A production process of a high-hardness box
By employing a three-layer co-extrusion process and zoned temperature control of the mold, the problems of insufficient hardness and poor barrier properties of blister packaging boxes have been solved, achieving a balance between high hardness and high barrier properties and improving the overall performance of the packaging boxes.
Patent Information
- Application Number
- CN202611222174.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-12
- Publication Date
- 2026-11-20
AI Technical Summary
Existing blister packaging boxes have insufficient rigidity and poor barrier properties, and it is difficult to balance rigidity and barrier properties. Furthermore, existing improvement methods result in increased material brittleness or high process complexity.
The process employs a three-layer co-extrusion technique. The outer layer enhances hardness through the synergistic effect of mineral fillers and nucleating agents. The middle layer uses EVOH or PVA to improve barrier properties. The inner layer improves toughness through toughening agents. Furthermore, the interlayer bonding force is optimized through mold temperature zone control and segmented cooling technology.
Without significantly increasing the wall thickness, the box's flexural modulus increases by 60-88%, compressive strength increases by 57-77%, oxygen permeability and water vapor permeability decrease by 89-91% and 75-80% respectively, and interlayer peel strength increases by 20-30%.
Smart Images

Figure REF-OBJ-1786515272574-000001
Abstract
Description
Technical Field
[0001] This application relates to the field of food plastic packaging technology, specifically to a manufacturing process for a high-hardness box. Background Technology
[0002] Plastic food packaging containers are widely used in catering, takeout, and pre-prepared meals, and their performance directly affects the shelf life, transportation safety, and user experience of food. Currently, blister packaging boxes are typically made of single-layer PVC, PET, or PP material through vacuum forming. The wall thickness is usually 0.3-0.6 mm, and the flexural modulus is only 1200-1800 MPa. During stacking and transportation, they are prone to collapse and deformation, leading to food damage from compression. Some manufacturers increase the wall thickness to improve rigidity, but this increases material consumption by 30-50% and prolongs the cooling time during vacuum forming, significantly reducing production efficiency.
[0003] In addition, the oxygen permeability of a single-layer PET box is approximately 3-5 cm. 3 / (m 2 (·d·atm), water vapor transmission rate is approximately 8-15 g / (m 2 •d) For foods containing oils and easily oxidized foods (such as fried foods, nuts, and baked goods), the shelf life at room temperature is only 7-15 days, which is insufficient to meet the packaging requirements for long-shelf-life foods. In existing technologies, methods to increase hardness often lead to increased material brittleness and decreased interfacial bonding strength of the barrier layer; while introducing a barrier layer requires multi-layer co-extrusion equipment, which is highly complex, and defects such as delamination and bubbles are prone to occur when the thickness control precision of the barrier layer is insufficient.
[0004] Therefore, how to make blister packaging boxes have both high hardness and high barrier properties without significantly increasing the wall thickness, and ensure the interlayer bonding force of the multi-layer structure, is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0005] To address the technical problems of insufficient rigidity, poor barrier properties, and difficulty in achieving both rigidity and barrier properties in existing blister packaging boxes, this application provides a manufacturing process for high-rigidity boxes.
[0006] The first aspect of this application provides a manufacturing process for a high-hardness box, comprising the following steps: providing a thermoplastic resin substrate with a mineral filler, a nucleating agent, and a coupling agent, mixing, melt-blending, and pelletizing to obtain a high-hardness outer layer masterbatch; drying an ethylene-vinyl alcohol copolymer or polyvinyl alcohol to a moisture content ≤0.5wt% to obtain a barrier layer raw material; mixing and melt-blending a thermoplastic resin substrate with a toughening agent to obtain an inner layer masterbatch; and separately feeding the outer layer masterbatch, the barrier layer raw material, and the inner layer masterbatch into... The material is melted in three extruders, merged by a manifold, and extruded through a T-die to obtain a three-layer composite sheet consisting of an outer layer, a middle layer, and an inner layer. The three-layer composite sheet is preheated and then vacuum-formed, with the mold temperature controlled in zones: 90-110℃ for the bottom of the box, 70-90℃ for the side walls, and 80-100℃ for the edge sealing area. Cooling and shaping are done in stages: the first stage cools to 80-100℃, and the second stage cools to room temperature. After demolding, the high-hardness box is obtained.
[0007] In the above technical solution, the outer layer, through the synergistic effect of mineral fillers and nucleating agents, enables the polymer matrix to achieve a grain-refining strengthening effect while being reinforced by filling, increasing the flexural modulus from 1500-1800 MPa of the matrix resin to 2800-3500 MPa. The middle layer uses EVOH or PVA, whose numerous hydroxyl groups in the molecular chain form a dense hydrogen bond network, providing strong barrier properties against oxygen and water vapor. The inner layer improves the overall toughness of the multilayer sheet by introducing toughening agents, avoiding the brittleness tendency caused by the high rigidity of the outer layer. During the vacuum forming stage, the mold temperature is controlled in zones to ensure that the bottom is fully crystallized at a higher mold temperature to withstand stacking pressure, the sidewalls retain molecular orientation at a lower mold temperature to improve bending stiffness, and the edges are sealed and flat at a moderate temperature. The segmented cooling process gradually releases the thermal stress generated by each layer during cooling, avoiding interlayer cracking caused by sudden cooling, and improving the interlayer peel strength by 20-30%.
