch tube to be repaired. Lay a prepreg material with the same material as the inner wall of the launch tube on the single-sided mold, and heat-press to cure it to obtain a skin. Drill holes on the surface of the skin to form perforations that penetrate the skin to obtain a prefabricated skin. The defect layer is removed by grinding on the inner wall of the launch tube to be repaired, and after cleaning, dry fiber cloth is laid. The number of layers in the dry fiber cloth satisfies the formula n= (h1-h2) / t , n is the number of layers, and t is the theoretical thickness of a single layer of dry fiber cloth after compaction. This indicates rounding up, where h1 is the thickness of the defect layer removed and h2 is the thickness of the prefabricated skin.

[0007] A prefabricated skin is laid on a dry fiber cloth, and an inner cavity limiting fixture is used to support the prefabricated skin. Then, a release cloth, a perforated isolation membrane, and a flow guide net are laid in sequence from the inside to the outside. An injection port and an air extraction port are set at both ends of the flow guide net. The vacuum bag is sealed, a vacuum is drawn, and resin is injected through the injection port. After the injection is completed, the resin is cured. After the resin is cured, the vacuum bag, the flow guide net, the perforated isolation membrane, the release cloth, and the inner cavity limiting fixture are removed in sequence to form a composite material repair layer on the inner wall of the launch tube.

[0008] Preferably, the composite material repair layer includes a dry fiber cloth that adheres to the inner wall of the launch tube and a prefabricated skin disposed on the dry fiber cloth. Each perforation of the prefabricated skin contains a resin nail, and one end of each resin nail protrudes from the perforation and adheres tightly to the dry fiber cloth.

[0009] Preferably, the cross-section of the perforation is a T-shaped hole.

[0010] Preferably, the curing temperature of the resin is 60℃~150℃, the heating rate is 2℃ / min~5℃ / min, and the holding time is 2h~6h; After the vacuum bag is sealed, the extraction port is connected to the vacuum pump through a pipeline. The vacuum is evacuated to -0.08MPa to -0.1MPa and held for 10 to 20 minutes.

[0011] Preferably, the inner cavity limiting fixture includes a support rod, with adjusting rods inserted at both ends of the support rod. One end of the adjusting rod is provided with a hole for insertion into the support rod, and the other end is provided with an arc-shaped plate with the same curvature as the inner wall of the launch tube. The adjusting rod is fixedly connected to the support rod by a limiting pin.

[0012] Preferably, the resin is epoxy resin or phenolic resin; the fiber cloth is carbon fiber cloth or glass fiber cloth with a surface density of 200g / ㎡ to 600g / ㎡.

[0013] Preferably, the prefabricated skin material is carbon fiber reinforced resin matrix composite or glass fiber reinforced resin matrix composite.

[0014] Preferably, the thickness of the skin is 0.5-2mm; the diameter of the perforation is 1-3mm; and the distance between two adjacent perforations is 10-30mm.

[0015] Preferably, before laying the skin, the defect layer on the inner surface of the launch tube to be repaired is removed by mechanical grinding or high-pressure water jetting. The initial thickness of the defect layer is determined according to the degree of defect. After removal, the inner surface of the launch tube is subjected to dust removal and degreasing treatment in sequence.

[0016] The in-situ repair method for the net dimensions of the inner cavity of a composite material launch tube provided by this invention has the following advantages compared with the prior art: 1. The present invention provides a method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube. By preparing a skin and drilling holes in the skin to obtain a prefabricated skin, and by accurately calculating the number of fiber cloth layers and coordinating the vacuum infusion process, the repair of the defective parts of the inner wall of the launch tube and the restoration of the net dimensions can be completed simultaneously. The repaired inner cavity surface of the tube is smooth and has high dimensional accuracy. Moreover, it does not require large heating and pressurization equipment, making it suitable for field operations, especially for field repairs and after-sales maintenance of large tubes, reducing transportation costs.

[0017] 2. The present invention provides a method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube. After repairing the defective parts of the inner wall of the launch tube, the repaired inner wall of the launch tube has high smoothness and the surface roughness Ra can reach below 1.6μm, which can meet the requirements without secondary grinding.

[0018] 3. The present invention provides an in-situ repair method for the net dimensions of the inner cavity of a composite material launch tube. After repair, the inner diameter accuracy is ≤ ±0.2mm, which effectively solves the problem of easy out-of-tolerance inner diameter in existing repair methods.

