Lightweight mirror blank and method of manufacturing the same
The lightweight mirror blank was prepared by 3D printing and two-step sintering and annealing process, which solved the problems of long preparation cycle and easy structural deformation in the existing technology, and achieved high-precision, non-destructive forming and good consistency of lightweight mirror blank.
Patent Information
- Application Number
- CN202611332338.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-20
AI Technical Summary
Existing mirror blank preparation methods suffer from long processing times, the easy introduction of air bubbles and residual stress, and difficulty in processing complex topological structures. Furthermore, thin-walled honeycomb structures are prone to deformation under thermal cycling, which limits lightweight design.
Lightweight mirror blanks are prepared using 3D printing technology. A printing paste is formed by mixing quartz glass powder, photocurable resin precursor, dispersant and binder, and then deep ultraviolet light is used for curing and printing. Combined with a two-step sintering and annealing process, a conformal support fixture is used to constrain the deformation, and the front panel and back panel are connected by a sealing method to achieve dimensional compensation and thermal stress management.
It shortens the preparation cycle, improves printing accuracy and mirror blank integrity, avoids bubbles and warping, ensures batch production consistency and mechanical properties, realizes non-destructive molding of complex topological structures, and meets the requirements of lightweighting and functionalization.
Smart Images

Figure CN123129502A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of additive manufacturing technology, specifically relating to a lightweight mirror blank and its preparation method. Background Technology
[0002] Reflectors are core components of optical systems such as aerospace optical remote sensing cameras and space telescopes; their surface accuracy and thermal stability directly determine image quality. To ensure surface stability under temperature fluctuations during on-orbit operation, mirror blanks are generally made of materials with low coefficients of thermal expansion. Quartz glass (high-purity SiO2, with a linear expansion coefficient of approximately 5.7 × 10⁻⁶) is a common example. -7 ( / ℃) and its doped systems (such as SiO2-TiO2 ultra-low expansion glass, with a thermal expansion coefficient as low as 0.03×10) -6 With a low coefficient of thermal expansion (below ℃), good temperature stability, and excellent optical processing and coating properties, it is the preferred material for high-performance aerospace mirrors. At the same time, to meet the weight reduction requirements of spacecraft, mirrors usually adopt lightweight structural designs such as honeycomb sandwich cores. The honeycomb sandwich core is welded to the face plate and the base plate to form a "sandwich" structure, which reduces the weight of the mirror blank while ensuring rigidity and surface accuracy.
[0003] However, existing methods for preparing mirror blanks have significant drawbacks: The traditional “cutting honeycomb + high-temperature welding” process takes several months. The welding process is prone to introducing air bubbles, residual stress and deformation. Furthermore, water cutting is difficult to process complex topological structures such as variable wall thickness and transition rounded corners. Thin-walled honeycomb structures are prone to deformation under the thermal cycle of water cutting and welding, which seriously restricts further lightweight design. Summary of the Invention
[0004] In view of this, the present invention provides a lightweight mirror blank and its preparation method. The preparation method provided by the present invention has the characteristics of short preparation cycle, prevention of thin-wall cracking, high printing accuracy, and controllable air bubbles in the printed mirror blank.
[0005] To address the above problems, the present invention provides the following technical solution: This invention provides a method for preparing a lightweight mirror blank, comprising the following steps: (1) The quartz glass system powder, the photocurable resin precursor, the dispersant and the binder are mixed and then dispersed and degassed to obtain the printing paste; (2) The printing paste is 3D printed to obtain an intermediate blank or a mirror blank; the structure of the intermediate blank includes a honeycomb sandwich layer, or a honeycomb sandwich layer and a face / back plate; the structure of the mirror blank includes a honeycomb sandwich layer, a face plate and a back plate; before 3D printing, the original three-dimensional model of the structure to be formed is pre-enlarged and compensated according to the volume shrinkage rate after degreasing and sintering of the paste, so that the size of the mirror blank after sintering falls back to the design value; the pre-enlargement compensation factor = 1 / (100% - shrinkage rate); (3) When the 3D printing yields an intermediate blank print body, the intermediate blank print body is degreased, sintered and annealed in sequence, then sealed with the panel and / or back plate and annealed again to obtain a lightweight mirror blank. When the 3D printing produces a mirror blank, the mirror blank is sequentially degreased, sintered, and annealed to obtain a lightweight reflective mirror blank.
[0006] Preferably, by weight, the printing paste comprises 100 parts of quartz glass system powder, 40-60 parts of photocurable resin precursor, 0.5-5 parts of dispersant and 0.5-3 parts of binder; the solid content of the printing paste is 40-60 vol.
[0007] Preferably, the dispersant is one or more of ammonium polyacrylate, polyvinylpyrrolidone, and polyethylene glycol; the binder is one or more of trimethylolpropane triacrylate, polyethylene glycol diacrylate, and hydroxyethyl acrylate.