[0008] Furthermore, in the preparation of the outer layer masterbatch, the weight ratio of the thermoplastic resin substrate, the mineral filler, the nucleating agent, and the coupling agent is 100:(8-15):(0.3-1.0):(0.5-1.5), the mixing temperature is 80-100℃, the mixing time is 5-10 min, the melt co-extrusion temperature is 180-220℃, and the screw speed is 200-350 r / min. Specifically, when the mineral filler content is 8-15 parts, hardness improvement can be achieved without significantly increasing brittleness; when the mineral filler content exceeds 15 parts, the elongation at break of the outer layer material decreases too quickly, and cracks are prone to occur during vacuum forming; when the mineral filler content is less than 8 parts, the hardness improvement effect is not obvious.
[0009] Furthermore, the thermoplastic resin substrate is one or more of polyethylene terephthalate (PET), polypropylene (PP), or polylactic acid (PLA). Specifically, PET, due to its high mechanical strength and good transparency, is suitable for food packaging requiring high light transmittance; PP has excellent heat resistance and chemical resistance, making it suitable for hot-fill food packaging; PLA is a biodegradable material, suitable for applications with high environmental protection requirements.
[0010] Furthermore, the mineral filler is one or more of nano-calcium carbonate, talc, or calcium sulfate whiskers, with a particle size ranging from 500 nm to 5 μm, and is surface-modified with a silane coupling agent. Specifically, nano-calcium carbonate is uniformly dispersed in the PET matrix and is inexpensive; talc has both filling and nucleation functions, exhibiting superior nucleation and reinforcement effects in the PET / PP system, enabling a flexural modulus of over 3100 MPa; calcium sulfate whiskers, due to their large aspect ratio, can enhance rigidity while maintaining a certain degree of toughness.
[0011] Further, the nucleating agent is one or more of sodium benzoate, talc, or sorbitol-based nucleating agents. Specifically, sodium benzoate is suitable for PET systems, significantly increasing the crystallization rate and refining the spherulite size from 50-100 μm to 5-15 μm; sorbitol-based nucleating agents are suitable for PP systems, improving crystallinity and crystal stability.
[0012] Furthermore, the coupling agent is one of the following: silane coupling agent KH-550, KH-560, or titanate coupling agent. Specifically, silane coupling agent KH-550 undergoes a condensation reaction with the hydroxyl groups on the surface of the mineral filler in the PET system to form stable Si-O-mineral covalent bonds, while its amino terminus forms hydrogen bonds with the PET ester groups, thereby improving interfacial adhesion; titanate coupling agent is suitable for PP systems and can form a chemical bridge between the mineral filler and PP.
[0013] Further, the ethylene-vinyl alcohol copolymer (EVOH) has an ethylene content of 29-44 mol% and a melt flow rate of 1.5-8.0 g / 10 min (190℃, 2.16 kg). Specifically, a ethylene content of 29-32 mol% provides optimal barrier properties but results in poor melt processability, requiring careful temperature control within the range of 200-230℃; a ethylene content of 38-44 mol% improves processability and makes it suitable for high-speed extrusion. The drying temperature is 80-100℃, and the drying time is 4-6 hours. Specifically, controlling the drying temperature at 80-100℃ effectively removes moisture while preventing thermal degradation of the material; a drying time of 4-6 hours reduces the moisture content to below 0.5 wt%, meeting the requirements for melt processing.
[0014] Furthermore, in the preparation of the inner layer masterbatch, the weight ratio of the thermoplastic resin substrate to the toughening agent is 100:(3-8), the mixing time is 3-5 min, and the melt co-extrusion temperature is 170-200℃. Specifically, when the toughening agent content is 3-8 parts, the elongation at break of the inner layer can be increased by 30-50% while maintaining sufficient rigidity to match the outer layer; when the toughening agent content exceeds 8 parts, the rigidity of the inner layer decreases excessively, affecting the overall bending resistance of the box. The toughening agent is one of ethylene-octene copolymer (POE), ethylene-vinyl acetate copolymer (EVA), or maleic anhydride graft compatibilizer. Specifically, POE has excellent toughening effect in the PET system and good compatibility with PET; maleic anhydride graft compatibilizer can further improve the interfacial bonding between the toughening agent and the matrix resin.
