A method and system for improving tire bead bubble defects
By establishing a systematic improvement scheme for controlling material compression rate and optimizing the insulated layer wrapping height in the tire bead area, the problem of air bubble defects in the tire bead and bead area was solved, achieving stable bonding and consistent molding in the bead area and avoiding edge defects caused by excessive material.
Patent Information
- Application Number
- CN202611628104.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-21
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies struggle to reliably and systematically address air bubble defects in the bead and ferrule areas of tires formed in a single process. This is especially true when there is insufficient or excessive material, making it difficult to simultaneously address both air bubble prevention and edge protrusion prevention, and a lack of quantifiable improvement methods.
A systematic improvement scheme was established to control the material compression rate at the bottom of the sub-hole, optimize the reverse wrapping height of the inner lining narrow layer, and constrain the position of the PA composite pressure roller. This included establishing a dual reference section, calculating the material compression rate, adjusting the material quantity and the reverse wrapping height of the inner lining, optimizing the continuous stacking relationship of materials, and controlling the position deviation of the pressure roller after the structure meets the standards.
It significantly reduces or eliminates air bubble defects in the tire bead area, improves the bonding quality and molding stability of the bead area, avoids edge protrusion problems caused by excessive material, and has good repeatability and scalability.
Smart Images

Figure CN123129507A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of tire production quality control technology, and in particular to a method and system for improving tire bead bubble defects. Background Technology
[0002] During tire molding and vulcanization, the bead, bead layer, and their adjacent areas are typically among the most structurally complex, have the most concentrated material layers, and are most prone to localized poor bonding. Especially in one-step tire molding processes, the inner liner, carcass ply, sidewall rubber, bead wire, and related reinforcing materials need to be bonded, wrapped, reversed, and compacted continuously within a short process chain. If any localized area has insufficient material configuration, discontinuous interlayer transitions, an unreasonable local compaction path, or an unstable subsequent pressing process window, residual air in that area may not be effectively expelled. This can ultimately manifest as defects such as air bubbles, voids, poor bonding, or localized abnormal appearance at the bead area after vulcanization. These defects not only affect the tire's appearance but can also weaken the interlayer bonding quality and reliability of the bead area. Therefore, they have always been a crucial technical problem that needs continuous resolution in tire manufacturing, particularly in one-step tire molding.
[0003] From the perspective of existing technological development paths, the industry has mainly developed two improvement approaches to address the issues of air bubbles or poor adhesion in the bead / nip area. The first approach focuses on localized compaction and venting at the equipment end. This involves applying additional internal and external clamping, compression, or rolling to the bead area to improve its air expulsion capacity. For example, existing technical document CN102267238A discloses a mechanical forming drum solution with inflatable expanding rubber rings on the inner and outer sides of the bead area of the tire blank. This solution utilizes the capsule structure formed after inflation to perform internal and external compression, wrapping, and compaction on the bead area, thereby improving the wrapping quality of the bead area and reducing the amount of air bubbles remaining on the inner and outer sides of the bead area as a key objective. In other words, the technical focus of this document is to use the forming drum structure and expandable rubber rings to create additional compaction and venting methods to compensate for the insufficient wrapping, compaction, and venting of the bead area during the traditional wrapping process.
[0004] The second approach focuses more on optimizing the pressure roller structure and rolling path. This involves increasing the targeted pressure rollers, changing the rolling process, or improving the rolling area to improve the adhesion between the layers of components near the bead and remove excess air between layers. For example, prior art document CN103144334A discloses a pressure roller device specifically designed for rolling the triangular rubber and its combined rolling method. This document emphasizes that by setting a dedicated pressure roller and improving the removal of excess air between the triangular rubber and the tire carcass ply during combined rolling, the adhesion quality between the layers can be improved, increasing the tightness of the fit between the tire carcass assembly and the bead, thereby enhancing tire manufacturing quality. Therefore, the main technical approach of this document is to enhance the local compaction effect in the area near the bead through the design of the pressure roller device and rolling method, thereby reducing the problem of residual air between layers caused by insufficient local rolling.
[0005] It should be said that the aforementioned existing technologies have a certain positive effect on improving problems such as air bubbles and poor adhesion in the tire bead and taper areas, and also reflect the long-standing understanding of this problem by those skilled in the art: that air bubble defects in the taper and bead areas are usually closely related to insufficient local air release, insufficient compaction, and poor interlayer adhesion. Existing technology document CN102267238A focuses on using a molding drum auxiliary structure capable of local bulging to enhance the wrapping and compaction of the taper area; existing technology document CN103144334A focuses on improving air release and adhesion of the triangular rubber on one side of the bead and related components through pressure roller device and rolling path design. The common point of both is that they mainly address the problem from the perspective of strengthening the equipment structure or the rolling process.
[0006] However, with the widespread application of one-step molding processes and the increasing complexity of product specifications, material combinations, and structural designs, simply relying on additional compaction or roller rolling optimization at the equipment end is often insufficient to reliably and systematically solve BBB (Blister Bead Base) defects that occur in actual production. This is because whether air bubbles occur at the bead area depends not only on whether subsequent rollers can expel the air, but also on whether the area has sufficient material filling during the initial design and molding stages, whether a continuous and reasonable material stacking path is formed, and whether there are sufficient compression and covering conditions in the area from the bottom to the middle of the bead. If the bead area itself has insufficient material or an unreasonable interlayer transition position in its structural design, even compensation through additional rollers, local rolling, or wrapping compaction often only provides some improvement and cannot fundamentally eliminate the conditions that easily trap air, cause air pockets, and hinder local low-pressure venting. In other words, existing technologies tend to view the problem as insufficient compression or venting, while paying insufficient attention to the design root cause of why this area is inherently prone to air pockets.
[0007] Furthermore, existing technical literature reveals that the focus remains on the equipment and processes themselves, such as the forming drum, rubber ring, pressure rollers, and rolling path, rather than on a systematic improvement approach centered on the material compression state of the bead region. Few existing technologies employ methods that first perform zonal quantitative analysis on the bottom and upper middle areas of the wire ring, and then use the analysis results to control the material configuration of the bead region, the inward wrapping position of the inner liner, and the allowable deviation of the subsequent pressure rollers. Especially in one-step forming processes, the bead region often faces both the risk of BBB defects and the risk of edge protrusion, local accumulation, or poor appearance caused by excessive material. Existing technologies have not provided a sufficient and clear solution for establishing a window control relationship that balances both air bubble prevention and edge protrusion prevention.