[0008] Preferably, the 3D printing is deep ultraviolet (DEUV) photopolymerization printing; the wavelength of the DEUV is 200-300 nm, the printing layer thickness is 20-100 μm, and the optical power density is 5-50 mW / cm². 2 The scanning speed is 10~200 mm / s.
[0009] Preferably, the wall thickness of the reinforcing ribs in the honeycomb sandwich layer is 0.2~10mm.
[0010] Preferably, the degreasing temperature is 200~600℃, the holding time is 1~4h, and the heating rate of the degreasing treatment is 1~10℃ / min.
[0011] Preferably, the sintering is a first sintering and a second sintering performed sequentially; the temperature of the first sintering is 1000~1200 ℃, and the holding time is 1~3h; the temperature of the second sintering is 1250~1500 ℃, the holding time is 2~6h, and the heating rate to the sintering temperature is 1~10℃ / min.
[0012] Preferably, the annealing is performed by holding at a preset temperature for 1 to 4 hours and then slowly cooling to room temperature at a rate of 1 to 5 °C / min; the preset temperature is the glass transition temperature of the sintered body ±50 °C.
[0013] Preferably, the sealing method is at least one of flame sealing, laser sealing, or low-expansion glass powder sealing; the sealing method is selected based on the matching degree of the thermal expansion coefficients of the panel / back panel and the sintered body of the printed part: when the difference in thermal expansion coefficients between the two is ≤1×10 -7 At a temperature of / ℃, laser sealing or low-expansion glass powder sealing should be used, with a sealing temperature ≤1000℃; when the difference in thermal expansion coefficients between the two is greater than 1×10 -7 At / ℃, low-expansion glass powder with a thermal expansion coefficient between the two is used for sealing.
[0014] The present invention also provides a lightweight mirror blank prepared by the preparation method described above, comprising a honeycomb core layer and a panel and a back plate connected to both sides of the honeycomb core layer; the honeycomb core layer comprises a plurality of honeycomb cells, the honeycomb cells being formed by reinforcing ribs surrounding each other.
[0015] Compared with the prior art, the present invention has the following advantages: (1) The mirror blank is formed by photopolymerization three-dimensional printing, eliminating the whole material water cutting process and welding process, and the preparation cycle of the 500 mm diameter mirror blank is shortened from about 3 months to 3~10 days; (2) Large-size thin-walled honeycomb structures have a large shrinkage rate during degreasing and sintering (up to 10%~30%). If printed directly according to the design size, systematic dimensional deviations and warping will occur. This invention eliminates shrinkage deformation by calibrating the shrinkage rate of the furnace test piece and implementing pre-deformation geometric compensation on the three-dimensional model, ensuring that the size of the mirror blank after sintering is consistent with the design, and the printing accuracy is ≤±0.2 mm, thus avoiding shrinkage and warping of large-size thin-walled structures. Furthermore, the deviation between the measured size and the design value after sintering can be fed back to correct the magnification factor of the subsequent batch printing model, realizing the closed-loop control of the size chain of "calibration-compensation-feedback-re-compensation" to ensure batch production consistency.
[0016] (3) Thin-walled honeycomb structures have a large specific surface area, and thermal stress concentration during sintering and sealing can easily lead to cracking. In this invention, after two-step sintering densification, annealing is carried out near the glass transition temperature and the temperature is slowly reduced. Combined with conformal support fixtures to constrain deformation, thermal stress is eliminated from the source, preventing thin-wall cracking and ensuring the integrity and mechanical properties of the mirror blank. At the same time, the conformal support fixture matches the shape of the corresponding part of the printed blank, constraining the deformation of the thin-walled structure throughout the sintering and annealing process. Combined with the gradient structure design (the size of the honeycomb cell and the thickness of the reinforcing ribs gradually change radially), the sintering shrinkage and thermal stress are released evenly in the radial direction, further suppressing warping and cracking.
[0017] (4) The printed part and the traditional solid glass part are connected by a sealing method that matches the thermal expansion of the base material. The air bubbles at the sealing interface are controllable, and the strength of the mirror blank is not lower than that of the traditional welding method. At the same time, it can avoid the problems of long cycle and many weld defects of the traditional waterjet cutting + welding. Specifically, the sealing method is selected according to the matching degree of the thermal expansion coefficients of the panel / back panel base material and the sintered body of the printed part: when the difference in thermal expansion coefficients between the base material and the printed part is ≤1×10 -7 At a temperature of / ℃, laser sealing or low-expansion glass powder sealing is used, with a sealing temperature ≤1000 ℃. When the thermal expansion coefficients of the two materials differ significantly, low-expansion glass powder with a thermal expansion coefficient between the two should be preferred to minimize thermal stress at the sealing interface. Furthermore, when the thermal expansion coefficients of the base material and the printed part differ significantly, low-expansion glass powder with a thermal expansion coefficient between the two should be used for sealing, and a thermal expansion transition layer can be set at the sealing interface to minimize thermal stress and control air bubbles.