[0015] Furthermore, in the extrusion of the three-layer composite sheet, the extrusion temperature of the outer layer masterbatch is 190-230℃, the extrusion temperature of the barrier layer raw material is 200-240℃, the extrusion temperature of the inner layer masterbatch is 180-210℃, and the T-die temperature is 210-230℃. Specifically, the outer layer extrusion temperature of 190-230℃ allows the mineral filler to be fully dispersed without causing thermal degradation; the middle layer extrusion temperature of 200-240℃ avoids the thermal degradation of EVOH at temperatures exceeding 250℃; and the T-die temperature of 210-230℃ ensures that the three-layer melt maintains good fluidity after merging to form a uniform composite sheet. In the three-layer composite sheet, the outer layer thickness accounts for 35-45% of the total sheet thickness, the middle layer thickness accounts for 10-20% of the total sheet thickness, and the inner layer thickness accounts for 35-55% of the total sheet thickness. Specifically, an outer layer of 35-45% can control costs while ensuring a sufficiently thick mineral-filled reinforcement layer; a middle layer of 10-20% achieves the optimal balance between barrier performance and cost; and an inner layer of 35-55% can provide sufficient base thickness for vacuum forming.
[0016] Furthermore, a melt distributor is provided within the T-shaped die head, ensuring that the melt flow rate ratio of the outer masterbatch to the inner masterbatch is (1.0-1.2):1.0, and the melt flow rate of the barrier layer material is 0.3-0.5 times that of the outer masterbatch. Specifically, by controlling this flow rate ratio, it can be ensured that the three melt layers maintain a stable layered structure after merging, avoiding intermediate layer segregation, uneven thickness, or interface fluctuations caused by flow rate mismatch.
[0017] Furthermore, in the vacuum forming process, the vacuum degree is -0.06 to -0.09 MPa, the forming time is 2-5 seconds, and the cooling and setting time is 5-10 seconds. Specifically, the vacuum degree of -0.06 to -0.09 MPa ensures that the sheet material fits tightly against the mold surface, forming a clear box outline; the forming time of 2-5 seconds enables efficient production while ensuring forming accuracy. The mold surface has a micro-grid texture with a groove depth of 0.05-0.15 mm, a groove width of 0.1-0.3 mm, and a spacing of 0.5-1.0 mm. Specifically, the groove depth of 0.05-0.15 mm, the groove width of 0.1-0.3 mm, and the spacing of 0.5-1.0 mm of the micro-grid texture can increase the bending stiffness by 15-25% without increasing the wall thickness, and without affecting the smoothness requirements of the food contact surface.
[0018] Furthermore, the first stage of the segmented cooling process has a cooling rate of 15-25°C / min, cooling to 80-100°C; the second stage has a cooling rate of 5-10°C / min, cooling to room temperature. Specifically, the rapid cooling in the first stage allows the outer and inner layers to quickly set, while the slow cooling in the second stage gradually releases the thermal stress between the barrier layer and the inner and outer layers, resulting in a 20-30% increase in interlayer peel strength compared to single-stage rapid cooling.
[0019] This application has the following beneficial effects: This application combines a mineral-filled modified high-hardness outer layer, an EVOH / PVA high-barrier intermediate layer, and a toughened inner layer through a three-layer co-extrusion vacuum forming process. This allows each layer to function synergistically, increasing the flexural modulus of the box from 1650MPa in traditional single-layer PET boxes to 2650-3100MPa, an increase of 60-88%, and the compressive strength by 57-77%, without significantly increasing the wall thickness.
[0020] This application improves the interfacial bonding between mineral fillers and matrix resin by introducing coupling agents and controls the thermal stress of each layer through segmented cooling, so that the interlayer peel strength of the three-layer composite structure reaches 4.2-4.8 N / 15 mm, which is significantly better than the optimized system without coupling agents, and solves the technical problem of easy delamination of multilayer structures.
[0021] This application reduces the oxygen permeability of the cartridge to 0.38-0.45 cm³ by introducing an EVOH / PVA interlayer and optimizing process parameters. 3 / (m 2 (·d·atm), water vapor transmission rate decreased to 1.6-2.0 g / (m 2 ·d) Compared to traditional single-layer PET boxes, this reduces costs by 89-91% and 75-80% respectively, extending the shelf life of oily foods from approximately 60 days to over 90 days. Detailed Implementation
[0022] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions in the embodiments of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.
[0023] Example 1:
[0024] This embodiment provides a high-hardness box and its manufacturing process.
[0025] Preparation of high-hardness outer layer masterbatch: Weigh 100 kg of PET resin, 10 kg of nano-calcium carbonate, 0.5 kg of sodium benzoate nucleating agent, and 1.0 kg of silane coupling agent KH-550. Add them to a high-speed mixer at a mixing temperature of 90℃ for 8 min. Then feed the mixture into a twin-screw extruder at an extrusion temperature of 200-220℃ and a screw speed of 280 r / min. The melt is then water-cooled and pelletized to obtain the outer layer masterbatch.
[0026] Preparation of intermediate barrier layer raw materials: Weigh 10 kg of EVOH and dry it in a vacuum drying oven at 90 °C for 5 h with a vacuum degree of -0.09 MPa. The moisture content after drying is 0.3 wt%.
[0027] Inner layer masterbatch preparation: Weigh 100 kg of PET resin and 5 kg of POE toughening agent, add them to a high-speed mixer, mix at 80℃ for 4 min. Then feed them into a twin-screw extruder, extrude at 190-210℃ and screw speed of 250 r / min to obtain the inner layer masterbatch.