[0019] 4. The present invention provides a method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube. A perforation is set on the skin, and after resin is injected, a resin nail is formed in the perforation. The resin nail forms a rivet structure, which improves the bonding strength between the skin and the fiber cloth layer, avoids the risk of skin debonding, and the bonding strength can reach more than 35MPa.

[0020] 5. The present invention provides a method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube. The skin is overlapped, which avoids stress concentration and improves the overall structural reliability of the repair area.

[0021] 6. The present invention provides a method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube, which can further increase the number of uses of the composite material launch tube, realize reuse, significantly reduce the scrap rate, save usage costs, and has high application value. Attached Figure Description

[0022] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0023] Figure 1 This is a schematic diagram (sectional view) of the composite material repair layer described in this invention. Figure 2 This is a structural schematic diagram (sectional view) of the internal cavity limiting tooling described in this invention. Figure 3 This is a schematic diagram (sectional view) of the structure of the prefabricated skin laying described in this invention.

[0024] Explanation of reference numerals in the attached figures: 1. Dry fiber cloth; 2. Prefabricated skin; 3. Resin nails; 51. Support rod; 52. Adjusting rod; 53. Curved plate; 54. Limiting pin. Detailed Implementation

[0025] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0026] In the description of this invention, it should be noted that the terms "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing the invention and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the invention. Furthermore, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0027] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.

[0028] The present invention provides a method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube, comprising the following steps: S1) Prepare a single-sided mold with the same curvature as the inner wall of the launch tube to be repaired, lay a prepreg of the same material as the inner wall of the launch tube on the single-sided mold, heat press and cure to obtain a skin, punch holes on the surface of the skin to form a perforation through the skin, and obtain a prefabricated skin. S2) Lay dry fiber cloth on the inner wall of the launch tube to be repaired; S3) Lay a prefabricated skin on the dry fiber cloth, support the prefabricated skin with an inner cavity limiting fixture, and then lay the release cloth, perforated isolation membrane and flow guide net in sequence from the inside to the outside. Set the glue injection port and air extraction port at both ends of the flow guide net, seal with vacuum bag film, draw a vacuum, and inject resin through the glue injection port. After the injection is completed, the resin is cured. After the resin is cured, remove the vacuum bag film, flow guide net, perforated isolation membrane, release cloth and inner cavity limiting fixture in sequence to form a composite material repair layer on the inner wall of the launch tube.

[0029] Specifically, the number of layers in the dry fiber cloth satisfies the formula n= (h1-h2) / t , n is the number of layers, and t is the theoretical thickness of a single layer of dry fiber cloth after compaction. This indicates rounding up, where h1 is the thickness of the defect layer removed and h2 is the thickness of the prefabricated skin.

[0030] Specifically, the composite material repair layer includes a dry fiber cloth 1 that is attached to the inner wall of the launch tube 901, a prefabricated skin 2 disposed on the dry fiber cloth 1, and a resin nail 3 in each perforation of the prefabricated skin 2, with one end of each resin nail 3 protruding from the perforation and tightly attached to the dry fiber cloth 1.

[0031] Specifically, the cross-section of the perforation is a T-shaped hole.

[0032] Specifically, the curing temperature of the resin is 60℃~150℃, the heating rate is 2℃ / min~5℃ / min, and the holding time is 2h~6h; After the vacuum bag is sealed, the extraction port is connected to the vacuum pump through a pipeline. The vacuum is evacuated to -0.08MPa to -0.1MPa and held for 10 to 20 minutes.

[0033] Specifically, the inner cavity limiting fixture includes a support rod 51, with adjusting rods 52 inserted at both ends of the support rod 51. One end of the adjusting rod 52 is provided with a hole for insertion into the support rod, and the other end is provided with an arc-shaped plate 53 with the same curvature as the inner wall of the launch tube. The adjusting rod 52 is fixedly connected to the support rod 51 by a limiting pin 54.

[0034] Specifically, the resin is epoxy resin or phenolic resin; the fiber cloth is carbon fiber cloth or glass fiber cloth with a surface density of 200g / ㎡~600g / ㎡; the prefabricated skin material is carbon fiber reinforced resin matrix composite material or glass fiber reinforced resin matrix composite material.

[0035] Specifically, the thickness of the skin is 0.5-2mm; the diameter of the perforation is 1-3mm; and the distance between two adjacent perforations is 10-30mm.