[0008] Furthermore, existing technologies often lack a quantifiable and applicable methodology that can be used across different tire specifications. In traditional production practices, improvements to many bead bubble defects still rely on on-site experience adjustments, such as tentatively moving the pressure roller position, locally altering the composite component position, fine-tuning the pre-form width, or simply increasing the amount of local rubber material to observe the results. While such approaches may produce temporary effects on a particular specification or batch of products, the lack of unified, calculable, and verifiable structural judgment criteria means that the improvement effect is usually not stable enough, and the same defects are prone to reappear once equipment status, material batches, operating conditions, or specification parameters change. Therefore, the field still needs an improvement method that differs from simply relying on pressure roller devices, rubber ring wrapping, or local rolling compensation. This method should start from the structural design source of the bead area, quantitatively determine whether the material configuration is sufficient and whether the inner liner wrapping is in place, and further limit the reasonable tolerance range of equipment parameters, thereby more stably improving tire bead bubble defects.
[0009] Therefore, how to establish a systematic improvement method for the bead area of one-piece molded tires, taking into account material configuration, structural coverage relationship and subsequent pressing window, in order to reduce or eliminate BBB defects, while avoiding new bead edge defects induced by excessive local material, remains a technical problem to be solved in this field. Summary of the Invention
[0010] The technical objective of this invention is to provide a method for improving tire bead bubble defects. Addressing the BBB bubble defect problem that easily occurs in the bead area of one-piece molded tires, this invention starts with the material compression state and interlayer arrangement structure at the bead area. It establishes a systematic improvement scheme centered on controlling the material compression rate at the bottom of the bead, optimizing the height of the inner liner's narrow layer reverse wrapping, and constraining the position of the PA composite roller. This reduces or eliminates residual air at the bead area, improves the bonding quality of the bead area and the stability of tire molding, while also preventing new defects such as bead edge protrusion caused by excessive local material.
[0011] Firstly, in order to achieve the above-mentioned objectives, the present invention adopts the following technical solution:
[0012] A method for improving tire bead bubble defects, the method comprising the following steps:
[0013] S1. Based on the material distribution diagram of the bead portion and the cross-sectional structure of the tire blank, establish the reference section at the bottom of the bead.
[0014] S2. Calculate the material compressibility of the reference section at the bottom of the sub-port;
[0015] S3. Using the material compression rate of the reference section at the bottom of the bead as the main structural control index, the bead material is reconstructed. When the material compression rate is less than 25%, the amount of material in the bead area is increased so that the actual material thickness of the reference section at the bottom of the bead is formed by continuously stacking at least a single layer of cord fabric, a wide inner liner layer, a narrow inner liner layer, and the outer sidewall rubber, and the material compression rate is adjusted to 25% to 30%.
[0016] S4. Based on step S3, increase the reverse wrapping height of the inner lining narrow layer so that the radial height of the reverse wrapping end of the inner lining narrow layer reaches at least the height of the center line of the wire ring.
[0017] S5. When the material compression rate of the reference section at the bottom of the nozzle is adjusted to 25% to 30%, and the radial height of the reverse wrapping end of the inner lining is not lower than the height of the center line of the steel wire ring, the pressing position of the PA composite pressure roller is set, and the absolute value of the lateral offset of the center line of the pressure roller relative to the preset reference line does not exceed 8mm.
[0018] S6. Under the condition of satisfying step S5, conduct trial production verification, and use the BBB sub-mouth bubble defect and the PB sub-mouth edge defect as the dual defect balance result for judgment; when the BBB sub-mouth bubble defect still exists, return to step S3 and step S4 to continue material reconstruction; when the PB sub-mouth edge defect appears, reduce the amount of material at the sub-mouth part, so that the material compression rate of the reference section at the bottom of the sub-mouth is restored to 25% to 30%.
[0019] As a further improvement, in step S2, the material compression ratio of the reference section at the bottom of the sub-port is calculated as follows: the difference between the actual material thickness and the theoretical material thickness is divided by the actual material thickness, and the resulting ratio is multiplied by 100 to obtain the percentage value of the material compression ratio.
[0020] The theoretical material thickness is the thickness value determined based on the theoretical occupancy thickness of the middle part to the bottom of the steel wire ring in the material distribution diagram; the actual material thickness is the sum of the thicknesses of each material layer that actually participates in compaction at the bottom position of the steel wire ring, and each material layer includes at least a single layer of cord fabric, a wide inner liner layer, a narrow inner liner layer, and a sidewall outer protective rubber.
[0021] As a further improvement, the increase in the amount of material at the bead portion in step S3 includes one or more of the following methods: increasing the width of the inner liner wide layer, increasing the width of the inner liner narrow layer, increasing the amount of sidewall outer protective rubber at the bead portion, and adjusting the covering position of the ply layer at the bead portion.
[0022] When the width of the inner lining wide layer and the width of the inner lining narrow layer are increased simultaneously, the width increment of the inner lining wide layer and the width increment of the inner lining narrow layer are independently 5mm to 15mm.
[0023] As a further improvement, in step S4, the radial height of the inverted end of the inner lining narrow layer is the radial height of the inverted end of the inner lining narrow layer relative to the bottom reference surface of the wire ring, and the centerline height of the wire ring is the radial height of the geometric center of the wire ring relative to the bottom reference surface of the wire ring.
[0024] When the radial height of the inverted end of the narrow inner lining is not lower than the height of the center line of the wire ring, it is determined that the inverted end of the narrow inner lining has reached or crossed the center line of the wire ring.
[0025] As a further improvement, when steps S3 and S4 have not yet been completed and it is necessary to temporarily reduce the risk of BBB sub-hole bubble defects, the predetermined width may be reduced by 1% to 5% or by no more than 5mm from the original setting value as a temporary emergency measure.
[0026] After adjusting the material compression rate of the reference section at the bottom of the liner to 25% to 30%, and ensuring that the radial height of the inner liner narrow layer reverse wrapping end is not lower than the height of the steel wire ring centerline, the pre-formed width is restored or recalibrated.