[0028] Three-layer co-extruded sheet: A three-layer co-extrusion extruder is used. The outer layer extrusion temperature is 200-220℃, the middle layer extrusion temperature is 210-230℃, and the inner layer extrusion temperature is 190-210℃. The T-die temperature is 220℃. The melt distributor inside the die controls the flow rate ratio of the outer layer to the inner layer to be 1.1:1.0, and the flow rate of the middle layer is 0.4 times that of the outer layer.
[0029] The extruded sheet has a total thickness of 0.6 mm, with an outer layer thickness of 0.24 mm, a middle layer thickness of 0.09 mm, and an inner layer thickness of 0.27 mm. The sheet is cooled and shaped using a three-roll calender at a roll temperature of 25-40℃ and a traction speed of 8 m / min.
[0030] Vacuum forming: The sheet material is preheated to 110℃ and vacuum forming is performed using a vacuum forming machine. The mold temperature is controlled in zones: bottom 100℃, side walls 80℃, and edge sealing area 90℃. Vacuum degree -0.08MPa, forming time 3s, cooling and setting time 8s. Cooling is performed in stages: the first stage cooling rate is 20℃ / min, cooling to 90℃; the second stage cooling rate is 8℃ / min, cooling to room temperature. The mold surface has a micro-mesh texture, with a groove depth of 0.1mm, a groove width of 0.2mm, and a spacing of 0.8mm. After demolding, a high-hardness box is obtained.
[0031] Post-processing: trimming, inspection, and packaging.
[0032] Example 2:
[0033] This embodiment provides a high-hardness box and its manufacturing process.
[0034] Preparation of high-hardness outer layer masterbatch: Weigh 100 kg of PET resin, 12 kg of talc powder, 0.8 kg of sodium benzoate nucleating agent, and 1.2 kg of titanate coupling agent, add them to a high-speed mixer, mix at 90℃ for 8 min. Then feed the mixture into a twin-screw extruder, extrude at 200-220℃ and screw speed of 280 r / min. The melt is then water-cooled and pelletized to obtain the outer layer masterbatch.
[0035] Preparation of intermediate barrier layer raw materials: Weigh 10 kg of EVOH and dry it in a vacuum drying oven at 90℃ for 5 h with a vacuum degree of -0.09 MPa. The moisture content after drying is 0.3 wt%.
[0036] Inner layer masterbatch preparation: Weigh 100 kg of PET resin and 5 kg of POE toughening agent, add them to a high-speed mixer, mix at 80℃ for 4 min. Then feed them into a twin-screw extruder, extrude at 190-210℃ and screw speed of 250 r / min to obtain the inner layer masterbatch.
[0037] Three-layer co-extruded sheet: A three-layer co-extrusion extruder is used. The outer layer extrusion temperature is 200-220℃, the middle layer extrusion temperature is 210-230℃, and the inner layer extrusion temperature is 190-210℃. The T-die temperature is 220℃. The melt distributor inside the die controls the flow rate ratio of the outer and inner layers to be 1.1:1.0, and the flow rate of the middle layer is 0.4 times that of the outer layer. The total thickness of the extruded sheet is 0.6mm, with the outer layer thickness being 0.24mm, the middle layer thickness being 0.09mm, and the inner layer thickness being 0.27mm. The sheet is cooled and shaped by a three-roll calender with a roll temperature of 25-40℃ and a traction speed of 8m / min.
[0038] Vacuum forming: The sheet material is preheated to 110℃ and vacuum forming is performed using a vacuum forming machine. The mold temperature is controlled in zones: bottom 100℃, side walls 80℃, and edge sealing area 90℃. Vacuum degree -0.08MPa, forming time 3s, cooling and setting time 8s. Cooling is performed in stages: the first stage cooling rate is 20℃ / min, cooling to 90℃; the second stage cooling rate is 8℃ / min, cooling to room temperature. The mold surface has a micro-mesh texture, with a groove depth of 0.1mm, a groove width of 0.2mm, and a spacing of 0.8mm. After demolding, a high-hardness box is obtained.
[0039] Post-processing: trimming, inspection, and packaging.
[0040] Example 3:
[0041] This embodiment provides a high-hardness box and its manufacturing process.
[0042] Preparation of high-hardness outer layer masterbatch: Weigh 100 kg of PP resin, 10 kg of nano-calcium carbonate, 0.5 kg of sodium benzoate nucleating agent, and 1.0 kg of silane coupling agent KH-550, add them to a high-speed mixer, mix at 90℃ for 8 min. Then feed the mixture into a twin-screw extruder, extrude at 190-210℃ and screw speed of 280 r / min. The melt is then water-cooled and pelletized to obtain the outer layer masterbatch.
[0043] Preparation of intermediate barrier layer raw materials: Weigh 10 kg of EVOH and dry it in a vacuum drying oven at 90℃ for 5 h with a vacuum degree of -0.09 MPa. The moisture content after drying is 0.3 wt%.