[0018] (5) Strong process controllability and good batch production consistency: Through the actual shrinkage rate of the calibrated specimens in the furnace, the pre-deformation geometric compensation and the feedback correction after sintering, combined with the coordinated control of the slurry rheology and photocuring parameters, the whole process of the thin-walled honeycomb structure from slurry to finished product can be controlled, and the batch production size fluctuation is ≤ ±0.2 mm. (6) Functionalization and Designable Thermal Expansion: By doping with functional components such as TiO2, CeO2, and alkali metal oxides, the thermal expansion coefficient of the mirror blank can be reduced to approximately 5.7 × 10⁻⁶. -7 / ℃ to negative expansion (approximately -0.1 to -0.3 × 10⁻⁶) -6 It features wide-range temperature control ( / ℃) and functions such as radiation resistance and refractive index control to meet the needs of different orbits and temperature ranges.
[0019] (7) Printing and molding controllability and non-destructive molding of complex topologies: The deep ultraviolet curing depth is controlled at 1.2 to 1.5 times the layer thickness, and a polymerization cross-linking zone is formed between adjacent cured layers to avoid delamination between layers; a grid support of the same material as the blank is set for the thin-walled suspended parts, and the grid is degreased and sintered together with the blank after printing, without the need for secondary demolding, so as to realize non-destructive molding of complex thin-walled topologies such as variable wall thickness and transition rounded corners. Attached Figure Description
[0020] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the accompanying drawings used in the embodiments will be briefly described below.
[0021] Figure 1 A schematic flowchart illustrating the lightweight mirror fabrication method provided by this invention; Figure 2 This is a schematic diagram of the structure of the lightweight mirror blank provided by the present invention; Figure 3A schematic diagram of the deep ultraviolet light curing three-dimensional printing process provided by the present invention; Figure 4 A schematic diagram of the temperature-time curve for the two-step sintering and annealing process provided by the present invention; Figure 5 A comparative structural diagram of the three printing schemes provided by this invention; Figure 6 This is a schematic diagram illustrating the relationship between titanium dioxide content and the coefficient of thermal expansion of glass provided by the present invention. In the diagram: 1-Panel; 2-Honeycomb sandwich; 3-Back plate; 4-Reinforcing rib; 5-Printing platform; 6-Slurry tank; 7-Scraper; 8-Deep ultraviolet light source; 9-Projection / scanning optical system; 10-Printed preform; 11-Curing interface. Detailed Implementation
[0022] This invention provides a method for preparing a lightweight mirror blank, comprising the following steps: (1) The quartz glass system powder, the photocurable resin precursor, the dispersant and the binder are mixed and then dispersed and degassed to obtain the printing paste; (2) The printing paste is 3D printed to obtain an intermediate blank or a mirror blank; the structure of the intermediate blank includes a honeycomb sandwich layer, or a honeycomb sandwich layer and a face / back plate; the structure of the mirror blank includes a honeycomb sandwich layer, a face plate and a back plate; before 3D printing, the original three-dimensional model of the structure to be formed is pre-enlarged and compensated according to the volume shrinkage rate after degreasing and sintering of the paste, so that the size of the mirror blank after sintering falls back to the design value; the pre-enlargement compensation factor = 1 / (100% - shrinkage rate); (3) When the 3D printing yields an intermediate blank print body, the intermediate blank print body is subjected to degreasing, sintering and annealing in sequence, and then sealed with the panel and / or back plate and annealed a second time to obtain a mirror blank. When the 3D printing produces a mirror blank, the mirror blank is sequentially degreased, sintered, and annealed to obtain a lightweight reflective mirror blank.
[0023] This invention mixes quartz glass system powder, photocurable resin precursor, dispersant and binder, and then disperses and degasses the mixture to obtain a printing paste.
[0024] In this invention, the printing paste comprises, by weight, 100 parts of quartz glass system powder, 40-60 parts of photocurable resin precursor, 0.5-5 parts of dispersant and 0.5-3 parts of binder.
[0025] In this invention, the quartz glass system material can be one or more of high-purity SiO2 powder, SiO2-based composite, or SiO2-based mixture; the purity of the high-purity SiO2 powder is ≥99.9%; the doping element in the SiO2-based composite can be at least one of titanium, alkali metal elements, alkaline earth metal elements, rare earth elements, transition metal elements, boron elements, and halogen elements; the alkali metal element can be at least one of lithium, sodium, and potassium; the alkaline earth metal element can be at least one of magnesium, calcium, strontium, and barium; the rare earth element can be at least one of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium, and yttrium; the transition metal element can be at least one of vanadium, chromium, manganese, iron, cobalt, nickel, copper, and zinc; the halogen element can be fluorine and / or chlorine; the SiO2-based composite is preferably a SiO2-TiO2 composite. In this invention, the doping component in the SiO2-based mixture can be an oxide or a compound of at least one of titanium, alkali metal, alkaline earth metal, rare earth, transition metal, and boron elements; the SiO2-based mixture is preferably a mixture of SiO2 and TiO2.