[0027] As a further improvement, the preset reference line in step S5 is the theoretical pressing center line of the PA composite, and the positive and negative values of the lateral offset of the center line of the pressure roller relative to the preset reference line correspond to the offset directions of the pressure roller towards both sides of the tire axis.
[0028] As a further improvement, in step S6, when the material compression rate of the reference section at the bottom of the bead is greater than 30%, it is determined that the material amount at the bead is too large, and the material amount at the bead is reduced by one or more of the following methods: reducing the width of the inner liner wide layer, reducing the width of the inner liner narrow layer, and reducing the amount of outer protective rubber on the tire sidewall, so as to suppress the PB bead edge defect.
[0029] As a further improvement, the standardized control scheme formed in step S6 includes at least the following parameters: material compression ratio of the reference section at the bottom of the sub-hole, radial height of the inner lining narrow layer reverse wrapping end, height of the steel wire ring centerline, offset of the pressure roller position, and corresponding target intervals for suppressing BBB sub-hole bubble defects and PB sub-hole edge defects.
[0030] In a second aspect, the present invention also provides a system for implementing the method, the system comprising:
[0031] The section creation and parameter analysis unit is used to create the reference section at the bottom of the tire bead based on the material distribution diagram, cross-sectional design diagram, and steel wire ring geometry parameters corresponding to the tire specifications. The theoretical material thickness is calculated; the actual thickness confirmation unit is used to calculate or measure the actual material thickness of each reference section based on the material configuration scheme, material thickness, wrapping relationship and cross-sectional stacking relationship of the bead area.
[0032] The material reconfiguration unit is used to perform actions such as adjusting the width of the inner liner wide layer and the inner liner narrow layer, adjusting the amount of outer protective rubber on the tire sidewall, and adjusting the position of the ply layer to establish a continuous stacked structure at the bottom of the bead.
[0033] The reverse wrapping height setting unit is used to control the radial height of the reverse wrapping end of the inner lining narrow layer, so that it at least reaches the center line of the wire ring;
[0034] The pressure roller position control unit is used to perform post-calibration of the pressing position of the PA composite pressure roller after the structure meets the standards, so that the pressure roller offset meets the tolerance window requirements.
[0035] The trial production verification and standardization unit is used to record the occurrence of BBB, PB, compression ratio range, reverse wrap height relationship and pressure roller offset range, and generate standardized operation plans applicable to the corresponding tire specifications.
[0036] Thirdly, the present invention also provides a computer-readable storage medium having a computer program or instructions stored thereon, which, when executed by a processor, implement the method.
[0037] Fourthly, the present invention also provides a computer program product, including a computer program or instructions that, when executed by a processor, implement the method.
[0038] Compared to existing improvement methods that mainly rely on partial wrapping and compaction by the forming drum, additional pressure roller rolling, or local venting enhancement, this invention shifts the focus of tire bead bubble defect control to the structural design stage of the bead bead area. By quantitatively evaluating the material compression state of the reference sections at the bottom and top of the bead, and optimizing the inner liner narrow layer back-wrapping height, the continuous stacking relationship of materials in the bead area, and the allowable deviation range of the PA composite component pressure roller, this invention reduces the probability of air pockets, trapped air, and poor local low-pressure venting in the bead area from the source. This allows for more stable defect control without solely relying on equipment experience adjustments. Furthermore, by controlling the material compression rate at the bottom of the bead within a reasonable window that balances preventing BBB and avoiding PB bead edge protrusion, this invention ensures that the bead area has sufficient... The material filling and interlayer compaction conditions are optimized without inducing new appearance and structural defects due to excessive local material. Therefore, it can significantly improve the bonding quality, molding consistency and process robustness of the bead area. According to the test results, in the 205 / 55R16RP18 / GR906 tire specification, after optimizing the bead material configuration and inner liner reverse wrapping structure, no BBB defects were found in 500 tires produced continuously. In another specification, the 215 / 60R16 tire, the BBB defect rate was reduced from 3.2% to 0.3%. Furthermore, the test also showed that when the material compression rate is between 25% and 30% and the pressure roller position deviation is controlled within ±8mm, the BBB occurrence rate can approach zero. This indicates that the present invention not only has a significant improvement effect, but also has good repeatability, scalability and industrial application value. Attached Figure Description
[0039] Figure 1 This is a photograph of a bubble defect.
[0040] Figure 2 This is a flowchart of the method of the present invention.
[0041] Figure 3 This is a schematic diagram illustrating the definition of the double reference cross-section in the tire bead area of this invention.
[0042] Figure 4 This is a schematic diagram of the position deviation control of the PA composite pressure roller in this invention.
[0043] Figure 5 This is a schematic diagram illustrating the relationship between material compressibility and defect occurrence in this invention.
[0044] Figure 6 This is a schematic diagram illustrating the relationship between the positional deviation of the pressure roller and the BBB in this invention. Detailed Implementation
[0045] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the protection scope of the present invention.
[0046] This invention addresses the BBB (Blister Bead Base) bubble defect that commonly occurs in the bead region of one-piece molded tires, proposing an improvement method that combines pre-design structural control with post-process parameter constraints. Unlike traditional improvement methods, this invention does not consider adjusting the PA composite component pressure roller position as the sole or primary solution. Instead, it first addresses the material configuration and interlayer stacking relationship in the bead region. By establishing dual reference sections, compression ratios are calculated for the bottom and centerline positions of the bead ring. Based on this, by simultaneously increasing the material quantity at the bead bottom and the inward wrapping height of the inner liner narrow layer, structural conditions conducive to venting are established. Only after these structural conditions are met is the PA composite component pressure roller position controlled within a specified deviation range. When material quantity is insufficient, adjusting the PA composite component pressure roller position alone can only partially improve the problem. With sufficient material quantity, an 8mm offset to the left or right of the pressure roller position does not cause bead bubbles, but once the offset reaches 10mm in mass production, the defect reappears. This fact supports the technical approach of this invention, which prioritizes structure and uses the pressure roller as a secondary measure.