[0044] Inner layer masterbatch preparation: Weigh 100 kg of PP resin and 5 kg of POE toughening agent, add them to a high-speed mixer, mix at 80℃ for 4 min. Then feed them into a twin-screw extruder, extrude at 180-200℃ and screw speed of 250 r / min to obtain the inner layer masterbatch.
[0045] Three-layer co-extruded sheet: A three-layer co-extrusion extruder is used. The outer layer extrusion temperature is 190-210℃, the middle layer extrusion temperature is 200-220℃, and the inner layer extrusion temperature is 180-200℃. The T-die temperature is 210℃. The melt distributor inside the die controls the flow rate ratio of the outer and inner layers to be 1.1:1.0, and the flow rate of the middle layer is 0.4 times that of the outer layer. The total thickness of the extruded sheet is 0.6mm, with the outer layer thickness being 0.24mm, the middle layer thickness being 0.09mm, and the inner layer thickness being 0.27mm. The sheet is cooled and shaped by a three-roll calender with a roll temperature of 25-40℃ and a traction speed of 8m / min.
[0046] Vacuum forming: The sheet material is preheated to 120℃ and vacuum forming is performed using a vacuum forming machine. The mold temperature is controlled in zones: bottom 110℃, side walls 90℃, and edge sealing area 100℃. Vacuum degree -0.08MPa, forming time 3s, cooling and setting time 8s. Cooling is performed in stages: the first stage cooling rate is 20℃ / min, cooling to 90℃; the second stage cooling rate is 8℃ / min, cooling to room temperature. The mold surface has a micro-mesh texture, with a groove depth of 0.1mm, a groove width of 0.2mm, and a spacing of 0.8mm. After demolding, a high-hardness box is obtained.
[0047] Post-processing: trimming, inspection, and packaging.
[0048] Example 4:
[0049] This embodiment provides a high-hardness box and its manufacturing process.
[0050] Preparation of high-hardness outer layer masterbatch: Weigh 100 kg of PET resin, 15 kg of nano-calcium carbonate, 0.5 kg of sodium benzoate nucleating agent, and 1.0 kg of silane coupling agent KH-550. Add them to a high-speed mixer at a mixing temperature of 90℃ for 8 min. Then feed the mixture into a twin-screw extruder at an extrusion temperature of 200-220℃ and a screw speed of 280 r / min. The melt is then water-cooled and pelletized to obtain the outer layer masterbatch.
[0051] Preparation of intermediate barrier layer raw materials: Weigh 10 kg of EVOH and dry it in a vacuum drying oven at 90 °C for 5 h with a vacuum degree of -0.09 MPa. The moisture content after drying is 0.3 wt%.
[0052] Inner layer masterbatch preparation: Weigh 5 kg of PET resin and add it to a high-speed mixer. Mix at 80°C for 4 min. Then feed it into a twin-screw extruder at 190-210°C and 250 r / min to obtain the inner layer masterbatch.
[0053] Three-layer co-extruded sheet: A three-layer co-extrusion extruder is used. The outer layer extrusion temperature is 200-220℃, the middle layer extrusion temperature is 210-230℃, and the inner layer extrusion temperature is 190-210℃. The T-die temperature is 220℃. The melt distributor inside the die controls the flow rate ratio of the outer and inner layers to be 1.1:1.0, and the flow rate of the middle layer is 0.4 times that of the outer layer. The total thickness of the extruded sheet is 0.6mm, with the outer layer thickness being 0.24mm, the middle layer thickness being 0.09mm, and the inner layer thickness being 0.27mm. The sheet is cooled and shaped by a three-roll calender with a roll temperature of 25-40℃ and a traction speed of 8m / min.
[0054] Vacuum forming: The sheet material is preheated to 110℃ and vacuum forming is performed using a vacuum forming machine. The mold temperature is controlled in zones: bottom 100℃, side walls 80℃, and edge sealing area 90℃. Vacuum degree -0.08MPa, forming time 3s, cooling and setting time 8s. Cooling is performed in stages: the first stage cooling rate is 20℃ / min, cooling to 90℃; the second stage cooling rate is 8℃ / min, cooling to room temperature. The mold surface has a micro-mesh texture, with a groove depth of 0.1mm, a groove width of 0.2mm, and a spacing of 0.8mm. After demolding, a high-hardness box is obtained.
[0055] Post-processing: trimming, inspection, and packaging.
[0056] Example 5:
[0057] This embodiment provides a high-hardness box and its manufacturing process.
[0058] Preparation of high-hardness outer layer masterbatch: Weigh 100 kg of PET resin, 10 kg of nano-calcium carbonate, 0.5 kg of sodium benzoate nucleating agent, and 1.0 kg of silane coupling agent KH-550. Add them to a high-speed mixer at a mixing temperature of 90℃ for 8 min. Then feed the mixture into a twin-screw extruder at an extrusion temperature of 200-220℃ and a screw speed of 280 r / min. The melt is then water-cooled and pelletized to obtain the outer layer masterbatch.
[0059] Preparation of intermediate barrier layer raw materials: Weigh 10kg of PVA and dry it in a vacuum drying oven at 90℃ for 5h with a vacuum degree of -0.09MPa. The moisture content after drying is 0.4wt%.