[0036] Specifically, before laying the skin, the defect layer on the inner surface of the launch tube to be repaired is removed by mechanical grinding or high-pressure water jetting. The initial thickness of the defect layer is determined according to the degree of defect. After removal, the inner surface of the launch tube is subjected to dust removal and degreasing treatment in sequence.

[0037] This invention provides a method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube. By preparing a skin and drilling holes in the skin to obtain a prefabricated skin, and by accurately calculating the number of fiber cloth layers and coordinating with the vacuum infusion process, the repair of defects in the inner wall of the launch tube and the restoration of net dimensions can be completed simultaneously. The repaired inner cavity surface is smooth and has high dimensional accuracy. Moreover, it does not require large heating and pressurizing equipment, making it suitable for field operations, especially for field repairs and after-sales maintenance of large tubes, reducing transportation costs.

[0038] The present invention provides a method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube. After repairing the defective parts of the inner wall of the launch tube, the repaired inner wall of the launch tube has high smoothness and the surface roughness Ra can reach below 1.6μm, which can meet the requirements without secondary grinding.

[0039] The present invention provides an in-situ repair method for the net dimensions of the inner cavity of a composite material launch tube. After repair, the inner diameter accuracy is ≤ ±0.2mm, which effectively solves the problem of easy out-of-tolerance inner diameter in existing repair methods.

[0040] The present invention provides a method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube. A perforation is set on the skin, and after resin is injected, a resin nail is formed in the perforation. The resin nail forms a rivet structure, which strengthens the bonding strength between the skin and the fiber cloth layer, avoids the risk of skin debonding, and the bonding strength can reach more than 35MPa.

[0041] The present invention provides a method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube. The skin is overlapped to avoid stress concentration and improve the overall structural reliability of the repair area.

[0042] The present invention provides an in-situ repair method for the net dimensions of the inner cavity of a composite material launch tube, which can further increase the number of uses of the composite material launch tube, realize reuse, significantly reduce the scrap rate, save usage costs, and has high application value.

[0043] Example 1 The present invention provides a method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube, comprising the following steps: 101) Prepare a single-sided mold with the same curvature as the inner wall of the launch tube to be repaired. The single-sided mold is made of aluminum alloy and has a curvature diameter of 500 mm, which is consistent with the curvature of the inner cavity of the launch tube. Lay a prepreg material with the same material as the inner wall of the launch tube on the single-sided mold. In this embodiment, carbon fiber reinforced phenolic resin prepreg is used. It is hot-pressed and cured to obtain a skin. Drill holes on the surface of the skin to form a through hole, and obtain a 1 mm thick prefabricated skin. The surface roughness of the prefabricated skin Ra≤0.8μm and the cross section of the through hole is a T-shaped hole. 102) An angle grinder was used to mechanically grind the impact defect area on the inner surface of the launch tube. The defect layer removal thickness h1 was 1.5mm. The grinding range covered the defect area and a 50mm transition area around it. After grinding, high-pressure air was used to blow away dust, followed by wiping with anhydrous ethanol for degreasing, and then drying for later use. Based on the design net dimension D=500mm of the launch tube inner diameter, the defect layer removal thickness h1=1.5mm, and the prefabricated skin thickness h2=1mm, the required number of dry fiber cloth layers was calculated. FP300 carbon fiber cloth (plain weave) with a surface density of 200g / ㎡ was selected. The theoretical thickness t of a single compacted layer is approximately 0.168mm. The number of dry fiber cloth layers satisfies the formula n= (h1-h2) / t Where n is the number of layers, and t is the theoretical thickness of a single layer of dry fiber cloth after compaction. This indicates rounding up, where h1 is the thickness of the defect layer removed and h2 is the thickness of the prefabricated skin. Specifically, n= (h1-h2) / t = (1.5-1) / (0.168) = 2.97 =3 (layers); Dry fiber cloth is laid on the inner wall of the launch tube to be repaired. Three layers of FP300 carbon fiber cloth (plain weave) are laid layer by layer on the treated inner surface. During the laying process, a scraper can be used to scrape and press from the middle to both sides to ensure that the fiber cloth is flat and wrinkle-free. The seams of adjacent dry fiber cloths are staggered by more than 100mm along the cylinder axis to avoid overlapping seams.