[0047] I. Terminology Explanation
[0048] To facilitate understanding of this invention, the main terms appearing in the embodiments are explained uniformly below; this section contains no more than 10 terms.
[0049] BBB stands for Blister Bead Base, which refers to air bubbles between the rubber layers at the bottom of the bead or between the rubber layer at the bottom of the bead and the cord fabric. This defect often occurs in tires manufactured using the one-step vulcanization process. Figure 1 As shown.
[0050] PB: refers to edge defects at the sub-mouth, which are abnormal appearances or structures caused by excessive material or local accumulation in the sub-mouth area.
[0051] Reference section at the bottom of the sub-mouth : This refers to the cross-section passing through the center of the bottom of the wire coil, used to evaluate the material compression state in the bottom region of the wire coil.
[0052] upper reference section of the sub-mouth The cross-section passing through the center line of the wire coil is used to evaluate the material compression state and exhaust channel formation in the vicinity and above the center line of the wire coil.
[0053] Theoretical material thickness : Refers to the process based on the material distribution diagram and the geometric relationship of the wire coil, in the first... The theoretical occupancy thickness calculated at each reference section, among which for or .
[0054] Actual material thickness : refers to the first The sum of the actual thicknesses of the material layers involved in compaction at each reference section.
[0055] Material compressibility : refers to the The degree of compression allowance of the actual material thickness at a reference section relative to the theoretical material thickness is an important criterion for this invention.
[0056] Inner liner narrow layer reverse wrapping end height : Refers to the radial height of the end of the narrow inner lining layer relative to the bottom reference surface of the wire ring.
[0057] Centerline height of steel wire ring : Refers to the radial height of the geometric center of the wire coil relative to the reference surface at the bottom of the wire coil.
[0058] pressure roller position offset : Refers to the lateral offset of the center line of the PA composite roller relative to the preset reference line.
[0059] II. System Structure for Implementing the Method of the Invention
[0060] While the subject matter of this invention is an improved method, for the convenience of those skilled in the art, this invention can also be understood as an improved system for performing the method. The system is not necessarily limited to a single device, but can be composed of a design analysis end, a prototyping execution end, and a verification and standardization end working together.
[0061] Specifically, the system may include:
[0062] Firstly, the section establishment and parameter analysis unit is used to establish the reference section at the bottom of the tire bead based on the material distribution diagram, cross-sectional design diagram, and steel wire ring geometric parameters corresponding to the tire specifications. upper reference section of the mortise And calculate the theoretical material thickness;
[0063] Secondly, the actual thickness confirmation unit is used to calculate or measure the actual material thickness of each reference section based on the material configuration scheme, material thickness, wrapping relationship and cross-sectional stacking relationship of the bead area.
[0064] Third, the material reconstruction unit is used to perform actions such as adjusting the width of the inner liner wide layer and the inner liner narrow layer, adjusting the amount of outer protective rubber on the tire sidewall, and adjusting the position of the ply layer covering, so as to establish a continuous stacked structure at the bottom of the bead.
[0065] Fourth, the reverse wrapping height setting unit is used to control the radial height of the reverse wrapping end of the inner lining narrow layer, so that it at least reaches the center line of the steel wire ring;
[0066] Fifth, the pressure roller position control unit is used to perform post-calibration of the pressing position of the PA composite pressure roller after the structure meets the standards, so that the pressure roller offset meets the tolerance window requirements.
[0067] Sixth, a trial production verification and standardization unit is used to record the occurrence of BBB, PB, compression ratio range, reverse wrapping height relationship and pressure roller offset range, and to generate a standardized operation plan applicable to the corresponding tire specifications.
[0068] Those skilled in the art will understand that the above-mentioned units can be implemented jointly by process engineers, design software, molding machines, measuring tools, and standardized documents, and it is not required to set up independent physical hardware modules. As long as the functional relationships described in this invention can be achieved, it should be considered as falling within the implementation of this invention.
[0069] III. Specific Technical Route for Implementing the Method of the Invention
[0070] 1. Step S1: Establish a double reference section
[0071] Step S1 is a preliminary identification step of this invention. Its purpose is not simply to find a general defect location, but to refine the original general experience-based judgment of the sub-mouth area into two functionally different analysis locations, namely the reference section at the bottom of the sub-mouth. Reference section at the upper end of the sub-mouth Among them, the reference section at the bottom of the sub-mouth. This mainly reflects whether the amount of material at the bottom of the wire ring is sufficient, whether air pockets easily form at the bottom, and whether there is sufficient compaction allowance between the mold heel and the blank; the reference section at the upper end of the die bead. This mainly reflects whether the wrapping state of the steel wire coil centerline and the area above it is continuous, whether the inner lining narrow layer is in place, and whether there are any breaks or insufficient compression areas when air is discharged upwards. Cross-sectional analysis shows that breaks and residual gas spaces exist in areas prone to this problem. Possible causes include insufficient material at the die head, resulting in a lower compression ratio; the die heel area, being similar in shape to the die blank, experiences low pressure, creating conditions for air pockets, and the air bubbles cannot be discharged smoothly due to lack of pressure. Therefore, simply observing the final surface phenomena is insufficient to accurately guide rectification; the bottom filling conditions and the upper venting conditions must be evaluated separately.
[0072] like Figure 3As shown, when establishing a dual-reference section in practice, technicians can follow the principles outlined below:
[0073] For the reference section at the bottom of the sub-port Preferably, the section plane is selected where the lowest point of the bottom of the wire ring passes through the geometric center of the wire ring; this section plane is usually located at the lowest radial position in the high bubble area, and can most sensitively reflect whether the material is full.
[0074] For the reference section at the upper end of the sub-port Preferably, a cross-section is selected that passes through the geometric center line of the wire coil; this cross-section reflects whether the reverse wrapping material can cross the middle of the wire coil and form a continuous transition from bottom to top.
[0075] The reason for establishing two sections simultaneously is that simply ensuring the material quantity at the bottom of the sub-hole meets the standard cannot automatically guarantee that the venting conditions above the centerline of the wire ring meet the standard.