[0060] Inner layer masterbatch preparation: Weigh 100 kg of PET resin and 5 kg of EVA toughening agent, add them to a high-speed mixer, mix at 80℃ for 4 min. Then feed them into a twin-screw extruder, extrude at 190-210℃ and screw speed of 250 r / min to obtain the inner layer masterbatch.
[0061] Three-layer co-extruded sheet: A three-layer co-extrusion extruder is used. The outer layer extrusion temperature is 200-220℃, the middle layer extrusion temperature is 200-220℃, and the inner layer extrusion temperature is 190-210℃. The T-die temperature is 215℃. The melt distributor inside the die controls the flow rate ratio of the outer and inner layers to be 1.1:1.0, and the flow rate of the middle layer is 0.4 times that of the outer layer. The total thickness of the extruded sheet is 0.6mm, with the outer layer thickness being 0.24mm, the middle layer thickness being 0.09mm, and the inner layer thickness being 0.27mm. The sheet is cooled and shaped by a three-roll calender with a roll temperature of 25-40℃ and a traction speed of 8m / min.
[0062] Vacuum forming: The sheet material is preheated to 110℃ and vacuum forming is performed using a vacuum forming machine. The mold temperature is controlled in zones: bottom 100℃, side walls 80℃, and edge sealing area 90℃. Vacuum degree -0.08MPa, forming time 3s, cooling and setting time 8s. Cooling is performed in stages: the first stage cooling rate is 20℃ / min, cooling to 90℃; the second stage cooling rate is 8℃ / min, cooling to room temperature. The mold surface has a micro-mesh texture, with a groove depth of 0.1mm, a groove width of 0.2mm, and a spacing of 0.8mm. After demolding, a high-hardness box is obtained.
[0063] Post-processing: trimming, inspection, and packaging.
[0064] Comparative Example 1: This comparative example provides a traditional single-layer PET box and its manufacturing process.
[0065] The difference from Example 1 is that only PET resin is used to extrude a sheet with a thickness of 0.6 mm using a single-screw extruder, without any mineral fillers, nucleating agents, or barrier layers. Specifically, 100 kg of PET resin is weighed and fed into a single-screw extruder at an extrusion temperature of 250-270°C and a T-die temperature of 260°C, resulting in a total sheet thickness of 0.6 mm. The sheet is cooled and shaped using a three-roll calender at a roller temperature of 25-40°C and a traction speed of 8 m / min. The sheet is preheated to 110°C and then vacuum-formed using a vacuum forming machine with a smooth die surface and a constant die temperature of 80°C. The vacuum degree is -0.08 MPa, the forming time is 3 seconds, the cooling and shaping time is 8 seconds, and the single-stage cooling rate is 15°C / min, cooling to room temperature. After demolding, a traditional single-layer PET box is obtained. Post-processing includes trimming, inspection, and packaging.
[0066] Comparative Example 2: This comparative example provides a barrier-free double-layer box and its manufacturing process.
[0067] The difference from Example 1 is that the intermediate barrier layer is eliminated, and only the outer and inner layers are co-extruded. Specifically, the preparation of the outer layer masterbatch and the inner layer masterbatch are the same as in Example 1. A double-layer co-extrusion extruder is used, with the outer layer extrusion temperature at 200-220℃ and the inner layer extrusion temperature at 190-210℃. The T-die temperature is 220℃, and the total thickness of the extruded sheet is 0.6mm, of which the outer layer thickness is 0.3mm and the inner layer thickness is 0.3mm. The sheet is cooled and shaped by a three-roll calender with a roll temperature of 25-40℃ and a traction speed of 8m / min. The thermoforming parameters are the same as in Example 1. After demolding, a double-layer box without a barrier layer is obtained. Post-processing: trimming, inspection, and packaging.
[0068] Comparative Example 3: This comparative example provides a control box with low mineral filler content and its manufacturing process.
[0069] The difference from Example 1 is that the amount of nano-calcium carbonate added to the outer layer material is reduced to 5 kg. Specifically, in the preparation of the outer layer masterbatch, 100 kg of PET resin, 5 kg of nano-calcium carbonate, 0.5 kg of sodium benzoate nucleating agent, and 1.0 kg of silane coupling agent KH-550 were weighed, the mixing temperature was 90℃, and the mixing time was 8 min. The twin-screw extrusion temperature was 200-220℃, and the screw speed was 280 r / min. The raw materials for the intermediate barrier layer, the preparation of the inner layer masterbatch, the three-layer co-extrusion sheet, the thermoforming, and the post-treatment were all the same as in Example 1. After demolding, a low-filling control box was obtained.
[0070] Comparative Example 4: This comparative example provides a control box without temperature zone control and its manufacturing process. The difference from Example 1 is that the mold temperature is kept constant at 90°C during vacuum forming, without zone control; the bottom, sidewalls, and edge sealing areas are all at 90°C. Specifically, the preparation of the outer masterbatch, the preparation of the intermediate barrier layer raw material, the preparation of the inner masterbatch, and the three-layer co-extruded sheet are all the same as in Example 1. During vacuum forming, the sheet is preheated to 110°C, the mold temperature is kept constant at 90°C, the vacuum degree is -0.08MPa, the forming time is 3s, the cooling and setting time is 8s, the segmented cooling parameters are the same as in Example 1, and the mold surface has a micro-mesh texture. After demolding, a control box without temperature zone control is obtained. Post-processing: trimming, inspection, and packaging.