[0026] In this invention, the mass of TiO2 in the SiO2-TiO2 composite is 0.1-15% of the mass of SiO2.
[0027] In this invention, the SiO2-TiO2 composite can be obtained by chemical vapor deposition + flame hydrolysis or liquid phase chemical synthesis; the SiO2-TiO2 mixture can be obtained by directly mixing SiO2 and TiO2 powders.
[0028] In this invention, by incorporating titanium dioxide into silica powder and precisely controlling its addition amount, a coefficient of thermal expansion of the glass material can be achieved at approximately 5.7 × 10⁻⁶. -7 / ℃ to 0 or even negative expansion (-0.1~-0.3×10) -6 Flexible adjustment within a wide range of / ℃ (see) (see) Figure 6Furthermore, this invention can achieve different functional properties by introducing different doping elements into the SiO2 matrix, such as radiation hardening, refractive index regulation, softening temperature regulation, improved chemical stability, and coloring, to meet the diverse needs of aerospace optical components. For example, introducing 0.5~3 wt% cerium oxide (CeO2) into the silicon dioxide matrix as a radiation hardening element improves the radiation resistance and optical stability of the mirror blank under space irradiation; introducing 1~5 wt% alkali metal oxides (such as lithium oxide, sodium oxide, and potassium oxide) regulates the glass softening temperature and refractive index; introducing small amounts of boron oxide and aluminum oxide improves chemical stability; and introducing transition metal oxides (such as iron oxide, cobalt oxide, copper oxide, and zinc oxide) achieves specific spectral transmission or coloring characteristics.
[0029] In this invention, the photocurable resin precursor is a photocurable polydimethylsiloxane (PDMS) resin (such as methacryloyloxy modified PDMS, acrylate modified PDMS); the dispersant is one or more of ammonium polyacrylate, polyvinylpyrrolidone and polyethylene glycol; and the binder is one or more of trimethylolpropane triacrylate, polyethylene glycol diacrylate and hydroxyethyl acrylate.
[0030] In this invention, the dispersant dosage mentioned above ensures improved powder dispersion and inhibits agglomeration; the binder dosage mentioned above ensures green body strength and debinding stability. In this invention, the solid content of the printing paste is 40~60 vol%; when the solid content of the printing paste is higher than 60 vol%, the viscosity is too high and light penetration is insufficient; when it is lower than 40 vol%, sintering shrinkage is large; the viscosity of the printing paste can be 0.5~20 Pa·s.
[0031] After obtaining the printing paste, the present invention performs 3D printing on the printing paste to obtain an intermediate blank or a mirror blank.
[0032] In this invention, the structure of the intermediate preform print body includes a honeycomb sandwich layer, or a honeycomb sandwich layer and a face / back plate; the structure of the mirror preform print body includes a honeycomb sandwich layer, a face plate, and a back plate (see...). Figure 5 ).
[0033] Before 3D printing, based on the volume shrinkage rate after slurry degreasing and sintering, the original three-dimensional model of the structure to be formed is pre-enlarged and compensated to make the size of the mirror blank after sintering fall back to the design value; the pre-enlargement compensation factor = 1 / (100% - shrinkage rate).
[0034] In this invention, determining the pre-amplification compensation factor includes the following steps: Before 3D printing, a shrinkage rate calibration specimen is printed and degreased and sintered in the same furnace as the mirror blank. The volume shrinkage rate is obtained based on the volume of the sintered body and the volume of the calibration specimen. Then, the pre-magnification compensation factor is determined according to the pre-magnification compensation factor = 1 / (100% - shrinkage rate). After sintering, the dimensions of the mirror blank are remeasured, and the deviation between the remeasurement result and the design value is fed back to correct the magnification factor of subsequent batches of printing, so as to realize the closed-loop control of the dimension chain.
[0035] In this invention, the 3D printing can be deep ultraviolet (DEUV) curing printing; the wavelength of the DEUV is 200-300 nm, the printing layer thickness is 20-100 μm, and the optical power density is 5-50 mW / cm². 2 The scanning speed is 10~200 mm / s. In this invention, the accuracy of the 3D printing is no greater than ±0.2 mm. In this invention, during the printing process, operations such as partitioned printing and gradient structure design can be selected according to the actual situation. The partitioned printing is to print simultaneously using multiple print heads; the gradient structure design can make the size of the honeycomb cell and the wall thickness of the reinforcing ribs gradually change along the radial direction of the mirror blank to match the radial distribution of sintering shrinkage and balance thermal stress.
[0036] In this invention, the curing depth of deep ultraviolet light curing printing is controlled at 1.2 to 1.5 times the thickness of the printed layer, so that there is a partially overlapping polymerization cross-linking zone between adjacent cured layers, which ensures the interlayer bonding strength and avoids delamination before sintering. During printing, the honeycomb reinforcing ribs are formed vertically along the direction of gravity, which can improve the forming stability of the thin-walled structure. The thin-walled suspended structure is provided with a grid support of the same material as the printed blank. The grid support is degreased and sintered together with the blank, eliminating the need for secondary demolding and realizing non-destructive forming of complex thin-walled topologies.