[0076] 2. Step S2: Calculate the compressibility of the two-section material
[0077] Step S2 is the quantitative evaluation step of this invention and is also the basis for subsequent material reconstruction and equipment control. The material compressibility is uniformly calculated according to the following formula:
[0078] ;
[0079] in, For the first Material compressibility of a reference section; for or ; For the first The actual material thickness of each reference section; For the first Theoretical material thickness of each reference section; Indicates the reference section at the bottom of the sub-port; This indicates the reference section at the upper end of the sub-port.
[0080] In this invention, the theoretical material thickness does not refer to an arbitrarily measured thickness value, but rather to the thickness of the space theoretically required at the corresponding position, calculated based on the material distribution diagram and the geometric relationship of the wire coil. The actual material thickness refers to the sum of the thicknesses of all material layers that actually participate in the stacking and compaction at the corresponding position. The significance of this definition is that it is not an absolute thickness measurement, but rather a comparison of whether the actual stacking thickness exceeds the geometrically required space. If the actual stacking thickness is too small, it indicates that there is insufficient margin to drive air out during compaction; if the actual stacking thickness is too large, it is prone to causing localized buildup at the nozzle and PB (partial pressure buildup).
[0081] In a preferred embodiment, the theoretical material thickness at the bottom of the tube can be calculated based on the geometric relationship between the middle portion and the bottom of the wire coil, for example:
[0082] ;
[0083] in, The theoretical material thickness is the reference cross-section at the bottom of the nozzle. The reference thickness from the middle part of the wire coil to the bottom; This is the transition angle of the sidewall; This is the corresponding horizontal reference length.
[0084] For a tire with specifications 205 / 55R16RP18 / GR906, the theoretical thickness of the bead base can be expressed as:
[0085] ;
[0086] Where 3.2mm is the reference thickness from the middle part of the wire coil to the bottom. This is the transition angle, and 14mm is the reference length. At this point, the actual material thickness at the bottom of the wire bead consists of a single layer of cord fabric, a wide inner liner layer, a narrow inner liner layer, and the outer sidewall rubber, as follows:
[0087] ;
[0088] Furthermore, the material compressibility of the reference section at the bottom of the sub-mouth is:
[0089] ;
[0090] In the above parameters, 1.1 mm is the thickness of the ply layer, 0.7 mm is the thickness of the wide inner liner layer, 0.8 mm is the thickness of the narrow inner liner layer, and 3.5 mm is the thickness of the outer sidewall rubber. This result indicates that, under the optimized state of Scheme 2, the compression ratio of the bead bottom material has entered the preferred control window of 25%–30% in this invention (e.g., Figure 5 (As shown).
[0091] Similarly, at the upper reference section of the sub-mouth... If the theoretical thickness consists of two layers of plywood, one inner liner, and the outer sidewall protector, then:
[0092] ;
[0093] Before optimization, since only the wide inner lining layer reaches the middle of the wire coil, while the narrow layer does not, the actual thickness can be expressed as:
[0094] ;
[0095] The compression ratio at the top of the sub-port before optimization is:
[0096] ;
[0097] After increasing the width of the inner liner, the narrow layer also wraps around the center of the wire coil, so the actual thickness becomes:
[0098] ;
[0099] The corresponding optimized sub-port compression ratio is:
[0100] ;
[0101] The compression ratio is relatively improved:
[0102] ;
[0103] This result indicates that simply increasing the amount of material at the bottom of the nozzle is insufficient; the narrow inner liner layer must be extended beyond the centerline of the wire ring to simultaneously improve the venting conditions in the area above the wire ring centerline. Therefore, this invention requires the simultaneous creation and evaluation of two cross-sections, rather than simply thickening the material at one location.
[0104] 3. Step S3: Material reconstruction is performed using the compression ratio at the bottom of the inlet as the main control index.
[0105] Step S3 is one of the steps that makes the greatest contribution to the inventiveness of this invention, and it is also the fundamental step of the entire method. Its core lies not in adding more material, but in reconstructing the continuous stacking relationship of the materials at the bottom of the ferrule, so that the bottom of the wire ring is transformed from a structure that is prone to air pockets, low pressure, and discontinuous into a structure with ample compaction and a continuous air venting foundation.
[0106] When material quantity is insufficient, even adjusting the position of the PA composite pressure roller or changing the composite position of the PA composite cannot fundamentally solve the problem of BBB (Body Bubbles). Specifically, in Scheme 3, while keeping the inner liner width unchanged, the sidewall was moved outward by 5mm and the PA width was changed from 630mm to 640mm, but bead bubbles still appeared after trial production, indicating that moving the composite position cannot eliminate the impact of insufficient material. Scheme 4, by reducing the pre-formed width to increase the compression ratio at the bead, showed significant improvement, but four bead bubbles still appeared after one day of trial production, indicating that this method can only be used as a temporary emergency measure, not a fundamental solution. Conversely, Scheme 2, by increasing the inner liner width from 395 / 410mm to 405 / 420mm, increased the bead compression ratio, making the material at the bottom of the wire bead more full, and no bead bubbles occurred after vulcanization of 68 tire blanks. Therefore, the truly decisive factor is the fullness of the material structure itself and the continuous stacking relationship.
[0107] Therefore, in this invention, when calculated according to step S2... In this case, instead of directly adjusting the pressure rollers, material reconstruction must be performed first. Preferably, the material reconstruction includes one or more of the following actions:
[0108] First, simultaneously increase the width of the inner lining wide layer and the width of the inner lining narrow layer;
[0109] Second, increase the amount of sidewall protective rubber in the bead area;
[0110] Third, adjust the position of the ply layer in the bead area so that it is continuously stacked with the inner liner and the sidewall outer protective rubber from the inside out or from the bottom up.
[0111] Fourth, if necessary, fine-tune the local plane width or transition boundary position to avoid forming interlayer discontinuities at the bottom of the wire ring.
[0112] In a preferred embodiment, the inner liner wide layer and the inner liner narrow layer are each increased by 10mm, adjusted from 395 / 410mm to 405 / 420mm. The significance of this action is not merely the increase in total width, but rather that it creates a continuous thickness chain at the bottom cross-section of the tire coil under compaction, consisting of a single layer of cord fabric, the inner liner wide layer, the inner liner narrow layer, and the sidewall outer protective layer. Once this continuous thickness chain is established, localized material collapse or significant low-pressure cavities no longer occur in the bottom area of the tire coil, thus providing a foundation for subsequent air expulsion. If only one layer is added while the other is inadequate, the total thickness may increase, but the critical stacking path may not be formed, thus diminishing the improvement effect.