[0044] 103) Lay a prefabricated skin on the dry fiber cloth, support the prefabricated skin with an inner cavity limiting fixture, and position and press the prefabricated skin axially and radially. Then, lay the release cloth, the perforated isolation membrane and the flow guide net in sequence from the inside to the outside. Set the glue injection port and the air extraction port at both ends of the flow guide net, seal with a vacuum bag film, draw a vacuum, and inject resin through the glue injection port. After the injection is completed, the resin is cured. After the resin is cured, remove the vacuum bag film, the flow guide net, the perforated isolation membrane, the release cloth and the inner cavity limiting fixture in sequence to form a composite material repair layer on the inner wall of the launch tube.

[0045] like Figure 1 As shown, the composite material repair layer includes a dry fiber cloth 1 that is attached to the inner wall of the launch tube 901, a prefabricated skin 2 disposed on the dry fiber cloth 1, and a resin nail 3 in each perforation of the prefabricated skin 2. One end of each resin nail 3 protrudes from the perforation and is tightly attached to the dry fiber cloth.

[0046] Specifically, the curing temperature of the resin is 150℃, the heating rate is 3℃ / min, and the holding time is 4h. After the vacuum bag is sealed, the extraction port is connected to the vacuum pump through a pipeline, and the vacuum is drawn to -0.09MPa and held for 15 minutes.

[0047] like Figure 2 As shown, the inner cavity limiting fixture of this embodiment includes a support rod 51, with adjusting rods 52 passing through both ends of the support rod 51. One end of the adjusting rod 52 is provided with an insertion hole for insertion with the support rod, and the other end is provided with an arc-shaped plate 53 with the same curvature as the inner wall of the launch tube. The adjusting rod 52 is fixed to the support rod 51 by a limiting pin 54. The side wall of one end of the support rod 51 through which the adjusting rod 52 passes is provided with first positioning holes at intervals, and the side wall of the adjusting rod 52 is provided with a second positioning hole. The limiting pin 54 passes through the second positioning hole and into the first positioning hole.

[0048] like Figure 3 As shown, in this embodiment, the adjacent prefabricated skins adopt a stepped interlocking structure with an overlap width of 500mm.

[0049] The thickness of the prefabricated skin in this embodiment is 1.0 mm; the diameter of the perforation is 2 mm, and the distance between two adjacent perforations is 25 mm.

[0050] During the curing process, the resin impregnates the perforations of the prefabricated skin, forming resin nails between the prefabricated skin and the dry fiber cloth. The resin nails have a rivet structure. At the same time, the inner cavity limiting tool restricts the position of the inner surface of the prefabricated skin, ensuring that the inner diameter reaches the designed net inner diameter dimension D after curing.

[0051] Eight measuring points were evenly selected along the circumference of the inner wall of the launch tube using an inside micrometer to detect the inner diameter of the repair area. The inner diameter of the repair area was found to be within the range of 500.0-500.4 mm, which is within the design net dimensional tolerance. The surface roughness of the repair area was detected using a surface roughness meter, and the Ra value was 1.2 μm.

[0052] The bonding strength of the repaired area was tested according to GB / T 7124-2008 "Determination of Tensile Shear Strength of Adhesives", and the result was 38 MPa, which meets the strength requirements.

[0053] Example 2 The present invention provides a method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube, comprising the following steps: 201) Prepare a single-sided mold with the same curvature as the inner wall of the launch tube to be repaired. The single-sided mold is made of Q235 steel and has a curvature diameter of 1400 mm, which is consistent with the curvature of the inner cavity of the launch tube. Lay a prepreg with the same material as the inner wall of the launch tube on the single-sided mold. In this embodiment, glass fiber reinforced resin prepreg is used. Hot pressing and curing are performed to obtain a 0.8 mm thick skin. Drill holes on the surface of the skin to form perforations that penetrate the skin, thereby obtaining a prefabricated skin. The surface roughness Ra of the prefabricated skin is ≤0.8 μm. 202) An angle grinder was used to mechanically grind the impact defect area on the inner surface of the launch tube. The defect layer removal thickness h1 was 1.5mm. The grinding range covered the defect area and a 50mm transition area around it. After grinding, high-pressure air was used to blow away dust, followed by wiping with anhydrous ethanol for degreasing, and then drying for later use. Based on the design net dimension D=1400mm of the launch tube inner diameter, the defect layer removal thickness h1=2.0mm, and the prefabricated skin thickness h2=0.8mm, the required number of dry fiber cloth layers was calculated. EW400 glass fiber cloth with a surface density of 400g / ㎡ was selected. The theoretical thickness t of a single layer is approximately 0.34mm. The number of dry fiber cloth layers satisfies the formula n= (h1-h2) / t Where n is the number of layers, and t is the theoretical thickness of a single layer of dry fiber cloth after compaction. This indicates rounding up, where h1 is the thickness of the defect layer removed and h2 is the thickness of the prefabricated skin. Specifically, n= (h1-h2) / t = (2.0-0.8) / (0.34) = 3.53 =4 floors; Dry fiber cloth is laid on the inner wall of the launch tube to be repaired. Four layers of EW400 glass fiber cloth are laid one by one on the treated inner surface. During the laying process, a scraper can be used to scrape and press from the middle to both sides to ensure that the fiber cloth is flat and wrinkle-free. The seams of adjacent fiber cloths are staggered by more than 150mm along the axial direction of the tube to avoid overlapping seams.