[0037] In this invention, the wall thickness of the reinforcing ribs in the honeycomb sandwich layer can be 0.2~10mm.
[0038] When the 3D printing yields an intermediate blank, the intermediate blank is sequentially degreased, sintered, and annealed. After being sealed with the panel and / or back plate, it is annealed again to obtain a lightweight mirror blank.
[0039] In this invention, the degreasing temperature can be 200~600℃, specifically 200℃, 300℃, 400℃, 500℃ or 600℃, and the holding time can be 1~4h, specifically 1h, 2h, 3h or 4h; the sintering can be a first sintering and a second sintering performed sequentially; the temperature of the first sintering can be 1000~1200℃, specifically 1000℃, 1100℃ or 1200℃, and the holding time can be 1~3h, specifically 1h, 2h or 3h; the temperature of the second sintering can be 1250~1500℃, specifically 1250℃, 1300℃, 1400℃ or 1500℃, and the holding time can be 2~6h, specifically 2h, 3h, 4h, 5h or 6h. In this invention, the heating rate for degreasing can be 1~10℃ / min; the heating rate to the sintering temperature can also be 1~10℃ / min. In this invention, the above heating rates can prevent the thin-walled structure from cracking due to thermal stress. In this invention, the sintering is carried out under a protective atmosphere. This invention, through the sintering parameters, can avoid cracking and bubble generation in the thin-walled honeycomb structure during sintering, thereby densifying the green body.
[0040] In this invention, the annealing involves holding at a preset temperature for 1-4 hours, followed by a slow cooling to room temperature at a rate of 1-5 °C / min; the preset temperature is the glass transition temperature of the sintered body ±50 °C. In this invention, the annealing treatment can eliminate thermal stress and prevent cracking; in this invention, the annealing treatment can be partial annealing or overall annealing; partial annealing refers to annealing stress concentration areas such as sealing interfaces and thickness transition zones; overall annealing refers to annealing the entire mirror blank preform.
[0041] Specifically, the first sintering, second sintering, and annealing are preferably performed by placing the degreased printed blank on a conformal support fixture for the first sintering, second sintering, and annealing. The conformal support fixture matches the shape of the corresponding parts of the printed blank, constraining the deformation of the thin-walled structure throughout the sintering and annealing process. The conformal support fixture is preferably made of high-purity porous alumina ceramic or high-purity quartz glass of the same material as the printed blank, and its surface in contact with the printed blank is processed to match the shape of the corresponding parts of the blank. To prevent the blank from sticking to the fixture during sintering, a boron nitride release coating is applied to the contact surface of the fixture. The conformal support fixture constrains the thin-walled structure throughout the degreasing, two-step sintering, and annealing processes, causing the blank to shrink along the designed contour during the densification shrinkage process, suppressing warping and cracking.
[0042] In this invention, the sealing method is at least one of flame sealing, laser sealing, or low-expansion glass powder sealing; the sealing method is selected based on the matching degree of the thermal expansion coefficients of the panel / back panel and the sintered body of the printed part: when the difference in thermal expansion coefficients between the two is ≤1×10-7 When the temperature is / ℃, laser sealing or low-expansion glass powder sealing is used, with a sealing temperature ≤1000℃, or further, 900~1000℃; when the difference in thermal expansion coefficients between the two is greater than 1×10 -7 At / ℃, low-expansion glass powder with a thermal expansion coefficient between the two is used for sealing.
[0043] In this invention, the conditions for the secondary annealing are the same as those for the initial annealing, and will not be repeated here.
[0044] In this invention, the secondary annealing process further includes optical processing and coating of the obtained mirror blank to form a finished mirror with an optical reflective surface; the optical processing includes grinding and polishing processes, and the coating process involves depositing a metal reflective film or a dielectric reflective film on the reflective surface.
[0045] When the 3D printing produces a mirror blank, the present invention sequentially performs degreasing, sintering, and annealing on the mirror blank to obtain a lightweight reflective mirror blank.
[0046] In this invention, when the 3D printing yields a mirror-shaped preform, its difference from the intermediate preform lies only in the absence of sealing and secondary annealing. The degreasing, sintering, and annealing conditions are the same as for the intermediate preform, and will not be repeated here. In this invention, during the 3D printing process, it is preferable to provide a mesh support of the same material as the printed preform for the thin-walled suspended structure. This mesh support is removed during degreasing and sintering along with the printed preform.
[0047] Figure 1 This is a schematic flowchart of the lightweight reflector fabrication method provided by the present invention.