[0113] When the material compression ratio is too low, BBB (Browning-Browning) is easily formed; while when the material compression ratio is too high, PB (Potentially Paralyzed-Browning) is easily formed. Therefore, this invention does not pursue the thickest possible thickness on one side, but rather determines a reasonable structural control range under the dual constraints of preventing BBB and PB. In other words, the goal of material reconstruction is not to add an arbitrary amount of material, but to ensure that the continuously stacked structure at the bottom of the wire coil has just enough venting margin, while avoiding excessive local material accumulation.
[0114] During implementation, technicians can operate as follows:
[0115] First, calculated based on S2 Determine whether the width of the inner lining wide and narrow layers needs to be adjusted;
[0116] Secondly, check the actual stacking relationship at the bottom of the wire bead to confirm whether it includes at least a single layer of cord fabric, a wide inner liner, a narrow inner liner, and the outer sidewall rubber. If a certain layer is not involved in the actual stacking of the reference section, it is necessary to adjust the width or the wrapping boundary to make it participate.
[0117] Secondly, by combining the partial cross-sectional diagram, determine whether there are still obvious slopes, breaks, or insufficiently compacted material voids at the bottom of the wire ring;
[0118] Finally, after completing a round of structural adjustments, the calculations were recalculated. Until it enters the 25% to 30% range.
[0119] The reason this invention treats this step as the key control step is that if this step is skipped and the pressure roller is directly modified, the defect can only be partially reduced, not completely eliminated. This is also the key difference between this invention and traditional pre-adjustment equipment.
[0120] 4. Step S4: Improve the compression ratio at the upper end of the ferrule by focusing on the height of the narrow inner lining layer.
[0121] Step S4 is also a step that makes a high contribution to the inventiveness of this invention. It solves a problem that is often overlooked in traditional experience rectification: even if the amount of material at the bottom of the ferrule has been increased, if the anti-wrapping material in the center line of the wire ring and the area above it is still interrupted or insufficient, the air will still be blocked when it moves upward and is discharged, so that the bottom improvement effect cannot be fully released.
[0122] This invention introduces a narrow inner lining layer with a reverse wrapping end height. Height of the center line of the wire ring By comparing the relationships between them, the compliance conditions for the upper structure of the sub-port are established. Preferably, the following requirements are met:
[0123] ;
[0124] in, The radial height of the narrow inner lining layer reverse wrapping end relative to the bottom reference plane of the wire ring; This is the radial height of the geometric center of the wire coil relative to the bottom reference surface of the wire coil.
[0125] The essential meaning of the above conditions is that the reverse-wrapped end of the narrow inner liner must at least reach the center line of the bead ring, preferably beyond it. This ensures that in the area at and above the center line of the bead ring, there is no longer only the wide layer in place while the narrow layer is missing, but rather a more complete overlapping structure is formed. Before optimization, the sidewall was already wrapped above the center of the bead ring, and only the wide layer of the inner liner reached the center of the bead ring. Therefore, the actual thickness at the upper end of the bead ring was 11.5mm, with a compression ratio of 37.39%. After increasing the width of the inner liner, the narrow layer also wraps above the center of the bead ring, increasing the actual thickness to 12.2mm and the compression ratio to 40.98%, a relative increase of 3.59%. This ensures sufficient material at the bead ring, making it easier to expel air.
[0126] Therefore, in this invention, step S4 is not simply an adjunct to step S3, but a crucial bridge determining whether bottom fullness can be transformed into smooth airflow at the top. Only when the bottom compression ratio meets the standard and the narrow layer reverse wrapping end crosses the center line of the wire coil can the two conditions of no air trapped at the bottom and no breakage at the top be simultaneously satisfied. If only step S3 is completed without executing step S4, a semi-improved state will occur where there is material at the bottom but the top is still weak; this state may seem effective in short-term trial production, but the defects may reappear when scaling up production or when there are minor fluctuations in the equipment.
[0127] In practice, it can be implemented as follows:
[0128] First, confirm the height of the centerline of the wire ring according to the cross-sectional design drawing. ;
[0129] Secondly, based on the change in the width of the narrow inner lining layer before and after optimization, and combined with the cross-sectional projection relationship, the height of the reverse end is calculated or confirmed. ;
[0130] Again, when At this time, by continuing to increase the width of the inner lining narrow layer, adjusting the reverse wrapping path, or changing the start and end points of local wrapping, so that... At least reach ;
[0131] Finally, the material compression ratio at the upper end of the nozzle was recalculated. It was confirmed that it was improved compared to the previous version, and together with the compression ratio at the bottom of the sub-port, it served as the basis for structural compliance.
[0132] 5. Step S5: After the structure meets the standards, control the position deviation of the PA composite pressure roller.
[0133] Step S5 is a post-processing step of this invention. Unlike traditional methods, this invention explicitly requires that the control of the pressure roller position deviation must be based on the premise that steps S3 and S4 have been completed, and cannot be treated as an earlier primary variable.
[0134] Preferably, the present invention adopts the following structural compliance determination formula:
[0135] ;
[0136] in, For structural compliance indicators; when When this occurs, it indicates that the material compression rate at the bottom of the nozzle has entered a reasonable window, and the narrow inner lining layer has reached or crossed the center line of the wire ring; when At that time, it indicates that the structural conditions are not yet stable.
[0137] Only when Only then is it permissible to set a tolerance window for the position of the PA composite pressure roller. For example... Figure 4, Figure 6 As shown, the positional deviation of the pressure roller satisfies the following formula:
[0138] ;
[0139] in, The lateral offset of the PA composite pressure roller centerline relative to the preset reference line; when A positive value indicates a shift to one side. A negative value indicates a shift to the other side.