[0054] 203) Lay a prefabricated skin on the dry fiber cloth, support the prefabricated skin with an inner cavity limiting fixture, and position and press the prefabricated skin axially and radially. Then, lay the release cloth, the perforated isolation membrane and the flow guide net in sequence from the inside to the outside. Set the glue injection port and the air extraction port at both ends of the flow guide net, seal with a vacuum bag film, draw a vacuum, and inject resin through the glue injection port. After the injection is completed, the resin is cured. After the resin is cured, remove the vacuum bag film, the flow guide net, the perforated isolation membrane, the release cloth and the inner cavity limiting fixture in sequence to form a composite material repair layer on the inner wall of the launch tube.

[0055] In this embodiment, adjacent prefabricated skins adopt a stepped interlocking structure with an overlap width of 500mm.

[0056] The composite material repair layer includes a dry fiber cloth that adheres to the inner wall of the launch tube and a prefabricated skin set on the dry fiber cloth. Each perforation of the prefabricated skin contains a resin nail, and one end of each resin nail protrudes from the perforation and adheres tightly to the dry fiber cloth.

[0057] Specifically, the cross-section of the perforation is a T-shaped hole.

[0058] Specifically, the resin curing temperature is 150℃, the heating rate is 3℃ / min, and the holding time is 6h; After the vacuum bag is sealed, the extraction port is connected to the vacuum pump through a pipeline, and the vacuum is drawn to -0.085MPa and held for 10 minutes.

[0059] Specifically, the internal cavity limiting tooling structure is the same as in Example 1.

[0060] In this embodiment, the resin is epoxy resin; the skin material is glass fiber reinforced epoxy resin-based composite material. In this embodiment, the thickness of the skin is 0.8 mm; the diameter of the perforation is 1.5 mm, and the distance between two adjacent perforations is 30 mm.

[0061] During the curing process, the resin impregnates the perforations of the prefabricated skin, forming a resin rivet structure between the prefabricated skin and the dry fiber cloth. At the same time, the inner cavity limiting tool restricts the position of the inner surface of the prefabricated skin, ensuring that the inner diameter reaches the designed net inner diameter dimension D after curing.

[0062] Eight measuring points were evenly selected along the circumference of the inner wall of the launch tube using an inside micrometer to detect the inner diameter of the repair area. The inner diameter of the repair area was found to be within the range of 1399.6-1400.2 mm, which is within the design net dimensional tolerance. The surface roughness of the repair area was detected using a surface roughness meter, and the Ra value was 0.9 μm.

[0063] The bonding strength of the repaired area was tested according to GB / T 7124-2008 "Determination of Tensile Shear Strength of Adhesives", and the result was 42 MPa, which meets the strength requirements.

[0064] Comparative Example 1 The launch tube of Example 1 was repaired using a traditional manual pasting method. After removing the defects, carbon fiber cloth and phenolic resin were directly hand-pasted onto the inner surface of the launch tube without using prefabricated skin or vacuum injection process. It was cured at room temperature for 24 hours.

[0065] The test was conducted according to the test method in Example 1. The inner diameter of the repaired area was measured to be in the range of 498.5 mm to 502.3 mm, which is a large dimensional deviation. The surface roughness Ra is 1.8 μm, which requires secondary grinding. The bonding strength is 22 MPa. Compared with Example 1, the traditional method is significantly inferior in terms of dimensional accuracy, surface quality and bonding strength.

[0066] Comparative Example 2 The only difference between this comparative example and Example 1 is that the prefabricated skin is not perforated.