[0048] This invention also provides a lightweight mirror blank prepared by the above-described method. Figure 2 The system includes a honeycomb core layer and a panel and a back plate connected to both sides of the honeycomb core layer. The honeycomb core layer comprises a plurality of honeycomb cells, which are formed by reinforcing ribs surrounding each other. In this invention, the honeycomb cells are regular hexagons or triangles; the lightweight mirror blank has an elastic modulus ≥50 GPa, a flexural strength ≥25 MPa, and a solid density of reinforcing ribs ≥1.8 g / cm³. 3 The size of the air bubbles in the honeycomb sandwich layer is no greater than 1 / 3 of the wall thickness of the reinforcing rib.
[0049] To further illustrate the present invention, the technical solutions provided by the present invention will be described in detail below with reference to the accompanying drawings and embodiments, but these should not be construed as limiting the scope of protection of the present invention.
[0050] Example 1 100 parts of SiO2 powder (purity ≥99.9%, particle size 0.5~2 μm), 45 parts of methacryloxy-modified PDMS resin (product number: Gelest MCR-M17, methacryloxypropyl-terminated polydimethylsiloxane, number average molecular weight approximately 2000), 2 parts of ammonium polyacrylate, and 1 part of trimethylolpropane triacrylate were ball-milled in a planetary ball mill at 200 rpm for 6 h (the grinding balls were...). 5 mm zirconia spheres (material-to-sphere mass ratio 1:2) were used, followed by degassing under a vacuum pressure of -0.09 MPa for 20 min to obtain a slurry with a solid content of 50 vol%. This slurry was then used to prepare a printing slurry with a solid content of 50 vol%. A batch of shrinkage calibration specimens were printed using this slurry. The calibration specimens were then used for subsequent degreasing and sintering processes, and the shrinkage rate was found to be 15%. Based on this shrinkage rate, the three-dimensional model of the honeycomb sandwich layer was pre-deformed geometrically compensated. The cell size, reinforcing rib wall thickness, and overall contour were pre-enlarged by the reciprocal of (100%-15%), i.e., enlarged by 1 / (1-15%)≈1.176 times, so that the mirror blank size after sintering returned to the design value. Figure 3 As shown, the printing paste is placed in a paste tank and scraped into a 50 μm thick layer using a scraper. A deep ultraviolet light source with a wavelength of 280 nm is used to irradiate the paste surface according to the slice pattern via a projection / scanning optical system, initiating polymerization and curing at the curing interface. The curing depth is controlled at 1.3 times the layer thickness to ensure interlayer bonding. The printing platform descends layer by layer, accumulating to obtain a honeycomb sandwich layer printing blank. During printing, the reinforcing ribs are formed vertically along the direction of gravity. A mesh support of the same material as the blank (support spacing 4 mm, which is removed by degreasing and sintering along with the blank after printing) is set at the thin-walled suspension points. The printing parameters are an optical power density of 30 mW / cm². 2 The scanning speed was 100 mm / s, the layer thickness was 50 μm, and the wavelength was 280 nm; the scraper speed was 10 mm / s; the wall thickness of the honeycomb reinforcing ribs was 2.0 mm; and the honeycomb cells were arranged in regular hexagonal shapes.
[0051] The honeycomb sandwich layer printed part was degreased (temperature 400 ℃, heating rate 2 ℃ / min, time 2 h, Ar atmosphere), and then placed on a conformal support fixture for first sintering, second sintering and annealing. The first sintering temperature was 1100 ℃, heating rate 3 ℃ / min, holding time 2 h, Ar atmosphere; the second sintering temperature was 1400 ℃, heating rate 3 ℃ / min, holding time 4 h, Ar atmosphere; the annealing temperature was 1050 ℃, holding time 2 h, and then slowly cooled to room temperature at a rate of 1 ℃ / min. The annealed honeycomb sandwich layer was placed between a solid front panel and a solid back panel (both were commercially available high-purity quartz glass solid panels that had been ground and polished to a surface accuracy of PV≤λ / 4) and flame-sealed. After sealing, it was annealed a second time (temperature 1050 ℃, time 1 h, Ar atmosphere). h), forming a lightweight reflective mirror blank with a "panel-honeycomb sandwich structure-backplate", was tested and found to have an elastic modulus of 52 GPa, a flexural strength of 28 MPa, and a solid density of 1.85 g / cm³ for the reinforcing ribs. 3 The honeycomb core bubble size is ≤1 / 3 of the rib thickness, and the coefficient of thermal expansion is 5.7×10. -7 / ℃, meeting acceptance requirements. Figure 4 This is the temperature-time curve for the two-step sintering and annealing process in this embodiment.
[0052] Example 2 In this embodiment, the SiO2 powder in Example 1 is replaced with SiO2-TiO2 composite powder. The doping mass of TiO2 in the composite powder is 7.5% of the total mass of the composite powder. The composite powder is prepared by chemical vapor deposition + flame hydrolysis.