[0071] Comparative Example 5: This comparative example provides a control box without micro-mesh texture mold and its manufacturing process.
[0072] The difference from Example 1 is that the surface of the vacuum forming mold is smooth and without micro-mesh texture. Specifically, the preparation of the outer masterbatch, the intermediate barrier layer raw material, the inner masterbatch, and the three-layer co-extruded sheet are all the same as in Example 1. During vacuum forming, the sheet is preheated to 110°C, the mold temperature is controlled in zones: bottom 100°C, sidewalls 80°C, and edges 90°C; vacuum degree -0.08MPa; forming time 3s; cooling and setting time 8s; and the mold surface is smooth. After demolding, a smooth-surfaced control box is obtained. Post-processing: trimming, inspection, and packaging.
[0073] The boxes prepared in Examples 1-5 and Comparative Examples 1-5 were subjected to performance tests, and the test methods are as follows: Flexural modulus: Tested according to GB / T9341-2008 "Determination of Flexural Properties of Plastics", with a sample size of 80mm×10mm×0.6mm, a span of 64mm, and a test speed of 2mm / min.
[0074] Oxygen permeability: Tested according to GB / T31354-2014 "Test method for oxygen permeability of packaging and containers - coulometric test method", with a test temperature of 23℃ and a relative humidity of 50%.
[0075] Water vapor transmission rate: Tested according to GB / T31355-2014 "Test method for water vapor transmission of packaging and containers - infrared sensor method", with a test temperature of 38℃ and a relative humidity of 90%.
[0076] Compression strength: Tested in accordance with GB / T1041-2008 "Determination of compressibility of plastics", the sample is a circular piece at the bottom of the box with a diameter of 50 mm, and the test speed is 5 mm / min.
[0077] Interlayer peel strength: Tested according to GB / T8808-1988 "Peel test method for flexible composite plastic materials", with a sample width of 15 mm and a peeling speed of 300 mm / min.
[0078] Table 1 Test results of the examples and comparative examples
[0079] The unit for oxygen permeability is cm. 3 / (m 2 (·d·atm); the unit of water vapor transmission rate is: g / (m 2 ·d).
[0080] As shown in Table 1, the flexural modulus of Examples 1-5 all reached 2650-3100 MPa, higher than that of Comparative Example 1 (1650 MPa), representing an increase of 60-88%; compared to Comparative Example 3 (2100 MPa), the increase was 26-48%, proving that the mineral filler content in the range of 8-15 parts has an enhancing effect on hardness, while the hardness decreases significantly when the content is below 8 parts. The oxygen permeability of Examples 1-5 was only 0.38-0.50 cm. 3 / (m 2 The interlayer peel strength (·d·atm) was reduced by 88-91% compared to Comparative Example 1 and by 87-90% compared to Comparative Example 2, indicating that the introduction of the EVOH / PVA interlayer can effectively improve the barrier performance of the housing. The interlayer peel strength of Examples 1-5 was 4.1-4.8 N / 15 mm, which was higher than 3.5 N / 15 mm of Comparative Example 2, proving that the optimization of coupling agent and toughening agent improved the interlayer interface bonding.
[0081] Comparative Example 1 is a traditional single-layer PET box, with all performance indicators being the worst. Comparative Example 2, after removing the intermediate barrier layer, showed a 10% reduction in oxygen permeability compared to Comparative Example 1, but it was still as high as 3.8 cm⁻¹. 3 / (m 2The flexural modulus (·d·atm) was significantly higher than that of the example, indicating that the introduction of the EVOH / PVA interlayer can effectively improve the barrier properties of the housing. In Comparative Example 3, after reducing the mineral filler to 5 parts, the flexural modulus decreased from 2850 MPa to 2100 MPa, and the compressive strength decreased from 58 MPa to 42 MPa, indicating that the hardness enhancement effect is insufficient when the filler content is below 8 parts. In Comparative Example 4, after temperature zoning without a mold, the compressive strength decreased from 58 MPa to 52 MPa, and the interlayer peel strength decreased from 4.5 N / 15 mm to 4.0 N / 15 mm, indicating that zoning temperature control makes a substantial contribution to the optimization of bottom crystallinity and thermal stress control. In Comparative Example 5, without micro-mesh texture, the properties were basically the same as in Example 1, with only a slight decrease in compressive strength, indicating that the contribution of micro-mesh texture to hardness improvement was relatively limited.