[0067] The bonding strength of the repaired area was tested according to GB / T 7124-2008 "Determination of Tensile Shear Strength of Adhesives". The result was 28 MPa. Compared with Example 1, the bonding strength decreased by 26.3%. This indicates that drilling holes in the prefabricated skin and injecting resin to form a rivet structure has a significant effect on enhancing the bonding force.

[0068] Comparative Example 3 The only difference between this comparative example and Example 1 is that the internal cavity limiting tool is not used.

[0069] Eight measuring points were evenly selected along the circumference of the inner wall of the launch tube using an inside micrometer to detect the inner diameter of the repair area. The inner diameter of the repair area was found to be within the range of 500.3-501.1 mm, which exceeded the tolerance range. The surface roughness of the repair area was detected using a surface roughness meter, and the Ra value was 1.2 μm.

[0070] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube, characterized in that: Includes the following steps: Prepare a single-sided mold with the same curvature as the inner wall of the launch tube to be repaired. Lay a prepreg material with the same material as the inner wall of the launch tube on the single-sided mold, and heat-press to cure it to obtain a skin. Drill holes on the surface of the skin to form perforations that penetrate the skin to obtain a prefabricated skin. Dry fiber cloth was laid on the inner wall of the launch tube to be repaired (1). A prefabricated skin (2) is laid on a dry fiber cloth (1). The prefabricated skin (2) is supported by an inner cavity limiting fixture. Then, a release cloth, a perforated isolation membrane, and a flow guide are laid from the inside out. An injection port and an air extraction port are set at both ends of the flow guide. The vacuum bag is sealed and a vacuum is drawn. Resin is injected from the injection port. After the resin has cured, the vacuum bag, the flow guide, the perforated isolation membrane, the release cloth, and the inner cavity limiting fixture are removed in sequence to form a composite material repair layer on the inner wall of the launch tube.

2. The method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube according to claim 1, characterized in that: The number of layers in the dry fiber cloth (1) satisfies the formula n= (h1-h2) / t ,in, n is the number of layers, and t is the theoretical thickness of a single layer of dry fiber cloth after compaction. This indicates rounding up, where h1 is the thickness of the defect layer removed and h2 is the thickness of the prefabricated skin.

3. The method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube according to claim 1, characterized in that: The composite material repair layer includes a dry fiber cloth (1) that is attached to the inner wall of the launch tube and a prefabricated skin (2) set on the dry fiber cloth (1). Each perforation of the prefabricated skin (2) contains a resin nail (3), and one end of each resin nail (3) protrudes from the perforation and is tightly attached to the dry fiber cloth (1).

4. The method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube according to claim 1, characterized in that: After the vacuum bag is sealed, the extraction port is connected to the vacuum pump through a pipeline. The vacuum is evacuated to -0.08MPa to -0.1MPa and held for 10 to 20 minutes.

5. The method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube according to claim 1, characterized in that: The curing temperature of the resin is 60℃~150℃, the heating rate is 2℃ / min~5℃ / min, and the holding time is 2h~6h.

6. The method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube according to claim 1, characterized in that: The inner cavity limiting fixture includes a support rod (51), and an adjusting rod (52) is installed at both ends of the support rod (51). One end of the adjusting rod (52) is provided with a hole for insertion into the support rod (51), and the other end is provided with an arc plate (53) with the same curvature as the inner wall of the launch tube. The adjusting rod (52) is fixed to the support rod (51) by a limiting pin (54).

7. The method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube according to claim 1, characterized in that: The resin is epoxy resin or phenolic resin; the fiber cloth is carbon fiber cloth or glass fiber cloth, with a surface density of 200g / ㎡~600g / ㎡.

8. The method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube according to claim 1, characterized in that: The prefabricated skin material is carbon fiber reinforced resin matrix composite or glass fiber reinforced resin matrix composite.

9. The method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube according to claim 1, characterized in that: The thickness of the prefabricated skin is 0.5-2mm; the diameter of the perforation is 1-3mm, and the distance between two adjacent perforations is 10-30mm.

10. The method for in-situ repair of the net dimensions of the inner cavity of a composite material launch tube according to claim 1, characterized in that: Before laying the skin, the defect layer on the inner surface of the launch tube to be repaired is removed by mechanical grinding or high-pressure water jetting. The initial thickness of the defect layer is determined according to the degree of defect. After removal, the inner surface of the launch tube is subjected to dust removal and degreasing treatment in sequence.