[0053] 100 parts of SiO2-TiO2 composite powder, 40 parts of methacryloxy-modified PDMS resin, 2 parts of ammonium polyacrylate, and 1 part of trimethylolpropane triacrylate were ball-milled in a planetary ball mill at 200 rpm for 6 hours (the grinding balls were...). 5 mm zirconia spheres (material-to-sphere mass ratio 1:2) were used, followed by degassing under a vacuum pressure of -0.09 MPa for 20 min to obtain a slurry with a solid content of 48 vol%. This slurry was used to print a batch of shrinkage calibration specimens. These specimens were then used for subsequent degreasing and sintering processes, and the shrinkage rate was measured to be 12%. Based on this shrinkage rate, pre-deformation geometric compensation was performed on the 3D model of the honeycomb sandwich layer-backplate, magnifying it by 1 / (1-12%)≈1.136 times, so that the size of the mirror blank after sintering returned to the design value. Figure 3As shown, the printing paste is placed in a paste tank, and a scraper spreads the paste into a thin layer of 40 μm thickness. A deep ultraviolet light source with a wavelength of 280 nm irradiates the paste surface according to the slice pattern through a projection / scanning optical system, initiating polymerization and curing at the curing interface. The curing depth is controlled at 1.3 times the layer thickness to ensure interlayer bonding. The printing platform descends layer by layer, accumulating to obtain a honeycomb sandwich layer printing blank. During printing, the reinforcing ribs are formed vertically along the direction of gravity, and a support structure is set to prevent the collapse of the thin-walled suspended structure. The printing parameters are an optical power density of 25 mW / cm². 2 The scanning speed was 80 mm / s, the layer thickness was 40 μm, and the wavelength was 280 nm; the scraping speed of the scraper was 10 mm / s; the wall thickness of the honeycomb reinforcing ribs was 1.0 mm, and the honeycomb cells were arranged in regular hexagons.
[0054] The honeycomb sandwich layer-back panel blanks were sequentially degreased (400 ℃, 2 ℃ / min, 2 h), first sintered (1100 ℃ for 2 h, 3 ℃ / min, Ar), and second sintered (1420 ℃ for 4 h, 3 ℃ / min, Ar). After holding at 1050 ℃ for 3 h, they were slowly cooled to room temperature at 2 ℃ / min. They were then laser-sealed with a commercially available high-purity quartz glass solid panel that had been ground and polished to a surface shape accuracy of PV≤λ / 4. After sealing, the sealing interface was annealed at 1050 ℃ for 1 h.
[0055] The lightweight mirror blank prepared in this embodiment has a coefficient of thermal expansion of 0.03 × 10⁻⁶. -6 / ℃, elastic modulus 62 GPa, flexural strength 38 MPa, and solid density of the reinforcing rib 1.87 g / cm³ 3 Printing accuracy ±0.15 mm, honeycomb core bubble size ≤1 / 3 rib thickness.
[0056] Example 3 In this embodiment, the SiO2 powder of Example 1 is replaced with a mixed powder of SiO2 and TiO2. The TiO2 doping amount in the composite powder is 9% of the total mass of the composite powder. The particle size of the SiO2 powder is 0.5~2 μm, and the particle size of the TiO2 powder is 20~50 nm. The sintering glass thermal expansion coefficient of this mixed powder is negative (approximately -0.1×10⁻⁶). -6 / ℃).
[0057] 100 parts of a mixed powder of SiO2 and TiO2, 45 parts of methacryloyloxy-modified PDMS, 2.5 parts of polyvinylpyrrolidone, and 1.5 parts of polyethylene glycol diacrylate were ball-milled in a planetary ball mill at 200 rpm for 6 hours (the grinding balls were...). 5 mm zirconia spheres (material-to-sphere mass ratio 1:2) were used, followed by degassing under vacuum pressure of -0.09 MPa for 20 min to obtain a printing slurry with a solid content of 50 vol%. A batch of shrinkage calibration specimens were printed using this slurry. The calibration specimens were then used for subsequent degreasing and sintering processes, and the shrinkage rate was found to be 18%. Based on this shrinkage rate, the integrated printing model was pre-deformed geometrically compensated, and the magnification was 1 / (1-18%)≈1.220 times. The printing paste was 3D printed using a gradient structure design (with the mirror blank center as the origin, the honeycomb cell size linearly changes radially from 8 mm to 12 mm, and the reinforcing rib wall thickness linearly changes from 1.2 mm to 0.8 mm; the slicing software generates slicing patterns layer by layer according to these parameters) to form an integrated panel-honeycomb sandwich layer-back panel. The printing parameters were a light power density of 30 mW / cm². 2 The scanning speed was 100 mm / s, the layer thickness was 50 μm, and the wavelength was 280 nm. The scraping speed was 10 mm / s. The wall thickness of the honeycomb reinforcing ribs was 1.2 mm at the center and 0.8 mm at the edge according to the gradient. The honeycomb cells were arranged in regular hexagons.