[0082] Example 2 uses talc, which has both filling and nucleation functions, achieving a flexural modulus of 3100 MPa, the highest among all examples. This indicates that the nucleation and strengthening effect of talc in the PET system is superior to that of sodium benzoate. In Example 3, changing the substrate to PP reduced the flexural modulus to 2650 MPa, indicating that the PET matrix has higher intrinsic rigidity under the same filling formulation. In Example 4, increasing the mineral filler content to 15 parts increased the flexural modulus to 3000 MPa, but the compressive strength was slightly lower than in Example 1, possibly due to increased outer layer brittleness caused by high filling. In Example 5, replacing EVOH with PVA increased the oxygen permeability to 0.50 cm⁻¹. 3 / (m 2 (·d·atm), water vapor transmission rate increased to 2.2 g / (m 2 (d) PVA's barrier properties are slightly lower than EVOH's, but still significantly better than the comparative example.
[0083] The above are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A manufacturing process for a high-hardness box, characterized in that, Includes the following steps: A high-hardness outer layer masterbatch is obtained by mixing, melt blending, and pelletizing thermoplastic resin base material with mineral fillers, nucleating agents, and coupling agents. Ethylene-vinyl alcohol copolymer or polyvinyl alcohol is dried to a moisture content of ≤0.5wt% to obtain barrier layer raw material; A thermoplastic resin substrate is mixed with a toughening agent and melt-blended to obtain an inner layer masterbatch; The outer layer masterbatch, the barrier layer raw material, and the inner layer masterbatch are respectively fed into three extruders for melting, and then combined by a manifold and extruded through a T-die to obtain a three-layer composite sheet, which includes an outer layer, a middle layer, and an inner layer. The three-layer composite sheet is preheated and then vacuum-formed, with the mold temperature controlled in zones: the bottom mold temperature is 90-110℃, the side wall mold temperature is 70-90℃, and the edge sealing area mold temperature is 80-100℃. The cooling and shaping process employs segmented cooling. The first stage involves cooling to 80-100℃, and the second stage involves cooling to room temperature. After demolding, the high-hardness box is obtained.
2. The production process according to claim 1, characterized in that, In the preparation of the outer layer masterbatch, the weight ratio of the thermoplastic resin substrate, the mineral filler, the nucleating agent and the coupling agent is 100:(8-15):(0.3-1.0):(0.5-1.5), the mixing temperature is 80-100℃, the mixing time is 5-10min, the melt co-extrusion temperature is 180-220℃, and the screw speed is 200-350r / min.
3. The production process according to claim 1, characterized in that, In the preparation of the outer masterbatch, the thermoplastic resin substrate is one or more of polyethylene terephthalate, polypropylene, or polylactic acid; the mineral filler is one or more of nano-calcium carbonate, talc, or calcium sulfate whiskers, with a particle size range of 500nm-5μm, and is surface modified by a silane coupling agent.
4. The production process according to claim 1, characterized in that, In the preparation of the outer layer masterbatch, the nucleating agent is one or more of sodium benzoate, talc, or sorbitol-based nucleating agents; the coupling agent is one of silane coupling agents KH-550, KH-560, or titanate coupling agents.
5. The production process according to claim 1, characterized in that, The ethylene-vinyl alcohol copolymer has an ethylene content of 29-44 mol% and a melt flow rate of 1.5-8.0 g / 10 min; the drying temperature is 80-100℃ and the drying time is 4-6 h.
6. The production process according to claim 1, characterized in that, In the preparation of the inner layer masterbatch, the weight ratio of the thermoplastic resin substrate to the toughening agent is 100:(3-8), the mixing time is 3-5 min, and the melt co-extrusion temperature is 170-200℃; the toughening agent is one of ethylene-octene copolymer, ethylene-vinyl acetate copolymer, or maleic anhydride graft compatibilizer.
7. The production process according to claim 1, characterized in that, In the extrusion of the three-layer composite sheet, the extrusion temperature of the outer layer masterbatch is 190-230℃, the extrusion temperature of the barrier layer raw material is 200-240℃, the extrusion temperature of the inner layer masterbatch is 180-210℃, and the T-die temperature is 210-230℃; in the three-layer composite sheet, the outer layer thickness accounts for 35-45% of the total sheet thickness, the middle layer thickness accounts for 10-20% of the total sheet thickness, and the inner layer thickness accounts for 35-55% of the total sheet thickness.
8. The production process according to claim 1, characterized in that, The T-shaped die head is equipped with a melt distributor, so that the melt flow rate of the outer masterbatch is (1.0-1.2):1.0 to the melt flow rate of the inner masterbatch, and the melt flow rate of the barrier layer raw material is 0.3-0.5 times the melt flow rate of the outer masterbatch.
9. The production process according to claim 1, characterized in that, In the vacuum forming process, the vacuum degree is -0.06 to -0.09 MPa, the forming time is 2-5 s, and the cooling and setting time is 5-10 s; the mold surface has a micro-mesh texture, the groove depth is 0.05-0.15 mm, the groove width is 0.1-0.3 mm, and the spacing is 0.5-1.0 mm.
10. The production process according to claim 1, characterized in that, The first stage of the segmented cooling process has a cooling rate of 15-25℃ / min, cooling to 80-100℃; the second stage has a cooling rate of 5-10℃ / min, cooling to room temperature.