[0140] Experiments show that after determining the width of the inner liner, Scheme 5, which shifts the pressing position of the pressure roller by 8mm to the right, produced 11 tires without any bead bubbles; Scheme 6, which shifts the pressing position of the pressure roller by 8mm to the left, produced 7 tires without any bead bubbles. However, during mass production, bead bubbles reappeared once the pressure roller position deviated by 10mm. Therefore, this invention uses ±8mm as the process tolerance window after the structure meets the standards. This is based on experimental evidence and demonstrates the correct positioning of the pressure roller in this invention: it is not a solution to the fundamental contradiction, but a process stabilizer after the structural conditions have been optimized.
[0141] More importantly, when the amount of bead material is insufficient, adjusting the position of the PA pressure roller and the composite position of the PA composite component have little effect on solving the bead bubble problem. Only by addressing the BBB (Body Bubble) issue from the perspective of bead compression ratio design can the pressure roller position be adjusted within a certain range without causing defects. Therefore, this invention, by placing pressure roller position control after the structure meets the standards, truly establishes a process logic of eliminating the root cause before controlling disturbances.
[0142] 6. Step S6: Verification and Standardization of Dual Defect Balance
[0143] Step S6 is used to solidify the aforementioned structural and process relationships into a standardized, repeatable scheme. In this step, it is necessary to observe not only whether the BBB disappears, but also whether the PB appears. This is because the present invention does not aim for simply higher compression ratios to be safer, but rather seeks to achieve a stable balance between BBB and PB.
[0144] In a preferred embodiment, step S6 can be designed with the following execution logic:
[0145] If BBB still exists after trial production, return to steps S3 and S4 to continue adjusting the material structure instead of directly relaxing the pressure roller deviation.
[0146] If PB (Pattern Breakdown) occurs after trial production, it indicates excessive material. The width of the inner liner (wide or narrow layer) should be adjusted accordingly, or the amount of outer sidewall rubber in certain areas should be reduced. It fell back to the range of 25% to 30%;
[0147] When there is neither BBB nor PB, record this state. , , , and This led to the development of standard operating procedures for tires of corresponding specifications.
[0148] When material is insufficient, reducing the pre-form width can provide some improvement and can be used as an emergency measure. Therefore, in some implementations, if production urgently needs to suppress defects in the short term and the entire structural reconstruction has not yet been completed, the pre-form width can be temporarily reduced by 1% to 5% or not exceeding 5mm to increase the instantaneous compression of the nozzle area during molding; however, this adjustment is only an emergency measure and not a fundamental improvement measure. After the structural conditions are perfected, the pre-form width should be restored or recalibrated so that the standardized scheme is still based on the structural conditions established in steps S3 and S4.
[0149] The foregoing description of embodiments of the present invention, through which those skilled in the art are able to implement or use the present invention, will be readily apparent to those skilled in the art. Various modifications to these embodiments will be readily apparent to those skilled in the art. The general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the present invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novelty disclosed herein.
[0150] Those skilled in the art will understand that embodiments of this application can be provided as methods, systems, or computer program products. Therefore, this application can take the form of a completely hardware embodiment, a completely software embodiment, or an embodiment combining software and hardware aspects. Furthermore, this application can take the form of a computer program product embodied on one or more computer-usable storage media (including but not limited to disk storage, CD-ROM, optical storage, etc.) containing computer-usable program code.
[0151] This application is described with reference to flowchart illustrations and / or block diagrams of methods, apparatus (systems), and computer program products according to embodiments of this application. It will be understood that each block of the flowchart illustrations and / or block diagrams, and combinations of blocks in the flowchart illustrations and / or block diagrams, can be implemented by computer program instructions. These computer program instructions can be provided to a processor of a general-purpose computer, special-purpose computer, embedded processor, or other programmable data processing apparatus to produce a machine, such that the instructions, which execute via the processor of the computer or other programmable data processing apparatus, generate instructions for implementing the flowchart... Figure 1 One or more processes and / or boxes Figure 1A device that provides the functions specified in one or more boxes.
[0152] These computer program instructions may also be stored in a computer-readable storage medium that can direct a computer or other programmable data processing device to function in a particular manner, such that the instructions stored in the computer-readable storage medium produce an article of manufacture including instruction means, which are implemented in a process Figure 1 One or more processes and / or boxes Figure 1 The function specified in one or more boxes.
[0153] These computer program instructions may also be loaded onto a computer or other programmable data processing equipment to cause a series of operational steps to be performed on the computer or other programmable equipment to produce a computer-implemented process, thereby providing instructions that execute on the computer or other programmable equipment for implementing the process. Figure 1 One or more processes and / or boxes Figure 1 The steps of the function specified in one or more boxes.
[0154] In a typical configuration, a computing device includes one or more processors (CPU), input / output interfaces, network interfaces, and memory.
[0155] Memory may include non-persistent memory in computer-readable media, such as random access memory (RAM) and / or non-volatile memory, such as read-only memory (ROM) or flash RAM. Memory is an example of computer-readable media.
[0156] Computer-readable media includes both permanent and non-permanent, removable and non-removable media that can store information using any method or technology. Information can be computer-readable instructions, data structures, modules of programs, or other data. Examples of computer storage media include, but are not limited to, phase-change memory (PRAM), static random access memory (SRAM), dynamic random access memory (DRAM), other types of random access memory (RAM), read-only memory (ROM), electrically erasable programmable read-only memory (EEPROM), flash memory or other memory technologies, CD-ROM, digital versatile optical disc (DVD) or other optical storage, magnetic tape, magnetic disk storage or other magnetic storage devices, or any other non-transferable medium that can be used to store information accessible by a computing device. As defined herein, computer-readable media does not include transient computer-readable media, such as modulated data signals and carrier waves.