[0058] The integrated printed part was degreased (400 ℃, heating rate 2 ℃ / min, time 2 h), first sintered (1100 ℃, holding for 2 h, heating rate 3 ℃ / min, Ar), and second sintered (1380 ℃, holding for 4 h, heating rate 3 ℃ / min, Ar). Then, it was annealed at 1030 ℃ for 3 h and slowly cooled to room temperature at 2 ℃ / min to directly obtain a lightweight reflective mirror blank integrating the panel, honeycomb sandwich layer and back plate. The reflective surface of the panel was ground and polished to a surface roughness Ra≤1 nm and coated (aluminum reflective film and SiO2 protective layer were deposited).
[0059] The lightweight mirror blank prepared in this embodiment has a coefficient of thermal expansion of -0.1×10⁻⁶. -6 / ℃, elastic modulus 58 GPa, flexural strength 32 MPa, and solid density of the reinforcing rib 1.84 g / cm³ 3 Printing accuracy ±0.15 mm, honeycomb core bubble size ≤1 / 3 rib thickness.
[0060] Although the above embodiments have provided a detailed description of the present invention, they are only some embodiments of the present invention, and not all embodiments. People can obtain other embodiments based on these embodiments without creative effort, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a lightweight mirror blank, comprising the following steps: (1) The quartz glass system powder, the photocurable resin precursor, the dispersant and the binder are mixed and then dispersed and degassed to obtain the printing paste; (2) 3D print the printing paste to obtain an intermediate blank or a mirror blank; The structure of the intermediate preform print includes a honeycomb sandwich layer, or a honeycomb sandwich layer and a face / back plate; the structure of the mirror preform print includes a honeycomb sandwich layer, a face plate, and a back plate; before 3D printing, based on the volume shrinkage rate after slurry degreasing and sintering, the original three-dimensional model of the structure to be formed is pre-scaled and compensated to ensure that the mirror preform size returns to the design value after sintering; the pre-scaled compensation factor = 1 / (100% - shrinkage rate). (3) When the 3D printing yields an intermediate blank print body, the intermediate blank print body is degreased, sintered and annealed in sequence, then sealed with the panel and / or back plate and annealed again to obtain a lightweight mirror blank. When the 3D printing produces a mirror blank, the mirror blank is sequentially degreased, sintered, and annealed to obtain a lightweight reflective mirror blank.
2. The preparation method according to claim 1, characterized in that, The printing paste comprises, by weight, 100 parts of quartz glass system powder, 40-60 parts of photocurable resin precursor, 0.5-5 parts of dispersant and 0.5-3 parts of binder; the solid content of the printing paste is 40-60 vol.
3. The preparation method according to claim 1, characterized in that, The dispersant is one or more of ammonium polyacrylate, polyvinylpyrrolidone, and polyethylene glycol; the binder is one or more of trimethylolpropane triacrylate, polyethylene glycol diacrylate, and hydroxyethyl acrylate.
4. The preparation method according to claim 1, characterized in that, The 3D printing is deep ultraviolet (DEUV) photopolymerization printing; the wavelength of DEUV is 200-300 nm, the printing layer thickness is 20-100 μm, and the optical power density is 5-50 mW / cm². 2 The scanning speed is 10~200 mm / s.
5. The preparation method according to claim 1, characterized in that, The wall thickness of the reinforcing ribs in the honeycomb sandwich layer is 0.2~10mm.
6. The preparation method according to claim 1, characterized in that, The degreasing treatment is carried out at a temperature of 200~600℃ for 1~4h; the heating rate of the degreasing treatment is 1~10℃ / min.
7. The preparation method according to claim 1, characterized in that, The sintering is a first sintering and a second sintering performed sequentially; the temperature of the first sintering is 1000~1200 ℃, and the holding time is 1~3h; the temperature of the second sintering is 1250~1500 ℃, and the holding time is 2~6h, with a heating rate of 1~10℃ / min to reach the sintering temperature.
8. The preparation method according to claim 1, characterized in that, The annealing process involves holding the material at a preset temperature for 1-4 hours and then slowly cooling it to room temperature at a rate of 1-5 °C / min; the preset temperature is the glass transition temperature of the sintered body obtained by sintering ±50 °C.
9. The preparation method according to claim 1, characterized in that, The sealing method is at least one of flame sealing, laser sealing, or low-expansion glass powder sealing; the sealing method is selected based on the matching degree of the thermal expansion coefficients of the panel / back panel and the sintered body of the printed part: when the difference in thermal expansion coefficients between the two is ≤1×10 -7 At a temperature of / ℃, laser sealing or low-expansion glass powder sealing should be used, with a sealing temperature ≤1000℃; when the difference in thermal expansion coefficients between the two is greater than 1×10 -7 At / ℃, low-expansion glass powder with a thermal expansion coefficient between the two is used for sealing.
10. The lightweight mirror blank prepared by the preparation method according to any one of claims 1 to 9, characterized in that, It includes a honeycomb sandwich layer and a panel and a back panel connected to both sides of the honeycomb sandwich layer; the honeycomb sandwich layer contains a plurality of honeycomb cells, which are formed by reinforcing ribs surrounding each other.