Claims
1. A method for improving tire bead bubble defects, characterized in that, The method includes the following steps: S1. Based on the material distribution diagram of the bead portion and the cross-sectional structure of the tire blank, establish the reference section at the bottom of the bead. S2. Calculate the material compressibility of the reference section at the bottom of the sub-port; S3. Using the material compression rate of the reference section at the bottom of the bead as the main structural control index, the bead material is reconstructed. When the material compression rate is less than 25%, the amount of material in the bead area is increased so that the actual material thickness of the reference section at the bottom of the bead is formed by continuously stacking at least a single layer of cord fabric, a wide inner liner layer, a narrow inner liner layer, and the outer sidewall rubber, and the material compression rate is adjusted to 25% to 30%. S4. Based on step S3, increase the reverse wrapping height of the inner lining narrow layer so that the radial height of the reverse wrapping end of the inner lining narrow layer reaches at least the height of the center line of the wire ring. S5. When the material compression rate of the reference section at the bottom of the nozzle is adjusted to 25% to 30%, and the radial height of the reverse wrapping end of the inner lining is not lower than the height of the center line of the steel wire ring, the pressing position of the PA composite pressure roller is set, and the absolute value of the lateral offset of the center line of the pressure roller relative to the preset reference line does not exceed 8mm. S6. Under the condition of satisfying step S5, conduct trial production verification, and use the BBB sub-hole bubble defect and PB sub-hole edge defect as the double defect balance result for judgment; when the BBB sub-hole bubble defect still exists, return to step S3 and step S4 to continue material reconstruction. When a defect occurs at the PB sub-mouth, reduce the amount of material at the sub-mouth, so that the material compression rate of the reference section at the bottom of the sub-mouth is reduced to 25% to 30%.
2. The improvement method according to claim 1, characterized in that, In step S2, the material compression ratio of the reference section at the bottom of the sub-port is calculated as follows: the difference between the actual material thickness and the theoretical material thickness is divided by the actual material thickness, and the resulting ratio is multiplied by 100 to obtain the percentage value of the material compression ratio. The theoretical material thickness is the thickness value determined based on the theoretical occupancy thickness of the middle part to the bottom of the steel wire ring in the material distribution diagram; the actual material thickness is the sum of the thicknesses of each material layer that actually participates in compaction at the bottom position of the steel wire ring, and each material layer includes at least a single layer of cord fabric, a wide inner liner layer, a narrow inner liner layer, and a sidewall outer protective rubber.
3. The improved method according to claim 1, characterized in that, The increase in material amount at the bead area mentioned in step S3 includes one or more of the following methods: increasing the width of the inner liner wide layer, increasing the width of the inner liner narrow layer, increasing the amount of sidewall outer protective rubber at the bead area, and adjusting the covering position of the ply layer at the bead area. When the width of the inner lining wide layer and the width of the inner lining narrow layer are increased simultaneously, the width increment of the inner lining wide layer and the width increment of the inner lining narrow layer are independently 5mm to 15mm.
4. The improvement method according to claim 1, characterized in that, In step S4, the radial height of the inverted end of the inner lining narrow layer is the radial height of the inverted end of the inner lining narrow layer relative to the bottom reference surface of the wire ring, and the centerline height of the wire ring is the radial height of the geometric center of the wire ring relative to the bottom reference surface of the wire ring. When the radial height of the inverted end of the narrow inner lining is not lower than the height of the center line of the wire ring, it is determined that the inverted end of the narrow inner lining has reached or crossed the center line of the wire ring.
5. The improved method according to claim 1, characterized in that, When steps S3 and S4 have not yet been completed and it is necessary to temporarily reduce the risk of bubble defects in the BBB nozzle, the pre-defined width may be reduced by 1% to 5% or by no more than 5mm from the original setting value as a temporary emergency measure. After adjusting the material compression rate of the reference section at the bottom of the liner to 25% to 30%, and ensuring that the radial height of the inner liner narrow layer reverse wrapping end is not lower than the height of the steel wire ring centerline, the pre-formed width is restored or recalibrated.
6. The improvement method according to claim 1, characterized in that, The preset reference line in step S5 is the theoretical pressing center line of the PA composite. The positive and negative values of the lateral offset of the center line of the pressure roller relative to the preset reference line correspond to the offset directions of the pressure roller towards both sides of the tire axis.
7. The improved method according to claim 1, characterized in that, In step S6, when the material compression rate of the reference section at the bottom of the bead is greater than 30%, it is determined that the material amount at the bead is too large. The material amount at the bead is reduced by one or more of the following methods: reducing the width of the inner liner wide layer, reducing the width of the inner liner narrow layer, and reducing the amount of outer protective rubber on the sidewall, so as to suppress the PB bead edge defect. And / or, the standardized control scheme formed in step S6 includes at least the following parameters: material compression ratio of the reference section at the bottom of the sub-hole, radial height of the inner liner narrow layer reverse wrapping end, height of the wire ring centerline, offset of the pressure roller position, and corresponding target intervals for suppressing BBB sub-hole bubble defects and PB sub-hole edge defects.
8. A system for implementing the method according to any one of claims 1 to 7, characterized in that, The system includes: The section establishment and parameter analysis unit is used to establish the reference section at the bottom of the tire bead based on the material distribution diagram, cross-sectional design diagram and steel wire ring geometric parameters corresponding to the tire specifications, and to calculate the theoretical material thickness. The actual thickness confirmation unit is used to calculate or measure the actual material thickness of each reference section based on the material configuration scheme, material thickness, wrapping relationship and cross-sectional stacking relationship of the bead area. The material reconfiguration unit is used to perform actions such as adjusting the width of the inner liner wide layer and the inner liner narrow layer, adjusting the amount of outer protective rubber on the tire sidewall, and adjusting the position of the ply layer to establish a continuous stacked structure at the bottom of the bead. The reverse wrapping height setting unit is used to control the radial height of the reverse wrapping end of the inner lining narrow layer, so that it reaches at least the height of the steel wire ring centerline; The pressure roller position control unit is used to perform post-calibration of the pressing position of the PA composite pressure roller after the structure meets the standards, so that the pressure roller offset meets the tolerance window requirements. The trial production verification and standardization unit is used to record the occurrence of BBB bead bubble defects, PB bead edge defects, compression ratio range, reverse wrapping height relationship and pressure roller offset range, and generate standardized operation plans applicable to the corresponding tire specifications.
9. A computer-readable storage medium having a computer program or instructions stored thereon, characterized in that, When the computer program or instructions are executed by a processor, they implement the method described in any one of claims 1 to 7.
10. A computer program product, comprising a computer program or instructions, characterized in that, When the computer program or instructions are executed by a processor, they implement the method described in any one of claims 1 to 7.
Citation Information
Patent Citations
Mechanical forming drum and method for achieving assisted reverse wrapping of embryo bud
CN102267238A
Press rolling device for tyre building, and combined rolling method thereof
CN103144334A